A solar cell and a method for preparing the same, and a photovoltaic module
By controlling the design of the molten silicon area and texture area, the problem of laser damage on the cutting surface of the segmented solar cell is solved, the photoelectric conversion efficiency and passivation effect are improved, and the light utilization rate is optimized.
Patent Information
- Application Number
- CN202410891549.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-07-04
AI Technical Summary
The laser-damaged area generated during the cutting process of the segmented solar cells causes silicon slag and silicon oxide to adhere, affecting the photoelectric conversion efficiency.
By controlling the relative area and distribution shape of the molten silicon area, combined with the design of the first texture area and the second texture area, the light trapping effect of the cutting side surface and the film formation quality of the passivation layer are optimized to improve the photoelectric conversion efficiency of the solar cell.
It effectively reduces the impact of laser damage areas, improves the photoelectric conversion efficiency and passivation effect of solar cells, and optimizes light utilization.
Smart Images

Figure CN118412390B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of solar cells, and in particular to a solar cell and a preparation method thereof, and a photovoltaic module. Background Art
[0002] Solar cells are devices that utilize solar energy and directly convert light energy into electrical energy through the photoelectric effect or photochemical effect. Solar cells include sliced solar cells. Currently, the production of sliced solar cells usually involves cutting a solar cell that has formed multiple film layers to cut the entire solar cell into at least two sliced solar cells, such as two half slices. Afterwards, the sliced solar cells are used to make photovoltaic modules.
[0003] However, after cutting, the cut surface of the sliced solar cell often has a laser damaged area. For example, the silicon substrate of the solar cell is partially melted by laser to open the guide groove for the split. At this time, the molten silicon recrystallizes and partially oxidizes during the temperature drop process, producing silicon slag and silicon oxide attached to the surface of the cut surface. The above situation will affect the passivation performance of the sliced solar cell, and then affect the photoelectric conversion efficiency of the sliced solar cell. Summary of the invention
[0004] The object of the present invention is to provide a solar cell and a preparation method thereof, and a photovoltaic module, which improves the passivation characteristics and light absorption characteristics of the laser lossy area by controlling the relative area and distribution morphology of the molten silicon area, thereby improving the photoelectric conversion efficiency of the solar cell.
[0005] In order to achieve the above object, in a first aspect, the present invention provides a solar cell. The solar cell comprises a first surface and a second surface opposite to each other, and a side surface connecting the first surface and the second surface. The side surface comprises at least one first region, the at least one first region comprises a plurality of molten silicon regions, and a first texture region located between at least two molten silicon regions.
[0006] In the actual production of solar cells, the side surface of a general solar cell includes a "non-cut side surface" that is not cut and a "cut side surface" formed after cutting. The non-cut side surface is generally not attached with silicon slag and silicon oxide, and even if it is attached, the amount of attachment is very small and can be ignored. Therefore, the silicon slag and silicon oxide on the cut side surface are discussed and analyzed here. An important source of the silicon slag and silicon oxide is that when cutting the cell sheet, the lossy laser used is used to irradiate the silicon substrate of the solar cell, and the silicon substrate absorbs the laser energy and melts and oxidizes to form. The portion of the silicon slag and silicon oxide that remains after treatment is the molten silicon area in the present invention. In the solar cell provided by the present invention, the cut side surface includes a first area, which is a guide groove area opened by the laser (laser lossy cutting area), and the first texture area is included between at least two molten silicon areas in the first area. At this time, compared with the situation in the prior art that the laser guide groove area on the cut surface is all silicon slag and silicon oxide, the present invention controls the area and distribution form of the molten silicon area on the cut side surface, so that the relative area of the molten silicon area is within a reasonable range. In addition, the first texture area is also included between the molten silicon areas. The first texture area and the side surface of the molten silicon area can improve the light trapping effect of the side surface of the solar cell and increase the light absorption rate. Furthermore, the relatively regular shape of the first texture area can improve the film quality of the passivation layer, thereby improving the passivation effect.
[0007] In one implementation, within the first region, a ratio of a total area of the molten silicon region to a total area of the first texture region is greater than or equal to 30% and less than or equal to 120%.
[0008] When the above technical solution is adopted, the ratio of the total area of the molten silicon region to the total area of the first texture region is within the above range, which can not only reduce the complexity of the manufacturing process caused by pursuing an excessively small total area of the molten silicon region, but also ensure the utilization rate of light on the side surface of the solar cell and optimize the overall passivation effect of the first region to improve the photoelectric conversion efficiency of the solar cell.
[0009] In one implementation, a plurality of molten silicon regions are distributed in the first region in an island shape; and / or a maximum width of the molten silicon region is less than 100 micrometers.
[0010] In the case of adopting the above technical solution, multiple molten silicon areas are distributed in the first area in an isolated island shape. Multiple island-shaped molten silicon areas are conducive to reflecting more light through their side walls to the first texture area, thereby improving the light trapping effect of the cut side surface of the solar cell and increasing the light absorption rate to improve the utilization rate of the side surface of the solar cell for light; the maximum width of the molten silicon area is less than 100 microns, which can further limit the size of the molten silicon area and optimize the light trapping effect and light absorption efficiency.
[0011] In one implementation, the ratio of the width of the first region to the thickness of the solar cell is greater than or equal to 30% and less than or equal to 100%; the width direction of the first region and the thickness direction of the solar cell are consistent with the direction from the first surface to the second surface.
[0012] When the above technical solution is adopted, when the ratio is greater than or equal to 30%, or when the ratio is equal to 100%, it can be ensured that the first area formed as a guide area effectively divides the entire solar cell into two solar cells. Further, when the ratio is less than 100%, the damage of the lossy laser to the solar cell can be reduced.
[0013] In one implementation, the first region includes a trench structure.
[0014] In one implementation, the groove structure extends in any one or more of a dendrite, a straight line, a broken line, or a curve; and / or the depth of the groove structure is 1 micron to 10 microns; and / or the cross-section of the groove structure is any one or more of a V-shape or a U-shape.
[0015] In one implementation, the molten silicon region includes a stacked multilayer structure; and / or, the molten silicon region includes a porous structure; and / or, the molten silicon region includes silicon oxide.
[0016] In one implementation, the side surface further includes a second region, and the second region includes a second texture area.
[0017] When the above technical solution is adopted, it is beneficial to improve the light trapping effect of the second area, which is beneficial for more light to be refracted into the solar cell through the second area and used by the solar cell. In addition, in the process of manufacturing the solar cell, a passivation layer is formed on the second area of the side surface of the solar cell, and the texture structure of the second texture area is beneficial to the passivation effect, so as to improve the photoelectric conversion efficiency of the solar cell.
[0018] In one implementation, the side surface includes a cutting side surface and a non-cutting side surface. The first area is located on the cutting side surface; and the second area is located on the cutting side surface and / or the non-cutting side surface.
[0019] When the above technical solution is adopted, when the first area and the second area are both located on the cut side surface of the solar cell, the above-mentioned cut side surface includes a molten silicon area, a first texture area and a second texture area. Compared with the situation in the prior art where the laser guide groove area on the cut surface is all silicon slag and silicon oxide, the present invention controls the area and distribution morphology of the molten silicon area on the cut side surface so that the relative area of the side molten silicon area is within a reasonable range. In addition, the first texture area is also included between the molten silicon areas, and the cut side surface also includes a second texture area. The first texture area and the second texture area can be used to improve the light trapping effect of the side surface of the solar cell and increase the light absorption rate. Furthermore, the relatively regular morphology of the first texture area and the second texture area can improve the film forming quality of the passivation layer, thereby improving the passivation effect.
[0020] In an implementation, the first texture area includes a suede structure, the second texture area includes a suede structure, and the suede structure included in the first texture area and the suede structure included in the second texture area both include a pyramid structure.
[0021] When the velvet structure on the first texture area and the second texture area is a pyramid structure, it is beneficial to increase the specific surface area of the side surface where the first texture area and the second texture area are located. Based on this, it is beneficial to make the side surface where the first texture area and the second texture area are located have a good light trapping effect, further improving the utilization rate of light by the solar cell.
