A process for preparing semiconductor silicon wafer for back contact solar cells

By using N-type silicon wafers with high resistivity in back-contact solar cells and adopting simplified preparation processes to form uniform diffusion layers and passivation layers, the problems of PID effect and high cost are solved, and high-efficiency photoelectric conversion efficiency and low cost production.

CN118380515BActive Publication Date: 2024-10-22JIANGSU FUTULA NEW ENERGY GRP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410816665.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-24
Publication Date
2024-10-22
Estimated Expiration
2044-06-24

AI Technical Summary

Technical Problem

Back-contact solar cells have a potential-induced decay (PID) effect in N-type solar cells, which leads to a decline in photoelectric conversion efficiency. The production process is complex, resulting in high costs and difficulty in industrial production.

Method used

An N-type silicon wafer with a resistivity of 15~20Ω·cm is used as the base material, and the steps are followed by surface cleaning of the silicon wafer, phosphorus diffusion, silicon nitride mask deposition, laser ablation, boron diffusion and double-sided deposition of silicon nitride film. , forming a uniform diffusion layer and passivation layer, simplifying the process, reducing costs, and preventing PID effects.

Benefits of technology

It improves the photoelectric conversion efficiency of back-contact solar cells, reduces production costs, ensures efficient cell performance, and effectively prevents potential-induced attenuation effects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118380515B_ABST
    Figure CN118380515B_ABST
Patent Text Reader

Abstract

The present invention proposes a preparation process of a semiconductor silicon wafer for preparing a back-contact solar cell. The resistivity of the silicon wafer substrate material is 15-20Ω·cm. The preparation process includes the steps of: cleaning and texturing the silicon wafer surface, phosphorus diffusion, silicon nitride mask, laser ablation, secondary cleaning, diffusion of boron tribromide on both sides of the silicon wafer, and double-sided deposition of silicon nitride film. The preparation process of the semiconductor silicon wafer of the present invention forms a uniform diffusion layer on the front surface of the silicon wafer by light doping; synchronous diffusion forms the front surface and back emitters on the N-type silicon substrate, and performs boron diffusion in a high-temperature oxygen atmosphere to form a borosilicate glass layer and a SiO2 layer as a passivation layer, eliminating the oxidation and passivation steps of the existing process and simplifying the process flow; selecting a silicon wafer material with a high resistivity, and depositing a SiNx film and SiO2 on the front surface of the battery to form a laminated passivation layer, which can effectively play an anti-PID effect; the prepared battery has a relatively large open circuit voltage and short circuit current, ensuring a high photoelectric conversion efficiency of the back-contact solar cell.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of solar photovoltaic power generation, and in particular to a process for preparing a semiconductor silicon wafer for preparing a back-contact solar cell. The solar cell prepared by the process has high conversion efficiency and low process cost. Background Art

[0002] The photovoltaic power generation system is a power generation system that directly converts solar energy into electrical energy. It can take into account both economic development and ecological protection while generating clean electricity. It is currently widely used in a variety of scenarios. It is one of the important clean energy sources to replace traditional fossil energy and has broad development prospects.

[0003] Photovoltaic power generation system is based on photovoltaic modules. The power generation units are connected by cables to form a module array. Then, the electricity generated by the photovoltaic modules is directly provided to the power load or connected to the power grid through branch lines, busbars, and DC / AC conversion. Since crystalline silicon solar cells and module technologies are the most mature and low-cost, and with the continuous improvement of technology and processes, the photoelectric conversion efficiency of crystalline silicon modules is getting higher and higher, so in the current photovoltaic power generation system, crystalline silicon modules are still the main type of modules used. Photovoltaic cells (or solar cells) are the main components of photovoltaic modules. The power generation efficiency of photovoltaic power generation systems is mainly determined by the photoelectric conversion efficiency of photovoltaic cells. For photovoltaic cells, increasing the effective light-receiving area of ​​the cell is always one of the important factors to improve the photoelectric conversion efficiency of photovoltaic cells. Since the electrode structure of back-contact solar cells is on the backlight side of the cell, there is no electrode shielding on the light-facing side. Therefore, it has higher short-circuit current and photoelectric conversion efficiency, and is one of the important development directions of high-efficiency solar cells. Compared with traditional crystalline silicon cells, the manufacturing process of back-contact solar cells is more complicated, and it uses processes such as photolithography, electroplating, and evaporation, resulting in higher battery costs and not conducive to market promotion. Therefore, how to simplify the preparation process, optimize process parameters, reduce production costs, and ensure high photoelectric conversion efficiency is a topic that needs to be continuously studied in the industrial production of back-contact solar cells.

