A high-performance environmentally friendly water-based paint and preparation method thereof
Through the combination of modified montmorillonite and copolymerized acrylate resin, the physical properties of water-based paint are solved, the hardness and anti-corrosion capabilities of the paint film are improved, and consumers' needs for decorative effects and construction techniques are met. , realizing the development of high-performance environmentally friendly water-based paint.
Patent Information
- Application Number
- CN202410611606.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-16
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-05-16
AI Technical Summary
Existing water-based paints have defects in physical properties such as difficulty in construction, water resistance, easy peeling, poor fullness, and poor hardness. They cannot meet consumers' decorative effect and construction technology needs, limiting their market development.
It uses components such as modified montmorillonite, copolymerized acrylate resin, ethylene glycol monobutyl ether and low-toxic alcohol ether solvents, and combines branched polymers and hexachlorocyclotriphosphazene through organic treatment and ultrasonic dispersion technology. A cross-linking reaction is carried out to form a high-performance environmentally friendly water-based paint, which improves the water solubility, flame retardancy, anti-corrosion ability and hardness of the paint film.
It achieves good physical properties of water-based paint, including improving the hardness, anti-corrosion and antibacterial properties of the paint film, reducing construction fire risks and air pollution, improving the working environment, and meeting consumer demands for decorative effects and construction techniques.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of water-based paints, in particular to a high-performance environmentally friendly water-based paint and a preparation method thereof. Background Art
[0002] With the continuous improvement of consumers' environmental awareness, especially the introduction of VOC emission limit standards in various provinces and cities across the country, encouraging the use of non-solvent coatings, it has brought opportunities for the development of environmentally friendly coatings such as water-based paints. The development and market share of water-based coatings are increasing year by year, and there is a trend of acceleration.
[0003] Although water-based paint is superior to traditional paint in environmental performance, in terms of physical properties, water-based paint products have defects such as difficult construction, poor water resistance, easy peeling, poor fullness, and poor hardness. Paint is still the preferred paint for many people to decorate and renovate because of its characteristics such as strong hardness, high fullness of paint film, and tolerance in construction. Only when the defects in physical properties are solved, or even surpass traditional paints, will consumers choose to use water-based paint more actively. It is still difficult to open the market for water-based paints if it only caters to consumers in terms of environmental performance and cannot satisfy consumers in terms of construction technology and decorative effects. This requires water-based paint manufacturers to make technical innovations in the performance of water-based paints. Therefore, this application does not solve the problem that the current water-based paint performance is poor and cannot meet the needs of existing consumers, and provides a high-performance environmentally friendly water-based paint. Summary of the invention
[0004] The purpose of the present invention is to provide a high-performance environmentally friendly water-based paint and a preparation method thereof, so as to solve the problems existing in the prior art.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0006] A high-performance environmentally friendly water-based paint comprises the following components: 5 to 10 parts by weight of modified montmorillonite, 0.1 to 0.5 parts by weight of a leveling agent, 0.1 to 0.6 parts by weight of a curing catalyst, 0.1 to 0.5 parts by weight of a defoamer, 20 to 40 parts by weight of a copolymerized polyacrylate resin, 2 to 10 parts by weight of ethylene glycol monobutyl ether and 40 to 60 parts by weight of deionized water.
[0007] As an optimization, the modified montmorillonite comprises the following preparation steps:
[0008] S1, adding the organic montmorillonite to deionized water 5 to 8 times the mass of the organic montmorillonite, ultrasonicating for 10 to 15 minutes, to prepare an organic montmorillonite suspension; adding a branched polymer 0.2 to 0.3 times the mass of the organic montmorillonite to deionized water 6 to 8 times the mass of the branched polymer, stirring evenly, to prepare a branched polymer aqueous solution; then adding the branched polymer aqueous solution to the organic montmorillonite suspension, stirring for 6 to 8 hours at a temperature of 80°C, filtering, washing with deionized water 2 to 3 times, and drying at a temperature of 110 to 120°C for 1 to 2 hours to prepare a branched montmorillonite;
[0009] S2. Add the branched montmorillonite to formaldehyde in an amount of 8 to 10 times the mass of the branched montmorillonite, then add a 5% sodium hydroxide solution in an amount of 0.02 to 0.05 times the mass of the formaldehyde solution, and react with stirring for 3 to 3.5 hours at a temperature of 60 to 70°C. After the reaction is completed, filter and centrifuge for dehydration, and dry for 4 to 5 hours at a temperature of 80 to 90°C to obtain a dry product; add the dry product to methanol in an amount of 6 to 8 times the mass of the dry product, add an acidic catalyst in an amount of 0.03 to 0.05 times the mass of the dry product while stirring, and react for 2 to 3 hours at a temperature of 45 to 55°C, then add a 5% sodium hydroxide solution in an amount of 0.04 to 0.06 times the mass of the dry product, terminate the reaction, and perform reduced pressure distillation. After the reduced pressure distillation is completed, filter and suck to obtain modified montmorillonite.