[0022] In one implementation, the average height of the pyramid structures in the first texture area is smaller than the average height of the pyramid structures in the second texture area, or the average bottom width of the pyramid structures in the first texture area is smaller than the average bottom width of the pyramid structures in the second texture area.
[0023] When the above technical solution is adopted, it is beneficial to form a passivation layer on the first texture area later, so as to improve the passivation effect of the solar cell and further improve the photoelectric conversion efficiency of the solar cell.
[0024] In one implementation, the first textured area includes a tower foundation structure, and the second textured area includes a tower foundation structure. The tower foundation structure of the first textured area has a tower foundation lateral dimension that is smaller than the tower foundation structure of the second textured area.
[0025] When the above technical solution is adopted, it is beneficial to form a passivation layer on the first texture area later, so as to improve the passivation effect of the solar cell and further improve the photoelectric conversion efficiency of the solar cell.
[0026] In one implementation, the tower base structure of the first texture area includes a boss-type structure or a recessed groove-like structure; the tower base structure of the second texture area includes a boss-type structure or a recessed groove-like structure.
[0027] When the above technical solution is adopted, the tower base structure of the above-mentioned boss-type structure or recessed groove-like structure can further increase the roughness of the side surface where the first texture area and the second texture area are located, which is beneficial to reduce the reflectivity of the side surface where the first texture area and the second texture area are located, so as to further improve the utilization rate of light by solar cells.
[0028] In one implementation, the solar cell comprises a first chamfer and a second chamfer opposite to each other, wherein a side surface of the first chamfer comprises a first region.
[0029] In one implementation, the first chamfer is smaller than the second chamfer.
[0030] When the above technical solution is adopted, the first chamfer and the second chamfer can reduce or avoid damage to the corners of the solar cell caused by external stress, reduce or eliminate the probability of damage to the solar cell due to corner loss, so as to ensure the quality of the solar cell.
[0031] In one implementation, the solar cell further includes a passivation layer, and the passivation layer includes a portion located on the side surface.
[0032] In one implementation, the passivation layer also includes portions located on the first surface and the second surface; the first surface is a light-facing surface, and the average thickness of the passivation layer located on the side surface is less than the average thickness of the passivation layer located on the first surface.
[0033] In one implementation, the solar cell also includes a passivation layer, the passivation layer includes a first passivation layer and a second passivation layer; the first passivation layer includes a portion located on the first surface or the second surface, the second passivation layer includes a portion located on the cut side surface, and the average thickness of the second passivation layer located on the cut side surface is greater than the average thickness of the first passivation layer located on the first surface or the second surface.
[0034] In one implementation, the second passivation layer further includes a portion located at an edge of the first surface and located above the first passivation layer, the edge of the first surface being close to the cut side surface; and / or,
[0035] The second passivation layer also includes a portion located at an edge of the second surface and located above the first passivation layer, wherein the edge of the second surface is close to the cut side surface.
[0036] In one implementation, the average thickness of the second passivation layer located at the cut side surface is greater than or equal to 10 nanometers and less than or equal to 120 nanometers; and / or, the average thickness of the second passivation layer located at the edge of the first surface is less than the average thickness of the second passivation layer located at the cut side surface; and / or, the average thickness of the second passivation layer located at the edge of the second surface is less than the average thickness of the second passivation layer located at the cut side surface.
[0037] In one implementation, the coverage of the passivation layer in the first region is smaller than that in the region of the side surface other than the first region; and / or the coverage of the passivation layer in the first region is greater than 80%.
[0038] In a second aspect, the present invention further provides a method for preparing a solar cell. The method for preparing a solar cell comprises:
[0039] First, a semiconductor substrate is provided, wherein the semiconductor substrate comprises a first surface and a second surface opposite to each other;
[0040] Next, the first surface is processed by a first laser process to form a groove on the first surface; the groove extends along a first direction;
[0041] Next, a second laser process is used to perform heat treatment on the first surface along the first direction, and a heat treatment path is formed;
[0042] Next, the semiconductor substrate is divided into at least two semiconductor substrate slices along the heat treatment path;
[0043] Next, the cut surface of the sliced semiconductor substrate is cleaned for damage; the cut surface includes at least one first region; the at least one first region includes a plurality of molten silicon regions and a first texture region located between at least two molten silicon regions.
[0044] When the above technical solution is adopted, the cut surface of the sliced semiconductor substrate is damaged and cleaned, and the laser damaged layer generated by the first laser process cutting can be removed to reduce lattice defects.
[0045] In the actual production of solar cells, the side surface of the sliced semiconductor substrate generally includes a "non-cut surface" that is not cut and a "cut surface" formed after cutting. The non-cut surface is generally not attached with silicon slag and silicon oxide, and even if it is attached, the amount of attachment is very small and can be ignored. Therefore, the focus of the discussion and analysis here is on the silicon slag and silicon oxide on the cut surface. An important source of the silicon slag and silicon oxide is that when cutting the cell, the lossy laser used is used to irradiate the silicon substrate of the solar cell, and the silicon substrate absorbs the laser energy and melts and oxidizes to form. The portion of the silicon slag and silicon oxide retained after treatment is the molten silicon area in the present invention. In the sliced semiconductor substrate provided by the present invention, the cut surface includes a first area, which is a guide groove area opened by the laser (laser lossy cutting area), and the first texture area is included between at least two molten silicon areas in the first area. At this time, compared with the situation in the prior art that the laser guide groove area on the cut surface is all silicon slag and silicon oxide, the present invention controls the area and distribution form of the molten silicon area on the cut surface, so that the relative area of the molten silicon area is within a reasonable range. In addition, the first texture area is also included between the molten silicon areas. The first texture area and the side surface of the molten silicon area can improve the light trapping effect of the side surface of the solar cell and increase the light absorption rate. Furthermore, the relatively regular shape of the first texture area can improve the film quality of the passivation layer, thereby improving the passivation effect.
[0046] In one implementation, after cleaning the damaged cut surfaces of the sliced semiconductor substrate, the method for preparing a solar cell further includes: forming a passivation layer at least on the cut surfaces of the sliced semiconductor substrate.
[0047] When the above technical solution is adopted, the passivation effect of the solar cell can be improved to improve the photoelectric conversion efficiency of the solar cell. In addition, since a passivation layer is formed on the cut surface of the sliced semiconductor substrate after cleaning, the surface dangling bonds generated by the cut surface of the sliced semiconductor substrate being directly exposed to the air can be saturated under the action of the passivation layer. Based on this, the minority carrier lifetime of the cut surface can be increased to reduce the recombination current, thereby improving the conversion efficiency and component power of the solar cell.
[0048] In one implementation, the groove includes a first part, a second part and a third part; the first end of the first part and the first end of the second part are both connected to one end of the third part; the distance between the first part and the second part gradually increases in a direction away from the third part; the second end of the first part and the second end of the second part are close to the edge of the semiconductor substrate.
[0049] When the above technical solution is adopted, the sliced semiconductor substrate formed by segmentation along the heat treatment path has a chamfer. Compared with the case where the angle of the cut side of the sliced semiconductor substrate is a right angle, the damage to the corner of the sliced semiconductor substrate caused by external stress can be reduced or avoided, and the probability of damage to the sliced semiconductor substrate due to corner chipping can be reduced or eliminated, thereby ensuring the quality of the sliced semiconductor substrate and further ensuring the quality of the solar cell.
[0050] In one implementation, the angle between the first portion and the third portion is equal to the angle between the second portion and the third portion.
[0051] In one implementation, a ratio of the depth of the groove to the thickness of the semiconductor substrate is greater than or equal to 30% and less than or equal to 100%, and a depth direction of the groove is consistent with a thickness direction of the semiconductor substrate.
[0052] When the above technical solution is adopted, when the ratio is greater than or equal to 30%, or when the ratio is equal to 100%, it can be ensured that the first region formed as a guide region effectively divides the entire semiconductor substrate into two semiconductor substrate slices. Furthermore, when the ratio is less than 100%, the damage of the lossy laser to the semiconductor substrate can be reduced.
