A saturation method for an LPCVD quartz boat and a quartz boat for Topcon batteries

By introducing a mixture of H2, N2O and H2O gases into the acid-washed LPCVD quartz boat for saturation treatment, the problem of EL quartz boat imprinting caused by polycrystalline silicon film deposition was solved, thereby extending the lifespan of the quartz boat, reducing cleaning costs, and improving the efficiency and yield of the solar cells.

CN118388147BActive Publication Date: 2026-11-17DONGFANG HUANSHENG PHOTOVOLTAIC (JIANGSU) CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410487471.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-22
Publication Date
2026-11-17
Estimated Expiration
2044-04-22

AI Technical Summary

Technical Problem

Existing quartz boats suffer from polycrystalline silicon film deposition during LPCVD, resulting in EL quartz boat imprints, poor cleaning performance, shortened boat life, and increased cleaning costs.

Method used

A mixed gas of H2, N2O and H2O is used to saturate the acid-washed LPCVD quartz boat to remove surface diffusion residues, reduce EL quartz boat imprints, and extend the life of the quartz boat. Only acid washing is required during cleaning.

Benefits of technology

It effectively reduces EL quartz boat stains, extends quartz boat life, reduces cleaning costs, and improves cell efficiency and yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118388147B_ABST
    Figure CN118388147B_ABST
Patent Text Reader

Abstract

This invention provides a saturation method for an LPCVD quartz boat and a quartz boat for Topcon batteries, relating to the field of Topcon battery technology. The saturation method includes the following steps: introducing a mixed gas into the acid-washed LPCVD quartz boat for saturation treatment; wherein the mixed gas includes H2, N2O, and H2O. The saturation method for the LPCVD quartz boat of this invention uses a mixed gas of H2, N2O, and H2O for saturation, reducing the amount of silane used and reducing EL quartz boat markings; the saturation method for the LPCVD quartz boat of this invention can extend the lifespan of the quartz boat; the saturation method for the LPCVD quartz boat of this invention eliminates the need for alkaline washing during cleaning, requiring only acid washing, thus reducing cleaning costs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of TOPCon battery technology, and in particular to a saturation method for an LPCVD quartz boat and a quartz boat for Topcon batteries. Background Technology

[0002] TOPCon (Tunnel Oxide Passivated Contact) solar cells are a novel type of silicon solar cell proposed by the Fraunhofer Institute in Germany in 2013. An ultrathin tunneling oxide layer and a highly doped polycrystalline silicon layer are fabricated on the back side, together forming a passivated contact structure that provides excellent surface passivation for the back of the silicon wafer. LPCVD is currently the most mature and widely used technology for fabricating tunneling oxide layers and polycrystalline silicon layers in industrial applications. The common fabrication method is LPCVD ion implantation, where a tunneling oxide layer is first deposited by LPCVD, followed by the deposition of intrinsic polycrystalline silicon in a furnace, and then ion implantation, impurity cleaning, and annealing.

[0003] Quartz boats, used in the semiconductor industry as quartz products, serve as carriers for silicon wafers. Made of pure quartz crystal, they possess extremely high water and corrosion resistance, and are commonly used in critical processes such as oxidation diffusion and LPCVD. Currently, in diffusion and LPCVD equipment production, quartz boats are typically placed within quartz boat holders. LPCVD quartz boats undergo silane deposition together with the holders. After deposition, the silicon wafers are removed from the quartz boat, and new wafers are inserted for the next batch of deposition. Therefore, quartz boats are reused during the production process.

[0004] Therefore, during the polycrystalline silicon deposition process, polycrystalline silicon thin films inevitably deposit onto the carrier boat, and the thickness of the polycrystalline silicon film on the carrier boat increases with the increase of process time and number of cycles. However, current quartz boat cleaning methods are ineffective, increasing the occurrence of EL quartz boat defects and shortening boat life. Furthermore, the need for alkaline washing followed by acid washing increases cleaning costs. EL quartz boat defects refer to defects found in crystalline silicon solar cells during electroluminescence (EL) testing. Inhomogeneous images in the cells indicate defects, such as darker colors at the contact points between the silicon wafer and the boat groove, commonly known as EL boat groove marks or EL quartz boat marks. If these defects exceed a certain area and number, the cell is downgraded, leading to a lower EL yield for crystalline silicon solar cells.

[0005] In view of this, the present invention is hereby proposed. Summary of the Invention

[0006] One objective of this invention is to provide a saturation method for LPCVD quartz boats. The saturation method includes the following steps: introducing a mixed gas into the acid-washed LPCVD quartz boat for saturation treatment. The saturation method of this invention uses a mixed gas of H2, N2O, and H2O to saturate the LPCVD quartz boat, reducing EL boat markings, extending its service life, and requiring only acid washing during cleaning, thus reducing cleaning costs.

