A battery with full-tab 38120 cylindrical structure

By adopting the cylindrical structure of the full-pole ear 38120 in large cylindrical lithium batteries and using kneading and welding technology, the problem of insufficient high and low temperature resistance resistance is solved, and the internal resistance is reduced and performance is improved, which is suitable for efficient electrochemical applications.

CN118367234BActive Publication Date: 2024-11-01JIANGSU SUNPOWER
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410782071.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2024-11-01
Estimated Expiration
2044-06-18

AI Technical Summary

Technical Problem

The existing large cylindrical lithium batteries have insufficient high and low temperature resistance, and further improvements are needed to improve the safety and performance of the battery.

Method used

Using the full-pole ear 38120 cylindrical structure battery, the hollow aluminum foil and empty copper foil are retained during the positive and negative electrode coating process, and the flattened after winding, welding the electrode ear or current collecting disk, and design uniform round holes to facilitate injection. shortens the electron migration path and reduces internal resistance.

Benefits of technology

It significantly reduces the internal resistance of the battery, improves the high and low temperature discharge performance and cycling performance, and has a wider application prospect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118367234B_ABST
    Figure CN118367234B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of cylindrical lithium-ion full-tab battery, in particular to a battery with a full-tab 38120 cylindrical structure; the positive and negative electrodes adopt a full-tab battery structure, which effectively reduces the internal resistance of the battery; during the coating process of the positive and negative electrodes, empty aluminum foil and empty copper foil are respectively retained on one side of the electrode sheet, and the empty aluminum foil and empty copper foil exposed on both sides of the diaphragm are flattened after winding, and then the flattened positive and negative electrode welding tabs or current collecting plates are assembled; the positive and negative electrode current collecting plates are designed with holes, and the circular holes are evenly distributed, which is convenient for liquid seepage during the liquid injection process; the tabs led out of the positive electrode current collecting plate can be directly welded on the cap, the operation is simple, the welding marks of the positive and negative electrode welding current collecting plates are evenly distributed, and the migration path of electrons in the charging and discharging process is shortened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of cylindrical lithium-ion full-tab batteries, in particular to a battery with a full-tab 38120 cylindrical structure. Background Art

[0002] In recent years, driven by the increasing terminal demand, the performance and application scope of cylindrical batteries have been continuously improved, and full-ear cylindrical batteries have come into being. There is no concentrated heating point inside the battery with full-ears, and the heat is evenly distributed inside, which has the advantage of thermal management for the whole battery pack. Therefore, the battery safety performance of the full-ear design is better. The full-ear technology can reduce the internal resistance and heating rate of the battery by orders of magnitude, and has an absolute advantage in solving the heat dissipation problem of high-energy density cells, helping to break through the bottleneck of cylindrical batteries. Large cylindrical lithium batteries have a large space in the development market of low-speed vehicles and small energy storage. As one of the positive electrode materials of lithium batteries, lithium iron phosphate has relative advantages over ternary materials in comprehensive indicators such as safety, cycle life, and production cost. Since its commercialization, it has been applied to many fields including automobiles, ships, and energy storage, becoming one of the most developed positive electrode materials at this stage; full-ear batteries have the advantages of strong current carrying capacity, excellent rate performance, effective reduction of internal resistance, and high power output. Large cylindrical batteries equipped with full-ear technology form a barrier with traditional cylindrical batteries. There will be huge demand in the low-speed vehicle and small energy storage markets, and it will also become the development direction of the next generation of cylindrical batteries.

[0003] As the size of large cylindrical battery cells increases, the energy density will also increase, the number of series and parallel connections will decrease, and flexible grouping will reduce pack costs. Compared with square batteries that are prone to bulging, cylindrical batteries have a stable structure and can remain stable for a long time in energy storage system applications. The full tabs of the battery cell can be completed through an ultrasonic flattening process, and the end surface processing technology is improved to solve the powder problem from the root and eliminate battery quality risks. The design structure and welding of the collector plate directly affect the effect of reducing the internal resistance of the full-tab battery. The Chinese patent with application number CN202223191478.6 discloses a full-tab cylindrical battery, which uses the annular groove of the collector plate with an oblique groove surface to fit the top of the tab, drive the tab to bend along the direction of the guide groove surface of the annular groove, increase the contact area between the tab and the collector plate, and avoid undesirable phenomena such as folding, reducing the risk of internal short circuit in the full-tab cylindrical battery.

