A glass substrate for solidifying high-calcium and high-titanium medium- and low-level radioactive waste ash, and its preparation method and application
By introducing specific components and process treatments into the glass substrate, the problem of vitrification of high-calcium, high-titanium, medium and low-level radioactive waste ash has been solved, stable glass solidification formation and long-term fixation of nuclides have been achieved, and the existing problems have been solved. Problems with crystallization and insufficient stability in technology.
Patent Information
- Application Number
- CN202410681586.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-29
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-05-29
AI Technical Summary
The existing glass solidification process is difficult to apply to medium and low radioactive waste ash with large composition fluctuations of high calcium and titanium, and it can easily lead to glass crystallization, affecting the long-term stable fixation of nuclides.
A glass substrate is used, containing components such as SiO2, B2O3, Al2O3, Na2O, BaO, ZnO and SnF2. Through high-temperature melting and annealing treatment, a stable glass network structure is formed to inhibit the formation of Ti-O-Ti enriched areas. , reduce the crystallization tendency of glass, and optimize the chemical stability and melting performance of glass.
It achieves effective solidification of high calcium, high titanium, medium and low radioactive waste ash, reduces the crystallization rate, ensures the chemical stability and long-term solidification performance of the glass body, is suitable for deep geological disposal of radioactive waste, and reduces disposal costs.
Smart Images

Figure CN118420218B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of radioactive waste treatment, and in particular to a glass substrate for solidifying high-calcium and high-titanium medium- and low-level radioactive waste ash, and a preparation method and application thereof. Background Art
[0002] As a key link in promoting the realization of the "dual carbon" strategic goal, my country's nuclear energy industry has developed rapidly in recent years, and the technical waste generated by nuclear power plants during operation and maintenance will also increase accordingly. Nuclear power plant technical waste is mainly composed of combustible solid wastes such as protective clothing (mainly cotton products), protective gloves (mainly rubber), polyethylene, and paper products. It has the characteristics of low radioactivity and large volume. Its safe and efficient treatment and disposal is the key to determining the sustainable development of my country's nuclear power.
[0003] Low- and medium-level radioactive solid waste is usually solidified and encapsulated before being disposed of in shallow landfills. In order to avoid occupying too much land resources, the volume of waste is generally reduced through pre-treatment methods such as compression, incineration or pyrolysis. However, compression and volume reduction are limited, and the nuclides are not effectively fixed; the ash produced by incineration or pyrolysis is solidified with cement before being disposed of in landfills, which leads to problems such as waste volume expansion and poor resistance to leaching of the solidified body. In order to efficiently reduce the volume of such combustible solid waste and safely solidify the toxic elements therein, in recent years, thermal plasma gasification and melting treatment technology for low- and medium-level combustible solid waste has gradually emerged. Thermal plasma technology decomposes organic matter in the waste through thermal plasma gasification, greatly reducing the volume of the waste. The residual inorganic gasified ash is mixed with glass additives and melted at high temperature to form a glass solidified body with stable chemical properties, which is then disposed of in shallow landfills. However, due to the wide sources of technical waste, the composition of the ash after gasification is complex and changeable, and the ash of some combustible solid wastes (such as cotton fabrics and paper products) contains not only a lot of Ca (generally greater than 50wt%, calculated as oxide), but also a high Ti content (generally not less than 30wt%, calculated as oxide). Such elements are prone to cause vitreous crystallization, which not only affects the normal operation of the furnace, but also may destroy the anti-leaching property of the vitreous body, leading to the risk of nuclide migration. Therefore, it is challenging to develop a corresponding glass solidification compatibility.
[0004] The existing patent technologies for glass solidification of combustible solid waste are as follows: ① The existing patent 201410534421.2 discloses a glass matrix composition for low- and medium-level radioactive combustible waste incineration ash and a glass solidified body prepared therefrom, which is a glass solidification treatment for the special physical and chemical properties of low- and medium-level radioactive combustible wastes such as absorbent paper, cotton products, plastic cloth, and rubber produced by nuclear facilities. However, the glass matrix in this technical solution is only for a single combustible waste incineration ash, and the ash does not contain Ti. ② The existing patent 201380081452.0 discloses a glass composition for the vitrification of mixed wastes and a method for vitrification of mixed wastes using the same. According to the actual combustible mixed wastes such as gloves, work clothes, plastics, and rubber, a glass additive composition suitable for solidifying combustible mixed waste incineration ash has been developed. However, this technical solution is only applicable to the glass solidification of waste ash with a titanium content of less than 5wt%. ③ The existing patent 202011278158.7 discloses a method for the coordinated glass solidification of medium and low-level radioactive glass fibers and combustible solid nuclear waste incineration ash. According to the composition characteristics of the wastes, a series of mixed formulas for the vitrification of medium and low-level radioactive waste incineration ash from nuclear power plants have been developed to minimize the amount of glass additives. However, this technical solution is applicable to medium and low-level radioactive waste with a certain waste ratio and a single ash composition, and cannot be applied to high-calcium and high-titanium waste ash with large composition fluctuations. Summary of the invention
[0005] In view of this, the present invention proposes a glass substrate for solidifying high-calcium and high-titanium low- and intermediate-level radioactive waste ash, and a preparation method and application thereof, so as to solve the technical problems that the existing glass solidification process is difficult to apply to high-calcium and high-titanium waste ash with large composition fluctuations and the existing glass solidification process is prone to cause crystallization of high-calcium and high-titanium low- and intermediate-level radioactive waste glass.