[0007] A second objective of this invention is to provide a quartz boat for Topcon batteries, wherein the quartz boat is obtained by saturation treatment of the LPCVD quartz boat as described above.

[0008] In order to achieve the above-mentioned objectives of the present invention, the following technical solution is adopted:

[0009] In a first aspect, the present invention provides a saturation method for an LPCVD quartz boat, the saturation method comprising the following steps:

[0010] A mixed gas was introduced into the acid-washed LPCVD quartz boat for saturation treatment;

[0011] The mixed gas includes H2, N2O and H2O.

[0012] In this invention, the LPCVD quartz boat is saturated with a mixture of H2, N2O and H2O, which reduces the amount of silane used, removes diffusion residues on the surface of the quartz boat, reduces EL quartz boat imprints, extends the life of the quartz boat, and thus improves the efficiency and yield of the solar cells. Furthermore, the quartz boat can be cleaned with acid only, without the need for alkaline cleaning, reducing cleaning costs and preventing damage to the LPCVD quartz boat.

[0013] Preferably, the flow rate ratio of H2, N2O and H2O is (0.5~1.5):(1~3):(0.5~1.5);

[0014] Among them, H2 "0.5~1.5" can be, for example, 0.5, 0.6, 0.8, 1, 1.2, 1.5, etc.;

[0015] Among them, N2O “1~3” can be, for example, 1, 1.5, 1.8, 2, 2.2, 2.5, 3, etc.;

[0016] Furthermore, the preferred ratio of the flow rates of H2, N2O and H2O is 1:2:1.

[0017] Preferably, the N2O gas flow rate is 5 to 20 slm, for example, it can be 5 slm, 6 slm, 8 slm, 10 slm, 12 slm, 14 slm, 16 slm, 18 slm, 20 slm, etc.

[0018] Preferably, the gas flow rate of H2 is 2.5 to 10 slm, for example, it can be 2.5 slm, 3 slm, 4 slm, 5 slm, 6 slm, 7 slm, 8 slm, 9 slm, 10 slm, etc.

[0019] Preferably, the gas flow rate of H2O is 2.5 to 10 slm, for example, it can be 2.5 slm, 3 slm, 4 slm, 5 slm, 6 slm, 7 slm, 8 slm, 9 slm, 10 slm, etc.

[0020] In this invention, by further limiting the flow ratio and absolute flow value of H2, N2O and H2O, the saturation treatment time is reduced, greatly improving efficiency. This is beneficial for reducing quartz boat imprints during normal production and can improve the efficiency and yield of battery cells.

[0021] Preferably, the pressure of the saturation treatment is 300 to 760 torr, for example, it can be 300 torr, 350 torr, 400 torr, 450 torr, 500 torr, 550 torr, 600 torr, 650 torr, 700 torr, 750 torr, 760 torr, etc.

[0022] Preferably, the temperature of the saturation treatment is 590 to 720°C, for example, it can be 590°C, 600°C, 610°C, 620°C, 630°C, 640°C, 650°C, 660°C, 670°C, 680°C, 690°C, 700°C, 710°C, 720°C, etc.

[0023] Preferably, the saturation treatment time is 1 to 2.5 hours, for example, it can be 1 hour, 1.2 hours, 1.4 hours, 1.6 hours, 1.8 hours, 2 hours, 2.2 hours, 2.4 hours, 2.5 hours, etc.

[0024] In this invention, by further limiting the saturation treatment temperature, pressure, and time, the efficiency of the saturation treatment is improved, so as to better remove diffusion residues on the surface of the quartz boat, reduce the generation of quartz boat imprints, and thus improve the efficiency and yield of the solar cells.

[0025] Preferably, the pickling process specifically includes the following steps:

[0026] The LPCVD quartz boat was sequentially acid-washed, water-washed, and dried to obtain the acid-washed LPCVD quartz boat.

[0027] Preferably, the pickling solution used is a mixture of HCl and HF.

[0028] Preferably, the pickling solution comprises, by mass percentage: 0.5-2% HCl, 0.5-2% HF, and the balance being water.

[0029] Based on the total mass of the pickling solution as 100%, the HCl content is 0.5% to 2%, for example, it can be 0.5%, 0.6%, 0.8%, 1%, 1.2%, 1.4%, 1.6%, 1.8%, 2%, etc.

[0030] Based on the total mass of the pickling solution as 100%, the HF content is 0.5% to 2%, for example, it can be 0.5%, 0.6%, 0.8%, 1%, 1.2%, 1.4%, 1.6%, 1.8%, 2%, etc.