[0010] As an optimization, the organic montmorillonite comprises the following preparation steps: adding allyltrimethylammonium bromide to deionized water with a mass of 18 to 20 times that of allyltrimethylammonium bromide, stirring for 1 to 1.5 hours at a temperature of 50 to 60°C and a rotation speed of 600 r / min, adding montmorillonite with a mass of 4 to 5 times that of allyltrimethylammonium bromide after stirring, keeping warm for 4 to 5 hours at a rotation speed of 600 r / min, then ultrasonicating for 0.2 to 0.3 hours, filtering after the ultrasonication, washing the filtered product with deionized water for 3 to 5 times, and drying at a temperature of 80 to 90°C for 4 to 5 hours to obtain the organic montmorillonite.
[0011] As an optimization, the branched polymer comprises the following preparation steps: adding ethylenediamine to methanol with a mass of 0.5 to 0.6 times that of ethylenediamine, and stirring for 2 to 2.5 hours in a light-proof and nitrogen-filled state at a temperature of 0 to 5°C to prepare an ethylenediamine methanol solution; adding hexachlorocyclotriphosphazene to methanol with a mass of 4 to 5 times that of hexachlorocyclotriphosphazene at a temperature of minus 10 to 15°C, and stirring evenly to prepare a hexachlorocyclotriphosphazene methanol solution; and uniformly dropping the hexachlorocyclotriphosphazene methanol solution into an ethylenediamine methanol solution with a mass of 2 to 3 times that of the hexachlorocyclotriphosphazene methanol solution at a temperature of 0 to 5°C, with a dropping time of 20 to 30 minutes. After the dropping is completed, stirring and reacting for 24 to 28 hours at a temperature of 25 to 30°C, filtering after the stirring reaction is completed, vacuum rotary evaporating the filtrate at a temperature of 40 to 50°C, and drying the rotary evaporation product at a temperature of 50 to 60°C for 2 to 3 hours to prepare a branched polymer.
[0012] As an optimization, the leveling agent is water-based coating leveling agent BYK333.
[0013] As an optimization, the curing catalyst is water-based coating catalyst BYK450.
[0014] As an optimization, the defoamer is water-based coating defoamer BYK028.
[0015] As an optimization, the copolymerized polyacrylate resin includes the following preparation steps: adding isopropanol to ethylene glycol diethyl ether in an amount of 1.6 to 1.8 times the mass of isopropanol, mixing and stirring evenly to obtain an ethylene glycol diethyl ether isopropanol solution; weighing methyl methacrylate, methacrylic acid, butyl acrylate and di-tert-amyl peroxide according to a mass ratio, mixing and stirring evenly to obtain a mixed solution; at a temperature of 90 to 100° C. and under nitrogen protection, uniformly adding the mixed solution dropwise to the ethylene glycol diethyl ether isopropanol solution within 3 to 3.5 hours, reacting at a temperature of 90 to 100° C. for 6 to 8 hours after the dropwise addition is completed, cooling to 60 to 70° C. after the reaction is completed, adding triethylamine in an amount of 3 to 5 times the mass of ethylene glycol diethyl ether, stirring evenly to obtain a copolymerized polyacrylate resin.
[0016] As an optimization, the mass ratio of the methyl methacrylate, methacrylic acid, butyl acrylate and di-tert-amyl peroxide is 30:8-10:10-12:2-2.5, and the mass of the methyl methacrylate is 10-12 times that of isopropanol.
[0017] A method for preparing a high-performance environmentally friendly water-based paint as described in any of the above items, comprising weighing modified montmorillonite, a curing catalyst, a defoaming agent, a copolymerized acrylate resin, ethylene glycol monobutyl ether and deionized water in proportion, stirring at a speed of 300 to 400 r / min for 15 minutes, adding a leveling agent, and continuing to stir for 15 minutes to obtain a high-performance environmentally friendly water-based paint.
