A fullerene derivative electron transport material and its preparation method
By preparing fullerene derivative materials for the electron transport layer of perovskite solar cells, the solubility and stability problems of existing materials were solved, thereby improving photoelectric conversion efficiency and device lifetime.
Patent Information
- Application Number
- CN202410480961.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-20
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-04-20
AI Technical Summary
Existing fullerene electron transport materials in perovskite solar cells suffer from problems such as limited solubility, insufficient passivation effect, weak intermolecular interactions, and unstable morphology, which lead to reduced device lifetime.
A fullerene derivative material and its preparation method are used to synthesize a mixture of monosubstituted or reasonably proportioned fullerene derivatives in a single process. This mixture is then used as the electron transport layer in perovskite solar cells to improve solubility and film formation, and enhance intermolecular interactions.
This improves the photoelectric conversion efficiency of perovskite solar cells, reduces production costs, and enhances the stability of the electron transport layer and device performance.
Smart Images

Figure CN118373789B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of fullerene materials and perovskite solar cell technology, specifically relating to a method for preparing a fullerene derivative electron transport material and its application in perovskite solar cells. Background Technology
[0002] Organic-inorganic hybrid halide perovskite solar cells possess advantages such as high photoelectric conversion efficiency, low manufacturing cost, and low-temperature fabrication capabilities, and have already laid the foundation for preliminary commercial applications. Inverse perovskite solar cells, due to their excellent operational stability, low hysteresis, and ability to be processed using low-temperature solution methods, have shown promising market prospects.
[0003] Currently, the fullerene electron transport materials mainly used in inverted perovskite solar cells include C 60 [6,6]phenyl-C 61 Isomethyl butyrate (PCBM), etc. Among them, PCBM has become one of the most widely used electron transport layer materials due to its energy level being well matched with that of conventional inverted perovskite solar cells with a band gap (1.53~1.55eV) and its advantages such as solution preparation. However, PCBM still has the following limitations: (1) PCBM has limited solubility in orthogonal solvents, resulting in highly disordered energy on the perovskite layer; (2) Insufficient passivation effect hinders device performance; (3) Weak intermolecular interactions, disordered orientation, weak adhesion to the perovskite surface, and unstable morphology under continuous light or heating, leading to reduced device lifetime. Therefore, developing fullerene electron transport materials with good film-forming properties, strong passivation ability, and long-term stability is one of the keys to the development of inverted perovskite solar cells. Summary of the Invention
[0004] The purpose of this invention is to provide a fullerene derivative electron transport material and its preparation method. This material exhibits excellent solubility and film-forming properties, which helps to improve the electron extraction and transport capabilities in devices, thereby enhancing the photoelectric conversion efficiency of perovskite solar cells.
[0005] In addition, monosubstituted fullerene derivatives or mixtures of fullerenes, monosubstituted fullerene derivatives and disubstituted fullerene derivatives in reasonable proportions can be obtained through a single synthesis, which can be directly applied to the electron transport layer of perovskite solar cells, eliminating the need for separate purification steps of each material and saving production costs.
[0006] Another object of the present invention is to provide the application of the above-mentioned fullerene derivative electron transport material in the preparation of perovskite solar cells.
[0007] The third objective of this invention is to provide a method for preparing perovskite solar cells that is simple, has controllable parameters, and is suitable for large-scale industrial production.
[0008] The fourth objective of this invention is to provide a perovskite solar cell that uses the fullerene derivatives of this invention as an electron transport layer, thereby improving the photoelectric conversion efficiency of the solar cell.
[0009] To achieve the above objectives, the present invention adopts the following technical solution:
[0010] This invention provides a fullerene derivative I and its preparation method.
[0011] Its chemical structural formula is:
[0012]
[0013] Where F is selected from C 60 C 70 Or C 84 C is preferred. 60 n = 1 to 6, preferably n = 1 or n = 2.
[0014] R1 is selected from straight-chain or branched alkoxy groups having at least one H atom substituted by an oxygen heterocycle, comprising 1 to 14 carbon atoms. Preferably, it is selected from...
[0015]
[0016] R2 is selected from H atoms, straight-chain or branched alkoxy groups having 1 to 14 carbon atoms, or straight-chain or branched alkoxy groups having 1 to 14 carbon atoms where at least one H atom is replaced by an oxygen heterocycle. Preferably, it is selected from -H, -CH3, -CH2CH3, -(CH2)2CH3, -(CH2)3CH3, -OCH3, or -O(CH2). n CH3, -OCH(CH3)2, -O(CH2) n CH(CH3)2、
[0017] The preparation method of the above fullerene derivatives is as follows:
[0018]
[0019] (1) Dissolve the corresponding compound P1 and formaldehyde in the first solvent in a reaction flask, add hydrogen bromide solution diluted with the first solvent, and react at room temperature for 12-24 h to obtain compound P2.