[0031] Preferably, the pickling temperature is 20-30℃, for example, 20℃, 22℃, 24℃, 26℃, 28℃, 30℃, etc., and the pickling time is 2-4h, for example, 2h, 2.2h, 2.4h, 2.6h, 2.8h, 3h, 3.2h, 3.4h, 3.6h, 3.8h, 4h, etc.

[0032] Preferably, the water washing temperature is 20-30℃, for example, 20℃, 22℃, 24℃, 26℃, 28℃, 30℃, etc., and the water washing time is 2-4 hours, for example, 2 hours, 2.2 hours, 2.4 hours, 2.6 hours, 2.8 hours, 3 hours, 3.2 hours, 3.4 hours, 3.6 hours, 3.8 hours, 4 hours, etc.

[0033] Preferably, the drying is carried out by blowing, and the gas used for blowing is nitrogen. The flow rate of the gas is 2 to 5 m / s, for example, 2 m / s, 2.5 m / s, 3 m / s, 3.5 m / s, 4 m / s, 4.5 m / s, 5 m / s, etc. The blowing time is 5 to 10 min, for example, 5 min, 5.5 min, 6 min, 6.5 min, 7 min, 7.5 min, 8 min, 8.5 min, 9 min, 9.5 min, 10 min, etc.

[0034] In this invention, the thickness of the polycrystalline silicon thin film on the surface of the LPCVD quartz boat is 0.10 to 0.13 μm, for example, it can be 0.10 μm, 0.105 μm, 0.11 μm, 0.115 μm, 0.12 μm, 0.125 μm, 0.13 μm, etc.

[0035] It should be noted that during the polycrystalline silicon deposition process, polycrystalline silicon films inevitably deposit onto the surface of the LPCVD quartz boat, and as the process time and number of cycles increase, the thickness of the polycrystalline silicon film on the surface of the quartz boat becomes thicker and thicker, generally 0.10 to 0.13 μm; the saturation method for the LPCVD quartz boat described in this invention can effectively solve this problem.

[0036] Secondly, the present invention provides a quartz boat for Topcon batteries, wherein the quartz boat is obtained by saturation treatment of the LPCVD quartz boat described in the first aspect.

[0037] Compared with the prior art, the present invention has the following beneficial effects:

[0038] (1) The saturation method of the LPCVD quartz boat described in this invention uses a mixed gas of H2, N2O and H2O for saturation, which reduces the amount of silane used and reduces EL quartz boat printing.

[0039] (2) The saturation method of the LPCVD quartz boat described in this invention can extend the life of the quartz boat;

[0040] (3) The saturation method of the LPCVD quartz boat described in this invention eliminates the need for alkali washing during the cleaning of the quartz boat, requiring only acid washing, thus reducing cleaning costs. Attached Figure Description

[0041] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.

[0042] Figure 1 This is a process flow diagram of the saturation method for the LPCVD quartz boat described in this invention. Detailed Implementation

[0043] Unless otherwise defined herein, the scientific and technical terms used in conjunction with this invention shall have the meanings commonly understood by one of ordinary skill in the art. The meaning and scope of terms shall be clear; however, in any case of potential ambiguity, the definitions provided herein shall prevail over any dictionary or foreign definitions. In this application, unless otherwise stated, the use of "or" means "and / or". Furthermore, the use of the term "comprising" and other forms is non-limiting.

[0044] It should be noted that specific details are set forth in the following description to provide a full understanding of the invention. However, the invention can be practiced in many ways other than those described herein, and those skilled in the art can make similar extensions without departing from the spirit of the invention. Therefore, the invention is not limited to the specific embodiments disclosed below.

[0045] The technical solution of the present invention will be clearly and completely described below with reference to the embodiments. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0046] The present invention will be further illustrated by the following examples. Unless otherwise specified, the materials in the examples are prepared according to existing methods or purchased directly from the market.

[0047] Example 1

[0048] This embodiment provides a saturation method for LPCVD quartz boats (such as...). Figure 1 As shown in the figure, the saturation method includes the following steps:

[0049] S1, pickling treatment

[0050] The LPCVD quartz boats that have reached the required number of process cycles were acid-washed using a mixture of HCl and HF (2 wt% HCl, 2 wt% HF, and the balance being water) (acid washing temperature: 25℃, time: 180 min); then the acid-washed LPCVD quartz boats were washed with pure water (washing temperature: 25℃, time: 180 min); finally, they were dried with nitrogen gas (gas flow rate: 3 m / s, drying time: 5 min).