[0018] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0019] The present invention adopts copolymerized polyacrylate resin as the main body, and adopts methyl methacrylate, methacrylic acid, butyl acrylate and di-tert-amyl peroxide to mix soft and hard monomers, so that the resin has good water solubility and excellent paint film performance, and uses water as solvent, which saves a lot of resources; eliminates the fire hazard during construction; reduces air pollution; only uses a small amount of low-toxic alcohol ether organic solvents, which improves the working environment conditions;
[0020] In addition, the present application uses modified montmorillonite as a filler for water-based paint. On the one hand, since montmorillonite has swelling properties and a unique layered structure, organic molecules can be inserted between its layers after organic treatment. In the present application, allyl trimethyl ammonium bromide is inserted into it through ultrasonic dispersion. Since allyl trimethyl ammonium bromide has the characteristics of a quaternary ammonium salt, the water-based paint has antibacterial ability.
[0021] In the later stage, the organic montmorillonite is grafted with a branched polymer. The branched polymer is used because the branched polymer has more bonding sites, thereby enhancing the overall cross-linking effect, and with hexachlorocyclotriphosphazene as the core, it also gives the water-based paint good flame retardancy; the final modified montmorillonite has many amino sites added thereto, and the present application also etherifies these numerous amino sites to make them the central sites in the later curing process of the water-based paint, which can not only act as a curing catalyst, but also form a surface structure physical barrier centered on montmorillonite, greatly enhancing the anti-corrosion ability of the water-based paint, and the montmorillonite is firmly fixed on the water-based paint through the curing cross-linking process, so that it can achieve sufficient cross-linking reaction at the molecular level, thereby improving the overall performance of the coating. DETAILED DESCRIPTION
[0022] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] In order to more clearly illustrate the method provided by the present invention, the following examples are provided in detail. The raw materials used in the experimental part of the following examples are as follows:
[0024] Table 1 - Raw materials used in the experimental part
[0025]
[0026]
[0027] Example 1
[0028] A high-performance environmentally friendly water-based paint comprises the following components: 5 parts by weight of modified montmorillonite, 0.1 parts by weight of a leveling agent, 0.1 parts by weight of a curing catalyst, 0.1 parts by weight of a defoamer, 20 parts by weight of a copolymerized polyacrylate resin, 2 parts by weight of ethylene glycol monobutyl ether and 40 parts by weight of deionized water.
[0029] The copolymerized polyacrylate resin comprises the following preparation steps:
[0030] Isopropyl alcohol was added to ethylene glycol diethyl ether in an amount of 1.6 times the mass of isopropyl alcohol, and the mixture was stirred evenly to obtain an ethylene glycol diethyl ether isopropyl alcohol solution. The mass of methyl methacrylate was 10 times that of isopropyl alcohol. Methyl methacrylate, methacrylic acid, butyl acrylate and di-tert-amyl peroxide were weighed in a mass ratio of 30:8:10:2, and the mixture was stirred evenly to obtain a mixed solution. At a temperature of 90°C and under nitrogen protection, the mixed solution was evenly added dropwise to the ethylene glycol diethyl ether isopropyl alcohol solution within 3 hours. After the addition was completed, the mixture was reacted at a temperature of 90°C for 6 hours. After the reaction was completed, the mixture was cooled to 60°C, and triethylamine in an amount of 3 times the mass of ethylene glycol diethyl ether was added, and the mixture was stirred evenly to obtain a copolymerized polyacrylate resin.
[0031] Example 2
[0032] A high-performance environmentally friendly water-based paint comprises the following components: 8 parts by weight of modified montmorillonite, 0.1 to 0.5 parts by weight of a leveling agent, 0.4 parts by weight of a curing catalyst, 0.13 parts by weight of a defoamer, 30 parts by weight of a copolymerized polyacrylate resin, 6 parts by weight of ethylene glycol monobutyl ether and 50 parts by weight of deionized water.
[0033] The copolymerized polyacrylate resin comprises the following preparation steps:
[0034] Isopropanol was added to ethylene glycol diethyl ether (1.7 times the mass of isopropanol), and the mixture was stirred evenly to obtain an ethylene glycol diethyl ether isopropanol solution. The mass of methyl methacrylate was 11 times that of isopropanol. Methyl methacrylate, methacrylic acid, butyl acrylate and di-tert-amyl peroxide were weighed in a mass ratio of 30:9:11:2.3, and the mixture was stirred evenly to obtain a mixed solution. At a temperature of 95°C and under nitrogen protection, the mixed solution was evenly added dropwise to the ethylene glycol diethyl ether isopropanol solution within 3.2 hours. After the addition was completed, the mixture was reacted at a temperature of 95°C for 7 hours. After the reaction was completed, the mixture was cooled to 65°C, and triethylamine (4 times the mass of ethylene glycol diethyl ether) was added and stirred evenly to obtain a copolymerized polyacrylate resin.