[0006] The technical solution of the present invention is achieved in this way:
[0007] In a first aspect, the present invention provides a glass substrate for solidifying high-calcium and high-titanium low- and medium-level radioactive waste ash, wherein the glass substrate comprises the following components in terms of oxide mass percentage: SiO 2 :35~60wt%、B 2 O 3 :10~25wt%、Al 2 O 3 :3~20wt%、Na 2 O: 5-25wt%, BaO: 12-30wt%, ZnO: 6-28wt% and SnF 2 :0.1~6wt%.
[0008] High calcium and high titanium low-level radioactive waste ash is composed of CaO, TiO 2The content of SiO is relatively high, which results in the formation of Ti-containing crystals during the vitrification process, thus affecting the stability of the final glass product. 2 With B 2 O 3 It is a glass network former and a basic component of glass; Al 2 O 3 It is a glass network intermediate and plays a role in enhancing the chemical stability of glass; Na 2 O and BaO are glass network modifiers, which are used to improve the glass melting process and reduce the glass viscosity. ZnO is a glass network intermediate. When there is enough free oxygen in the glass, [ZnO 4 ] enter the glass network, making the glass structure more stable.
[0009] TiO 2 In glass, [TiO 4 ]、[TiO 5 ] or [TiO 6 ] is connected to the glass network. 4 ] can replace [SiO 4 ] forms a Si-O-Ti network connection, but Na + It will also promote [TiO 5 ] or [TiO 6 ] to form a balanced charge, resulting in the Ti-O-Ti enriched region, resulting in the precipitation of Ti-containing phase. 2 , which can effectively reduce the precipitation of Ti-containing phase, among which F - Can be used to balance the charge and reduce [TiO 5 ] or [TiO 6 ], thereby reducing the tendency of Ti-O-Ti enrichment and inhibiting the tendency of glass crystallization. 4+ It can be used as a glass clarifier to reduce bubbles in the glass melt and reduce the possibility of non-uniform nucleation of glass at the bubble interface. 2 It will cause glass phase separation, destroy the chemical stability of the glass solid body, and make it unable to meet the requirements of radioactive waste disposal. 2 The addition of will also enhance the volatilization of nuclides such as Cs and Sr during high-temperature melting.
[0010] On the basis of the above technical solution, preferably, the glass substrate comprises the following components in terms of oxide mass percentage: SiO 2 :35~50wt%、B 2 O 3 :12~20wt%、Al 2 O 3:3~12wt%、Na 2 O: 5-15wt%, BaO: 15-20wt%, ZnO: 8-15wt% and SnF 2 : 1~5wt%.
[0011] SiO 2 and B 2 O 3 The total content of Al is increased to 47-70wt%, which enhances the formation of glass network and the overall structural stability; 2 O 3 The upper limit of the content is increased to 12wt%, further improving the chemical stability of the glass; Na 2 Maintaining the total content of O and BaO at 20-35wt% can better optimize the melting properties of the glass; increasing the content of ZnO to 8-15wt% is conducive to the formation of more [ZnO 4 ]Structural reinforcement glass network; SnF 2 The content of Ti is controlled at 1-5wt%, which can effectively inhibit the precipitation of Ti-containing crystal phase, while not causing excessive glass phase separation and increased volatilization of radionuclides.
[0012] In a second aspect, the present invention provides a method for preparing a glass substrate for solidifying high-calcium and high-titanium low- and medium-level radioactive waste ash, comprising the following steps:
[0013] S1, the proportion of the configuration containing SiO 2 , B 2 O 3 、Al 2 O 3 、Na 2 O, BaO, ZnO and SnF 2 The glass base material batch materials are mixed evenly and then melted at high temperature to obtain a glass melt;
[0014] S2. Pour the molten glass into the preheated mold, and after annealing and cooling, obtain a glass substrate.
[0015] On the basis of the above technical solution, preferably, the high temperature melting temperature is 1150-1400°C, the high temperature melting time is 1-8h, the annealing temperature is 300-600°C, and the annealing time is 1-6h, which are used to release thermal stress in the glass.