[0004] Although the cylindrical battery manufactured by the above patent document has advantages such as avoiding short circuit, its high and low temperature resistance is relatively insufficient and still needs further improvement. Based on this, the present invention provides a battery with a full-tab 38120 cylindrical structure to solve the above technical problems! Summary of the invention

[0005] The object of the present invention is to provide a battery with a full-ear 38120 cylindrical structure. The positive and negative electrodes adopt a full-ear battery structure to effectively reduce the internal resistance of the battery. During the coating process of the positive and negative electrodes, empty aluminum foil and empty copper foil are respectively retained on one side of the electrode piece. After winding, the empty aluminum foil and empty copper foil exposed on both sides of the diaphragm are flattened, and then the flattened positive and negative electrode welding ears or current collecting plates are assembled. The positive and negative electrode current collecting plates are designed with holes, and the circular holes are evenly distributed, which is convenient for liquid seepage during the injection process. The ears led out of the positive electrode current collecting plate can be directly welded on the cap, which is simple to operate. The weld marks of the positive and negative electrode welding collecting plates are evenly distributed, shortening the migration path of electrons during charging and discharging.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] The first aspect of the present invention provides a method for preparing a battery with a full-tab 38120 cylindrical structure, comprising the following steps:

[0008] S1, homogenization: 20-30 parts of lithium iron phosphate, 5-9 parts of polyvinylidene fluoride PVDF, 3-5 parts of carbon black conductive agent SP, 3-5 parts of functional additives and 40-50 parts of N-methylpyrrolidone are mixed evenly to obtain positive electrode slurry; 12-14 parts of graphite, 3-5 parts of binder CMC, 3-5 parts of carbon black conductive agent SP, 4-6 parts of dispersant SBR and 40-50 parts of deionized water are mixed evenly to obtain negative electrode slurry;

[0009] The preparation process of the functional additive is as follows:

[0010] The carbon-containing plant material is placed in a carbonization device and heated to 230-240°C at a heating rate of 6-8°C / min, and kept warm for 180-200 minutes; then heated to 400°C at a heating rate of 1-3°C / min, and kept warm for 260-280 minutes to obtain a pre-carbonized carbon material;

[0011] The obtained pre-carbonized carbon material is placed in a grinding device and ground to 150-200 meshes, the obtained ground carbon powder is placed in an appropriate amount of potassium hydroxide solution at a solid-liquid ratio of 0.02-0.05 g / mL, and ultrasonically dispersed at 90-92° C. for 20-30 minutes. After suction filtration, the filter cake is placed in a drying oven at 80-90° C. and dried to constant weight to obtain a carbonized product;

[0012] The obtained carbonized product is placed in an activation furnace, treated under vacuum, nitrogen atmosphere, 820-840° C. for 60-80 min, cooled and discharged, washed with deionized water until the pH value reaches 7.2-7.4, and then dried in a drying oven at 80-90° C. to constant weight to obtain an activated carbon auxiliary material;

[0013] The activated carbon auxiliary material obtained is placed in an appropriate amount of carbon disulfide solution at a solid-liquid ratio of 0.02-0.05 g / mL, stirred at 30-50 r / min for 120-130 min, and allowed to stand for 22-24 h, then washed with deionized water 2-4 times, placed in a drying oven at 80-90° C. and dried to constant weight to obtain a functional auxiliary agent;

[0014] The carbon-containing plant material is prepared by mixing corn silk and Euryale ferox shell in a mass ratio of 1:0.2-0.4;

[0015] The potassium hydroxide solution is prepared by mixing potassium hydroxide and deionized water at a solid-liquid ratio of 0.22 to 0.32 g / mL;

[0016] The carbon disulfide solution is prepared by mixing carbon disulfide and anhydrous ethanol at a mass ratio of 0.32 to 0.42:1;

[0017] S2, coating: coating the positive electrode and the negative electrode respectively using a continuous coating mode;

[0018] S3, rolling and slitting: after coating is completed, the rolling thickness is controlled to roll and slitting the positive electrode and the negative electrode respectively;

[0019] S4, winding and flattening: When winding, wrap the negative electrode material area on both sides of the diaphragm, and wrap the positive electrode material area on both sides of the negative electrode material area. After winding, 4-5 mm of empty aluminum foil and empty copper foil are exposed at both ends of the core, and then use a flattening machine to flatten the exposed empty aluminum foil and empty copper foil at both ends of the core;

[0020] S5, foil surface welding: weld the pole ear or collector plate on the flattened aluminum foil and copper foil surface, and then perform grooving, spot welding, liquid injection, sealing and assembly.