[0004] In addition, the potential induced degradation (PID) effect was first discovered in N-type back-contact solar cells, that is, when the N-type solar cell generates a positive potential to the ground, its output power will continue to decline, which shows that the influence of the potential on the base material of the solar cell leads to the decline of the solar cell efficiency. The base material of the N-type solar cell is an N-type silicon wafer, and a layer of silicon nitride film and silicon oxide film are deposited on the surface of the silicon wafer, which is mainly to achieve the effect of anti-reflection passivation. When the N-type solar cell / cell module generates a positive potential to the ground, due to the grounding of the metal frame of the module, a high voltage is generated between the solar cell and the metal frame, which will form a leakage current from the solar cell through the frame to the ground, and induce negative charges in the silicon nitride film. When the density of negative charges gradually increases and eventually exceeds the density of the original positive charge of the film, it will cause the energy band to bend upward, attracting photogenerated minority carriers to the surface, exacerbating the surface recombination of minority carriers. Due to the large ratio of the surface area (effective light receiving area) to the volume of the back-contact solar cell, the surface recombination will be more serious, which will significantly reduce the minority carrier lifetime and the open circuit voltage of the battery, thereby affecting the conversion efficiency of the battery. The performance of solar cells is mainly determined by the semiconductor silicon wafers used to make the cells. Therefore, how to improve the photoelectric conversion efficiency of back-contact solar cells and significantly reduce or avoid the potential induced degradation effect of the cells are issues that require special attention during silicon wafer processing. Summary of the invention

[0005] The purpose of the present invention is to address the problems in the existing back-contact solar cell applications and to propose a preparation process for semiconductor silicon wafers for back-contact solar cells, which can reduce production costs, ensure that the solar cells prepared by the process have high photoelectric conversion efficiency and can effectively prevent the PID effect.

[0006] To achieve the above object, the present invention adopts the following technical solutions:

[0007] A preparation process for a semiconductor silicon wafer for a back-contact solar cell, wherein the substrate material of the solar cell is an N-type silicon wafer with a resistivity of 15-20Ω·cm, and the preparation process comprises the following steps:

[0008] S1. Cleaning and texturing of the damaged layer on the silicon wafer surface: The cut silicon wafer is cleaned in ozone water, and then the surface is corroded and texturized with an alkaline solution with a concentration of about 20% to form a velvet structure on the surface of the silicon wafer;

[0009] S2. Phosphorus diffusion: The pressure in the diffusion furnace is set at 10~25Kpa. The reaction temperature is first controlled at about 795℃. A mixed gas of N2 and O2 carrying POCl3 is pre-deposited on the surface of the silicon wafer to form a phosphorus silicon glass layer. The deposition reaction time is controlled at about 15 minutes. Then the temperature is raised to about 945℃. The reaction time does not exceed 15 minutes. At high temperature, the phosphorus dopant is diffused into the silicon wafer to form a back field layer on the surface of the silicon wafer.

[0010] S3, depositing a silicon nitride mask and forming a p+ doping window by laser ablation: after phosphorus diffusion, use tubular PECVD to deposit SiNx to form a mask layer, and then use high-energy laser ablation to form a specific pattern on the back of the battery according to the designed pattern, and etch the SiNx film formed in the step to form a p+ doping window;

[0011] S4, secondary cleaning, removing the phosphorus dopant on the front surface of the silicon wafer and the n+ doping at the groove on the back surface, to obtain a silicon wafer with a clean surface;

[0012] S5. Use furnace tube thermal diffusion to diffuse boron tribromide on both sides of the silicon wafer after texturing, forming a floating emitter on the front surface and an emitter in the grooved area on the back; the diffusion process is to first deposit a layer of borosilicate glass on the surface of the silicon wafer at 890-910°C, and then perform high-temperature oxidation at 980°C-1000°C in an oxygen atmosphere, and produce a SiO2 layer between the borosilicate glass layer formed in the diffusion process and the doped silicon interface in a high-temperature oxygen atmosphere; then use an HF acid solution corrosion process to thin the borosilicate glass layer formed on the surface of the silicon wafer during the boron diffusion process to make the surface smooth;

[0013] S6. Double-sided deposition of silicon nitride film: SiH4 and NH3 are stimulated to react through tubular PECVD to form SiNx film, and a SiO2 / SiNx stacked passivation anti-reflection film is formed on the surface of the battery.