[0016] Specifically, the high temperature melting treatment is carried out at 1150-1400°C to ensure that all components are fully melted and evenly mixed to form a uniform glass melt. Too low a temperature will cause some high melting point components (such as SiO 2 ) is difficult to melt completely, and too high a temperature will aggravate the volatilization loss of glass components (such as Na 2O). Appropriate high-temperature melting helps to fully form the glass network and obtain a uniform and stable glass body. When the glass product is cooled from the high-temperature melt to room temperature, the temperature difference between the inside and outside causes thermal stress inside the glass. This stress will reduce the strength of the glass and increase the risk of cracking. Annealing at 300-600℃ can provide a certain amount of heat energy to the glass molecular segments, thereby releasing internal stress.
[0017] In the third aspect, the present invention provides an application of a glass substrate for solidifying high-calcium, high-titanium, intermediate and low-level radioactive waste ash. The glass substrate is mixed with the high-calcium, high-titanium, intermediate and low-level radioactive waste ash, kept warm at 1150-1300°C for 1-6 hours, and the glass liquid is poured into a preheated metal mold, annealed and cooled, the annealing temperature is 300-600°C, and the annealing time is 1-6 hours, to prepare a high-calcium, high-titanium, intermediate and low-level radioactive waste glass solidified body.
[0018] On the basis of the above technical solution, preferably, the high calcium and high titanium low-level and intermediate-level waste ash comprises the following components by weight percentage of oxides: CaO: 35-55wt%, TiO 2 :15~28wt%、SiO 2 :10~15wt%、Al 2 O 3 :2~7wt%、Na 2 O: 1~4wt%, MgO: 0~5wt%, BaO: 2~5wt%, ZnO: 1~3wt%, K 2 O: 0-1 wt%, B 2 O 3 :0~1wt%、Fe 2 O 3 :0~1wt%、P 2 O 5 :0~2wt%、SO 3 : 1-3wt%, and less than 1wt% of oxides of radioactive elements.
[0019] On the basis of the above technical solution, preferably, the radioactive elements include Cs, Sr and Co.
[0020] The present invention selects CaO and TiO in the high-calcium and high-titanium medium and low-level radioactive waste ash. 2 The content is very high (35-55wt% and 15-28wt%), which easily leads to glass crystallization. 2 (1~5wt%), F - Balanced charge suppression [TiO 5 ] or [TiO 6 ] formation and enrichment, Sn 4+As a clarifier, it reduces non-uniform nucleation and effectively inhibits the precipitation of Ti-containing crystal phase. 2 、Al 2 O 3 、Na 2 O, BaO and other components can be well integrated into the glass matrix network, and B 2 O 3 、Na 2 The presence of O and other elements can lower the melting temperature of glass and reduce the volatilization of radioactive elements.
[0021] On the basis of the above technical solution, preferably, calculated by mass percentage of oxides, the glass substrate accounts for 50-80wt% in the glass solid body, and the high-calcium and high-titanium low- and medium-level radioactive waste ash accounts for 20-50wt% in the glass solid body.
[0022] On the basis of the above technical solution, preferably, calculated by mass percentage of oxides, the glass substrate accounts for 60-70wt% in the glass solid body, and the high-calcium and high-titanium low- and medium-level radioactive waste ash accounts for 30-40wt% in the glass solid body.
[0023] On the one hand, the glass substrate is the main body of the solidified body, and its proportion needs to be high enough (≥50wt%) to form a stable glass network structure, ensuring that the solidified body has good chemical stability and a low crystallization rate. A too low proportion of the substrate will lead to an incomplete glass network and reduced performance. On the other hand, from the perspective of volume reduction and capacity increase, the glass substrate has a good match with high-calcium and high-titanium ash slag, and the ash slag proportion can reach 20-50wt%. Compared with the general medium and low-level waste borosilicate glass substrate (waste load ~30wt%), it effectively increases the waste load and saves the final radioactive waste package disposal space.
[0024] On the basis of the above technical solution, preferably, the glass substrate is spherical or granular, and the particle size of the glass substrate is 0.1 mm to 3 mm.
[0025] In order to make the glass substrate and the ash fully contact and interact with each other, accelerate the diffusion of components and chemical reactions, thereby promoting the uniform melting of the melt and obtaining a homogeneous glass solidification body with stable quality, the particle size of the glass substrate is set to 0.1-3 mm in the present invention. If the particle size of the glass substrate is too small (such as <0.1 mm), it will cause dust pollution, feed port blockage and other problems; if the particle size of the glass substrate is too large (such as >3 mm), the contact area between the glass substrate and the ash will be reduced, the melting time will be prolonged, and the glass melting efficiency will be reduced.