[0035] Example 3
[0036] A high-performance environmentally friendly water-based paint comprises the following components: 10 parts by weight of modified montmorillonite, 0.5 parts by weight of a leveling agent, 0.6 parts by weight of a curing catalyst, 0.5 parts by weight of a defoamer, 40 parts by weight of a copolymerized polyacrylate resin, 10 parts by weight of ethylene glycol monobutyl ether and 60 parts by weight of deionized water.
[0037] The copolymerized polyacrylate resin comprises the following preparation steps:
[0038] Isopropyl alcohol is added to ethylene glycol diethyl ether in an amount of 1.8 times the mass of isopropyl alcohol, and the mixture is mixed and stirred to obtain an ethylene glycol diethyl ether isopropyl alcohol solution. The mass of methyl methacrylate is 12 times that of isopropyl alcohol, and methyl methacrylate, methacrylic acid, butyl acrylate and di-tert-amyl peroxide are weighed in a mass ratio of 30:10:12:2.5, and the mixture is mixed and stirred to obtain a mixed solution. At a temperature of 100°C and under nitrogen protection, the mixed solution is uniformly added dropwise to the ethylene glycol diethyl ether isopropyl alcohol solution within 3.5 hours. After the addition is completed, the mixture is reacted at a temperature of 100°C for 8 hours. After the reaction is completed, the mixture is cooled to 70°C, and triethylamine in an amount of 5 times the mass of ethylene glycol diethyl ether is added, and the mixture is stirred to obtain a copolymerized polyacrylate resin.
[0039] Example 4
[0040] The modified montmorillonite comprises the following preparation steps:
[0041] S1. Add allyl trimethyl ammonium bromide to deionized water with a mass of 18 times that of allyl trimethyl ammonium bromide, stir for 1 hour at a temperature of 50°C and a rotation speed of 600 r / min, add montmorillonite with a mass of 4 times that of allyl trimethyl ammonium bromide after stirring, keep warm for 4 hours at a rotation speed of 600 r / min, and then ultrasonicate for 0.2 hours. After ultrasonication, filter and wash the filtered product with deionized water for 3 times, and dry at a temperature of 80°C for 4 hours to obtain an organic montmorillonite;
[0042] S2, adding ethylenediamine to methanol with a mass of 0.5 times that of ethylenediamine, under the condition of temperature of 0°C, avoiding light and stirring with nitrogen for 2h to prepare ethylenediamine methanol solution; under the condition of temperature of minus 10°C, adding hexachlorocyclotriphosphazene to methanol with a mass of 4 times that of hexachlorocyclotriphosphazene, stirring evenly to prepare hexachlorocyclotriphosphazene methanol solution; under the condition of temperature of 0°C, adding hexachlorocyclotriphosphazene methanol solution evenly dropwise to ethylenediamine methanol solution with a mass of 2 times that of hexachlorocyclotriphosphazene methanol solution, the dropping time is 20min, after the dropwise addition is completed, stirring the reaction at a temperature of 25°C for 24h, filtering after the stirring reaction is completed, vacuum rotary evaporating the filtrate at a temperature of 40°C, and drying the rotary evaporation product at a temperature of 50°C for 2h to obtain a branched polymer;
[0043] S3, adding the organized montmorillonite to deionized water 5 times the mass of the organized montmorillonite, ultrasonicating for 10 minutes, to prepare an organized montmorillonite suspension; adding a branched polymer 0.2 times the mass of the organized montmorillonite to deionized water 6 times the mass of the branched polymer, stirring evenly, to prepare a branched polymer aqueous solution; then adding the branched polymer aqueous solution to the organized montmorillonite suspension, stirring and reacting at a temperature of 80°C for 6 hours, filtering, washing with deionized water twice, and drying at a temperature of 110°C for 1 hour to prepare a branched montmorillonite;
[0044] S4. Add the branched montmorillonite to formaldehyde in an amount of 8 times the mass of the branched montmorillonite, then add a 5% sodium hydroxide solution in an amount of 0.02 times the mass of the formaldehyde solution, and stir the reaction at a temperature of 60°C for 3 hours. After the reaction is completed, filter and centrifuge for dehydration, and dry at a temperature of 80°C for 4 hours to obtain a dry product; add the dry product to methanol in an amount of 6 times the mass of the dry product, add an acidic catalyst in an amount of 0.03 times the mass of the dry product while stirring, and react at a temperature of 45°C for 2 hours, then add a 5% sodium hydroxide solution in an amount of 0.04 times the mass of the dry product, terminate the reaction, and perform reduced pressure distillation. After the reduced pressure distillation is completed, filter and filter to obtain modified montmorillonite.