[0053] And / or, the second laser process uses a non-destructive laser.
[0054] When the above technical solution is adopted, the portion of the entire semiconductor substrate located in the middle of the guide groove is subjected to non-destructive laser heat treatment, which can reduce damage to the semiconductor substrate.
[0055] In a third aspect, the present invention further provides a photovoltaic module. The photovoltaic module comprises:
[0056] A plurality of solar cells as described in the first aspect, or a plurality of solar cells prepared by the method for preparing a solar cell as described in the second aspect; an encapsulation layer covering the surfaces of the plurality of solar cells; and a cover plate covering the surface of the encapsulation layer away from the solar cells. BRIEF DESCRIPTION OF THE DRAWINGS
[0057] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0058] Figure 1 is a schematic structural diagram of a partially cut side surface of a solar cell when the ratio of the width of the first region to the thickness of the solar cell is less than 100% in an embodiment of the present invention;
[0059] Figure 2is a schematic structural diagram of a partially cut side surface of a solar cell when the ratio of the width of the first region to the thickness of the solar cell is equal to 100% in an embodiment of the present invention;
[0060] Figure 3 is a SEM image of a partially cut side surface when the ratio of the width of the first region to the thickness of the solar cell is equal to 100% in an embodiment of the present invention;
[0061] Figure 4 is a SEM image of other areas of the cut side surface when the ratio of the width of the first area to the thickness of the solar cell is equal to 100% in the embodiment of the present invention;
[0062] Figure 5 A schematic diagram of the relationship between light and a solar cell in an embodiment of the present invention;
[0063] Figure 6 This is a SEM image of the second texture area in the embodiment of the present invention when it is a tower base structure;
[0064] Figure 7 is a top view of a solar cell in an embodiment of the present invention;
[0065] Figure 8 A schematic diagram of the relationship between a semiconductor substrate, a groove, and a heat treatment path in an embodiment of the present invention;
[0066] Fig. 9 is a top view of a groove in an embodiment of the present invention;
[0067] Fig.10 is a SEM image of a portion of a cut surface of a sliced semiconductor substrate after the semiconductor substrate is processed by a lossy laser in an embodiment of the present invention;
[0068] Fig.11 This is a SEM image of a portion of the cut surface of a sliced semiconductor substrate after the semiconductor substrate is processed by non-destructive laser in an embodiment of the present invention.
[0069] Reference numerals:
[0070] 1-side surface, 2-first region, 20-molten silicon region, 21-first texture region, 22-groove structure, 3-second region, 4-first chamfer, 5-second chamfer, 6-solar cell, 7-semiconductor substrate, 70-sliced semiconductor substrate, 8-groove, 80-first part, 81-second part, 82-third part. DETAILED DESCRIPTION
[0071] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0072] It should be noted that when an element is referred to as being "fixed to" or "disposed on" another element, it can be directly on the other element or indirectly on the other element. When an element is referred to as being "connected to" another element, it can be directly connected to the other element or indirectly connected to the other element.
[0073] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined. The meaning of "several" is one or more, unless otherwise clearly and specifically defined.
[0074] In the description of the present invention, it is necessary to understand that the directions or positional relationships indicated by the terms "up", "down", "front", "back", "left", "right", etc. are based on the directions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific direction, be constructed and operated in a specific direction, and therefore cannot be understood as a limitation on the present invention.
[0075] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0076] In a first aspect, an embodiment of the present invention provides a solar cell. Figures 1 to 5 The solar cell comprises a first surface and a second surface opposite to each other, and a side surface 1 connecting the first surface and the second surface. The side surface 1 comprises at least one first region 2, and the at least one first region 2 comprises a plurality of molten silicon regions 20, and a first texture region 21 located between at least two molten silicon regions 20.
[0077] The above-mentioned solar cell may include a semiconductor substrate. Exemplarily, the above-mentioned semiconductor substrate may be a silicon substrate. In terms of conductivity type, the solar cell may be an intrinsic conductive substrate, an N-type conductive substrate or a P-type conductive substrate. Preferably, the semiconductor substrate is an N-type conductive substrate or a P-type conductive substrate. Compared with the intrinsic conductive substrate, the N-type conductive substrate or the P-type conductive substrate has a higher conductivity, which is beneficial to reduce the series resistance of the solar cell and improve the efficiency of the solar cell. From a structural point of view, the first surface of the solar cell may be a velvet surface to improve the light trapping effect of the solar cell toward the light surface, thereby improving the utilization rate of light by the solar cell. Of course, the first surface of the solar cell may also be a plane. As for the second surface of the solar cell, it may be a polished surface or a velvet surface, which is not specifically limited here.
[0078] In the actual production of solar cells, the side surfaces of solar cells generally include "non-cut side surfaces" that are not cut and "cut side surfaces" formed after cutting. Silicon slag and silicon oxide are generally not attached to the non-cut side surfaces, and even if they are attached, the amount attached is very small and can be ignored. Therefore, the silicon slag and silicon oxide on the cut side surfaces are discussed and analyzed here. An important source of the silicon slag and silicon oxide is that when cutting the cell sheet, the lossy laser is used to irradiate the silicon substrate of the solar cell, and the silicon substrate absorbs the laser energy and melts and oxidizes to form. The area where the silicon slag and silicon oxide are retained after treatment is the molten silicon area in the embodiment of the present invention.
[0079] The number of the first regions can be determined according to actual conditions, for example, it can be one, two, three, four or more. Further, the position of the first region on the side surface of the solar cell can also be set according to actual conditions, for example, in the upper right corner region, lower right corner region, upper left corner region, lower left corner region, middle upper region, middle lower region, left region, right region, middle region, etc. of the cut side surface included in the side surface, which depends on the specific method of slicing, such as laser grooving from the light-facing side or the backlight side of the solar cell, and the depth of the laser grooving.
[0080] The following description uses three possible situations as examples. It should be understood that the following description is only for understanding and is not intended to be a specific limitation.
[0081] Example 1: When cutting a whole solar cell, if there is only one cutting side surface (i.e., a whole solar cell is divided into two split solar cells along its length), and a non-penetrating guide groove is opened at both ends of the first surface of the whole solar cell using a laser. At this time, the side surface (or the cutting side surface) includes two first areas, and the two first areas are respectively located in the upper right corner area and the upper left corner area of the cutting side surface; of course, the guide groove can also be opened from the second surface of the solar cell opposite to the first surface using a laser. At this time, the two first areas are respectively located in the lower right corner area and the lower left corner area of the cutting side surface. That is, the solar cell can have a guide groove opened from the light-facing side or from the backlight side.
[0082] Example 2: When cutting a whole solar cell, if there are two cut side surfaces (i.e., a whole solar cell is divided into three sliced solar cells along its length direction), and both cut side surfaces have non-penetrating guide grooves opened by laser at both ends of the first surface of the whole solar cell, then the side surface of the middle sliced solar cell includes four first areas, wherein the four first areas are respectively located in the upper right corner area and the upper left corner area of the two cut side surfaces.
[0083] Example 3: When cutting a whole solar cell, if there are two cut side surfaces (i.e., a whole solar cell is divided into three sliced solar cells along its length), and both cut side surfaces are provided with non-penetrating guide grooves by laser at both ends of the first surface of the whole solar cell, and further, a guide groove is added in the middle position of one of the cut side surfaces, then the side surface of the middle sliced solar cell includes five first regions. Among them, for the first cut side surface, the two first regions are respectively located in the upper right corner region and the upper left corner region of the first cut side surface. For the second cut side surface, the three first regions are respectively located in the upper right corner region, the upper left corner region and the middle upper region of the second cut side surface.