[0026] The glass substrate for solidifying high-calcium and high-titanium low- and medium-level radioactive waste ash and its preparation method and application of the present invention have the following beneficial effects compared with the prior art:
[0027] (1) The glass substrate composition of the present invention is optimized and designed, and has wide applicability and good inclusion effect for high-calcium and high-titanium medium- and low-level radioactive waste ash from different sources and compositions. 2 O 3 , ZnO and other components can react with CaO, TiO 2 etc. are well compatible to form a uniform and stable glass network structure. The ash proportion can be flexibly adjusted within the range of 20-50wt%, which effectively increases the waste load and reflects the advantages of glass solidification and volume reduction;
[0028] (2) By introducing SnF into the glass substrate 2 As a crystallization inhibitor, the content of BaO, ZnO and other components is precisely controlled at the same time, effectively inhibiting the precipitation of Ti-containing crystal phase. The prepared high-calcium and high-titanium waste glass solid has a low crystallization rate. The low crystallization rate means that the glass matrix structure is intact and has excellent chemical stability, which can ensure the long-term stable fixation of radioactive nuclides and avoid the risk of nuclide release caused by crystallization.
[0029] (3) The high-calcium and high-titanium waste glass solid body prepared from the glass substrate of the present invention has excellent chemical durability, meets the strict requirements for radioactive waste disposal, and is suitable for long-term deep geological disposal; at the same time, while ensuring the excellent mechanical properties and chemical stability of the glass solid body, it significantly increases the waste load and reduces the disposal cost to a certain extent, reflecting the high practicality and economy of the glass solidification technology. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0031] Figure 1 The solidified bodies obtained in Example 1 and Comparative Example 2 of the present invention are shown in FIG.
[0032] Figure 2 The XRD diffraction spectra of the glass solidified bodies prepared in Example 1, Example 2 and Comparative Example 1 of the present invention are shown;
[0033] Figure 3 The XRD diffraction patterns of the glass solidified bodies prepared in Example 1 and Comparative Example 1 of the present invention after heat treatment are shown. DETAILED DESCRIPTION
[0034] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0035] Example 1
[0036] This embodiment provides a glass substrate for solidifying high-calcium and high-titanium low- and medium-level radioactive waste ash and a preparation method and application thereof, which specifically includes the following steps:
[0037] S1. Weigh 100g of the mixture according to the composition of the glass substrate. The glass substrate, calculated by oxide mass percentage, includes the following components: SiO 2 :38.3wt%、B 2 O 3 :14.36wt%,Al 2 O 3 :4.79wt%, Na 2 O: 9.57wt%, BaO: 19.15wt%, ZnO: 9.57wt% and SnF 2 :4.26wt%of which SiO 2 、Al 2 O 3 and ZnO is introduced in the form of oxide, B 2 O 3 H 3 BO 3 Form introduction, Na 2 O with Na 2 CO 3 In the form of BaO, BaCO 3 Form introduction, SnF 2 SnF 2 The mixture was fully mixed and placed in a 150 mL corundum crucible, and then moved to a 1300 ° C muffle furnace for 2 hours. The crucible was then quickly taken out, and the glass liquid was poured into a metal mold preheated at 500 ° C. The cooled solid glass was quickly moved to a 500 ° C muffle furnace for annealing for 4 hours, and cooled with the furnace. Finally, 1-3 mm glass substrate particles were obtained by crushing and screening.
[0038] S2, simulated high calcium and high titanium low-level radioactive waste ash oxides, including the following components by oxide mass percentage: CaO: 44.52wt%, TiO 2 :22.4wt%、SiO 2 :12.15wt%,Al 2 O 3:4.74wt%, Na 2 O: 1.98wt%, MgO: 3.44wt%, BaO: 4.08wt%, ZnO: 1.56wt%, K 2 O: 0.71wt%, B 2 O 3 :0.21wt%, Fe 2 O 3 :0.37wt%、P 2 O 5 :1.43wt%、SO 3 :2.41wt%. The glass substrate oxide accounts for 70wt%, the simulated high calcium and high titanium medium and low radioactive waste ash oxide accounts for 30wt% and a small amount of simulated nuclides (Co 2 O 3 、SrO、Cs 2 O each accounting for 0.2wt% of the glass solid body) are weighed and proportioned, 100g of the mixture is weighed and placed in a 150mL corundum crucible, moved to a 1300℃ muffle furnace and kept warm for 2h, and the glass liquid is poured into a metal mold preheated at 500℃, and annealed at 500℃ for 4h to obtain a simulated high-calcium and high-titanium medium- and low-level radioactive waste glass solid body.