[0051] S2, saturation treatment

[0052] A mixed gas, comprising H2, N2O and H2O, is introduced into the acid-washed LPCVD quartz boat for saturation treatment.

[0053] The gas flow rate of H2 was 5 slm, the gas flow rate of N2O was 10 slm, and the gas flow rate of H2O was 5 slm; the saturation treatment pressure was 500 torr, the temperature was 620℃, and the time was 1.5h.

[0054] Example 2

[0055] This embodiment provides a saturation method for an LPCVD quartz boat, the saturation method comprising the following steps:

[0056] S1, pickling treatment

[0057] The LPCVD quartz boats that have reached the required number of process cycles were acid-washed using a mixture of HCl and HF (2 wt% HCl, 2 wt% HF, and the balance being water) (acid washing temperature: 25℃, time: 180 min); then the acid-washed LPCVD quartz boats were washed with pure water (washing temperature: 25℃, time: 180 min); finally, they were dried with nitrogen gas (gas flow rate: 3 m / s, drying time: 5 min).

[0058] S2, saturation treatment

[0059] A mixed gas, comprising H2, N2O and H2O, is introduced into the acid-washed LPCVD quartz boat for saturation treatment.

[0060] The gas flow rate of H2 was 2.5 slm, the gas flow rate of N2O was 5 slm, and the gas flow rate of H2O was 2.5 slm; the saturation treatment pressure was 300 torr, the temperature was 600℃, and the time was 1.8h.

[0061] Example 3

[0062] This embodiment provides a saturation method for an LPCVD quartz boat, the saturation method comprising the following steps:

[0063] S1, pickling treatment

[0064] The LPCVD quartz boats that have reached the required number of process cycles were acid-washed using a mixture of HCl and HF (2 wt% HCl, 2 wt% HF, and the balance being water) (acid washing temperature: 25℃, time: 180 min); then the acid-washed LPCVD quartz boats were washed with pure water (washing temperature: 25℃, time: 180 min); finally, they were dried with nitrogen gas (gas flow rate: 3 m / s, drying time: 5 min).

[0065] S2, saturation treatment

[0066] A mixed gas, comprising H2, N2O and H2O, is introduced into the acid-washed LPCVD quartz boat for saturation treatment.

[0067] The gas flow rate of H2 was 10 slm, the gas flow rate of N2O was 20 slm, and the gas flow rate of H2O was 10 slm; the saturation treatment pressure was 760 torr, the temperature was 640℃, and the time was 1.2h.

[0068] Example 4

[0069] This embodiment provides a saturation method for an LPCVD quartz boat, which differs from Embodiment 1 only in that the gas flow rate of H2 is 5 slm, the gas flow rate of N2O is 5 slm, and the gas flow rate of H2O is 5 slm; the other steps are completely consistent with Embodiment 1.

[0070] Example 5

[0071] This embodiment provides a saturation method for an LPCVD quartz boat, which differs from Embodiment 1 only in that the gas flow rate of H2 is 2 slm, the gas flow rate of N2O is 6 slm, and the gas flow rate of H2O is 2 slm; the other steps are completely consistent with Embodiment 1.

[0072] Comparative Example 1

[0073] This comparative example provides a saturation method for an LPCVD quartz boat, the saturation method comprising the following steps:

[0074] S1, pickling treatment

[0075] The LPCVD quartz boats that have reached the required number of process cycles were acid-washed using a mixture of HCl and HF (2 wt% HCl, 2 wt% HF, and the balance being water) (acid washing temperature: 25℃, time: 180 min); then the acid-washed LPCVD quartz boats were washed with pure water (washing temperature: 25℃, time: 180 min); finally, they were dried with nitrogen gas (gas flow rate: 3 m / s, drying time: 5 min).

[0076] S2, saturation treatment

[0077] A mixed gas, comprising nitrogen, oxygen, and small amounts of nitrogen, is introduced into the acid-washed LPCVD quartz boat for saturation treatment.

[0078] The flow rate of nitrogen was 10 slm, the flow rate of oxygen was 20 slm, and the flow rate of small nitrogen was 10 slm; the saturation treatment pressure was 760 torr, the temperature was 620℃, and the time was 1.5h.

[0079] Comparative Example 2

[0080] This comparative example provides a saturation method for an LPCVD quartz boat, the saturation method comprising the following steps:

[0081] S1, pickling treatment

[0082] The LPCVD quartz boats that have reached the required number of process cycles were acid-washed using a mixture of HCl and HF (2 wt% HCl, 2 wt% HF, and the balance being water) (acid washing temperature: 25℃, time: 180 min); then the acid-washed LPCVD quartz boats were washed with pure water (washing temperature: 25℃, time: 180 min); finally, they were dried with nitrogen gas (gas flow rate: 3 m / s, drying time: 5 min).