[0021] Furthermore, in step S2, when the positive electrode is coated, 7 to 9 mm of empty aluminum foil is retained on one side of the electrode to form a material area and an empty aluminum foil, and when the negative electrode is coated, 6 to 8 mm of empty copper foil is retained on one side of the electrode to form a material area and an empty copper foil.

[0022] Furthermore, in step S3, the cutting width of the positive electrode is 111-113 mm, wherein the material area width of the positive electrode is 103-104 mm, and the width of the empty aluminum foil of the positive electrode is 7-9 mm.

[0023] Furthermore, in step S3, the cutting width of the negative electrode is 114-115 mm, wherein the material area width of the negative electrode is 106-108 mm, and the empty copper foil width of the negative electrode is 6-8 mm.

[0024] Furthermore, in the step S4, during the kneading, the kneading machine is kept to absorb dust.

[0025] Furthermore, in step S4, after being flattened, the foil surfaces of the empty aluminum foil and the empty copper foil are exposed by 1 to 2 mm.

[0026] The second aspect of the present invention: also provides a battery with a full-tab 38120 cylindrical structure, which is prepared by the above-mentioned preparation method.

[0027] Furthermore, the battery has a diameter of 37.5-38.5 mm, a height of 119-121 mm, and a capacity of 13.0-14.0 Ah.

[0028] Compared with the prior art, the present invention has the following beneficial effects:

[0029] The full-ear 38120 cylindrical structure battery prepared by the present invention reduces the film-making steps after the normal process slitting, and the preparation process is simple. In addition, the full-ear and the new collector plate structure effectively reduce the internal resistance of the battery, and the internal resistance of the battery is more than 70% lower than that of the conventional cylindrical battery. At the same time, the new collector plate structure is convenient for welding the cap, and the operation is simple. The full-ear 38120 cylindrical structure battery prepared by the present invention shows good electrochemical performance in tests such as high and low temperature discharge performance and cycle performance, has broad application prospects, and is worthy of promotion. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 Schematic diagram of cutting the full-tab pole piece of the full-tab 38120 cylindrical battery (sample A) of Example 1;

[0031] Figure 2 Schematic diagram of the positive electrode current collector of the full-tab 38120 cylindrical battery (sample A) of Example 1;

[0032] Figure 3 Schematic diagram of the negative electrode current collector of the full-tab 38120 cylindrical battery (sample A) of Example 1;

[0033] Figure 4 Schematic diagram of the full-tab positive electrode welded current collector of the full-tab 38120 cylindrical battery (sample A) of Example 1;

[0034] Figure 5 Schematic diagram of the full-tab negative electrode welded current collector of the full-tab 38120 cylindrical battery (sample A) of Example 1;

[0035] Figure 6 This is the high and low temperature 0.5C discharge curve of full-tab 38120 cylindrical battery;

[0036] Figure 7 This is the 25°C cycle curve of a full-tab 38120 cylindrical battery;

[0037] Legend: 1. Current collecting plate; 2. Round hole; 3. Ear. DETAILED DESCRIPTION

[0038] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0039] Embodiment 1: This embodiment provides a method for preparing a battery with a full-tab 38120 cylindrical structure, comprising the following steps:

[0040] S1, homogenization: 25 parts of lithium iron phosphate, 7 parts of polyvinylidene fluoride PVDF, 4 parts of carbon black conductive agent SP, 3-5 parts of functional additives and 45 parts of N-methylpyrrolidone are mixed evenly to obtain positive electrode slurry; 13 parts of graphite, 4 parts of binder CMC, 4 parts of carbon black conductive agent SP, 5 parts of dispersant SBR and 45 parts of deionized water are mixed evenly to obtain negative electrode slurry;

[0041] The preparation process of the functional additive is as follows:

[0042] The carbon-containing plant material is placed in a carbonization device and heated to 230°C at a heating rate of 6°C / min, and kept warm for 180 minutes; then heated to 400°C at a heating rate of 1°C / min, and kept warm for 260 minutes to obtain a pre-carbonized carbon material;

[0043] The obtained pre-carbonized carbon material was placed in a grinding device and ground to 150 mesh, and the ground carbon powder was placed in an appropriate amount of potassium hydroxide solution at a solid-liquid ratio of 0.02 g / mL, and ultrasonically dispersed at 90°C for 20 minutes. After suction filtration, the filter cake was placed in a drying oven at 80°C and dried to constant weight to obtain a carbonized product;

[0044] The obtained carbonized product was placed in an activation furnace, treated under vacuum, nitrogen atmosphere, and 820° C. for 60 min, cooled and discharged, washed with deionized water until the pH value reached 7.2-7.4, and then dried in a drying oven at 80° C. to constant weight to obtain an activated carbon auxiliary material;