[0039] Example 2
[0040] This embodiment provides a glass substrate for solidifying high-calcium and high-titanium low- and medium-level radioactive waste ash and a preparation method and application thereof, which specifically includes the following steps:
[0041] S1. Weigh 200g of the mixture according to the composition of the glass substrate. The glass substrate, calculated by oxide mass percentage, includes the following components: SiO 2 :38.3wt%、B 2 O 3 :14.36wt%,Al 2 O 3 :4.79wt%, Na 2 O: 9.57wt%, BaO: 19.15wt%, ZnO: 9.57wt% and SnF 2 :4.26wt%of which SiO 2 and ZnO is introduced in the form of oxide, Al 2 O 3 Al(OH) 3 Form introduction, B 2 O 3 B 2 O 3 Form introduction, Na 2 O with Na 2 CO 3 In the form of BaO, BaCO3 Form introduction, SnF 2 SnF 2 The mixture was fully mixed and placed in a 200 mL corundum crucible, and then moved to a 1300 ° C muffle furnace for 4 hours. The crucible was then quickly taken out, and the glass liquid was poured into a metal mold preheated at 500 ° C. The cooled solid glass was quickly moved to a 500 ° C muffle furnace for annealing for 6 hours, and cooled with the furnace. Finally, 1-3 mm glass substrate particles were obtained by crushing and screening.
[0042] S2, simulated high calcium and high titanium low-level radioactive waste ash oxides, including the following components by oxide mass percentage: CaO: 36.09wt%, TiO 2 :27.08wt%、SiO 2 :13.71wt%, Al 2 O 3 :5.46wt%, Na 2 O: 2.38wt%, MgO: 3.59wt%, BaO: 4.92wt%, ZnO: 1.22wt%, K 2 O: 0.84wt%, B 2 O 3 :0.27wt%, Fe 2 O 3 :0.43wt%、P 2 O 5 :1.66wt%、SO 3 :2.35wt%. According to the glass substrate oxide weight accounting for 70wt%, the simulated high calcium and high titanium medium and low radioactive waste ash oxide weight accounting for 30wt% and a small amount of simulated nuclides (Co 2 O 3 、SrO、Cs 2 O each accounting for 0.2wt% of the glass solid body) are weighed and proportioned, 100g of the mixture is weighed and placed in a 150mL corundum crucible, moved to a 1300℃ muffle furnace and kept warm for 2h, and the glass liquid is poured into a metal mold preheated at 500℃, and annealed at 500℃ for 4h to obtain a simulated high-calcium and high-titanium simulated low- and intermediate-level waste glass solid body.
[0043] Example 3
[0044] This embodiment provides a glass substrate for solidifying high-calcium and high-titanium low- and medium-level radioactive waste ash and a preparation method and application thereof, which specifically includes the following steps:
[0045] S1. Weigh 500g of the mixture according to the composition of the glass substrate. The glass substrate, calculated by oxide mass percentage, includes the following components: SiO 2 :60wt%、B 2 O 3:10wt%,Al 2 O 3 :3wt%、Na 2 O: 5wt%, BaO: 12wt%, ZnO: 9.9wt% and SnF 2 :0.1wt% SiO 2 、Al 2 O 3 and ZnO is introduced in the form of oxide, B 2 O 3 H 3 BO 3 Form introduction, Na 2 O with Na 2 CO 3 In the form of BaO, BaCO 3 Form introduction, SnF 2 SnF 2 The mixture was fully mixed and placed in a 800 mL corundum crucible, and then moved to a 1400 ° C muffle furnace for 8 hours. The crucible was then quickly taken out, and the glass liquid was poured into a metal mold preheated at 600 ° C. The cooled solid glass was quickly moved to a 600 ° C muffle furnace for annealing for 6 hours, and cooled with the furnace. Finally, 1-3 mm glass substrate particles were obtained by crushing and screening.
[0046] S2, simulated high calcium and high titanium low-level radioactive waste ash oxides, including the following components by oxide mass percentage: CaO: 36wt%, TiO 2 :17wt%、SiO 2 :15wt%、Al 2 O 3 :7wt%、Na 2 O: 4wt%, MgO: 5wt%, BaO: 5wt%, ZnO: 3wt%, K 2 O: 1wt%, B 2 O 3 :1wt%,Fe 2 O 3 :1wt%、P 2 O 5 :2wt%、SO 3 :3wt%. According to the weight of glass substrate oxide accounting for 50wt%, the weight of simulated high calcium and high titanium medium and low radioactive waste ash oxide accounting for 50wt% and a small amount of simulated nuclides (Co 2 O 3 、SrO、Cs 2O each accounting for 0.2wt% of the glass solid body) are weighed and proportioned, 100g of the mixture is weighed and placed in a 150mL corundum crucible, moved to a 1300℃ muffle furnace and kept warm for 1h, and the glass liquid is poured into a metal mold preheated at 500℃, and annealed at 500℃ for 4h to obtain a simulated high-calcium and high-titanium medium- and low-level radioactive waste glass solid body.
