A method for preparing paraformaldehyde by spray drying

By adding polymerization agents multiple times during the concentration stage of paraformaldehyde and using spray drying, the problem of excessive polymerization caused by self-polymerization of paraformaldehyde is solved, and the preparation of low-polymerization products is achieved, and the water solubility of the products is improved and stability.

CN118344542BActive Publication Date: 2024-11-01ANHUI RUIBAI NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410549820.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-06
Publication Date
2024-11-01
Estimated Expiration
2044-05-06

AI Technical Summary

Technical Problem

In the process of preparing paraformaldehyde using a spray drying device, paraformaldehyde is prone to excessive polymerization due to self-polymerization reaction, thereby reducing water solubility.

Method used

By adding a polymerization agent multiple times during the concentration stage, the self-polymerization of paraformaldehyde was inhibited, and the formaldehyde solution was spray granulated and fluidized bed dried by spray drying, and the reaction conditions were controlled to obtain paraformaldehyde with low polymerization.

Benefits of technology

It effectively inhibits the self-polymerization of paraformaldehyde, reduces its polymerization degree, improves the water solubility and stability of the product, and avoids the self-polymerization reaction caused by overheating.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a method for preparing paraformaldehyde by spray drying, and belongs to the technical field of paraformaldehyde preparation. The method comprises the following steps: refluxing a formaldehyde solution with a mass concentration of 45-60%; cooling the refluxed formaldehyde solution, adding a telogen, and performing a first-stage evaporation concentration; mixing the formaldehyde solution and the telogen after the first-stage evaporation concentration, and performing a second-stage evaporation concentration; mixing the concentrated formaldehyde solution and the catalyst, spray granulating, and sending to a fluidized bed for drying to obtain the paraformaldehyde; and adding the telogen multiple times in the concentration stage to inhibit the self-polymerization of the paraformaldehyde, and obtain the paraformaldehyde with a low degree of polymerization.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of paraformaldehyde preparation, and particularly relates to a method for preparing paraformaldehyde by a spray drying method. Background Art

[0002] The initial production method of paraformaldehyde in my country was the rake dryer process, but there were problems such as poor operating environment, serious dust pollution, insufficient water solubility of the product, and low single-set output. With the rapid development of the national economy, especially the sharp increase in demand for paraformaldehyde in the pesticide, resin, coating and other industries, my country has introduced several sets of spray granulation drying devices to meet market demand and improve product quality.

[0003] These devices produce finished paraformaldehyde through the process of concentrating the formaldehyde aqueous solution, spray granulation and fluidized bed drying. After the introduction of the spray granulation drying device, the production process of paraformaldehyde in my country has been significantly improved. The core of this process is to concentrate the formaldehyde aqueous solution and quickly dry the formaldehyde aqueous solution in hot air through spray granulation to form granular paraformaldehyde. This process not only improves the water solubility of paraformaldehyde, but also makes the particle size of the product more uniform, thereby improving the stability and fluidity of the product.

[0004] However, in the process of preparing paraformaldehyde using a spray drying device, there is also a risk of local overheating. When paraformaldehyde is heated to a certain temperature, it may initiate a self-polymerization reaction, resulting in a high degree of polymerization of the paraformaldehyde. As the degree of polymerization increases, the length of the molecular chain increases, and the interaction force between molecules increases, resulting in a decrease in the solubility of the paraformaldehyde in water. Summary of the invention

[0005] The invention discloses a method for preparing paraformaldehyde by spray drying, and belongs to the technical field of paraformaldehyde preparation. The method comprises the following steps: refluxing a formaldehyde solution with a mass concentration of 45-60%; cooling the refluxed formaldehyde solution, adding a telogen, and performing a first-stage evaporation concentration; mixing the formaldehyde solution and the telogen after the first-stage evaporation concentration, and performing a second-stage evaporation concentration; mixing the concentrated formaldehyde solution and the catalyst, spraying granulation, and sending to a fluidized bed for drying to obtain the paraformaldehyde; and adding the telogen multiple times in the concentration stage to inhibit the self-polymerization of the paraformaldehyde, and obtain the paraformaldehyde with a low degree of polymerization.