[0045] The activated carbon auxiliary material obtained was placed in an appropriate amount of carbon disulfide solution at a solid-liquid ratio of 0.02 g / mL, stirred at 30 r / min for 120 min, and allowed to stand for 22 h, then washed twice with deionized water, placed in a drying oven at 80 ° C and dried to constant weight to obtain a functional auxiliary agent;

[0046] In addition, the carbon-containing plant material is mixed with corn silk and Euryale ferox shell in a mass ratio of 1:0.2;

[0047] The potassium hydroxide solution was prepared by mixing potassium hydroxide and deionized water at a solid-liquid ratio of 0.22 g / mL;

[0048] The carbon disulfide solution is prepared by mixing carbon disulfide and anhydrous ethanol in a mass ratio of 0.32:1.

[0049] S2. Coating: The positive electrode and the negative electrode are coated separately using a continuous coating mode.

[0050] Among them, when coating the positive electrode, 7~9mm of empty aluminum foil is retained on one side of the electrode to form a material area and an empty aluminum foil. When coating the negative electrode, 6~8mm of empty copper foil is retained on one side of the electrode to form a material area and an empty copper foil, which are reserved for the flattened full electrode ear.

[0051] S3, rolling and slitting: After coating, the rolling thickness is controlled to roll and slitting the positive electrode and the negative electrode respectively.

[0052] Among them, the cutting width of the positive electrode is 111-113 mm, the width of the material area of ​​the positive electrode is 103-104 mm, and the width of the empty aluminum foil of the positive electrode is 7-9 mm.

[0053] The slitting width of the negative electrode is 114-115 mm, of which the material area of ​​the negative electrode is 106-108 mm wide and the empty copper foil of the negative electrode is 6-8 mm wide.

[0054] In addition, the slitting process avoids wavy edges and material falling off, and the positive and negative electrode sheets and diaphragms (diaphragm width 110~112mm) are baked and then wound.

[0055] S4. Winding and flattening: When winding, wrap the negative electrode material area on both sides of the diaphragm, and wrap the positive electrode material area on both sides of the negative electrode material area. After winding, 4~5mm of empty aluminum foil and empty copper foil are exposed at both ends of the core respectively, and then use a flattening machine to flatten the exposed empty aluminum foil and empty copper foil at both ends of the core.

[0056] When kneading, keep the kneading machine vacuumed.

[0057] After being flattened, the foil surfaces of the empty aluminum foil and the empty copper foil are exposed by 1 to 2 mm.

[0058] S5, foil surface welding: weld the pole ear or collector plate on the flattened aluminum foil and copper foil surface, and then perform grooving, spot welding, liquid injection, sealing and assembly.

[0059] In addition, the current collecting plates 1 of the positive and negative electrodes are designed as follows Figure 2 and Figure 3 As shown in the figure, the circular hole 2 is the punching position, and the circular holes 2 are evenly distributed, which is convenient for rapid liquid infiltration during the injection process. The pole ear 3 led out of the positive electrode collector plate 1 can be directly welded on the cap, which is simple to operate. Figure 4 and Figure 5As shown, the dotted line in the figure is the welding position.

[0060] In addition, this embodiment also provides a battery with a full-tab 38120 cylindrical structure, which is prepared using the above-mentioned preparation method, namely sample A (full-tab structure).

[0061] Among them, the battery has a diameter of 37.5-38.5mm, a height of 119-121mm, and a capacity of 13.0-14.0Ah.

[0062] Embodiment 2: The battery with full-electrode tab 38120 cylindrical structure provided in this embodiment is basically the same as that in Embodiment 1, except that: the specific preparation method of the battery with full-electrode tab 38120 cylindrical structure in this embodiment is different; the specific preparation method of the battery with full-electrode tab 38120 cylindrical structure in this embodiment is as follows:

[0063] S1, homogenization: 25 parts of lithium iron phosphate, 7 parts of polyvinylidene fluoride PVDF, 4 parts of carbon black conductive agent SP, 4 parts of functional additives and 45 parts of N-methylpyrrolidone are mixed evenly to obtain a positive electrode slurry; 13 parts of graphite, 4 parts of binder CMC, 4 parts of carbon black conductive agent SP, 5 parts of dispersant SBR and 45 parts of deionized water are mixed evenly to obtain a negative electrode slurry;

[0064] The preparation process of the functional additive is as follows:

[0065] The carbon-containing plant material is placed in a carbonization device and heated to 235°C at a heating rate of 7°C / min, and kept warm for 190 minutes; then heated to 400°C at a heating rate of 2°C / min, and kept warm for 270 minutes to obtain a pre-carbonized carbon material;