[0020] (2) Compound P2 was reacted with fullerene, potassium iodide and 18-crown ether-6 in a second solvent to obtain fullerene derivative I.
[0021] The above preparation method also has the following feature: the first solvent is selected from acetic acid, ethanol or dichloromethane, preferably acetic acid.
[0022] The above preparation method also has the following feature: the second solvent is selected from one of chlorobenzene, o-dichlorobenzene, p-dichlorobenzene, m-dichlorobenzene, and toluene, preferably toluene.
[0023] The present invention further provides the application of the fullerene derivative electron transport material in the preparation of perovskite solar cells.
[0024] This invention provides an inverted perovskite solar cell, comprising, in sequence, an FTO conductive substrate, a hole transport layer, a perovskite active layer, an electron transport layer, a buffer layer, and a metal electrode; the electron transport layer comprises the fullerene derivative described in the above technical solution.
[0025] The fabrication method of the above perovskite solar cells is as follows:
[0026] In this invention, there are no special provisions regarding the FTO conductive substrate used in the fabrication of inverted perovskite solar cells; any FTO conductive substrate well-known to those skilled in the art for fabricating solar cells can be used. Preferred cleaning conditions for the FTO conductive substrate are as follows: The cleaning step includes sequential ultrasonic cleaning with deionized water, isopropanol, and ethanol, followed by ultraviolet ozone cleaning to obtain a pretreated FTO conductive substrate. In this invention, the ultrasonic cleaning time for each reagent is independently 10–30 min, preferably 20 min; the ultraviolet ozone cleaning time is 10–30 min, preferably 15 min.
[0027] The inverted perovskite solar cell of this invention includes a hole transport layer on an FTO substrate. In this invention, the hole transport layer is [2-(3,6-dimethoxy-9H-carbazole-9-yl)ethyl]phosphonic acid (MeO-2PACz). The concentration of the MeO-2PACz ethanol solution is preferably 0.2–1 mg / mL, more preferably 0.5 mg / mL. This invention does not specify a particular method for preparing the hole transport layer; any preparation method well-known to those skilled in the art can be used.
[0028] The perovskite active layer in this invention is a mixture of methylamine hydrobromide, methylamine hydrochloride, formamidinium hydroiodide, lead bromide, cesium iodide, and lead iodide, dissolved to obtain a perovskite active solution. After filtration, this solution is spin-coated onto the surface of the hole transport layer to obtain the perovskite active layer. Preferably, the perovskite active solution is filtered before spin-coating. The filter screen pore size is preferably 0.10–0.45 μm, more preferably 0.22 μm.
[0029] In this invention, the electron transport layer of the perovskite is a fullerene derivative, and the selected solvent is chlorobenzene, which is prepared as a chlorobenzene solution and then spin-coated. In this invention, the concentration of the electron transport layer solution is preferably 10–30 mg / mL, more preferably 20 mg / mL.
[0030] The inverted perovskite solar cell of this invention includes a buffer layer on the surface of the electron transport layer. In this invention, the buffer layer is preferably tin oxide (ALD-SnO2) deposited by atomic layer deposition. In this invention, the ALD-SnO2 deposition thickness is preferably 10–20 nm, more preferably 15 nm.
[0031] The inverted perovskite solar cell of this invention includes a metallic silver electrode on the surface of the buffer layer. In this invention, the thickness of the silver electrode is 80–100 nm, more preferably 95 nm. In this invention, the silver electrode is prepared by vacuum thermal evaporation deposition, with a vacuum level of 5.5 × 10⁻⁶. -4 Pa.
[0032] The beneficial effects of this invention are as follows:
[0033] (1) The fullerene derivatives provided by the present invention have good solubility and film-forming properties, and can be used as electron transport layers in solar cell devices to improve the photoelectric conversion efficiency of the corresponding perovskite solar cells.
[0034] (2) Monosubstituted fullerene derivatives or a mixture of fullerenes, monosubstituted fullerene derivatives and disubstituted fullerene derivatives in a reasonable ratio can be obtained by one synthesis. When applied to the electron transport layer of perovskite solar cells, it can not only improve the efficiency of the device, but also save the separation and purification steps of each material and save production costs. Attached Figure Description
[0035] Figure 1 MALDI-TOF-MS image of F30;
[0036] Figure 2 This is a schematic diagram of an inverted perovskite solar cell structure.