[0006] The technical problem to be solved by the present invention is: how to inhibit the self-polymerization of paraformaldehyde and obtain paraformaldehyde with a low degree of polymerization.

[0007] The purpose of the present invention can be achieved by the following technical solutions:

[0008] A method for preparing paraformaldehyde by spray drying comprises the following steps:

[0009] S1. Pass a formaldehyde solution with a mass concentration of 45-60% into a depolymerization kettle at 50-60°C, control the temperature of the formaldehyde in the depolymerization kettle at 100°C, and reflux for 3-4 hours under boiling state;

[0010] S2, cooling the refluxed formaldehyde solution, when the temperature of the formaldehyde solution reaches 55-65°C, adding a telogen accounting for 0.5-1.5% of the mass content of formaldehyde in the formaldehyde solution, stirring for 10-15 minutes, feeding into a primary falling film evaporator, and performing a stage of evaporation and concentration;

[0011] S3, mixing the formaldehyde solution after one-stage evaporation concentration and a telogen accounting for 0.5-0.8% of the mass content of formaldehyde in the formaldehyde solution after the one-stage evaporation concentration, stirring for 10-15 minutes, feeding into a secondary falling film evaporator, and performing two-stage evaporation concentration;

[0012] S4, mixing the formaldehyde solution after the second stage evaporation concentration and the catalyst accounting for 1.2-1.5% of the mass content of formaldehyde in the formaldehyde solution after the second stage evaporation concentration for 10-15 minutes, and then passing it into a spray granulation tower for spray granulation to obtain a polyformaldehyde solid phase, wherein the temperature in the spray granulation tower is 40-45° C. and the pressure is 270-300 Pa;

[0013] S5, sending the paraformaldehyde solid phase to a fluidized bed for drying to obtain the paraformaldehyde.

[0014] As a preferred technical solution of the present invention, the preparation of the telogen comprises the following steps:

[0015] S231, gallic acid, polyvinyl alcohol, 4-dimethylaminopyridine and toluene were mixed, stirred for 2-3 hours, dicyclohexylcarbodiimide was added, stirred for 2-3 hours, centrifuged, the supernatant was added to a 95% ethanol solution by volume, n-octyl hydrazide was added, stirred for 2-3 hours, a 2-4 mol / L hydrochloric acid solution was added, and the mixture was purified by gradient precipitation with ethyl acetate and petroleum ether, washed, and dried to obtain material A;

[0016] S232, take the material A, methanol and deionized water and put them in a reactor, stir for 1-2 hours, add a formaldehyde solution with a mass fraction of 49.8-52.3% and a sulfuric acid solution with a concentration of 2-4 mol / L, react at 50-55°C for 6-8 hours, then treat with an ion exchange resin, and take the liquid phase to obtain the polymerization agent.

[0017] As a preferred technical solution of the present invention, in step S231, the dosage ratio of gallic acid, polyvinyl alcohol, 4-dimethylaminopyridine, toluene, dicyclohexylcarbodiimide, ethanol solution, n-octyl hydrazide, and hydrochloric acid solution is 4-6 mmol: 3-4 mmol: 0.5-0.6 mmol: 30-40 mL: 5-6 mmol: 20-30 mL: 14-16 mmol: 4-6 mmol.

[0018] As a preferred technical solution of the present invention, in step S232, the dosage ratio of material A, methanol, deionized water, formaldehyde solution and sulfuric acid solution is 4-6 mg: 30-40 mL: 30-40 mL: 15-20 mL: 6-8 mL.

[0019] As a preferred technical solution of the present invention, the preparation of the catalyst comprises the following steps:

[0020] S41, in a nitrogen atmosphere, 1-vinylimidazole, 1,4-dibromobutane and anhydrous ethanol were mixed, stirred in a water bath at 55-60° C. for 12-16 h, filtered, the solid phase was washed and dried to obtain material B;

[0021] S42, take the material B and deionized water, mix them, stir for 1-2 hours, add lithium bis(trifluoromethanesulfonyl imide), stir in a water bath at 65° C. for 20-24 hours, filter, wash the solid phase, and vacuum dry to obtain the catalyst.