[0047] Example 4
[0048] This embodiment provides a glass substrate for solidifying high-calcium and high-titanium low- and medium-level radioactive waste ash and a preparation method and application thereof, which specifically includes the following steps:
[0049] S1. Weigh 100g of the mixture according to the composition of the glass substrate. The glass substrate, calculated by oxide mass percentage, includes the following components: SiO 2 :35wt%、B 2 O 3 :15wt%、Al 2 O 3 :10wt%, Na 2 O: 15wt%, BaO: 12wt%, ZnO: 7wt% and SnF 2 :6wt% SiO 2 、Al 2 O 3 and ZnO is introduced in the form of oxide, B 2 O 3 H 3 BO 3 Form introduction, Na 2 O with Na 2 CO 3 In the form of BaO, BaCO 3 Form introduction, SnF 2 SnF 2 The mixture was fully mixed and placed in a 150 mL corundum crucible, and then moved to a 1150 ° C muffle furnace for 1 hour. The crucible was then quickly taken out and the glass liquid was poured into a metal mold preheated at 300 ° C. The cooled solid glass was quickly moved to a 300 ° C muffle furnace for annealing for 1 hour, and cooled with the furnace. Finally, 1-3 mm glass substrate particles were obtained by crushing and screening.
[0050] S2, simulated high calcium and high titanium low-level radioactive waste ash oxides, including the following components by oxide mass percentage: CaO: 55wt%, TiO 2 :28wt%、SiO 2 :10wt%,Al 2 O 3 :2wt%, Na 2 O: 1wt%, BaO: 2wt%, ZnO: 1wt%, SO3 :1wt%. The glass substrate oxide accounts for 80wt%, the simulated high calcium and high titanium medium and low radioactive waste ash oxide accounts for 20wt% and a small amount of simulated nuclides (Co 2 O 3 、SrO、Cs 2 O each accounting for 0.2wt% of the glass solid body) are weighed and proportioned, 100g of the mixture is weighed and placed in a 150mL corundum crucible, moved to a 1150℃ muffle furnace and kept warm for 2h, and the glass liquid is poured into a metal mold preheated at 300℃, and annealed at 300℃ for 1h to obtain a simulated high-calcium and high-titanium medium- and low-level radioactive waste glass solid body.
[0051] Example 5
[0052] This embodiment provides a glass substrate for solidifying high-calcium and high-titanium intermediate and low-level radioactive waste ash and a preparation method and application thereof. The specific steps are the same as those in Example 1, except that: in step S2, the weight of the glass substrate oxide accounts for 45wt%, the weight of the simulated high-calcium and high-titanium intermediate and low-level radioactive waste ash oxide accounts for 55wt% and a small amount of simulated nuclides (Co 2 O 3 、SrO、Cs 2 O each accounting for 0.2wt% of the glass solid body) are weighed and 100g of the mixture is weighed.
[0053] Comparative Example 1
[0054] This comparative example provides a glass substrate for solidifying high-calcium and high-titanium low- and medium-level radioactive waste ash and a preparation method and application thereof, which specifically comprises the following steps:
[0055] S1. Weigh 100g of the mixture according to the composition of the glass substrate. The glass substrate, calculated by oxide mass percentage, includes the following components: SiO 2 :40wt%、B 2 O 3 :15wt%、Al 2 O 3 :5wt%, Na 2 O: 10wt%, BaO: 20wt%, ZnO: 10wt%. Among them, SiO 2 、Al 2 O 3 and ZnO is introduced in the form of oxide, B 2 O 3 H 3 BO 3 Form introduction, Na 2 O with Na 2 CO 3 In the form of BaO, BaCO 3The mixture was fully mixed and placed in a 150 mL corundum crucible, and then moved to a 1300 ° C muffle furnace for 2 hours. The crucible was then quickly taken out, and the glass liquid was poured into a metal mold preheated at 500 ° C. The cooled solid glass was quickly moved to a 500 ° C muffle furnace for annealing for 4 hours, and cooled with the furnace. Finally, 1-3 mm glass substrate particles were obtained by crushing and screening.
[0056] The glass substrate oxide accounts for 70wt% by weight, and the simulated high-calcium and high-titanium low- and intermediate-level radioactive waste ash oxide accounts for 30wt% by weight (the chemical composition of the simulated high-calcium and high-titanium low- and intermediate-level radioactive waste ash oxide is the same as that in Example 1). 100g of the mixture is weighed and placed in a 150mL corundum crucible, moved to a 1300℃ muffle furnace and kept warm for 2h, and the glass liquid is poured into a metal mold preheated at 500℃, and annealed at 500℃ for 4h to obtain a simulated high-calcium and high-titanium simulated low- and intermediate-level radioactive waste glass solid body.