[0037] Figure 3JV curves of the inverted perovskite solar cells described in Examples 1-4 and Comparative Example 1;
[0038] Figure 4 For the application of the inverse perovskite solar cells described in Examples 1-4 and Comparative Example 1, V OC Statistical chart;
[0039] Figure 5 For the application of the inverse perovskite solar cells described in Examples 1-4 and Comparative Example 1, J SC Statistical chart;
[0040] Figure 6 FF statistics of the inverted perovskite solar cells described in Examples 1-4 and Comparative Example 1;
[0041] Figure 7 PCE statistics for the inverted perovskite solar cells described in Examples 1-4 and Comparative Example 1. Detailed Implementation
[0042] To make the content of this invention easier to understand, the technical solution of this invention will be further described below with reference to specific embodiments, but this invention is not limited thereto.
[0043] Unless otherwise specified in the examples, the procedures should be performed under standard conditions or conditions recommended by the manufacturer. Reagents or instruments whose manufacturers are not specified are all commercially available products.
[0044] Example 1
[0045] The preparation route and method for a fullerene derivative F30 are as follows:
[0046]
[0047] Benzoic acid (compound a1, 1221.2 mg, 10 mmol) and formaldehyde (750.8 mg, 25 mmol) were dissolved in acetic acid (50 mL), and hydrobromic acid (2427.3 mg, 30 mmol) dissolved in acetic acid was added dropwise. The reaction was allowed to proceed at room temperature for 24 h, and the precipitate formed during the reaction was collected to give product a2 (1693.4 mg, 5.5 mmol), with a yield of 55%. Compound a2 (1539.5 mg, 5 mmol), dicyclohexylcarbodiimide (1031.7 mg, 5 mmol), and 4-dimethylaminopyridine (61.0 mg, 0.5 mmol) were dissolved in N,N-dimethylformamide (50 mL), and 3-methyl-3-oxetane-methanol (510.4 mg, 5 mmol) was added. The reaction was allowed to proceed at room temperature for 24 h, and column chromatography was used to give compound a3 (1666.0 mg, 4.25 mmol), with a yield of 85%. Take compound a3 (544.0 mg, 1.39 mmol) and C 60 Dissolved in toluene (1000 mg, 1.39 mmol), potassium iodide (115.2 mg, 0.69 mmol) and 18-crown ether-6 (91.7 mg, 0.35 mmol) were added, and the mixture was refluxed for 24 h. After removing the solvent, column chromatography was used to give the brownish-red product F30 (766.3 mg, 0.80 mmol), with a yield of 58%.
[0048] Example 2
[0049] Preparation of a mixture F30-1, the mixture comprising C 60 Monosubstituted fullerene derivative F30 and disubstituted fullerene derivative FB-30, and C 60 The molar percentages of F30:FB-30 are 33%:47%:20%. The reaction route and preparation method are as follows:
[0050]
[0051] Take compound a3 (544.0 mg, 1.39 mmol) prepared in Example 1 and C 60 (1000 mg, 1.39 mmol) was dissolved in toluene, and potassium iodide (115.2 mg, 0.69 mmol) and 18-crown ether-6 (91.7 mg, 0.35 mmol) were added. The mixture was refluxed for 16 h, and after removing the solvent, column chromatography was used to obtain unreacted C. 60 (310.0 mg, 0.43 mmol), brownish-red product F30 (583.7 mg, 0.61 mmol), brown product FB-30 (308.9 mg, 0.26 mmol), C 60 The molar percentages of :F30:FB-30 are 33%:47%:20%. [The following appears to be a separate, unrelated sentence:] [The product] contains the above C... 60A mixture of F30 and FB-30 is designated as F30-1, with a yield of 94%.