[0066] The obtained pre-carbonized carbon material was placed in a grinding device and ground to 175 mesh, and the ground carbon powder was placed in an appropriate amount of potassium hydroxide solution at a solid-liquid ratio of 0.03 g / mL, and ultrasonically dispersed at 91°C for 25 minutes. After filtration, the filter cake was placed in a drying oven at 85°C and dried to constant weight to obtain a carbonized product;

[0067] The obtained carbonized product was placed in an activation furnace, treated under vacuum, nitrogen atmosphere, and 830° C. for 70 min, cooled and discharged, washed with deionized water until the pH value reached 7.3, and then dried in a drying oven at 85° C. to constant weight to obtain an activated carbon auxiliary material;

[0068] The activated carbon auxiliary material was placed in an appropriate amount of carbon disulfide solution at a solid-liquid ratio of 0.03 g / mL, stirred at 40 r / min for 125 min, and allowed to stand for 23 h, then washed with deionized water 3 times, placed in a drying oven at 85 ° C and dried to constant weight to obtain a functional auxiliary agent;

[0069] In addition, the carbon-containing plant material is mixed with corn silk and Euryale ferox shell in a mass ratio of 1:0.3;

[0070] The potassium hydroxide solution is prepared by mixing potassium hydroxide and deionized water at a solid-liquid ratio of 0.27 g / mL;

[0071] The carbon disulfide solution is prepared by mixing carbon disulfide and anhydrous ethanol in a mass ratio of 0.37:1.

[0072] S2. Coating: The positive electrode and the negative electrode are coated separately using a continuous coating mode.

[0073] Among them, when coating the positive electrode, 12~14mm of empty aluminum foil is retained on one side of the electrode to form a material area and an empty aluminum foil. When coating the negative electrode, 11~13mm of empty copper foil is retained on one side of the electrode to form a material area and an empty copper foil, which are reserved for die-cutting the electrode ears.

[0074] S3. Die-cutting: The rolling thickness and slitting width of the positive and negative electrodes are controlled within the process design range. After slitting, the empty aluminum foil and empty copper foil of the positive and negative electrodes are die-cut, and 6 empty foil tabs are die-cut for the positive and negative electrodes respectively.

[0075] S4. Winding and flattening: When winding, the two sides of the diaphragm wrap around the negative electrode material area, and the two sides of the negative electrode material area wrap around the positive electrode material area.

[0076] S5, Foil surface welding: After winding, the die-cut empty foil tab is welded to the tab or collector plate. Finally, groove rolling, spot bottom welding, liquid injection, and sealing assembly are performed according to the set size. It is recorded as sample B (multi-tab structure).

[0077] Embodiment 3: The battery with full-electrode tab 38120 cylindrical structure provided in this embodiment is basically the same as that in Embodiment 1, except that: the specific preparation method of the battery with full-electrode tab 38120 cylindrical structure in this embodiment is different; the specific preparation method of the battery with full-electrode tab 38120 cylindrical structure in this embodiment is as follows:

[0078] S1, homogenization: 25 parts of lithium iron phosphate, 7 parts of polyvinylidene fluoride PVDF, 4 parts of carbon black conductive agent SP, 5 parts of functional additives and 45 parts of N-methylpyrrolidone are mixed evenly to obtain a positive electrode slurry; 13 parts of graphite, 4 parts of binder CMC, 4 parts of carbon black conductive agent SP, 5 parts of dispersant SBR and 45 parts of deionized water are mixed evenly to obtain a negative electrode slurry;

[0079] The preparation process of the functional additive is as follows:

[0080] The carbon-containing plant material is placed in a carbonization device and heated to 240°C at a heating rate of 8°C / min, and kept warm for 200 minutes; then heated to 400°C at a heating rate of 3°C / min, and kept warm for 260-280 minutes to obtain a pre-carbonized carbon material;

[0081] The obtained pre-carbonized carbon material was placed in a grinding device and ground to 200 meshes, and the ground carbon powder was placed in an appropriate amount of potassium hydroxide solution at a solid-liquid ratio of 0.05 g / mL, and ultrasonically dispersed at 92°C for 30 minutes. After filtration, the filter cake was placed in a drying oven at 90°C and dried to constant weight to obtain a carbonized product;

[0082] The obtained carbonized product is placed in an activation furnace, treated for 80 minutes under vacuum, nitrogen atmosphere, and 820-840° C., cooled and discharged, washed with deionized water until the pH value reaches 7.2-7.4, and then dried in a drying oven at 90° C. to constant weight to obtain an activated carbon auxiliary material;