[0014] More preferably, in the step S1, it also includes a step of cleaning the silicon wafer with ozone water after the textured structure is formed.

[0015] More preferably, in the step S5, the thickness of SiO2 grown in a high temperature oxygen atmosphere is controlled to be 20±3 nm, and the thickness of the borosilicate glass layer is controlled to be 4-8 nm.

[0016] More preferably, in the step S6, the thickness of the formed SiNx and SiO2 stacked passivation layer is controlled to be 50±5 nm.

[0017] More preferably, the preparation process also includes the steps of printing electrodes on the back of the silicon wafer and sintering, first printing the fine grid lines, then printing the insulating paste to form an isolation layer, and finally printing the main grid line paste, the main grid line and the fine grid line have multiple connection points for current collection; then the battery silicon wafer is formed through a sintering process.

[0018] More preferably, the preparation process also includes the steps of quality inspection and efficiency inspection of the prepared solar cell silicon wafers, slicing the cell silicon wafers with local defects into half-cells; and sorting the cell silicon wafers into grades and storing them according to conversion efficiency.

[0019] The beneficial effects of the present invention are as follows: the preparation process of semiconductor silicon wafers for preparing back-contact solar cells forms a uniform diffusion layer on the front surface of the silicon wafer by light doping; the front surface and back emitters are formed by synchronous diffusion on an N-type silicon substrate with a large resistivity, and boron diffusion is used to form a borosilicate glass layer and a SiO2 layer as a passivation layer, thereby eliminating the oxidation and passivation steps of the existing process and simplifying the process flow; a high-resistivity silicon wafer material is selected, and a SiNx film and SiO2 are deposited on the front surface of the battery to form a stacked passivation layer, which can effectively play an anti-PID effect; the prepared battery has a relatively large open-circuit voltage and short-circuit current, thereby ensuring a high photoelectric conversion efficiency of the back-contact solar cell. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 Shown is a process for preparing a semiconductor silicon wafer for a back-contact solar cell according to an embodiment of the present invention. DETAILED DESCRIPTION

[0021] In order to provide a further understanding of the purpose, structure, features, and functions of the present invention, the following detailed description is given in conjunction with the embodiments.

[0022] In the description of the present invention, it should be noted that the terms "center", "up", "down", "left", "right", "vertical", "horizontal", "inside", "outside", etc. indicate directions or positional relationships based on the directions or positional relationships shown in the accompanying drawings. They are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific direction, be constructed and operated in a specific direction. Therefore, they cannot be understood as limitations on the present invention.

[0023] According to the purpose of the present invention, a preparation process of a semiconductor silicon wafer for preparing a back contact solar cell of the present invention uses an N-type Cz silicon wafer as a base material. Since the resistivity of the silicon wafer will have a certain influence on the PID effect of the N-type solar cell, the larger the resistivity, the better the anti-PID effect. Therefore, the silicon wafer base material of the present invention selects a silicon wafer with a resistivity of 15~20Ω·cm. The specific preparation process is as follows:

[0024] S1: Cleaning and texturing of the damaged layer on the surface of silicon wafers: Since a damaged layer will be formed on the surface of the silicon wafer during the cutting process, there are a large number of defects and recombination centers, which have a great impact on the conversion efficiency and yield of the battery. Therefore, it is necessary to clean the surface of the silicon wafer to remove the damaged layer first; specifically, the silicon wafer is first thoroughly cleaned in ozone water, and then the surface is corroded and texturized by an alkaline solution with a concentration of about 20%, such as KOH or NaOH, to form a pyramid structure on the surface of the silicon wafer, namely the so-called velvet structure to increase the light-receiving surface of the silicon wafer; in a preferred embodiment, after the velvet structure is formed, it can be cleaned once with ozone water. Since ozone water is obtained by passing ozone gas into high-purity water, a silicon wafer with a clean surface can be obtained by cleaning with ozone water, which is convenient for subsequent processes;