[0052] Example 3
[0053] Preparation of a mixture F30-2, the mixture comprising C 60 Monosubstituted fullerene derivative F30 and disubstituted fullerene derivative FB-30, and C 60 The molar percentages of F30:FB-30 are 33%:47%:20%. The preparation method is as follows:
[0054] Take compound a3 (652.8 mg, 1.67 mmol) prepared in Example 1 and C 60 (1000 mg, 1.39 mmol) was dissolved in toluene, and potassium iodide (230.4 mg, 1.39 mmol) and 18-crown ether-6 (366.8 mg, 1.39 mmol) were added. The mixture was refluxed for 24 h. After removing the solvent, column chromatography was used to obtain unreacted C. 60 (179.9 mg, 0.25 mmol), brownish-red product F30 (594.5 mg, 0.62 mmol), brown product FB-30 (443.6 mg, 0.37 mmol), C 60 The molar percentage of :F30:FB-30 is 20%:50%:30%. This will contain the above C... 60 A mixture of F30 and FB-30 is designated as F30-2, with a yield of 90%.
[0055] Example 4
[0056] Preparation of a mixture F30-3, the mixture comprising C 60 Monosubstituted fullerene derivative F30 and disubstituted fullerene derivative FB-30, and C 60 The molar percentage of F30:FB-30 is 15%:45%:40%. The preparation method is as follows:
[0057] Compound a3 (870.4 mg, 2.22 mmol) prepared in Example 1 and C were taken. 60 (1000 mg, 1.39 mmol) was dissolved in toluene, and potassium iodide (460.7 mg, 2.78 mmol) and 18-crown ether-6 (733.6 mg, 2.78 mmol) were added. The mixture was refluxed for 24 h. After removing the solvent, column chromatography was used to obtain unreacted C. 60 (131.9 mg, 0.18 mmol), brownish-red product F30 (523.2 mg, 0.55 mmol), brown product FB-30 (578.4 mg, 0.49 mmol), C 60The molar percentages of F30:FB-30 are 15%:45%:40%. [The following appears to be a separate, unrelated sentence:] [The product / service] contains the above C... 60 A mixture of F30 and FB-30 is designated as F30-3, with a yield of 88%.
[0058] Application Example 1
[0059] The specific steps for fabricating an inverted perovskite solar cell with the structure FTO / SAM / perovskite / F30 / ALD-SnO2 / Ag are as follows:
[0060] Cleaning the FTO substrate: The FTO substrate was ultrasonically cleaned with deionized water, isopropanol and ethanol for 20 min respectively, and then cleaned with ultraviolet ozone for 15 min after cleaning to obtain the pretreated FTO substrate.
[0061] Spin-coating hole transport layer: MeO-2PACz(SAM) was spin-coated onto a pretreated FTO substrate. After spin-coating, the substrate was placed at 100°C and annealed for 10 min.
[0062] Preparation of the perovskite active layer: A perovskite active solution with a concentration of 1.46 mol / L was prepared, wherein the molar ratio of lead iodide, formamidinium hydroiodate, lead bromide, methylamine hydrochloride, cesium iodide, and methylamine hydrobromide was (0.95:0.9:0.05:0.2:0.05:0.05), and the solvent was a mixed polar solvent of DMF:DMSO (volume ratio 4:1). The solution was stirred at 60 °C for 2 h to obtain the perovskite active solution. The perovskite active solution was filtered through a polytetrafluoroethylene filter with a pore size of 0.22 μm to obtain a perovskite spin-coating solution. 60 μL of the perovskite spin-coating solution was dropped onto the hole transport layer. After adding anhydrous anisole to the perovskite spin-coating solution, the spin-coated substrate was annealed at 100 °C for 30 min to obtain the perovskite active layer.
[0063] Preparation of electron transport layer: Prepare a 20 mg / mL solution of the fullerene derivative chlorobenzene of the present invention, spin-coat it onto the above perovskite active layer, place the spin-coated substrate at 100°C and anneal for 10 min to obtain an electron transport layer of about 30 nm on the perovskite active layer.
[0064] Preparation of the buffer layer: The substrate obtained above was transferred to the ALD system, and 15 nm of SnO2 was deposited while maintaining the substrate temperature at 85 °C.
[0065] Electrode fabrication: The substrate is placed in a vacuum evaporation chamber, and the vacuum level is increased to 5.5 × 10⁻⁶. -4 After Pa, metallic silver (95 nm thick) is deposited on the buffer layer to obtain the structure of an inverted perovskite solar cell as shown below. Figure 2 As shown, it is denoted as F30.
[0066] Application Example 2
[0067] An inverted perovskite solar cell with the structure FTO / SAM / perovskite / F30-1 / ALD-SnO2 / Ag was prepared according to the preparation method described in Application Example 1, denoted as F30-1, with the only difference being that the electron transport layer is a mixture of fullerene derivatives, F30-1.