[0083] The activated carbon auxiliary material was placed in an appropriate amount of carbon disulfide solution at a solid-liquid ratio of 0.05 g / mL, stirred at 50 r / min for 130 min, and allowed to stand for 24 h, then washed with deionized water 4 times, placed in a drying oven at 90 ° C and dried to constant weight to obtain a functional auxiliary agent;

[0084] In addition, the carbon-containing plant material is mixed with corn silk and Euryale ferox shell in a mass ratio of 1:0.4;

[0085] The potassium hydroxide solution is prepared by mixing potassium hydroxide and deionized water at a solid-liquid ratio of 0.32 g / mL;

[0086] The carbon disulfide solution is prepared by mixing carbon disulfide and anhydrous ethanol in a mass ratio of 0.42:1.

[0087] S2. Coating: The intermittent coating mode is used to coat the positive electrode and the negative electrode respectively. The intermittent coating mode is used during coating, leaving a 13mm gap for welding the pole ear, and the surface density of the material area is controlled within the process design range.

[0088] S3. Slitting: The rolling thickness of positive and negative electrodes is controlled within the process design range. The positive electrode slitting width is 105-107mm (material area 105-107mm), and the negative electrode slitting width is 109-111mm (material area 109-111mm). The slitting process should avoid wavy edges and material falling.

[0089] S4. Welding: After cutting, the electrode tabs are welded and the positive and negative electrodes are welded with two tabs respectively. After the production, the positive and negative electrode sheets and diaphragms (diaphragm width 113 ~ 115mm) are baked.

[0090] S5. Winding: When winding, the two sides of the diaphragm wrap around the negative electrode material area, and the two sides of the negative electrode material area wrap around the positive electrode material area. Finally, according to the set size, groove rolling, spot welding, liquid injection, and sealing assembly are performed. Recorded as sample C (bipolar ear structure).

[0091] Embodiment 4: The battery with full-electrode tab 38120 cylindrical structure provided in this embodiment is basically the same as that in Embodiment 1, except that: the specific preparation method of the battery with full-electrode tab 38120 cylindrical structure in this embodiment is different; the specific preparation method of the battery with full-electrode tab 38120 cylindrical structure in this embodiment is as follows:

[0092] S1. Homogenization: Mix 25 parts of lithium iron phosphate, 7 parts of polyvinylidene fluoride PVDF, 4 parts of carbon black conductive agent SP and 45 parts of N-methylpyrrolidone to obtain positive electrode slurry; mix 13 parts of graphite, 4 parts of binder CMC, 4 parts of carbon black conductive agent SP, 5 parts of dispersant SBR and 45 parts of deionized water to obtain negative electrode slurry.

[0093] S2. Coating: The positive electrode and the negative electrode are coated separately using a continuous coating mode.

[0094] Among them, when coating the positive electrode, 7~9mm of empty aluminum foil is retained on one side of the electrode to form a material area and an empty aluminum foil. When coating the negative electrode, 6~8mm of empty copper foil is retained on one side of the electrode to form a material area and an empty copper foil, which are reserved for the flattened full electrode ear.

[0095] S3, rolling and slitting: After coating, the rolling thickness is controlled to roll and slitting the positive electrode and the negative electrode respectively.

[0096] Among them, the cutting width of the positive electrode is 111-113 mm, the width of the material area of ​​the positive electrode is 103-104 mm, and the width of the empty aluminum foil of the positive electrode is 7-9 mm.

[0097] The slitting width of the negative electrode is 114-115 mm, of which the material area of ​​the negative electrode is 106-108 mm wide and the empty copper foil of the negative electrode is 6-8 mm wide.

[0098] In addition, the slitting process avoids wavy edges and material falling off, and the positive and negative electrode sheets and diaphragms (diaphragm width 110~112mm) are baked and then wound.

[0099] S4. Winding and flattening: When winding, wrap the negative electrode material area on both sides of the diaphragm, and wrap the positive electrode material area on both sides of the negative electrode material area. After winding, 4~5mm of empty aluminum foil and empty copper foil are exposed at both ends of the core respectively, and then use a flattening machine to flatten the exposed empty aluminum foil and empty copper foil at both ends of the core.

[0100] When kneading, keep the kneading machine vacuumed.

[0101] After being flattened, the foil surfaces of the empty aluminum foil and the empty copper foil are exposed by 1 to 2 mm.

[0102] S5, foil surface welding: weld the pole ear or collector plate on the flattened aluminum foil and copper foil surface, and then perform grooving, spot welding, liquid injection, sealing and assembly.