[0025] S2: Phosphorus diffusion, doping on the surface of the silicon wafer to form a back field (n+ layer). Specifically, the reaction temperature is first controlled at about 795°C, and a mixed gas of N2 and O2 carrying POCl3 is pre-deposited on the surface of the silicon wafer to form a phosphorus silicon glass layer, and the deposition reaction time is controlled at about 15 minutes; then the temperature is raised to about 945°C, and the reaction time does not exceed 15 minutes. At high temperature, the phosphorus dopant is diffused into the silicon wafer to form a back field layer on the surface of the silicon wafer;

[0026] S3: Deposit a silicon nitride mask and form a p+ doping window by laser ablation. Since the emitter and back field of the back-contact solar cell are integrated on the back of the cell, two different dopings need to be performed on the same side of the cell. Therefore, after phosphorus diffusion, SiNx is deposited using tubular PECVD to form a mask layer. Using SiNx as a mask can better block the diffusion of the inversion layer; then high-energy laser ablation is used to form a specific pattern on the back of the cell according to the designed pattern, and the SiNx film formed in the step is etched to form a p+ doping window;

[0027] S4: Secondary cleaning. The cleaning process removes the phosphorus dopant on the front surface of the silicon wafer and the n+ doping at the groove on the back surface, making the silicon wafer surface clean;

[0028] S5: Use furnace tube thermal diffusion to diffuse boron tribromide on both sides of the silicon wafer after texturing, forming a floating emitter on the front surface and an emitter in the grooved area on the back; then use HF acid solution etching process to thin and smooth the silicon glass layer formed on the surface of the silicon wafer during the boron diffusion process;

[0029] S6: Double-sided deposition of silicon nitride film, that is, through tubular PECVD to stimulate SiH4 and NH3 to react to form SiNx film, forming SiO2 / SiNx stacked passivation anti-reflection film on the surface of the silicon wafer.

[0030] In the above step S2, in the traditional silicon wafer processing process of solar cells, in order to form a good ohmic contact between the silicon surface of the emitter region and the metal grid line, and reduce the contact resistance and series resistance loss, the emitter region needs to be heavily doped, but heavy doping is prone to produce large surface recombination and a decrease in short-wave spectrum response, resulting in voltage and current losses. For silicon wafers used for back-contact solar cells, since the metal grid lines are all arranged on the back surface of the silicon wafer and there are no grid lines on the front surface, the preparation process of the present application, for silicon wafers used for back-contact solar cells, adopts a light doping process to reduce the recombination of minority carriers when P diffusion doping is performed on the surface of the silicon wafer. In a preferred embodiment, the pressure in the diffusion furnace is set at 10~25KPa, which can effectively ensure the uniformity and stability of the atmosphere in the furnace and improve the uniformity of diffusion on the surface of the silicon wafer; in addition, the silicon wafer preparation process of the present application adopts a low temperature in the initial stage of deposition, and controls the deposition time to about 15 minutes; a higher temperature and a shorter time are used in the advancement stage to increase the temperature difference between the two times, which can form a better concentration gradient distribution on the surface of the silicon wafer, obtain an ideal doping curve, and obtain a low-concentration emitter junction. The square resistance of the silicon wafer after diffusion can reach more than 180Ω / □; and the overall diffusion time of the silicon wafer can be shortened, thereby improving the production efficiency of the process.

[0031] In the boron tribromide diffusion process of step S5, according to the existing boron tribromide diffusion process, boron tribromide vapor is first mixed with oxygen to form B2O3 and bromine vapor, and then the B2O3 deposited on the surface of the silicon wafer reacts with the underlying silicon substrate layer to form boron atoms and SiO2. At the conventional deposition temperature (about 950°C), the vapor pressure of B2O3 is relatively low, and the liquid B2O3 condenses on the surface of the silicon wafer and inside the diffusion furnace. During the reaction process at this stage, a glass layer rich in B2O3, i.e., a borosilicate glass layer, is formed on the surface of the boron-doped silicon wafer. During the boron diffusion process, if the reaction atmosphere and temperature are not uniform, the thickness of the borosilicate glass layer inside the solar cell will be uneven. If the SiNx layer directly deposited on the borosilicate glass layer is combined with the borosilicate glass layer as a laminated passivation and anti-reflection film, it will lead to differences in properties between different regions of the cell, reducing the short-circuit current of the cell. Therefore, the current process requires first removing the borosilicate glass layer by pickling, growing a passivation layer on the p+ doped surface, and then depositing the SiNx passivation layer. The process is relatively complicated, and the quality of the generated surface passivation layer cannot be guaranteed.