[0045] Example 5
[0046] The modified montmorillonite comprises the following preparation steps:
[0047] S1. Add allyl trimethyl ammonium bromide to deionized water with a mass of 19 times that of allyl trimethyl ammonium bromide, stir for 1.2 hours at a temperature of 40°C and a rotation speed of 600 r / min, add montmorillonite with a mass of 4.5 times that of allyl trimethyl ammonium bromide after stirring, keep warm for 4.5 hours at a rotation speed of 600 r / min, and then ultrasonicate for 0.25 hours. After ultrasonication, filter the filtered product, wash it with deionized water 4 times, and dry it at a temperature of 85°C for 4.5 hours to obtain an organic montmorillonite;
[0048] S2, adding ethylenediamine to methanol with a mass of 0.55 times that of ethylenediamine, under the condition of temperature of 3°C, avoiding light and stirring with nitrogen for 2.2h to prepare ethylenediamine methanol solution; under the condition of temperature of minus 13°C, adding hexachlorocyclotriphosphazene to methanol with a mass of 4.5 times that of hexachlorocyclotriphosphazene, stirring evenly to prepare hexachlorocyclotriphosphazene methanol solution; under the condition of temperature of 3°C, adding hexachlorocyclotriphosphazene methanol solution evenly dropwise to ethylenediamine methanol solution with a mass of 2.5 times that of hexachlorocyclotriphosphazene methanol solution, the dropping time is 25min, after the dropwise addition is completed, under the condition of temperature of 28°C, stirring the reaction for 26h, after the stirring reaction is completed, filtering, under the condition of temperature of 45°C, vacuum rotary evaporation of the filtrate, drying the rotary evaporation product at a temperature of 55°C for 2.5h, to obtain a branched polymer;
[0049] S3, adding the organized montmorillonite to deionized water 6 times the mass of the organized montmorillonite, ultrasonicating for 12 minutes, to prepare an organized montmorillonite suspension; adding a branched polymer 0.25 times the mass of the organized montmorillonite to deionized water 7 times the mass of the branched polymer, stirring evenly, to prepare a branched polymer aqueous solution; then adding the branched polymer aqueous solution to the organized montmorillonite suspension, stirring for 7 hours at a temperature of 80°C, filtering, washing with deionized water 3 times, and drying at a temperature of 110°C for 1.5 hours to prepare a branched montmorillonite;
[0050] S4. Add the branched montmorillonite to formaldehyde in an amount of 9 times the mass of the branched montmorillonite, then add a 5% sodium hydroxide solution in an amount of 0.035 times the mass of the formaldehyde solution, and stir the reaction at a temperature of 65°C for 3 hours. After the reaction is completed, filter and centrifuge for dehydration, and dry at a temperature of 90°C for 5 hours to obtain a dry product; add the dry product to methanol in an amount of 7 times the mass of the dry product, and add an acidic catalyst in an amount of 0.04 times the mass of the dry product while stirring. After the reaction is carried out at a temperature of 45°C for 2.5 hours, add a 5% sodium hydroxide solution in an amount of 0.05 times the mass of the dry product, terminate the reaction, and perform reduced pressure distillation. After the reduced pressure distillation is completed, filter and filter to obtain modified montmorillonite.