[0084] See also Figures 1 to 3In the solar cell provided in the embodiment of the present invention, the cutting side surface includes a first area 2, which is a guide groove area opened by the laser (laser lossy cutting area), and a first texture area 21 is included between at least two molten silicon areas 20 in the first area 2. At this time, compared with the situation in the prior art that the laser guide groove area on the cutting surface is all silicon slag and silicon oxide, in the embodiment of the present invention, the area and distribution form of the molten silicon area 20 on the cutting side surface are controlled, so that the relative area of the molten silicon area 20 is within a reasonable range. In addition, the first texture area 21 is also included between the molten silicon areas 20. The light trapping effect of the side surface 1 of the solar cell can be improved by using the first texture area 21 and the side of the molten silicon area to increase the light absorption rate. Furthermore, the relatively regular shape of the first texture area 21 can improve the film forming quality of the passivation layer, thereby improving the passivation effect.
[0085] In terms of materials, the molten silicon region 20 includes silicon and silicon oxides.
[0086] As a possible implementation, see Figure 1 , in the first region 2, the ratio of the total area of the molten silicon region 20 to the total area of the first texture region 21 is greater than or equal to 30% and less than or equal to 120%. For example, the ratio of the total area of the molten silicon region 20 to the total area of the first texture region 21 may be 30%, 40%, 50%, 60%, 70%, 80%, 90%, 100% or 120%, etc.
[0087] The ratio of the total area of the molten silicon region 20 to the total area of the first texture region 21 is within the above range, which can not only reduce the complexity of the manufacturing process caused by pursuing an excessively small total area of the molten silicon region 20, but also ensure the utilization rate of light by the side surface 1 of the solar cell, and optimize the overall passivation effect of the first region, so as to improve the photoelectric conversion efficiency of the solar cell.
[0088] In an optional manner, a plurality of molten silicon regions 20 are dispersedly distributed in the first region.
[0089] In an optional manner, the maximum width of the molten silicon zone 20 is widely distributed, including both smaller molten silicon zones and larger molten silicon zones. The maximum width of a single molten silicon zone 20 is preferably less than 100 microns, and the average maximum width of the molten silicon zone 20 in the first region 2 is preferably greater than or equal to 10 microns and less than or equal to 80 microns. For example, the average maximum width is 10 microns, 20 microns, 50 microns, 60 microns, 70 microns or 80 microns, etc. The maximum width of the above-mentioned molten silicon zone is the maximum line segment length passing through the molten silicon zone 20.
[0090] See also Figures 1 to 5In an embodiment of the present invention, a plurality of molten silicon regions are distributed in the first region in an isolated island shape. The plurality of molten silicon regions distributed in an island shape are conducive to reflecting more light through its side wall to the first texture region, thereby improving the light trapping effect of the cut side surface of the solar cell, increasing the light absorption rate, and improving the utilization rate of the side surface of the solar cell for light, thereby improving the photoelectric conversion efficiency of the solar cell. Preferably, the molten silicon region is an irregular polygon and is evenly distributed in the first region.
[0091] See also Figure 5 According to the foregoing description, the solar cell includes a first surface and a second surface relative to each other. When the first surface S1 is the light-facing surface and the second surface is the backlight surface, in order to better utilize the light, the incident angle of the first surface of the solar cell is as close to 0 as possible. However, this will cause the incident light on the side surface to have a large angle of incidence on the side surface, for example, close to 90°, which will result in a very low utilization rate of the light on the side surface. In an embodiment of the present invention, the first region includes a plurality of molten silicon zones, and a first textured zone between the molten silicon zones, and the shape of the molten silicon zone is an irregular polygonal shape, and is distributed in an isolated island shape with a relatively uniform distribution. This is beneficial to improving the utilization rate of the light on the side surface of the solar cell. For example, the attached Figure 5 After the incident light L1 and L2 pass through the molten silicon area, more light can be reflected to the first texture area, thereby improving the utilization rate of light on the side surface of the solar cell. Further, the maximum width of a single molten silicon area 20 is preferably less than 100 microns, and the average maximum width of the molten silicon area 20 in the first region 2 is preferably greater than or equal to 10 microns and less than or equal to 80 microns, which can balance the absorption and light trapping effects of light.
[0092] Preferably, the thickness of the molten silicon region on the side surface is greater than or equal to 1 micron and less than or equal to 50 microns, and the thickness of the molten silicon region is the height difference between the top surface of the molten silicon region and the first texture region. For example, the thickness of the molten silicon region on the side surface can be 1 micron, 5 microns, 10 microns, 15 microns, 20 microns, 25 microns, 30 microns, 35 microns, 40 microns, 45 microns or 50 microns, etc.
[0093] Furthermore, the first region includes microcracks, namely, groove structures 22, and the groove structures 22 extend in any one or more shapes such as dendrite extension, straight line extension, broken line extension, and curved line extension. Figure 3 and Figure 5As shown, the groove structure 22 is conducive to the light entering deeper into the side surface of the solar cell and into the silicon substrate, thereby improving the utilization rate of the light. Preferably, the depth of the groove structure is 1 micron-10 microns, and the profile of the groove structure is any one or more of a V-type and a U-type. The bottom and sidewall of the groove can be a relatively flat plane structure or a velvet structure. For example, the depth of the groove structure can be 1 micron, 2 microns, 3 microns, 4 microns, 5 microns, 6 microns, 7 microns, 8 microns, 9 microns or 10 microns, etc.
[0094] Furthermore, the molten silicon region may include a multilayer structure stacked in layers, and the edges of the molten silicon region are staggered. The stacked multilayer structure is conducive to increasing the scattering of light by the edge of the molten silicon region. In addition, the molten silicon region includes a porous structure, which is more conducive to enhancing the utilization of light.
[0095] As a possible implementation, see Figure 1 , the ratio of the width W of the first region 2 to the thickness D of the solar cell is greater than or equal to 30% and less than or equal to 100%; the width direction of the first region 2 and the thickness direction of the solar cell are both consistent with the direction from the first surface to the second surface. For example, the ratio of the width of the first region to the thickness of the solar cell can be 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95% or 100%, etc.
[0096] When the above technical solution is adopted, when the ratio is greater than or equal to 30%, or when the ratio is equal to 100%, it can be ensured that the first area formed as a guide area effectively divides the entire solar cell into two solar cells. Further, when the ratio is less than 100%, the damage of the lossy laser to the solar cell can be reduced.
[0097] For example, see Figure 1 , Figure 1 It is a schematic structural diagram of a partially cut side surface when the ratio of the width W of the first region 2 to the thickness D of the solar cell is less than 100%.
[0098] See also Figure 2 , Figure 2 It is a schematic structural diagram of a partially cut side surface when the ratio of the width W of the first region 2 to the thickness D of the solar cell is equal to 100%. Figure 3 is a SEM image of a partially cut side surface when the ratio of the width of the first region 2 to the thickness of the solar cell is equal to 100%; Figure 4 It is a SEM image of other areas of the cut side surface when the ratio of the width of the first area to the thickness of the solar cell is equal to 100%.
[0099] As a possible implementation, see Figure 1 The side surface 1 also includes a second region 3, and the second region 3 includes a second texture region, which is beneficial to improving the light trapping effect of the second region 3. In addition, in the process of manufacturing the solar cell, a passivation layer will be formed on the second region 3 of the side surface 1 of the solar cell, and the texture structure of the second texture region is beneficial to the passivation effect, so as to improve the photoelectric conversion efficiency of the solar cell.
[0100] In combination with the above description, the side surface includes a cutting side surface and a non-cutting side surface. The first area is located on the cutting side surface; and the second area is located on the cutting side surface and / or the non-cutting side surface.
[0101] For example, the first region and the second region are both located on the cut side surface of the solar cell. Or, the second region is located on the non-cut side surface of the solar cell, and the first region is located on the cut side surface of the solar cell. Or, the first region is located on the cut side surface of the solar cell, and the second region is located on the non-cut side surface and the cut side surface of the solar cell.