[0103] In addition, the current collecting plates 1 of the positive and negative electrodes are designed as follows Figure 2 and Figure 3 As shown in the figure, the circular hole 2 is the punching position, and the circular holes 2 are evenly distributed, which is convenient for rapid liquid infiltration during the injection process. The pole ear 3 led out of the positive electrode collector plate 1 can be directly welded on the cap, which is simple to operate. Figure 4 and Figure 5 As shown, the dotted line in the figure is the welding position.

[0104] In addition, this embodiment also provides a battery with a full-tab 38120 cylindrical structure, which is prepared using the above-mentioned preparation method, namely, sample D (full-tab structure).

[0105] The battery has a diameter of 37.5 to 38.5 mm, a height of 119 to 121 mm, and a capacity of 13.0 to 14.0 Ah. This is referred to as sample D.

[0106] Performance test: The relevant performance of the battery with full-tab 38120 cylindrical structure provided in Examples 1 to 4 was tested as follows:

[0107] 1. Charge and discharge test: Use a charge and discharge tester to test the battery's cycle performance.

[0108] 2. High and low temperature test: Use a charge and discharge tester with a high and low temperature oven to test the high and low temperature discharge performance of the battery.

[0109] The obtained test data are recorded in the following Tables 1, 2, and Figure 6 and Figure 7 .

[0110]

[0111]

[0112] As shown in Table 1, the AC internal resistance ACR of sample A (full-ear structure) is 2.1mΩ@100%SOC, and the 3C discharge DCR and 3C charge DCR are 5.7mΩ and 4.5mΩ respectively at 25%SOC. The internal resistance is lower than that of sample B (multi-ear structure), sample C (bipolar ear structure) and sample D. Compared with the conventional bipolar ear structure (sample C), the ACR of the full-ear structure (sample A) is reduced by 77.9% and the DCR is reduced by 79%. The battery with full-ear structure turns the entire foil current collector into an ear, and the current is changed from the conventional lateral transmission along the current collector to the ear to the longitudinal transmission of the current collector, which shortens the migration path of the electrons and effectively reduces the internal resistance of the 38120 cylindrical battery; functional additives help shorten the migration path of the electrons.

[0113] Depend on Figure 6It can be seen that the battery is fully charged to 3.65V at 0.5C constant current and constant voltage at 25℃, and then discharged at 0.5C constant current after being left for 4 hours at 25℃, 55℃, -10℃ and -20℃. The discharge cut-off voltage at 25℃ and 55℃ is 2.0V, and the discharge cut-off voltage at -10℃ and -20℃ is 1.5V.

[0114] As shown in Table 2, the discharge capacities of sample A (full-ear) at 25℃, 55℃, -10℃ and -20℃ are 13.1Ah, 13.0Ah, 12.4Ah, 11.6Ah, respectively, and the -10℃ discharge capacity retention rate is 94.3%, and the -20℃ discharge capacity retention rate is 88.1%. The discharge capacities of sample B (multi-ear) at 25℃, 55℃, -10℃ and -20℃ are 13.3Ah, 13.1Ah, 11.2Ah, 9.6Ah, respectively, and the -10℃ discharge capacity retention rate is 84.0%, and the -20℃ discharge capacity retention rate is 72.0%. The high and low temperature discharge capacity retention rate of sample A (full-ear) is relatively high; functional additives help to improve the high and low temperature discharge capacity retention rate.

[0115] Depend on Figure 7 It can be seen that the 1C constant current and constant voltage fully charges to 3.65V, and the 1C constant current discharges to 2.0V. The initial capacity of sample A (full-electrode ear) is 13.1Ah, and the capacity retention rate is 93.6% after 1200 cycles of +1C / -1C at 25°C. The initial capacity of sample B (multi-electrode ear) is 13.0Ah, and the capacity retention rate is 90.2% after 1200 cycles of +1C / -1C at 25°C. The capacity retention rate of sample A (full-electrode ear) is higher in room temperature cycles.