[0068] Application Example 3
[0069] An inverted perovskite solar cell with the structure FTO / SAM / perovskite / F30-2 / ALD-SnO2 / Ag was prepared according to the preparation method described in Application Example 1. It is denoted as F30-2, except that the electron transport layer is a mixture of fullerene derivatives, F30-2.
[0070] Application Example 4
[0071] An inverted perovskite solar cell with the structure FTO / SAM / perovskite / F30-3 / ALD-SnO2 / Ag was prepared according to the preparation method described in Application Example 1, denoted as F30-3, except that the electron transport layer is a mixture of fullerene derivatives F30-3.
[0072] Comparative Example 1
[0073] An inverted perovskite solar cell with the structure FTO / SAM / perovskite / PCBM / ALD-SnO2 / Ag was prepared according to the preparation method described in Application Example 1, denoted as PCBM, except that the electron transport layer is PCBM.
[0074] Test Example 1
[0075] The photoelectric conversion efficiency of the inverted perovskite solar cells described in Application Examples 1-4 and Comparative Example 1 was tested, and the results are shown in the figure below.
[0076] Figure 3 JV curves for inverted perovskite solar cells used in Examples 1-4 and Comparative Example 1; Figure 4 For the V of the inverted perovskite solar cells used in Examples 1-4 and Comparative Example 1 OC Statistical chart; Figure 5 J is used in the inverse perovskite solar cells of Examples 1-4 and Comparative Example 1. SC Statistical chart; Figure 6 FF statistics for inverted perovskite solar cells used in Examples 1-4 and Comparative Example 1; Figure 7 The PCE statistics are shown in Table 1 for the inverted perovskite solar cells used in Examples 1-4 and Comparative Example 1. The photoelectric performance parameters of each inverted perovskite solar cell in Examples 1-4 and Comparative Example 1 are shown in Table 1.
[0077] Table 1. Photoelectric performance parameters of the best devices for each type of inverted perovskite solar cell.
[0078]
[0079] from Figures 3-7 As shown in Table 1, using F30 in Example 1 as the electron transport layer of an inverted perovskite solar cell, the device exhibits better open-circuit voltage, short-circuit current, fill factor, and efficiency than Comparative Example 1. This indicates that the fullerene derivative has a more ordered molecular arrangement, improving its electron transport capability and the passivation effect of functional groups on perovskite defects, reducing open-circuit voltage loss, increasing the fill factor, and improving the photoelectric conversion efficiency of the inverted perovskite solar cell. Using mixed fullerene derivatives in Examples 2-4 as the electron transport layer of inverted perovskite solar cells, the devices exhibit better short-circuit current and fill factor than in Example 1. This indicates that in the mixed fullerene derivatives, the disubstituted fullerene derivatives have a stronger interaction with the perovskite, more effectively passivating perovskite active layer defects, resulting in lower interfacial open-circuit voltage loss, improved stability of the electron transport layer, and C... 60 Enhancing the charge extraction capability of the electron transport layer improves the photoelectric conversion efficiency of inverted perovskite solar cells.
[0080] The above description is only a preferred embodiment of the present invention. All equivalent changes and modifications made within the scope of the claims of the present invention should be included in the scope of the present invention.
Claims
1. A fullerene derivative, characterized by: The structure is as follows: , wherein F is a fullerene C 60 , C 70 , C 84 ; n = 1-6; R1is one of , , ; R2 is one of -H, -CH3, -CH2CH3, -(CH2)2CH3, -(CH2)3CH3, -OCH3, or -OCH(CH3)2.
2. A method of preparing the fullerene derivative according to claim 1, characterized by: Includes the following steps: ; (1) Compound P1, formaldehyde, hydrogen bromide and the first solvent were mixed and reacted at room temperature for 12-24 h to obtain compound P2; (2) Compound P2, fullerene dissolved in a second solvent, potassium iodide and 18-crown ether-6 are mixed and reacted for 12-24 h to obtain the fullerene derivative I.
3. The method of claim 2, wherein: The first solvent is one of acetic acid, ethanol, and dichloromethane.
4. The method of claim 2, wherein: The second solvent is one of chlorobenzene, o-dichlorobenzene, p-dichlorobenzene, m-dichlorobenzene, and toluene.
5. The application of a fullerene derivative as described in claim 1 in the preparation of an electron transport layer for an inverted perovskite solar cell.
Citation Information
Patent Citations
Fullerene derivative and application of fullerene derivative in perovskite solar cells
CN106380380A
Polymer / fullerene formations and their use in electronic / photonic devices
US20160322575A1