[0022] As a preferred technical solution of the present invention, in step S41, the dosage ratio of 1-vinylimidazole, 1,4-dibromobutane and anhydrous ethanol is 0.15-0.25 mol: 0.1-0.12 mol: 10-15 mL.

[0023] As a preferred technical solution of the present invention, in step S42, the dosage ratio of the material B, deionized water, and lithium bis(trifluoromethanesulfonyl)imide is 0.1-0.15 mol:150 mL:0.2-0.22 mol.

[0024] As a preferred technical solution of the present invention, in step S5, the drying temperature is 55-60°C.

[0025] As a preferred technical solution of the present invention, in step S2, the one-stage evaporation concentration refers to concentration to 50-65% of the mass of the formaldehyde solution in step S1.

[0026] As a preferred technical solution of the present invention, in step S3, the two-stage evaporation concentration refers to concentration to 75-85% of the mass of the formaldehyde solution in step S2.

[0027] Beneficial effects of the present invention:

[0028] The method for preparing paraformaldehyde by spray drying disclosed by the present invention introduces a large number of hydroxyl groups into the molecular structure of the polymerization agent to form a complex with the iron ions dropped from the pipeline during the formaldehyde transportation process, so that the iron ions lose their activity and their catalytic effect on the paraformaldehyde is reduced, thereby inhibiting the irreversible self-polymerization reaction of the paraformaldehyde; by introducing a polycyclic structure into the molecular structure of the polymerization agent, the steric hindrance of the self-polymerization of the paraformaldehyde is increased, the chain growth of the paraformaldehyde is hindered, the self-polymerization reaction of the paraformaldehyde is inhibited, and the polymerization degree of the paraformaldehyde is reduced; at the same time, the alkyl side chain of the imidazole ring of the ionic liquid catalyst is shortened, the distance between the anion and the cation is reduced, and the molecular volume of the ionic liquid will gradually decrease. The ionic liquid with a short alkyl side chain is helpful to regulate the product selectivity in the reaction process, and promotes the formaldehyde polymerization process to develop in the direction of paraformaldehyde with a low polymerization degree. DETAILED DESCRIPTION

[0029] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with the embodiments.

[0030] Example 1

[0031] A method for preparing paraformaldehyde by spray drying comprises the following steps:

[0032] S1. Pass a formaldehyde solution with a mass concentration of 45% into a depolymerization kettle at 50°C, control the temperature of the formaldehyde in the depolymerization kettle at 100°C, and reflux under boiling conditions for 3 hours;

[0033] S2, cooling the refluxed formaldehyde solution, when the temperature of the formaldehyde solution reaches 55°C, adding a telogen accounting for 0.5% of the mass content of formaldehyde in the formaldehyde solution, stirring for 10 minutes, feeding the material into a primary falling film evaporator, and performing a stage of evaporation and concentration to 50% of the mass of the formaldehyde solution in step S1;

[0034] S3, mixing the formaldehyde solution after one stage evaporation concentration and a telogen accounting for 0.5% of the mass content of formaldehyde in the formaldehyde solution after the one stage evaporation concentration, stirring for 10 minutes, feeding into a secondary falling film evaporator, and performing two-stage evaporation concentration to concentrate to 75% of the mass of the formaldehyde solution in step S2;

[0035] S4, mixing the formaldehyde solution after the second stage evaporation concentration and the catalyst accounting for 1.2% of the formaldehyde mass content in the formaldehyde solution after the second stage evaporation concentration for 10 minutes, and then passing it into a spray granulation tower for spray granulation to obtain a polyformaldehyde solid phase, the temperature in the spray granulation tower is 40° C., and the pressure is 270 Pa;

[0036] S5. Sending the paraformaldehyde solid phase to a fluidized bed for drying at a drying temperature of 55° C. to obtain paraformaldehyde with a degree of polymerization of 9.