[0102] See also Figure 1 , when the first region 2 and the second region 3 are both located on the cut side surface of the solar cell, the above-mentioned cut side surface includes a molten silicon region 20, a first texture region 21 and a second texture region. Compared with the prior art in which the laser guide groove area on the cut surface is all silicon slag and silicon oxide, in the embodiment of the present invention, the area and distribution morphology of the molten silicon region on the cut side surface are controlled so that the relative area of the side molten silicon region is within a reasonable range. In addition, the first texture region is also included between the molten silicon regions, and the cut side surface also includes a second texture region. The first texture region and the second texture region can be used to improve the light trapping effect of the side surface of the solar cell and increase the light absorption rate. Furthermore, the relatively regular morphology of the first texture region and the second texture region can improve the film forming quality of the passivation layer, thereby improving the passivation effect.
[0103] The structure included in the first texture area and the structure included in the second texture area may be the same or different. Further, the structure included in the first texture area and the structure included in the second texture area may be a velvet structure or a tower base structure. The following description is given by taking two possible situations as examples. It should be understood that the following description is only for understanding and is not intended to be specifically limited.
[0104] The first type: the first texture area includes a suede structure, and the second texture area includes a suede structure (for example Figure 4 The suede structure included in the first texture area and the suede structure included in the second texture area both include a pyramid structure.
[0105] When the velvet structure on the first texture area and the second texture area is a pyramid structure, it is beneficial to increase the specific surface area of the side surface where the first texture area and the second texture area are located. Based on this, it is beneficial to make the side surface where the first texture area and the second texture area are located have a good light trapping effect, further improving the utilization rate of light by the solar cell.
[0106] Furthermore, the average height of the pyramid structure in the first texture area is smaller than the average height of the pyramid structure in the second texture area, or the average bottom width of the pyramid structure in the first texture area is smaller than the average bottom width of the pyramid structure in the second texture area. In this case, it is beneficial to form a passivation layer on the first texture area later to improve the passivation effect of the solar cell and further improve the photoelectric conversion efficiency of the solar cell.
[0107] The second type: the first texture area includes a tower base structure, and the second texture area includes a tower base structure (for example Figure 6 The structure shown). The transverse dimension of the tower base structure of the first texture area is smaller than the transverse dimension of the tower base structure of the second texture area. At this time, it is beneficial to form a passivation layer on the first texture area later to improve the passivation effect of the solar cell and further improve the photoelectric conversion efficiency of the solar cell. It should be noted that when the top view of the tower base is a quadrilateral, the transverse dimension of the tower base can be the length of any side or diagonal of the quadrilateral.
[0108] In an optional manner, the tower base structure of the first texture area includes a boss-type structure or a recessed groove-like structure, and the tower base structure of the second texture area includes a boss-type structure or a recessed groove-like structure.
[0109] The tower base structure with the above-mentioned boss-type structure or recessed groove-like structure can further increase the roughness of the side surface where the first texture area and the second texture area are located, which is beneficial to reduce the reflectivity of the side surface where the first texture area and the second texture area are located, so as to further improve the utilization rate of light by solar cells.
[0110] As a possible implementation, see Figure 7 The solar cell 6 includes a first chamfer 4 and a second chamfer 5. The side surface of the first chamfer 4 includes a first region 2, and the first chamfer 4 is smaller than the second chamfer 5. The first chamfer 4 and the second chamfer 5 can reduce or avoid damage to the corner of the solar cell caused by external stress, reduce or eliminate the probability of damage to the solar cell due to corner loss, so as to ensure the quality of the solar cell.
[0111] Exemplarily, the solar cell 6 generally includes two first chamfers 4 and two second chamfers 5 , wherein the two first chamfers 4 are close to the cut side surfaces, the two second chamfers 5 are close to the surfaces opposite to the cut side surfaces, and the first chamfers 4 are smaller than the second chamfers 5 .
[0112] In one implementation, the solar cell further includes a passivation layer, and the passivation layer may be located on the cut side surface, the non-cut side surface, the first surface, and the second surface. The following description is given by taking several possible situations as examples, and it should be understood that the following description is only for understanding and is not intended to be a specific limitation.
[0113] Example 1: A passivation layer is provided on the side surfaces (including the cut side surfaces and the non-cut side surfaces) of the solar cell.
[0114] Example 2: The side surfaces (including the cut side surfaces and the non-cut side surfaces), the first surface, and the second surface of the solar cell all have a passivation layer, and are formed in the same process. That is, the passivation layer on the side surface is integrally formed with the passivation layer on the first surface and the passivation layer on the second surface and is continuously distributed. When the first surface is the light-facing surface and the second surface is the backlight surface, the passivation layer on the second surface may be located only within a certain range of the edge of the second surface, for example, within 5 microns of the edge of the second surface. At the same time, the average thickness of the passivation layer located on the side surface is less than the average thickness of the passivation layer located on the first surface. The passivation layer preferably includes at least one of aluminum oxide, silicon oxide, and silicon nitride.
[0115] Example 3: The passivation layer of the solar cell includes a first passivation layer and a second passivation layer. The first passivation layer includes a portion located on the first surface or the second surface, the second passivation layer includes a portion located on the cut side surface, and the average thickness of the second passivation layer located on the cut side surface is greater than the average thickness of the first passivation layer located on the first surface or the second surface.
[0116] Example 4: The passivation layer of the above-mentioned solar cell includes a first passivation layer and a second passivation layer. The first passivation layer includes a portion located on the first surface and / or the second surface, the second passivation layer includes a portion located on the cut side surface, and the average thickness of the second passivation layer located on the cut side surface is greater than the average thickness of the first passivation layer located on the first surface or the second surface. The second passivation layer also includes a portion located on the edge of the first surface, and is located above the first passivation layer, and the edge of the first surface is close to the cut side surface; and / or, the second passivation layer also includes a portion located on the edge of the second surface, and is located above the first passivation layer, and the edge of the second surface is close to the cut side surface.
[0117] Exemplarily, the passivation layer of the solar cell includes a first passivation layer and a second passivation layer. The first passivation layer includes a portion located on the first surface and / or the second surface; the second passivation layer includes a portion located on the cut side surface, and a portion located in a certain range of the first surface and / or the second surface close to the edge of the cut side surface; the second passivation layer covers the first passivation layer within a certain range of the edge of the first surface and / or the second surface close to the cut side surface, so as to realize a stacked structure of the first passivation layer and the second passivation layer. The first passivation layer and the second passivation layer can be formed in different process steps. Since the cut side surface includes a first region, and the first region has a molten silicon region, a second passivation layer covering the cut side surface can be formed in an independent step, so as to better meet the passivation requirements of the first region. Preferably, the average thickness of the second passivation layer located on the cut side surface is greater than the average thickness of the first passivation layer located on the first surface or the second surface. The average thickness of the second passivation layer located on the cut side surface is greater than or equal to 10 nanometers and less than or equal to 120 nanometers. For example, the average thickness of the second passivation layer located on the cut side surface can be 10 nanometers, 30 nanometers, 50 nanometers, 80 nanometers, 90 nanometers, 100 nanometers or 120 nanometers. The first passivation layer and the second passivation layer can be selected from at least one of aluminum oxide, silicon oxide and silicon nitride; the material and structure of the first passivation layer can be the same as or different from that of the second passivation layer; the first passivation layer and the second passivation layer can be a single-layer film or a stack of multiple films. Further, the average thickness of the second passivation layer located at the edge of the first surface is less than the average thickness of the second passivation layer located at the cut side surface; and / or, the average thickness of the second passivation layer located at the edge of the second surface is less than the average thickness of the second passivation layer located at the cut side surface.
[0118] As a possible implementation, regarding the passivation layer formed at different positions, in the side surface of the solar cell, the coverage of the passivation layer in the first area is less than that in the area other than the first area of the side surface; or, in the cut side surface, the coverage of the passivation layer in the first area 2 is less than that in the second area 3. Since there is a molten silicon area in the first area, its surface structure is more complex than that in the second area 3. After the passivation layer is formed, the overall coverage of the first area is less than that of the second area. Preferably, the coverage of the passivation layer in the first area 2 is greater than 80%, so that the overall passivation effect of the first area can be guaranteed, while also avoiding other problems caused by excessive setting of the passivation layer, such as increased process time and increased materials.