[0032] Therefore, in step S5 of the present invention, the boron diffusion process is to first deposit a layer of borosilicate glass layer on the surface of the silicon wafer at a low temperature (890-910°C), and then perform high temperature (980°C-1000°C) oxidation in an oxygen atmosphere. Under this process condition, the borosilicate glass layer is in a low viscosity state, oxygen and silicon react at the interface between the borosilicate glass layer and the doped silicon, and SiO2 is produced between the borosilicate glass layer and the doped silicon interface. When the concentration of B2O3 in the borosilicate glass layer is lower than a certain concentration, the growth of SiO2 stops, and SiO2 with a certain thickness is formed. Moreover, since the solubility of boron in SiO2 is higher than that of Si, this oxidation process also reduces the surface concentration of boron, forms boron doping in silicon dioxide, and avoids the formation of a surface boron-rich layer. In this oxidation process, the surface borosilicate glass layer will be relatively loose, which will affect the formation of the subsequent passivation layer. Therefore, after the boron is diffused, it is necessary to use HF acid solution to etch away the loose borosilicate glass layer of a certain thickness on the surface. In addition, according to the experimental results, when the thickness of the formed SiOx:B is small, its structure is not dense enough, and there are pores and induced defects. Only when it reaches a certain thickness can the external environment be effectively prevented from affecting the SiOx:B / Si interface. Compared with the thickness of SiO2 formed by the traditional wet chemical process, which generally does not exceed 10nm, the thickness of SiO2 grown in the high-temperature oxygen atmosphere of the present application can reach up to 30nm. Considering the overall performance and manufacturing process of the solar cell, the thickness of SiO2 grown in the high-temperature oxygen atmosphere of the present invention is preferably controlled at about 22nm (20±3nm), and the thickness of the borosilicate glass layer is controlled at 4-8nm. Therefore, compared with the existing diffusion process, the process steps of the present invention are simpler, the cost is low, and the passivation effect is excellent.

[0033] In step S6, the preparation process of the present invention deposits SiNx film and SiO2 on the front surface of the battery to form a laminated passivation layer, and the high-quality Si-SiO2 passivation layer formed in the diffusion process of step S5 can effectively reduce the silicon interface state density. The H atoms introduced when depositing the SiNx passivation anti-reflection film diffuse into the silicon wafer during the sintering process, which can saturate the silicon dangling bonds and passivate the silicon wafer body defects. In addition, the formed SiO2 / SiNx laminated passivation film has a higher fixed positive charge concentration than the single-layer SiO2 film, thereby playing a better field passivation role and can effectively play an anti-PID role. In a preferred embodiment, the thickness of the formed SiNx and SiO2 laminated passivation layer is controlled at 50±5nm.

[0034] Furthermore, the process for preparing semiconductor silicon wafers for preparing back-contact solar cells of the present invention also includes the steps of printing and sintering electrodes on the back of the silicon wafer. Since the electrodes (i.e., grid lines) of the back-contact solar cells are all arranged on the back of the cells, when printing the electrodes, the fine grid lines are printed first, then the insulating paste is printed to form an isolation layer, and finally the main grid line paste is printed, and the main grid line and the fine grid line have multiple connection points for current collection; then the solar cell is formed through a sintering process.

[0035] Furthermore, the process for preparing semiconductor silicon wafers for back-contact solar cells of the present invention also includes quality inspection and efficiency inspection of the cell wafers after the above-mentioned solar cell production is completed. Cell wafers with local defects can be sliced ​​to form half-cells that can be directly used in components; the cell wafers are sorted and stored according to the conversion efficiency.

[0036] The preparation process of semiconductor silicon wafers for preparing back-contact solar cells of the present invention forms a uniform diffusion layer on the front surface of the silicon wafer by light doping; the front surface and back emitters are formed by synchronous diffusion on an N-type silicon substrate with a large resistivity, and boron diffusion is used to form a borosilicate glass layer and a SiO2 layer as a passivation layer, thereby eliminating the oxidation and passivation steps of the existing process and simplifying the process flow; a high-resistivity silicon wafer material is selected, and a SiNx film and SiO2 are deposited on the front surface of the battery to form a laminated passivation layer, which can effectively play an anti-PID effect; the prepared battery has a relatively large open-circuit voltage and short-circuit current, thereby ensuring a high photoelectric conversion efficiency of the back-contact solar cell.