[0037] The preparation of the telogen comprises the following steps:

[0038] Gallic acid, polyvinyl alcohol, 4-dimethylaminopyridine and toluene are mixed, stirred for 2 hours, dicyclohexylcarbodiimide is added, stirred for 2 hours, and the supernatant is centrifuged and added to an ethanol solution with a volume fraction of 95%, n-octyl hydrazide is added, stirred for 2 hours, and a hydrochloric acid solution with a concentration of 2 mol / L is added, and the mixture is purified by gradient precipitation of ethyl acetate and petroleum ether, washed, and dried to obtain material A; the dosage ratio of gallic acid, polyvinyl alcohol, 4-dimethylaminopyridine, toluene, dicyclohexylcarbodiimide, ethanol solution, n-octyl hydrazide and hydrochloric acid solution is 4mmo l: 3mmo l: 0.5mmo l: 30mL: 5mmo l: 20mL: 14mmo l: 4mmo l; the ethyl acetate and petroleum ether gradient precipitation refers to that the volume ratios of petroleum ether and ethyl acetate in the gradient precipitation process are 4:1, 1:3, and 0:1 respectively;

[0039] The material A, methanol and deionized water are placed in a reactor, stirred for 1 hour, a formaldehyde solution with a mass fraction of 49.8% and a sulfuric acid solution with a concentration of 2 mol / L are added, reacted at 50°C for 6 hours, and then treated with an ion exchange resin to obtain the liquid phase to obtain the polymerization agent; the dosage ratio of the material A, methanol, deionized water, formaldehyde solution and sulfuric acid solution is 4 mg: 30 mL: 30 mL: 15 mL: 6 mL.

[0040] The preparation of the catalyst comprises the following steps:

[0041] 1-vinylimidazole, 1,4-dibromobutane and anhydrous ethanol were mixed in a nitrogen atmosphere, stirred in a water bath at 55°C for 12 hours, filtered, the solid phase was washed and dried to obtain material B; the dosage ratio of 1-vinylimidazole, 1,4-dibromobutane and anhydrous ethanol was 0.15 mol: 0.1 mol: 10 mL;

[0042] The material B and deionized water are mixed, stirred for 1 hour, lithium bis(trifluoromethanesulfonyl imide) is added, stirred in a water bath at 65° C. for 20 hours, filtered, the solid phase is washed, and vacuum dried to obtain the catalyst; the dosage ratio of the material B, deionized water, and lithium bis(trifluoromethanesulfonyl imide is 0.1 mol:150 mL:0.2 mol.

[0043] Example 2

[0044] A method for preparing paraformaldehyde by spray drying comprises the following steps:

[0045] S1. Pass a formaldehyde solution with a mass concentration of 55% into a depolymerization kettle at 55°C, control the temperature of the formaldehyde in the depolymerization kettle at 100°C, and reflux under boiling conditions for 3.5 hours;

[0046] S2, cooling the refluxed formaldehyde solution, when the temperature of the formaldehyde solution reaches 60°C, adding a 1% telogen to the mass content of formaldehyde in the formaldehyde solution, stirring for 12 minutes, feeding the material into a primary falling film evaporator, and performing a stage of evaporation and concentration to 60% of the mass of the formaldehyde solution in step S1;

[0047] S3, mixing the formaldehyde solution after one stage evaporation concentration and a telogen accounting for 0.65% of the mass content of formaldehyde in the formaldehyde solution after the one stage evaporation concentration, stirring for 12 minutes, feeding into a secondary falling film evaporator, and performing two-stage evaporation concentration to concentrate to 80% of the mass of the formaldehyde solution in step S2;

[0048] S4, the formaldehyde solution after the second stage evaporation concentration and the catalyst accounting for 1.35% of the formaldehyde mass content in the formaldehyde solution after the second stage evaporation concentration are mixed for 12 minutes, and then passed into a spray granulation tower for spray granulation to obtain a polyformaldehyde solid phase, the temperature in the spray granulation tower is 42° C., and the pressure is 285 Pa;

[0049] S5. Sending the paraformaldehyde solid phase to a fluidized bed for drying at a drying temperature of 58° C. to obtain paraformaldehyde with a degree of polymerization of 11.