[0057] Comparative Example 2
[0058] This comparative example provides a glass substrate for solidifying high-calcium and high-titanium low- and medium-level radioactive waste ash and a preparation method and application thereof, which specifically comprises the following steps:
[0059] S1. Weigh 100g of the mixture according to the composition of the glass substrate. The glass substrate, calculated by oxide mass percentage, includes the following components: SiO 2 :35.55wt%、B 2 O 3 :13.33wt%, Al 2 O 3 :4.44wt%, Na 2 O: 8.89wt%, BaO: 17.78wt%, ZnO: 8.89wt% and SnF 2 :11.12wt% SiO 2 、Al 2 O 3 and ZnO is introduced in the form of oxide, B 2 O 3 H 3 BO 3 Form introduction, Na 2 O with Na 2 CO 3 In the form of BaO, BaCO 3 Form introduction, SnF 2 SnF 2The mixture was fully mixed and placed in a 150 mL corundum crucible, and then moved to a 1300 ° C muffle furnace for 2 hours. The crucible was then quickly taken out, and the glass liquid was poured into a metal mold preheated at 500 ° C. The cooled solid glass was quickly moved to a 500 ° C muffle furnace for annealing for 4 hours, and cooled with the furnace. Finally, 1-3 mm glass substrate particles were obtained by crushing and screening.
[0060] S2, simulated high calcium and high titanium low-level radioactive waste ash oxides, including the following components by oxide mass percentage: CaO: 44.52wt%, TiO 2 :22.4wt%、SiO 2 :12.15wt%,Al 2 O 3 :4.74wt%, Na 2 O: 1.98wt%, MgO: 3.44wt%, BaO: 4.08wt%, ZnO: 1.56wt%, K 2 O: 0.71wt%, B 2 O 3 :0.21wt%, Fe 2 O 3 :0.37wt%、P 2 O 5 :1.43wt%、SO 3 :2.41wt%. The glass substrate oxide accounts for 70wt%, the simulated high calcium and high titanium medium and low radioactive waste ash oxide accounts for 30wt% and a small amount of simulated nuclides (Co 2 O 3 、SrO、Cs 2 O each accounting for 0.2wt% of the glass solid body) are weighed, 100g of the mixture is weighed and placed in a 150mL corundum crucible, moved to a 1300℃ muffle furnace and kept warm for 2h, and the glass liquid is poured into a metal mold preheated at 500℃ to obtain a solid body.
[0061] Performance Testing
[0062] The chemical stability of the prepared glass solid body was evaluated using the internationally accepted solid body chemical stability test method: Product Consistency Test (PCT) (ASTM C 1285-02). The test results are shown in Table 1.
[0063] Table 1
[0064] <![CDATA[Total leaching value of Element PCT-7 (g / m 2 )]]> Example 1 0.5587 Example 2 0.4537 Example 3 0.2873 Example 4 0.8729 Example 5 3.2542 Comparative Example 1 0.4511 Comparative Example 2 5.8732
[0065] The solidified bodies obtained in Examples 1-5 and Comparative Examples 1-2 were observed under an optical microscope, and no other inclusions were found in Examples 1-5 and Comparative Example 1.
[0066] Figure 1 The solidification of the glass solidified bodies obtained in Example 1 and Comparative Example 2 is shown. It can be seen from the figure that the solidified bodies did not form a homogeneous glass body, indicating that the excessive SnF 2 It is impossible to make the simulated high-calcium and high-titanium low- and medium-level radioactive waste ash form a homogeneous glass solid body.
[0067] Figure 2 The XRD diffraction spectra of the glass solidified bodies prepared in Example 1, Example 2 and Comparative Example 1 are shown. It can be seen from the figure that the XRD diffraction spectrum of Example 1 shows a typical amorphous steamed bun peak, proving that the prepared solidified body is in a glassy state. The XRD diffraction spectrum of Example 2 shows a typical amorphous steamed bun peak, proving that the prepared solidified body is in a glassy state. The XRD diffraction spectrum of Comparative Example 1 shows a typical amorphous steamed bun peak, proving that the prepared solidified body is in a glassy state.
[0068] The crystallization rate of the samples (Example 1 and Comparative Example 1) after heat treatment was calculated using XRD patterns combined with Jade 6.0. Figure 3 The XRD diffraction patterns of the glass solidified bodies of Example 1 and Comparative Example 1 after heat treatment are shown (CaF 2 As shown in Table 1, the consistency test results of the glass solidified product prepared by the present invention for 7 days show that the total leaching value of the element PCT-7-day test in Example 1 is less than 0.6 g / m 2 , indicating that the prepared glass solid has excellent chemical stability. The glass solid in Comparative Example 1 was heat treated at 800°C for 3 days and the crystallization rate of the glass solid was ~3 vol%, which was higher than the crystallization rate of the sample in Example 1 (~0.8 vol%), indicating that the addition of SnF 2 It has the effect of inhibiting glass crystallization.