[0083] S2, saturation treatment

[0084] A mixed gas, comprising nitrogen, oxygen, and small amounts of nitrogen, is introduced into the acid-washed LPCVD quartz boat for saturation treatment.

[0085] The flow rate of nitrogen was 10 slm, the flow rate of oxygen was 20 slm, and the flow rate of phosphorus oxychloride was 10 slm; the saturation treatment pressure was 760 torr, the temperature was 620℃, and the time was 1.5h.

[0086] Test case

[0087] Test samples: LPCVD quartz boats after saturation treatment provided in Examples 1-5, and LPCVD quartz boats after saturation treatment provided in Comparative Examples 1-2;

[0088] Test method:

[0089] (1) Quartz boat lifespan: the time from when it goes online to when it goes offline;

[0090] (2) EL Quartz Boat Print: Statistical proportions obtained through EL testing;

[0091] The specific test results are shown in Table 1 below:

[0092] Table 1

[0093]

[0094]

[0095] As shown in Table 1, the saturation method for the LPCVD quartz boat described in this invention uses a mixed gas of H2, N2O, and H2O for saturation, reducing the amount of silane used and decreasing EL quartz boat stains; the saturation method for the LPCVD quartz boat described in this invention can extend the life of the quartz boat; the saturation method for the LPCVD quartz boat described in this invention eliminates the need for alkaline washing during quartz boat cleaning, requiring only acid washing, thus reducing cleaning costs.

[0096] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A saturation method for an LPCVD quartz boat, characterized in that, The saturation method includes the following steps: A mixed gas was introduced into the acid-washed LPCVD quartz boat for saturation treatment; The mixed gas includes H2, N2O and H2O; The flow rate ratio of H2, N2O and H2O is (0.5~1.5):(1~3):(0.5~1.5).

2. The saturation method for the LPCVD quartz boat according to claim 1, characterized in that, The flow rates of H2, N2O, and H2O are in the ratio of 1:2:

1.

3. The saturation method for an LPCVD quartz boat according to claim 1 or 2, characterized in that, The flow rate of N2O is 5~20 slm.

4. The saturation method for an LPCVD quartz boat according to claim 1 or 2, characterized in that, The gas flow rate of H2 is 2.5~10 slm.

5. The saturation method for an LPCVD quartz boat according to claim 1 or 2, characterized in that, The gas flow rate of H2O is 2.5~10 slm.

6. The saturation method for an LPCVD quartz boat according to claim 1 or 2, characterized in that, The pressure of the saturation treatment is 300~760 torr.

7. The saturation method for the LPCVD quartz boat according to claim 1 or 2, characterized in that, The saturation treatment temperature is 590~720℃.

8. The saturation method for an LPCVD quartz boat according to claim 1 or 2, characterized in that, The saturation treatment time is 1~2.5 h.

9. The saturation method for an LPCVD quartz boat according to claim 1, characterized in that, The pickling process specifically includes the following steps: The LPCVD quartz boat was sequentially acid-washed, water-washed, and dried to obtain the acid-washed LPCVD quartz boat.

10. The saturation method for the LPCVD quartz boat according to claim 9, characterized in that, The pickling solution used is a mixture of HCl and HF.

11. The saturation method for the LPCVD quartz boat according to claim 10, characterized in that, The pickling solution comprises, by mass percentage: 0.5-2% HCl, 0.5-2% HF, and the balance being water.

12. The saturation method for an LPCVD quartz boat according to claim 9, characterized in that, The pickling temperature is 20~30℃, and the pickling time is 2~4 h.

13. The saturation method for an LPCVD quartz boat according to claim 9, characterized in that, The water washing temperature is 20~30℃, and the washing time is 2~4 minutes.

14. The saturation method for an LPCVD quartz boat according to claim 9, characterized in that, The drying process is carried out by blowing, and the gas used for blowing is nitrogen. The gas flow rate is 2~5 m / s, and the blowing time is 5~10 min.

15. The saturation method for an LPCVD quartz boat according to claim 9, characterized in that, The thickness of the polycrystalline silicon thin film on the surface of the LPCVD quartz boat is 0.10~0.13 μm.

16. A quartz boat for Topcon batteries, characterized in that, The quartz boat is obtained by saturation treatment of the LPCVD quartz boat as described in any one of claims 1 to 15.

Citation Information

Patent Citations

  • Cleaning and saturation process of quartz boat for silicon wafer diffusion

    CN115216848A

  • Thin film depositing method

    JP1997027457A