[0050] The preparation of the telogen comprises the following steps:

[0051] Gallic acid, polyvinyl alcohol, 4-dimethylaminopyridine and toluene are mixed, stirred for 2.5 hours, dicyclohexylcarbodiimide is added, stirred for 2.5 hours, the supernatant is centrifuged and poured into an ethanol solution with a volume fraction of 95%, n-octyl hydrazide is added, stirred for 2.5 hours, a hydrochloric acid solution with a concentration of 3 mol / L is added, and the mixture is purified by gradient precipitation of ethyl acetate and petroleum ether, washed and dried to obtain material A; the dosage ratio of gallic acid, polyvinyl alcohol, 4-dimethylaminopyridine, toluene, dicyclohexylcarbodiimide, ethanol solution, n-octyl hydrazide and hydrochloric acid solution is 5 mmol: 3.5 mmol: 0.55 mmol: 35 mL: 5.5 mmol: 25 mL: 15 mmol: 5 mmol; the gradient precipitation of ethyl acetate and petroleum ether refers to that the volume ratios of petroleum ether and ethyl acetate in the gradient precipitation process are 4: 1, 1: 3 and 0: 1 respectively;

[0052] The material A, methanol and deionized water are placed in a reactor, stirred for 1.5 hours, a formaldehyde solution with a mass fraction of 50.7% and a sulfuric acid solution with a concentration of 3 mol / L are added, and the mixture is reacted at 53° C. for 7 hours, and then treated with an ion exchange resin to obtain the liquid phase to obtain the polymerization agent; the dosage ratio of the material A, methanol, deionized water, formaldehyde solution and sulfuric acid solution is 5 mg: 35 mL: 35 mL: 18 mL: 7 mL.

[0053] The preparation of the catalyst comprises the following steps:

[0054] 1-vinylimidazole, 1,4-dibromobutane and anhydrous ethanol were mixed in a nitrogen atmosphere, stirred in a water bath at 58°C for 14 hours, filtered, the solid phase was washed and dried to obtain material B; the dosage ratio of 1-vinylimidazole, 1,4-dibromobutane and anhydrous ethanol was 0.2 mol: 0.11 mol: 13 mL;

[0055] The material B and deionized water are mixed, stirred for 1.5 hours, lithium bis(trifluoromethanesulfonyl imide) is added, stirred in a water bath at 65°C for 22 hours, filtered, the solid phase is washed, and vacuum dried to obtain the catalyst; the dosage ratio of the material B, deionized water, and lithium bis(trifluoromethanesulfonyl imide is 0.13 mol:150 mL:0.21 mol.

[0056] Example 3

[0057] A method for preparing paraformaldehyde by spray drying comprises the following steps:

[0058] S1. Pass a formaldehyde solution with a mass concentration of 60% into a depolymerization kettle at 60°C, control the temperature of the formaldehyde in the depolymerization kettle at 100°C, and reflux under boiling conditions for 4 hours;

[0059] S2, cooling the refluxed formaldehyde solution, when the temperature of the formaldehyde solution reaches 65°C, adding a telogen accounting for 1.5% of the mass content of formaldehyde in the formaldehyde solution, stirring for 15 minutes, feeding the material into a primary falling film evaporator, and performing a stage of evaporation and concentration to 65% of the mass of the formaldehyde solution in step S1;

[0060] S3, mixing the formaldehyde solution after one stage evaporation concentration and a telogen accounting for 0.8% of the mass content of formaldehyde in the formaldehyde solution after the one stage evaporation concentration, stirring for 15 minutes, feeding into a secondary falling film evaporator, and performing two-stage evaporation concentration to concentrate to 85% of the mass of the formaldehyde solution in step S2;

[0061] S4, the formaldehyde solution after the second stage evaporation concentration and the catalyst accounting for 1.5% of the formaldehyde mass content in the formaldehyde solution after the second stage evaporation concentration are mixed for 15 minutes, and then introduced into a spray granulation tower for spray granulation to obtain a polyformaldehyde solid phase, the temperature in the spray granulation tower is 45° C., and the pressure is 300 Pa;

[0062] S5. Sending the paraformaldehyde solid phase to a fluidized bed for drying at a drying temperature of 60° C. to obtain paraformaldehyde with a degree of polymerization of 14.