[0119] In a second aspect, an embodiment of the present invention further provides a method for preparing a solar cell. Figures 8 to 11 , the preparation method of the solar cell comprises:
[0120] First, a semiconductor substrate 7 is provided. The semiconductor substrate 7 includes a first surface and a second surface opposite to each other.
[0121] Exemplarily, the semiconductor substrate may be a silicon substrate. In terms of conductivity type, the semiconductor substrate may be an intrinsic conductive substrate, an N-type conductive substrate or a P-type conductive substrate. Preferably, the semiconductor substrate is an N-type conductive substrate or a P-type conductive substrate. Compared with the intrinsic conductive substrate, the N-type conductive substrate or the P-type conductive substrate has a higher conductivity, which is beneficial to reduce the series resistance of the solar cell and improve the efficiency of the solar cell.
[0122] Next, the slices are cut and the first surface is processed by a first laser process to form a groove 8 on the first surface, wherein the groove 8 extends along a first direction;
[0123] Exemplarily, the first laser process uses lossy laser to cut the grooves formed on the semiconductor substrate as guide grooves, which is conducive to the subsequent segmentation of the semiconductor substrate along the guide grooves to ensure that the shapes of the segmented semiconductor substrates meet actual requirements.
[0124] In one example, the ratio of the depth of the groove to the thickness of the semiconductor substrate is greater than or equal to 30% and less than or equal to 100%, and the depth direction of the groove is consistent with the thickness direction of the semiconductor substrate. For example, the ratio can be 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95% or 100%.
[0125] When the above technical solution is adopted, when the ratio is greater than or equal to 30%, or when the ratio is equal to 100%, it can be ensured that the first region formed as a guide region effectively divides the entire semiconductor substrate into two semiconductor substrate slices. Furthermore, when the ratio is less than 100%, the damage of the lossy laser to the semiconductor substrate can be reduced.
[0126] Further, see Fig. 9 As an optional solution, the groove 8 includes a first portion 80, a second portion 81 and a third portion 82, and the first end of the first portion 80 and the first end of the second portion 81 are both connected to one end of the third portion 82. Along the direction away from the third portion 82, the distance between the first portion 80 and the second portion 81 gradually increases, and the second end of the first portion 80 and the second end of the second portion 81 are close to the edge of the semiconductor substrate 7. Exemplarily, the groove may be a Y-shaped groove.
[0127] When the above technical solution is adopted, the sliced semiconductor substrate formed by segmentation along the heat treatment path has chamfers. Compared with the case where at least two corners of the sliced semiconductor substrate are right angles, the damage to the corners of the sliced semiconductor substrate caused by external stress can be reduced or avoided, and the probability of damage to the sliced semiconductor substrate due to corner loss can be reduced or eliminated, thereby ensuring the quality of the sliced semiconductor substrate and further ensuring the quality of the solar cell.
[0128] As a possible implementation, see Fig. 9 , the angle A between the first portion 80 and the third portion 82 is equal to the angle B between the second portion 81 and the third portion 82. As for the sizes of the above two angles, they can be set according to actual conditions and are not specifically limited here.
[0129] Next, a second laser process is used to perform heat treatment on the first surface along the first direction, and a heat treatment path L is formed;
[0130] Exemplarily, the second laser process uses a non-destructive heat laser. Using a non-destructive heat laser to heat-treat the portion of the entire semiconductor substrate located in the middle of the guide groove can reduce damage to the semiconductor substrate.
[0131] Next, along the heat treatment path L, the semiconductor substrate 7 is divided into at least two semiconductor substrate slices 70;
[0132] Exemplarily, after the heat treatment path and the two grooves are formed on the first surface of the semiconductor substrate, water is sprayed on the semiconductor substrate, and the semiconductor substrate is naturally split to form two or more semiconductor substrates. Fig.10 , Fig.10 This is the situation of a part of the cut surface of a sliced semiconductor substrate after the semiconductor substrate is processed by a lossy laser. Fig.10 Silicon slag and silicon oxide can be observed in the Fig.11 , Fig.11 This is the situation of the partially cut surface of the sliced semiconductor substrate after the semiconductor substrate is processed by non-destructive laser. Fig.11 It can be observed that there is no silicon slag and silicon oxide on the cut surface.
[0133] Next, the cut surface of the sliced semiconductor substrate is cleaned for damage, and the laser damaged layer generated by the first laser process cutting can be removed to reduce lattice defects.
[0134] Exemplarily, in a chain cleaning machine, the sliced semiconductor substrate is placed in a HF and HNO3 tank, and a roller-liquid method or a water-floating method is used to remove part of the silicon slag and silicon oxide on the cut surface of the sliced semiconductor substrate. Since the cut surface is not protected by the phosphorus-silicon glass layer, the concentration of HF and HNO3 is increased to increase the corrosion of the cut surface, thereby increasing the cleaning of the cut surface, making the cut surface smoother than the cut surface in the prior art, and making the cleaning effect of the cut surface similar to the cleaning effect of other surfaces of the sliced semiconductor substrate. Next, the ratio of alkali texturing and additives is adjusted when passing through the tank cleaning machine, and the cut surface is texturized and corroded, so that the texturing effect on each surface of the sliced semiconductor substrate is similar, so that after the passivation layer is formed on the sliced semiconductor substrate later, the passivation effect of the solar cell is improved.
[0135] The cutting surface includes at least one first region, and the at least one first region includes multiple molten silicon regions and a first texture region located between at least two molten silicon regions. The number and position of the first regions can be referred to the description of the first aspect, and will not be repeated here.
[0136] In the actual production of solar cells, the side surface of the sliced semiconductor substrate generally includes the "non-cut surface" that is not cut (i.e., the "non-cut side surface" described in the first aspect) and the "cut surface" formed after cutting (i.e., the "cut side surface" described in the first aspect). Silicon slag and silicon oxide are generally not attached to the above non-cut surface, and even if attached, the amount attached is very small and can be ignored. Therefore, the focus of discussion and analysis here is on the silicon slag and silicon oxide on the cut surface. An important source of the silicon slag and silicon oxide is that when cutting the cell sheet, the lossy laser used is used to irradiate the silicon substrate of the solar cell, and the silicon substrate absorbs the laser energy and melts and oxidizes to form. The portion of the silicon slag and silicon oxide that is retained after being processed is the molten silicon area in the present invention. In the sliced semiconductor substrate provided by the present invention, the cutting surface includes a first area, which is a guide groove area opened by the laser (laser lossy cutting area), and a first texture area is included between at least two molten silicon areas in the first area. At this time, compared with the situation in the prior art that the laser guide groove area on the cutting surface is all silicon slag and silicon oxide, in the embodiment of the present invention, the distribution area and shape of the molten silicon area on the cutting surface are controlled so that the relative area of the molten silicon area is within a reasonable range, and the first area also includes a first texture area, which can improve the light trapping effect of the side surface 1 of the solar cell by utilizing the first texture area 21 and the side of the molten silicon area, increase the absorbance, and the relatively regular shape of the first texture area 21 can improve the film forming quality of the passivation layer, thereby improving the passivation effect.
[0137] In an optional manner, in the first region, the ratio of the total area of the molten silicon region to the total area of the first texture region is greater than or equal to 30% and less than or equal to 120%. For example, the ratio of the total area of the molten silicon region to the total area of the first texture region can be 30%, 40%, 50%, 60%, 70%, 80%, 90%, 100%, 110% or 120%, etc.
[0138] The ratio of the total area of the molten silicon zone 20 to the total area of the first texture zone 21 is within the above range, which can not only reduce the complexity of the manufacturing process caused by pursuing an overly small total area of the molten silicon zone 20. At the same time, it can also ensure the utilization rate of light by the side surface 1 of the solar cell, and optimize the overall passivation effect of the first area to improve the photoelectric conversion efficiency of the solar cell. Multiple molten silicon zones are distributed in the first area in isolated island shapes. Multiple island-shaped molten silicon zones are conducive to reflecting more light through their side walls to the first texture zone, thereby improving the light trapping effect of the cut surface of the solar cell and increasing the absorbance to improve the utilization rate of light by the side surface of the solar cell, thereby improving the photoelectric conversion efficiency of the solar cell. Preferably, the molten silicon zone is an irregular polygon and is evenly distributed in the first area.