[0051] Example 6
[0052] The modified montmorillonite comprises the following preparation steps:
[0053] S1. Add allyl trimethyl ammonium bromide to deionized water 20 times the mass of allyl trimethyl ammonium bromide, stir for 1.5 hours at a temperature of 60°C and a speed of 600 r / min, add montmorillonite 5 times the mass of allyl trimethyl ammonium bromide after stirring, keep warm for 5 hours at a speed of 600 r / min, and then ultrasonicate for 0.3 hours. After the ultrasonication is completed, filter and wash the filtered product with deionized water 5 times, and dry at a temperature of 90°C for 5 hours to obtain an organic montmorillonite;
[0054] S2, adding ethylenediamine to methanol with a mass of 0.6 times that of ethylenediamine, at a temperature of 5 ° C, avoiding light and stirring with nitrogen for 2.5 hours to prepare an ethylenediamine methanol solution; at a temperature of minus 15 ° C, adding hexachlorocyclotriphosphazene to methanol with a mass of 5 times that of hexachlorocyclotriphosphazene, stirring evenly, to prepare a hexachlorocyclotriphosphazene methanol solution; at a temperature of 5 ° C, the hexachlorocyclotriphosphazene methanol solution was uniformly added dropwise to the ethylenediamine methanol solution with a mass of 3 times that of the hexachlorocyclotriphosphazene methanol solution, the dropping time was 30 minutes, after the dropwise addition was completed, at a temperature of 30 ° C, stirring the reaction for 28 hours, after the stirring reaction was completed, filtering, at a temperature of 50 ° C, the filtrate was vacuum evaporated, and the rotary evaporated product was dried at a temperature of 60 ° C for 3 hours to obtain a branched polymer;
[0055] S3, adding the organized montmorillonite to 8 times the mass of the organized montmorillonite in deionized water, ultrasonicating for 15 minutes, to prepare an organized montmorillonite suspension; adding a branched polymer of 0.3 times the mass of the organized montmorillonite to 8 times the mass of the branched polymer in deionized water, stirring evenly, to prepare a branched polymer aqueous solution; then adding the branched polymer aqueous solution to the organized montmorillonite suspension, stirring for 8 hours at a temperature of 80°C, filtering, washing with deionized water 3 times, and drying at a temperature of 120°C for 2 hours to prepare a branched montmorillonite;
[0056] S4. Add the branched montmorillonite to formaldehyde in an amount 10 times the mass of the branched montmorillonite, then add a 5% sodium hydroxide solution in an amount 0.05 times the mass of the formaldehyde solution, and react with stirring at a temperature of 70°C for 3.5 hours. After the reaction is completed, filter and centrifuge for dehydration, and dry at a temperature of 90°C for 5 hours to obtain a dry product. Add the dry product to methanol in an amount 8 times the mass of the dry product, add an acidic catalyst in an amount 0.05 times the mass of the dry product while stirring, and react at a temperature of 55°C for 3 hours, then add a 5% sodium hydroxide solution in an amount 0.06 times the mass of the dry product, terminate the reaction, and perform reduced pressure distillation. After the reduced pressure distillation is completed, filter and filter to obtain modified montmorillonite.
[0057] Comparative Example 1
[0058] The only difference from Example 5 is that steps (2), (3) and (4) are not performed.
[0059] Comparative Example 2
[0060] The only difference from Example 5 is that step (4) is not performed.
[0061] Comparative Example 3
[0062] The difference from Example 2 is that the modified montmorillonite therein is the modified montmorillonite in Example 5.
[0063] Comparative Example 4
[0064] The difference from Example 2 is that the modified montmorillonite therein adopts the modified montmorillonite in Comparative Example 1.
[0065] Comparative Example 5
[0066] The difference from Example 2 is that the modified montmorillonite therein adopts the modified montmorillonite in Comparative Example 2.
[0067] Test Example 1
[0068] Sample preparation: The water-based paint prepared in the above comparative examples 3 to 5 was evenly coated on the surface of the tinplate / Q235 carbon steel using a wire rod applicator; after coating, it was placed at room temperature for 15 minutes, and then cured at a temperature of 80°C for 2 hours. The coating thickness was 45 (± 5) μm.
[0069] Water resistance test: refer to GB / T1733-93 standard, place 2 / 3 of the coated test board in a deionized water tank, dry the coated water after 72 hours, and then observe whether the coating loses gloss, bubbles, changes color, wrinkles, falls off, rusts, etc., so as to judge whether it is qualified. Three parallel samples are required, and only those that meet the standard are qualified.
[0070] Salt water resistance test: refer to GB / T1763-79 standard, place 2 / 3 of the coated test board in a container filled with 3% sodium chloride solution, and keep the temperature at 25℃. After 100 hours, remove the salt stains with deionized water and wipe it dry with filter paper. Observe whether the coating has peeling, gloss loss, blistering, discoloration, rust, etc. 3 parallel samples are required, and only those that meet the standard are qualified.
[0071] Acid and alkali resistance test: According to the standard of GB / T9274-88, the coating is placed in a 10% sulfuric acid solution and observed for abnormal conditions after 100 hours. The coating is placed in a 50g / L sodium hydroxide solution and observed for abnormal conditions after 24 hours.