[0063] The preparation of the telogen comprises the following steps:

[0064] Gallic acid, polyvinyl alcohol, 4-dimethylaminopyridine and toluene are mixed, stirred for 3 hours, dicyclohexylcarbodiimide is added, stirred for 3 hours, and the supernatant is centrifuged and poured into an ethanol solution with a volume fraction of 95%, and n-octyl hydrazide is added, stirred for 3 hours, and a hydrochloric acid solution with a concentration of 4 mol / L is added, and the mixture is purified by gradient precipitation of ethyl acetate and petroleum ether, washed, and dried to obtain material A; the dosage ratio of gallic acid, polyvinyl alcohol, 4-dimethylaminopyridine, toluene, dicyclohexylcarbodiimide, ethanol solution, n-octyl hydrazide and hydrochloric acid solution is 6mmol:4mmol:0.6mmol:40mL:6mmol:30mL:16mmol:6mmol; the gradient precipitation of ethyl acetate and petroleum ether refers to that the volume ratios of petroleum ether and ethyl acetate in the gradient precipitation process are 4:1, 1:3, and 0:1 respectively;

[0065] The material A, methanol and deionized water are placed in a reactor, stirred for 2 hours, a formaldehyde solution with a mass fraction of 52.3% and a sulfuric acid solution with a concentration of 4 mol / L are added, and the mixture is reacted at 55° C. for 8 hours, and then treated with an ion exchange resin to obtain the liquid phase to obtain the polymerization agent; the dosage ratio of the material A, methanol, deionized water, formaldehyde solution and sulfuric acid solution is 6 mg: 40 mL: 40 mL: 20 mL: 8 mL.

[0066] The preparation of the catalyst comprises the following steps:

[0067] 1-vinylimidazole, 1,4-dibromobutane and anhydrous ethanol were mixed in a nitrogen atmosphere, stirred in a water bath at 60°C for 16 hours, filtered, the solid phase was washed and dried to obtain material B; the dosage ratio of 1-vinylimidazole, 1,4-dibromobutane and anhydrous ethanol was 0.25 mol: 0.12 mol: 15 mL;

[0068] The material B and deionized water are mixed, stirred for 2 hours, lithium bis(trifluoromethanesulfonyl imide) is added, stirred in a water bath at 65°C for 24 hours, filtered, the solid phase is washed, and vacuum dried to obtain the catalyst; the dosage ratio of the material B, deionized water, and lithium bis(trifluoromethanesulfonyl imide is 0.15 mol:150 mL:0.22 mol.

[0069] Comparative Example 1

[0070] The difference from Example 1 is that a method for preparing paraformaldehyde by spray drying comprises the following steps:

[0071] S1. Pass a formaldehyde solution with a mass concentration of 45% into a depolymerization kettle at 50°C, control the temperature of the formaldehyde in the depolymerization kettle at 100°C, and reflux under boiling conditions for 3 hours;

[0072] S2, cooling the refluxed formaldehyde solution, and when the temperature of the formaldehyde solution reaches 55°C, feeding it into a primary falling film evaporator for a stage of evaporation and concentration to 50% of the mass of the formaldehyde solution in step S1;

[0073] S3, mixing the formaldehyde solution after one stage evaporation concentration and a telogen accounting for 0.5% of the mass content of formaldehyde in the formaldehyde solution after the one stage evaporation concentration, stirring for 10 minutes, feeding into a secondary falling film evaporator, and performing two-stage evaporation concentration to concentrate to 75% of the mass of the formaldehyde solution in step S2;

[0074] S4, mixing the formaldehyde solution after the second stage evaporation concentration and the catalyst accounting for 1.2% of the formaldehyde mass content in the formaldehyde solution after the second stage evaporation concentration for 10 minutes, and then passing it into a spray granulation tower for spray granulation to obtain a polyformaldehyde solid phase, the temperature in the spray granulation tower is 40° C., and the pressure is 270 Pa;

[0075] S5. Sending the paraformaldehyde solid phase to a fluidized bed for drying at a drying temperature of 55° C. to obtain paraformaldehyde with a degree of polymerization of 38.