[0037] The present invention has been described by the above-mentioned relevant embodiments, however, the above-mentioned embodiments are only examples for implementing the present invention. It must be pointed out that the disclosed embodiments do not limit the scope of the present invention. On the contrary, changes and modifications made without departing from the spirit and scope of the present invention are all within the scope of patent protection of the present invention.

Claims

1. A process for preparing a semiconductor silicon wafer for a back-contact solar cell, characterized in that: The substrate material of the silicon wafer is an N-type silicon wafer with a resistivity of 15-20Ω·cm, and the preparation process comprises the following steps: S1. Cleaning and texturing of the damaged layer on the silicon wafer surface: The cut silicon wafer is cleaned in ozone water, and then the surface is corroded and texturized by an alkaline solution with a concentration of 20% to form a velvet structure on the surface of the silicon wafer; S2. Phosphorus diffusion: The pressure in the diffusion furnace is set at 10~25Kpa. The reaction temperature is first controlled at 795℃. A mixed gas of N2 and O2 carrying POCl3 is pre-deposited on the surface of the silicon wafer to form a phosphorus silicon glass layer. The deposition reaction time is controlled at 15min. The temperature is then raised to 945℃. The reaction time does not exceed 15min. The phosphorus dopant is diffused into the silicon wafer at high temperature to form a back field layer on the surface of the silicon wafer. S3, depositing a silicon nitride mask and forming a p+ doping window by laser ablation: after phosphorus diffusion, use tubular PECVD to deposit SiNx to form a mask layer, then use high-energy laser ablation to form a pattern on the back of the battery according to the designed pattern, and etch the formed SiNx mask layer to form a p+ doping window; S4, secondary cleaning, removing the phosphorus dopant on the front surface of the silicon wafer and the n+ doping at the groove on the back surface, to obtain a silicon wafer with a clean surface; S5. Use furnace tube thermal diffusion to diffuse boron tribromide on both sides of the silicon wafer after texturing, forming a floating emitter on the front surface and an emitter in the grooved area on the back; the diffusion process is to first deposit a layer of borosilicate glass on the surface of the silicon wafer at 890-910°C, and then perform high-temperature oxidation at 980°C-1000°C in an oxygen atmosphere, and produce a SiO2 layer between the borosilicate glass layer formed in the diffusion process and the doped silicon interface in a high-temperature oxygen atmosphere; then use an HF acid solution etching process to thin the borosilicate glass layer formed on the surface of the silicon wafer during the boron diffusion process to make the surface smooth; and, S6. Double-sided deposition of silicon nitride film: SiH4 and NH3 are stimulated to react through tubular PECVD to form SiNx film, and a SiO2 / SiNx stacked passivation anti-reflection film is formed on the surface of the battery.

2. A process for preparing a semiconductor silicon wafer for preparing a back contact solar cell according to claim 1, characterized in that: In the step S1, there is also a step of cleaning the silicon wafer with ozone water after the textured structure is formed.

3. The process for preparing a semiconductor silicon wafer for preparing a back contact solar cell according to claim 1, characterized in that: In step S5, the thickness of SiO2 grown in a high-temperature oxygen atmosphere is controlled to be 20±3 nm, and the thickness of the borosilicate glass layer is controlled to be 4-8 nm.

4. A process for preparing a semiconductor silicon wafer for preparing a back contact solar cell according to claim 3, characterized in that: In step S6, the thickness of the formed SiNx and SiO2 stacked passivation layer is controlled to be 50±5 nm.

5. A process for preparing a semiconductor silicon wafer for preparing a back contact solar cell according to claim 4, characterized in that: It also includes the steps of printing electrodes and sintering to form solar cells after step S6, specifically: first printing fine grid lines, then printing insulating paste to form an isolation layer, and finally printing main grid line paste, the main grid lines and fine grid lines have multiple connection points for current collection; then the solar cells are formed through a sintering process.

6. A process for preparing a semiconductor silicon wafer for preparing a back contact solar cell according to claim 5, characterized in that: The method also includes the steps of quality inspection and efficiency inspection of the manufactured solar cells, specifically: slicing the cells with local defects into half-cells; and sorting the cells into grades and storing them according to conversion efficiency.