[0139] As a possible implementation manner, the above-mentioned cutting surface also includes a third area, and the third area includes a third texture area, which is beneficial to improving the light trapping function and passivation effect of the third area.
[0140] The structure included in the first texture area and the structure included in the third texture area may be the same or different. Further, the structure included in the first texture area and the structure included in the third texture area may be a velvet structure or a tower base structure. The following description is given by taking two possible cases as examples. It should be understood that the following description is only for understanding and is not intended to be specifically limited.
[0141] Example 1: The first texture area includes a suede structure, the third texture area includes a suede structure, and the suede structure included in the first texture area and the suede structure included in the third texture area both include a pyramid structure.
[0142] When the velvet structure on the first texture area and the third texture area is a pyramid structure, it is beneficial to increase the specific surface area of the cut surface. Based on this, it is beneficial to make the cut surface have a good light trapping effect, further improving the utilization rate of light by the solar cell.
[0143] Since the first region includes a plurality of molten silicon regions, during the wet process, the growth time of the first texture region in the first region is shorter than the growth time of the third texture region in the third region. Therefore, the average height of the pyramid structure of the first texture region is smaller than the average height of the pyramid structure of the third texture region, or the average bottom width of the pyramid structure of the first texture region is smaller than the average bottom width of the pyramid structure of the third texture region.
[0144] The second type: the first texture area includes a tower base structure, and the third texture area includes a tower base structure. The tower base transverse dimension of the tower base structure of the first texture area is smaller than the tower base transverse dimension of the tower base structure of the third texture area. It should be noted that when the top view of the tower base is a quadrilateral, the tower base transverse dimension can be the length of any side or diagonal of the quadrilateral.
[0145] In an optional manner, the tower base structure of the first texture area includes a boss-type structure or a recessed groove-like structure, and the tower base structure of the third texture area includes a boss-type structure or a recessed groove-like structure.
[0146] Compared with a tower base structure that forms a plane, the tower base structure with the above-mentioned boss-shaped structure or recessed groove-shaped structure can further increase the roughness of the cut surface, thereby helping to reduce the reflectivity of the cut surface, so as to further improve the utilization rate of light by the solar cell.
[0147] It should be understood that the semiconductor substrate also includes a side surface connecting the first surface and the second surface. According to the final result of the cutting, the side surface includes a cutting surface and a non-cutting surface. For the description of the cutting surface, reference can be made to the previous text and will not be repeated here. For the non-cutting surface, a fourth texture area may be included, and the fourth texture area may include a velvet structure and a tower base structure. Among them, the velvet structure may include a pyramid structure, and the tower base structure may include a boss-type structure or a recessed groove-like structure. The sizes of the velvet structure and tower base structure in the above-mentioned third texture area and the velvet structure and tower base structure in the fourth texture area may be the same or different. The sizes of the velvet structure and tower base structure in the fourth texture area must be larger than the sizes of the velvet structure and tower base structure in the first texture area.
[0148] After cleaning the damaged cut surfaces of the sliced semiconductor substrate, the method for preparing a solar cell further includes: forming a passivation layer at least on the cut surfaces of the sliced semiconductor substrate.
[0149] At this time, the passivation effect of the solar cell can be improved to improve the photoelectric conversion efficiency of the solar cell. In addition, since a passivation layer is formed on the cut surface of the sliced semiconductor substrate after cleaning, the surface dangling bonds generated by the cut surface of the sliced semiconductor substrate being directly exposed to the air can be saturated under the action of the passivation layer. Based on this, the minority carrier lifetime of the cut surface can be increased to reduce the recombination current, thereby improving the conversion efficiency of the solar cell and the component power.
[0150] In an optional manner, the passivation layer comprises a stacked multilayer structure, such as a stacked film of aluminum oxide and silicon nitride, and the passivation layer is located on the cut surface of the semiconductor substrate to enhance the protection of the cut surface.
[0151] When the above technical solution is adopted, the stacked aluminum oxide passivation layer and silicon nitride passivation layer can passivate the cut surface, reduce the recombination rate of carriers at the cut surface, and further improve the photoelectric conversion efficiency of the solar cell. Furthermore, the silicon nitride passivation layer can play an anti-reflection role, which is conducive to refracting more light from the cut surface into the semiconductor substrate, so as to further improve the utilization rate of light by the solar cell.
[0152] The following takes the manufacturing process of two types of solar cells as an example to describe the location of the step of "slicing" described above. It should be understood that the following description is only for understanding and is not intended to be a specific limitation.
[0153] The first category is for TOPCon batteries. The production process of TOPCon batteries includes:
[0154] S1, providing a semiconductor substrate;
[0155] S2, cleaning and texturing the semiconductor substrate;
[0156] S3, performing boron diffusion and etching on the textured semiconductor substrate to form a PN junction on the light-receiving side of the semiconductor substrate;
[0157] S4, polishing the backlight surface of the semiconductor substrate to remove the diffusion layer on the backlight surface of the semiconductor substrate;
[0158] S5, sequentially forming a tunneling oxide layer and a doped polysilicon layer on the backlight surface of the semiconductor substrate;
[0159] S6, cleaning the semiconductor substrate to remove the light-receiving surface of the semiconductor substrate and the PSG layer that is expanded on the side, as well as the BSG layer on the light-receiving surface and the PSG layer on the backlight surface;
[0160] S7, forming a passivation anti-reflection layer on the surface of the structure formed in the above steps.
[0161] The step of "slicing" described above can be located at any position after S1 and before S6, for example, after S1 and before S2, or after S2 and before S3, or after S3 and before S4, or after S4 and before S5, or after S5 and before S6; after the slicing is completed, the liquid and process parameters in the cleaning process of step S6 can be controlled to obtain the solar cell described in the first aspect of the present invention. In this embodiment, it is preferred that the first texture area includes a tower base structure, and the second texture area includes a tower base structure; in addition, in another case, the semiconductor substrate provided in step S1 is already a pre-sliced semiconductor substrate, for example, it has been sliced before entering the cell production process.
[0162] The second category is for BC batteries. The production process of the first BC battery includes:
[0163] S1, providing a semiconductor substrate, wherein the semiconductor substrate comprises a first surface and a second surface opposite to each other;
[0164] S2, cleaning the semiconductor substrate;
[0165] S3, forming a first doped semiconductor material layer on the second surface;
[0166] S4, performing patterning on the first doped semiconductor material layer to form a first doped semiconductor layer on a partial area of the second surface;
[0167] S5, forming a second doped semiconductor material layer on the second surface;
[0168] S6, performing patterning on the second doped semiconductor material layer so that the first doped semiconductor layers and the second doped semiconductor layers are alternately arranged;
[0169] S7, cleaning and / or texturing the semiconductor substrate;
[0170] S8, forming a passivation anti-reflection layer on the first surface of the semiconductor substrate, the first doped semiconductor material layer and the second doped semiconductor material layer.
[0171] The step of "slicing" described above can be located at any position after S1 and before S7, such as after S1, before S2, or after S2, before S3, or after S3, before S4, or after S4, before S5, or after S5, before S6, or after S5, before S6, or after S6, before S7; after the slicing is completed, the chemical solution, process parameters, etc. in step S7 can be controlled to obtain the solar cell described in the first aspect of the present invention. In addition, in another case, the semiconductor substrate provided in step S1 is already a pre-sliced semiconductor substrate, for example, it has been sliced before entering the cell production process.
[0172] The production process of the second BC battery includes:
[0173] S1, providing a semiconductor substrate, wherein the semiconductor substrate comprises a first surface and a second surface opposite to each other;
[0174] S2, cleaning the semiconductor substrate;
[0175] S3, forming a first doped semiconductor material layer on the second surface;
[0176] S4, patterning the first doped semiconductor material layer to form a first doped semiconductor layer on a partial region of the semiconductor substrate;
[0177] S5, cleaning and / or texturing the semiconductor substrate;
[0178] S6, forming a passivation anti-reflection layer on the first surface of the semiconductor substrate, the first doped semiconductor material layer, and the area of the second surface of the semiconductor substrate exposed outside the first doped semiconductor layer.