[0076] Comparative Example 2

[0077] The difference from Example 1 is that a method for preparing paraformaldehyde by spray drying comprises the following steps:

[0078] S1. Pass a formaldehyde solution with a mass concentration of 45% into a depolymerization kettle at 50°C, control the temperature of the formaldehyde in the depolymerization kettle at 100°C, and reflux under boiling conditions for 3 hours;

[0079] S2, cooling the refluxed formaldehyde solution, when the temperature of the formaldehyde solution reaches 55°C, adding a telogen accounting for 0.5% of the mass content of formaldehyde in the formaldehyde solution, stirring for 10 minutes, feeding the material into a primary falling film evaporator, and performing a stage of evaporation and concentration to 50% of the mass of the formaldehyde solution in step S1;

[0080] S3, feeding the formaldehyde solution after the first stage evaporation concentration into a secondary falling film evaporator, and performing second stage evaporation concentration to concentrate to 75% of the mass of the formaldehyde solution in step S2;

[0081] S4, mixing the formaldehyde solution after the second stage evaporation concentration and the catalyst accounting for 1.2% of the formaldehyde mass content in the formaldehyde solution after the second stage evaporation concentration for 10 minutes, and then passing it into a spray granulation tower for spray granulation to obtain a polyformaldehyde solid phase, the temperature in the spray granulation tower is 40° C., and the pressure is 270 Pa;

[0082] S5. Sending the paraformaldehyde solid phase to a fluidized bed for drying at a drying temperature of 55° C. to obtain paraformaldehyde with a degree of polymerization of 41.

[0083] Comparative Example 3

[0084] The difference from Comparative Example 1 is that a method for preparing paraformaldehyde by spray drying comprises the following steps:

[0085] S1. Pass a formaldehyde solution with a mass concentration of 45% into a depolymerization kettle at 50°C, control the temperature of the formaldehyde in the depolymerization kettle at 100°C, and reflux under boiling conditions for 3 hours;

[0086] S2, cooling the refluxed formaldehyde solution, and when the temperature of the formaldehyde solution reaches 55°C, feeding it into a primary falling film evaporator for a stage of evaporation and concentration to 50% of the mass of the formaldehyde solution in step S1;

[0087] S3, feeding the formaldehyde solution after the first stage evaporation concentration into a secondary falling film evaporator, and performing second stage evaporation concentration to concentrate to 75% of the mass of the formaldehyde solution in step S2;

[0088] S4, mixing the formaldehyde solution after the second stage evaporation concentration and the catalyst accounting for 1.2% of the formaldehyde mass content in the formaldehyde solution after the second stage evaporation concentration for 10 minutes, and then passing it into a spray granulation tower for spray granulation to obtain a polyformaldehyde solid phase, the temperature in the spray granulation tower is 40° C., and the pressure is 270 Pa;

[0089] S5. Sending the paraformaldehyde solid phase to a fluidized bed for drying at a drying temperature of 55° C. to obtain paraformaldehyde with a degree of polymerization of 53.

[0090] Comparative Example 4

[0091] The difference from Example 1 is that the catalyst is triethylamine, and paraformaldehyde with a polymerization degree of 40 is obtained.