[0072] Referring to the above test method, the test results of chemical properties of water-based paint are shown in Table 1 below;
[0073] Table 1- Experimental data of chemical performance test of water-based paint
[0074]
[0075] It can be seen from the comparative examples 3 to 5 in the above table that when the modified montmorillonite in Example 5 is used, the various chemical performance indicators reach the optimal level, while in comparative example 4, there is a significant decline, which is mainly because the modified montmorillonite used does not play a cross-linking role, and the lack of a curing cross-linking agent leads to a decline in the chemical properties of the final paint film. There is also a partial decline in comparative example 5, which is mainly because the final cross-linking curing effect is poor, and the lack of etherification leads to a lack of a cross-linking agent in the final curing process, resulting in a decline in the performance of the paint film.
[0076] Test Example 2
[0077] Sample preparation: All samples were prepared according to GB1727-92 "General preparation method for paint film".
[0078] Hardness test: According to the "GB / T6739-1996 Coating Pencil Hardness Determination Method", a group of high-grade Chinese brand drawing pencils with different hardness ratings are used to manually determine the pencil hardness of the coating. Place the coating test plate on a horizontal table with the coating fixed upward. Hold the pencil at an angle of about 45°, push about 1 cm on the coating surface at a uniform speed of about 1 cm / s, and scratch the coating. Repeat the scratching 5 times with the pencil of the same hardness rating. If 2 or more scratches do not reach the bottom plate of the sample, use a pencil with a higher hardness rating until the coating is scratched or more. The pencil with a lower hardness rating is the pencil hardness of the coating.
[0079] Impact resistance test: The product of the mass of a falling hammer and the maximum height at which it falls on the sample without causing damage (kg.cm). It is measured according to GB / T1731-93 "Determination of paint film flexibility". The larger the value, the better the impact resistance.
[0080] Adhesion test: Determine according to GB / T9286-1998, ISO2409: 1992. Use a blade to scratch 100 small squares of 1mm×1mm on the paint film sample, stick them with transparent tape, and observe the degree of damage to the paint film to determine the level of paint film adhesion. The results are expressed in 0 to 5 levels, with 0 being the best and 5 being the worst.
[0081] Referring to the above test method, the performance test results are shown in Table 2 below;
[0082] Table 2 - Performance test data
[0083]
[0084]
[0085] From the above table, it can be seen from Examples 3 to 5 that when the modified montmorillonite in Example 5 is used, the hardness is the highest mainly because a cross-linked network is formed at this time, and its overall cross-linking strength is the highest, while the subsequent cross-linking curing degree is weak, so the subsequent performance is not good, which is related to the subsequent impact resistance. The higher the cross-linking curing degree, the stronger the impact resistance. The adhesion is similar to the above situation. It may be mainly because there are more uncross-linked parts, and they are mostly concentrated on the surface of the paint film, which makes it easy to destroy the surface during the bonding process of the transparent tape, resulting in poor performance of the paint film in Examples 4 and 5.
[0086] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A high-performance environmentally friendly water-based paint, characterized in that: The invention comprises the following components: 5 to 10 parts by weight of modified montmorillonite, 0.1 to 0.5 parts by weight of a leveling agent, 0.1 to 0.6 parts by weight of a curing catalyst, 0.1 to 0.5 parts by weight of a defoaming agent, 20 to 40 parts by weight of a copolymerized polyacrylate resin, 2 to 10 parts by weight of ethylene glycol monobutyl ether and 40 to 60 parts by weight of deionized water; The modified montmorillonite comprises the following preparation steps: S1, adding the organic montmorillonite to deionized water 5 to 8 times the mass of the organic montmorillonite, ultrasonicating for 10 to 15 minutes, to prepare an organic montmorillonite suspension; adding a branched polymer 0.2 to 0.3 times the mass of the organic montmorillonite to deionized water 6 to 8 times the mass of the branched polymer, stirring evenly, to prepare a branched polymer aqueous solution; then adding the branched polymer aqueous solution to the organic montmorillonite suspension, stirring for 6 to 8 hours at a temperature of 80°C, filtering, washing with deionized water 2 to 3 times, and drying at a temperature of 110 to 120°C for 1 to 2 hours to prepare a branched montmorillonite; S2, adding the branched montmorillonite to formaldehyde in an amount of 8 to 10 times the mass of the branched montmorillonite, and then adding a 5% sodium hydroxide solution in an amount of 0.02 to 0.05 times the mass of the formaldehyde solution, stirring