[0179] The step of "slicing and slicing" described above can be located at any position after S1 and before S5, for example, after S1 and before S2, or after S2 and before S3, or after S3 and before S4, or after S4 and before S5; after the slicing and slicing is completed, the chemical solution, process parameters, etc. in step S5 can be controlled to obtain the solar cell described in the first aspect of the present invention. In addition, in another case, the semiconductor substrate provided in step S1 is already a pre-sliced semiconductor substrate, for example, it has been sliced and sliced before entering the cell production process.
[0180] In a third aspect, an embodiment of the present invention further provides a photovoltaic module. The photovoltaic module comprises: a plurality of solar cells as described in the first aspect, or solar cells prepared by the second aspect; and an encapsulation layer covering the surfaces of the plurality of solar cells; and a cover plate covering the surface of the encapsulation layer away from the solar cells.
[0181] In the description of the above embodiments, specific features, structures, materials or characteristics may be combined in a suitable manner in any one or more embodiments or examples.
[0182] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A solar cell, characterized in that: The solar cell includes a first surface and a second surface opposite to each other, and a side surface connecting the first surface and the second surface; The side surface includes at least one first region; at least one of the first regions includes a plurality of molten silicon regions, and a first texture region located between at least two of the molten silicon regions; the molten silicon region has a thickness on the side surface; A passivation layer is also included, and the passivation layer includes a portion located on the side surface.
2. The solar cell according to claim 1, characterized in that In the first region, a ratio of a total area of the molten silicon region to a total area of the first texture region is greater than or equal to 30% and less than or equal to 120%.
3. The solar cell according to claim 1, characterized in that The plurality of molten silicon regions are distributed in the first region in an island shape; and / or the maximum width of the molten silicon region is less than 100 micrometers.
4. The solar cell according to claim 1, characterized in that A ratio of a width of the first region to a thickness of the solar cell is greater than or equal to 30% and less than or equal to 100%; a width direction of the first region and a thickness direction of the solar cell are both consistent with a direction from the first surface to the second surface.
5. The solar cell according to claim 1, characterized in that: The first region includes a trench structure.
6. The solar cell according to claim 5, characterized in that: The groove structure extends in any one or more of a dendrite, a straight line, a broken line, and a curve; and / or the depth of the groove structure is 1 micron to 10 microns; and / or the cross-section of the groove structure is any one or more of a V-shape and a U-shape.
7. The solar cell according to claim 1, characterized in that The molten silicon region includes a multilayer structure arranged in a stacked manner; and / or, the molten silicon region includes a porous structure; and / or, the molten silicon region includes silicon oxide.
8. The solar cell according to any one of claims 1 to 7, characterized in that: The side surface further includes a second region including a second textured area.
9. The solar cell according to claim 8, characterized in that The side surfaces include cutting side surfaces and non-cutting side surfaces; The first area is located on the cutting side surface; The second region is located on the cutting side surface and / or the non-cutting side surface.
10. The solar cell according to claim 8, characterized in that The first texture area includes a velvet structure, and the second texture area includes a velvet structure; the velvet structure included in the first texture area and the velvet structure included in the second texture area both include pyramid structures; the average height of the pyramid structures in the first texture area is smaller than the average height of the pyramid structures in the second texture area, or the average bottom width of the pyramid structures in the first texture area is smaller than the average bottom width of the pyramid structures in the second texture area.
11. The solar cell according to claim 8, characterized in that The first texture area includes a tower foundation structure, and the second texture area includes a tower foundation structure; the tower foundation transverse dimension of the tower foundation structure of the first texture area is smaller than the tower foundation transverse dimension of the tower foundation structure of the second texture area.
12. The solar cell according to claim 11, characterized in that: The tower base structure of the first texture area includes a boss-shaped structure or a recessed groove-shaped structure; The tower base structure of the second texture area includes a boss-shaped structure or a recessed groove-shaped structure.
13. The solar cell according to any one of claims 1 to 7, characterized in that: The solar cell includes a first chamfer and a second chamfer opposite to each other; a side surface of the first chamfer includes the first region.
14. The solar cell according to claim 13, characterized in that: The first chamfer is smaller than the second chamfer.
15. The solar cell according to claim 1, characterized in that The passivation layer also includes portions located on a first surface and a second surface; the first surface is a light-facing surface, and an average thickness of the passivation layer located on the side surface is less than an average thickness of the passivation layer located on the first surface.
16. The solar cell according to claim 9, characterized in that It also includes a passivation layer, which includes a first passivation layer and a second passivation layer; the first passivation layer includes a portion located on the first surface or the second surface, the second passivation layer includes a portion located on the cut side surface, and the average thickness of the second passivation layer located on the cut side surface is greater than the average thickness of the first passivation layer located on the first surface or the second surface.
17. The solar cell according to claim 16, wherein the second passivation layer further comprises a portion located at an edge of the first surface and located above the first passivation layer, the edge of the first surface being close to the cut side surface; and / or, The second passivation layer also includes a portion located at an edge of a second surface and located above the first passivation layer, wherein the edge of the second surface is close to the cut side surface.
18. The solar cell according to claim 17, wherein the average thickness of the second passivation layer located on the cut side surface is greater than or equal to 10 nanometers and less than or equal to 120 nanometers; and / or the average thickness of the second passivation layer located on the edge of the first surface is less than the average thickness of the second passivation layer located on the cut side surface; and / or the average thickness of the second passivation layer located on the edge of the second surface is less than the average thickness of the second passivation layer located on the cut side surface.
19. The solar cell according to claim 1, wherein the coverage of the passivation layer in the first region is smaller than that in the region of the side surface other than the first region; and / or the coverage of the passivation layer in the first region is greater than 80%.
20. A method for preparing a solar cell, comprising: Providing a semiconductor substrate, the semiconductor substrate comprising a first surface and a second surface opposite to each other; Processing the first surface with a first laser process to form a groove on the first surface, wherein the groove extends along a first direction; Using a second laser process to perform heat treatment on the first surface along the first direction and form a heat treatment path; dividing the semiconductor substrate into at least two semiconductor substrate slices along the heat treatment path; Cleaning the cut surface of the sliced semiconductor substrate for damage; the cut surface includes at least one first region; at least one first region includes a plurality of molten silicon regions and a first texture region located between at least two of the molten silicon regions; the molten silicon region has a thickness on the side surface; After cleaning the cut surfaces of the sliced semiconductor substrate, the method for preparing a solar cell further comprises: A passivation layer is formed at least on the cut surface of the sliced semiconductor substrate.
21. The method for preparing a solar cell according to claim 20, characterized in that: The groove comprises a first portion, a second portion and a third portion; the first end of the first portion and the first end of the second portion are both connected to one end of the third portion; the distance between the first portion and the second portion gradually increases in a direction away from the third portion; the second end of the first portion and the second end of the second portion are close to the edge of the semiconductor substrate; The angle between the first portion and the third portion is equal to the angle between the second portion and the third portion.
22. The method for preparing a solar cell according to claim 20, characterized in that: The ratio of the depth of the groove to the thickness of the semiconductor substrate is greater than or equal to 30% and less than or equal to 100%, and the depth direction of the groove is consistent with the thickness direction of the semiconductor substrate; And / or; the second laser process uses lossless thermal cracking laser.
23. A photovoltaic module, characterized in that: include: A plurality of solar cells according to any one of claims 1 to 19, or a plurality of solar cells prepared by the method for preparing a solar cell according to any one of claims 20 to 22; An encapsulation layer, covering the surface of the plurality of solar cells; A cover plate covers a surface of the encapsulation layer away from the solar cell.
Citation Information
Patent Citations
Fragmented battery, formation method thereof and photovoltaic module
CN118016739A
Photovoltaic device
JP2006286820A