[0092] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A method for preparing paraformaldehyde by spray drying, It is characterized in that The following steps are involved: S1. Pass a formaldehyde solution with a mass concentration of 45-60% into a depolymerization kettle at 50-60°C, control the temperature of the formaldehyde in the depolymerization kettle at 100°C, and reflux for 3-4 hours under boiling state; S2, cooling the refluxed formaldehyde solution, when the temperature of the formaldehyde solution reaches 55-65°C, adding a telogen accounting for 0.5-1.5% of the mass content of formaldehyde in the formaldehyde solution, stirring for 10-15 minutes, feeding into a primary falling film evaporator, and performing a stage of evaporation and concentration; S3, mixing the formaldehyde solution after one-stage evaporation concentration and a telogen accounting for 0.5-0.8% of the mass content of formaldehyde in the formaldehyde solution after the one-stage evaporation concentration, stirring for 10-15 minutes, feeding into a secondary falling film evaporator, and performing two-stage evaporation concentration; S4, mixing the formaldehyde solution after the second stage evaporation concentration and the catalyst accounting for 1.2-1.5% of the mass content of formaldehyde in the formaldehyde solution after the second stage evaporation concentration for 10-15 minutes, and then passing it into a spray granulation tower for spray granulation to obtain a polyformaldehyde solid phase, wherein the temperature in the spray granulation tower is 40-45° C. and the pressure is 270-300 Pa; S5, sending the paraformaldehyde solid phase to a fluidized bed for drying to obtain the paraformaldehyde; Wherein, the preparation of the telogen comprises the following steps: S231, take gallic acid, polyvinyl alcohol, 4-dimethylaminopyridine, toluene, mix, stir for 2-3h, add dicyclohexylcarbodiimide, stir for 2-3h, centrifuge, take the supernatant, add it to 95% ethanol solution by volume, add n-octyl hydrazide, stir for 2-3h, add hydrochloric acid solution with a concentration of 2-4mol / L, purify by gradient precipitation of ethyl acetate and petroleum ether, wash, and dry to obtain material A; the dosage ratio of gallic acid, polyvinyl alcohol, 4-dimethylaminopyridine, toluene, dicyclohexylcarbodiimide, ethanol solution, n-octyl hydrazide, and hydrochloric acid solution is 4-6mmol:3-4mmol:0.5-0.6mmol:30-40mL:5-6mmol:20-30mL:14-16mmol:4-6mmol; S232, taking the material A, methanol and deionized water and placing them in a reaction kettle, stirring for 1-2h, adding a formaldehyde solution with a mass fraction of 49.8-52.3% and a sulfuric acid solution with a concentration of 2-4mol / L, reacting at 50-55°C for 6-8h, and then treating with an ion exchange resin, taking the liquid phase to obtain the polymerization agent; the dosage ratio of the material A, methanol, deionized water, formaldehyde solution and sulfuric acid solution is 4-6mg:30-40mL:30-40mL:15-20mL:6-8mL; The preparation of the catalyst comprises the following steps: S41. Mix 1-vinylimidazole, 1,4-dibromobutane and anhydrous ethanol in a nitrogen atmosphere, stir in a water bath at 55-60° C. for 12-16 hours, filter, wash and dry the solid phase to obtain material B; the ratio of 1-vinylimidazole, 1,4-dibromobutane and anhydrous ethanol is 0.15-0.25 mol: 0.1-0.12 mol: 10-15 mL; S42. Mix the material B and deionized water, stir for 1-2 hours, add lithium bis(trifluoromethanesulfonyl imide), stir in a water bath at 65°C for 20-24 hours, filter, wash the solid phase, and vacuum dry to obtain the catalyst; the dosage ratio of the material B, deionized water, and lithium bis(trifluoromethanesulfonyl imide is 0.1-0.15 mol: 150 mL: 0.2-0.22 mol.

2. The method for preparing paraformaldehyde by spray drying according to claim 1, It is characterized in that In step S5, the drying temperature is 55-60°C.

3. The method for preparing paraformaldehyde by spray drying according to claim 1, It is characterized in that In step S2, the one-stage evaporation concentration refers to concentration to 50-65% of the mass of the formaldehyde solution in step S1.

4. The method for preparing paraformaldehyde by spray drying according to claim 1, It is characterized in that In step S3, the second stage evaporation concentration refers to concentration to 75-85% of the mass of the formaldehyde solution in step S2.