[0116] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0117] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A method for preparing a battery with a full-tab 38120 cylindrical structure, characterized in that: The following steps are involved: S1, homogenization: 20-30 parts by weight of lithium iron phosphate, 5-9 parts by weight of polyvinylidene fluoride PVDF, 3-5 parts by weight of carbon black conductive agent SP, 3-5 parts by weight of functional additives and 40-50 parts by weight of N-methylpyrrolidone are mixed evenly to obtain a positive electrode slurry; 12-14 parts by weight of graphite, 3-5 parts by weight of binder CMC, 3-5 parts by weight of carbon black conductive agent SP, 4-6 parts by weight of dispersant SBR and 40-50 parts by weight of deionized water are mixed evenly to obtain a negative electrode slurry; The preparation process of the functional additive is as follows: The carbon-containing plant material is placed in a carbonization device and heated to 230-240°C at a heating rate of 6-8°C / min, and kept warm for 180-200 minutes; then heated to 400°C at a heating rate of 1-3°C / min, and kept warm for 260-280 minutes to obtain a pre-carbonized carbon material; The obtained pre-carbonized carbon material is placed in a grinding device and ground to 150-200 meshes, the obtained ground carbon powder is placed in an appropriate amount of potassium hydroxide solution at a solid-liquid ratio of 0.02-0.05 g / mL, and ultrasonically dispersed at 90-92° C. for 20-30 minutes. After suction filtration, the filter cake is placed in a drying oven at 80-90° C. and dried to constant weight to obtain a carbonized product; The obtained carbonized product is placed in an activation furnace, treated under vacuum, nitrogen atmosphere, 820-840° C. for 60-80 min, cooled and discharged, washed with deionized water until the pH value reaches 7.2-7.4, and then dried in a drying oven at 80-90° C. to constant weight to obtain an activated carbon auxiliary material; The activated carbon auxiliary material obtained is placed in an appropriate amount of carbon disulfide solution at a solid-liquid ratio of 0.02-0.05 g / mL, stirred at 30-50 r / min for 120-130 min, and allowed to stand for 22-24 h, then washed with deionized water 2-4 times, placed in a drying oven at 80-90° C. and dried to constant weight to obtain a functional auxiliary agent; The carbon-containing plant material is prepared by mixing corn silk and Euryale ferox shell in a mass ratio of 1:0.2-0.4; The potassium hydroxide solution is prepared by mixing potassium hydroxide and deionized water at a solid-liquid ratio of 0.22 to 0.32 g / mL; The carbon disulfide solution is prepared by mixing carbon disulfide and anhydrous ethanol at a mass ratio of 0.32 to 0.42:1; S2, coating: coating the positive electrode and the negative electrode respectively using a continuous coating mode; S3, rolling and slitting: after coating is completed, the rolling thickness is controlled to roll and slitting the positive electrode and the negative electrode respectively; S4, winding and flattening: When winding, wrap the negative electrode material area on both sides of the diaphragm, and wrap the positive electrode material area on both sides of the negative electrode material area. After winding, 4-5 mm of empty aluminum foil and empty copper foil are exposed at both ends of the core, and then use a flattening machine to flatten the exposed empty aluminum foil and empty copper foil at both ends of the core; S5, foil surface welding: weld the pole ear or collector plate on the flattened aluminum foil and copper foil surface, and then perform grooving, spot welding, liquid injection, sealing and assembly.

2. The method for preparing a battery with a full-tab 38120 cylindrical structure according to claim 1, characterized in that: In step S2, when coating the positive electrode, a 7-9 mm empty aluminum foil is retained on one side of the electrode to form a material area and an empty aluminum foil. When coating the negative electrode, a 6-8 mm empty copper foil is retained on one side of the electrode to form a material area and an empty copper foil.

3. The method for preparing a battery with a full-tab 38120 cylindrical structure according to claim 2, characterized in that: In step S3, the cutting width of the positive electrode is 111-113 mm, wherein the material area width of the positive electrode is 103-104 mm, and the width of the empty aluminum foil of the positive electrode is 7-9 mm.

4. The method for preparing a battery with a full-tab 38120 cylindrical structure according to claim 2, characterized in that: In step S3, the cutting width of the negative electrode is 114-115 mm, wherein the material area width of the negative electrode is 106-108 mm, and the empty copper foil width of the negative electrode is 6-8 mm.

5. The method for preparing a battery with a full-tab 38120 cylindrical structure according to claim 1, characterized in that: In the step S4, during the flattening, the flattening machine is kept to absorb dust.

6. The method for preparing a battery with a full-tab 38120 cylindrical structure according to claim 1, characterized in that: In step S4, after being flattened, the foil surfaces of the empty aluminum foil and the empty copper foil are exposed by 1 to 2 mm.

7. A battery with a full-tab 38120 cylindrical structure, characterized in that: Prepared according to any one of the preparation methods of claims 1 to 6.

8. A battery with a full-tab 38120 cylindrical structure according to claim 7, characterized in that: The battery has a diameter of 37.5 to 38.5 mm, a height of 119 to 121 mm, and a capacity of 13.0 to 14.0 Ah.