[0069] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A glass substrate for solidifying high-calcium and high-titanium low- and medium-level radioactive waste ash, Features: The glass substrate comprises the following components, calculated by oxide mass percentage: SiO 2 :35~60wt%、B 2 O 3 :10~25wt%、Al 2 O 3 :3~20wt%、Na 2 O: 5-25wt%, BaO: 12-30wt%, ZnO: 6-28wt% and SnF 2 :0.1~6wt%.
2. A glass substrate for solidifying high-calcium and high-titanium low- and medium-level radioactive waste ash as claimed in claim 1, Features: The glass substrate comprises the following components, calculated by oxide mass percentage: SiO 2 :35~50wt%、B 2 O 3 :12~20wt%、Al 2 O 3 :3~12wt%、Na 2 O: 5-15wt%, BaO: 15-20wt%, ZnO: 8-15wt% and SnF 2 :1~5wt%.
3. A method for preparing a glass substrate for solidifying high-calcium and high-titanium low- and medium-level radioactive waste ash according to any one of claims 1 to 2, Features: The following steps are involved: S1, the proportion of the configuration containing SiO 2 , B 2 O 3 、Al 2 O 3 、Na 2 O, BaO, ZnO and SnF 2 The glass base material batch materials are mixed evenly and then melted at high temperature to obtain a glass melt; S2. Pour the molten glass into the preheated mold, and after annealing and cooling, obtain a glass substrate.
4. A glass substrate for solidifying high-calcium and high-titanium low- and medium-level radioactive waste ash as claimed in claim 3, Features: The high temperature melting temperature is 1150-1400° C., the high temperature melting time is 1-8 hours, the annealing temperature is 300-600° C., and the annealing time is 1-6 hours.
5. Use of a glass substrate for solidifying high-calcium and high-titanium low- and medium-level radioactive waste ash as claimed in any one of claims 1 to 2, Features: The glass substrate is mixed with high-calcium and high-titanium low- and intermediate-level radioactive waste ash, kept at 1150-1300°C for 1-6 hours, and the glass liquid is poured into a preheated metal mold, annealed and cooled at a temperature of 300-600°C for 1-6 hours to prepare a high-calcium and high-titanium low- and intermediate-level radioactive waste glass solidification body.
6. A glass substrate for solidifying high-calcium and high-titanium low- and medium-level radioactive waste ash as claimed in claim 5, Features: The high-calcium and high-titanium low- and medium-level radioactive waste ash comprises the following components in terms of oxide mass percentage: CaO: 35-55wt%, TiO 2 :15~28wt%、SiO 2 :10~15wt%、Al 2 O 3 :2~7wt%、Na 2 O: 1~4wt%, MgO: 0~5wt%, BaO: 2~5wt%, ZnO: 1~3wt%, K 2 O: 0-1 wt%, B 2 O 3 :0~1wt%、Fe 2 O 3 :0~1wt%、P 2 O 5 :0~2wt%、SO 3 : 1-3wt%, and less than 1wt% of oxides of radioactive elements.
7. A glass substrate for solidifying high-calcium and high-titanium low- and medium-level radioactive waste ash as claimed in claim 6, Features: The radioactive elements include Cs, Sr and Co.
8. A glass substrate for solidifying high-calcium and high-titanium low- and medium-level radioactive waste ash as claimed in claim 5, Features: Calculated by oxide mass percentage, the glass substrate accounts for 50-80wt% in the glass solid body, and the high-calcium and high-titanium low- and medium-level radioactive waste ash accounts for 20-50wt% in the glass solid body.
9. A glass substrate for solidifying high-calcium and high-titanium low- and medium-level radioactive waste ash as claimed in claim 5, Features: Calculated by oxide mass percentage, the glass substrate accounts for 60-70wt% in the glass solid body, and the high-calcium and high-titanium low- and medium-level radioactive waste ash accounts for 30-40wt% in the glass solid body.
10. A glass substrate for solidifying high-calcium and high-titanium low- and medium-level radioactive waste ash as claimed in claim 5, Features: The glass substrate is spherical or granular, and the particle size of the glass substrate is 0.1 mm to 3 mm.
Citation Information
Patent Citations
A glass matrix composition for incineration ash of low-to-medium level radioactive combustible waste and a glass-cured body prepared therefrom.
CN104310781B
Glass composition for vitrifying mixed waste product and method for vitrifying mixed waste product using same
CN105814000A
A method for co-vitrifying low- and medium-level radioactive glass fibers with combustible solid nuclear waste incineration ash.
CN112382429B
Optical glass
CN107399906A
Optical compound glass
CN108395095A
Cited By
A solidification matrix and method for solidification of radioactive waste in titaniosilicate glass
CN122916426A