the reaction at a temperature of 60 to 70°C for 3 to 3.5 hours, filtering and centrifuging for dehydration after the reaction is completed, and drying at a temperature of 80 to 90°C for 4 to 5 hours to obtain a dry product; adding the dry product to methanol in an amount of 6 to 8 times the mass of the dry product, adding an acidic catalyst in an amount of 0.03 to 0.05 times the mass of the dry product while stirring, reacting at a temperature of 45 to 55°C for 2 to 3 hours, adding a 5% sodium hydroxide solution in an amount of 0.04 to 0.06 times the mass of the dry product, terminating the reaction and performing reduced pressure distillation, and filtering after the reduced pressure distillation is completed to obtain a modified montmorillonite; The organic montmorillonite comprises the following preparation steps: adding allyl trimethyl ammonium bromide to deionized water with a mass of 18 to 20 times that of allyl trimethyl ammonium bromide, stirring for 1 to 1.5 hours at a temperature of 50 to 60° C. and a rotation speed of 600 r / min, adding montmorillonite with a mass of 4 to 5 times that of allyl trimethyl ammonium bromide after stirring, keeping the temperature for reaction for 4 to 5 hours at a rotation speed of 600 r / min, ultrasonicating for 0.2 to 0.3 hours, filtering after ultrasonicating, washing the filtered product with deionized water for 3 to 5 times, and drying at a temperature of 80 to 90° C. for 4 to 5 hours to obtain the organic montmorillonite; The branched polymer comprises the following preparation steps: adding ethylenediamine to methanol with a mass of 0.5 to 0.6 times that of ethylenediamine, stirring for 2 to 2.5 hours in a nitrogen atmosphere in a light-proof state at a temperature of 0 to 5°C to prepare an ethylenediamine methanol solution; adding hexachlorocyclotriphosphazene to methanol with a mass of 4 to 5 times that of hexachlorocyclotriphosphazene at a temperature of -10 to 15°C, stirring evenly to prepare a hexachlorocyclotriphosphazene methanol solution; evenly dropping the hexachlorocyclotriphosphazene methanol solution into an ethylenediamine methanol solution with a mass of 2 to 3 times that of the hexachlorocyclotriphosphazene methanol solution at a temperature of 0 to 5°C, the dropping time being 20 to 30 minutes, stirring for reaction for 24 to 28 hours at a temperature of 25 to 30°C after the dropping is completed, filtering after the stirring reaction is completed, vacuum rotary evaporating the filtrate at a temperature of 40 to 50°C, and drying the rotary evaporation product at a temperature of 50 to 60°C for 2 to 3 hours to prepare the branched polymer.
2. The high performance environmentally friendly water-based paint according to claim 1, characterized in that: The leveling agent is water-based coating leveling agent BYK333.
3. The high performance environmentally friendly water-based paint according to claim 1, characterized in that: The curing catalyst is water-based coating catalyst BYK450.
4. The high performance environmentally friendly water-based paint according to claim 1, characterized in that: The defoamer is water-based paint defoamer BYK028.
5. The high performance environmentally friendly water-based paint according to claim 1, characterized in that: The copolymerized polyacrylate resin comprises the following preparation steps: adding isopropanol to ethylene glycol diethyl ether in an amount of 1.6 to 1.8 times the mass of the isopropanol, mixing and stirring uniformly to obtain an ethylene glycol diethyl ether isopropanol solution; weighing methyl methacrylate, methacrylic acid, butyl acrylate and di-tert-amyl peroxide according to a mass ratio, mixing and stirring uniformly to obtain a mixed solution; at a temperature of 90 to 100° C. and under nitrogen protection, uniformly dropping the mixed solution into the ethylene glycol diethyl ether isopropanol solution within 3 to 3.5 hours, reacting at a temperature of 90 to 100° C. for 6 to 8 hours after the dropping is completed, cooling to 60 to 70° C. after the reaction is completed, adding triethylamine in an amount of 3 to 5 times the mass of the ethylene glycol diethyl ether, stirring uniformly to obtain the copolymerized polyacrylate resin.
6. The high performance environmentally friendly water-based paint according to claim 5, characterized in that: The mass ratio of the methyl methacrylate, methacrylic acid, butyl acrylate and di-tert-amyl peroxide is 30:8-10:10-12:2-2.5; the mass of the methyl methacrylate is 10-12 times that of isopropanol.
7. A method for preparing a high-performance environmentally friendly water-based paint according to any one of claims 1 to 6, characterized in that: Weigh modified montmorillonite, curing catalyst, defoaming agent, copolymerized acrylate resin, ethylene glycol monobutyl ether and deionized water in proportion, stir at a speed of 300-400 r / min for 15 minutes, then add the leveling agent, and continue stirring for 15 minutes to obtain a high-performance environmentally friendly water-based paint.
Citation Information
Patent Citations
Environment-friendly fireproof water-based paint for woodware, and preparation method thereof
CN112094551A