A method for preparing oxygen-barrier polyvinyl alcohol packaging material
By modifying graphene oxide with a polyphenol surface modifier and compounding it with polyvinyl alcohol, the problem of insufficient oxygen barrier properties of polyvinyl alcohol was solved, and a coated polyvinyl alcohol with excellent oxygen barrier properties and slightly higher mechanical properties was prepared. Vinyl alcohol oxygen barrier biodegradable film, suitable for packaging materials.
Patent Information
- Application Number
- CN202410661494.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-27
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-05-27
AI Technical Summary
Polyvinyl alcohol has limited ability to block small molecules of oxygen, making it difficult to meet actual engineering needs. Existing methods to improve oxygen blocking performance require high equipment or complicated processes, and the products are not sufficiently controllable.
A synthetic polyphenol surface modifier is designed to modify graphene oxide to enhance its interfacial compatibility and interfacial force with polyvinyl alcohol. The modified polyvinyl alcohol coating liquid is processed through an extrusion blow molding film forming process. Coated on the PLA film, a coated polyvinyl alcohol oxygen barrier biodegradable film was prepared.
Significantly reduces oxygen permeability, improves oxygen barrier properties, and slightly improves mechanical properties, making it suitable for packaging materials.
Smart Images

Figure CN118420958B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of research and development of coated polyvinyl alcohol oxygen barrier films, in particular to a method for preparing an oxygen barrier polyvinyl alcohol packaging material. Background Art
[0002] Today, energy shortage and environmental pollution are becoming increasingly prominent. Polyvinyl alcohol (PVA) has great potential application value in food, medicine, electronics, aerospace and other packaging fields due to its wide source and biodegradability. For example, dissolving it in water and coating it on biodegradable polylactic acid (PLA) packaging film can significantly improve the barrier properties of the material. However, the barrier capacity of polyvinyl alcohol for small molecules (such as oxygen) is limited and it is difficult to meet the actual engineering needs.
[0003] At present, the common methods for improving the oxygen barrier performance of polyvinyl alcohol include: multilayer composite, blending modification, biaxial stretching, etc. Among them, blending modification is to use impermeable layered nanofillers (such as montmorillonite, hydrotalcite, molybdenum disulfide, graphene, graphene oxide, etc.) and disperse them into polyvinyl alcohol to prepare nanocomposites by blending. The addition of layered fillers can reduce the polymer content in the composite material and reduce the solubility coefficient of the permeating small molecules on the one hand; on the other hand, it can extend the permeation path of the permeating molecules and reduce the diffusion coefficient, thereby improving the oxygen barrier performance of the composite material from these two aspects. Compared with other methods, blending modification has low equipment requirements, simple process, strong product controllability and few defects, and is a method widely used in industrial production. For example, the patent with publication number CN117510956A discloses a coating process and a high barrier film of a high barrier film, in which a coating liquid made of polyvinyl alcohol, deionized water, graphene oxide, cellulose nanofibrils and polyethyleneimine is applied to a polymer base film, which can significantly improve the barrier performance of the base film.
[0004] The search found that graphene derivatives have a higher diameter-to-thickness ratio and better barrier properties than other layered nanofillers. Among them, graphene oxide (GO) is an ideal filler for improving the oxygen barrier properties of polymers because it is easy to achieve functional modification and improve its interfacial compatibility and interfacial force with the polymer matrix due to its rich functional groups. Summary of the invention
[0005] The present invention provides a method for preparing an oxygen-barrier polyvinyl alcohol packaging material, designs and synthesizes a novel polyphenol-type surface modifier, utilizes the novel polyphenol-type surface modifier to modify graphene oxide and composites it with polyvinyl alcohol, enhances the interface compatibility and interface interaction force between graphene oxide and polyvinyl alcohol matrix, and applies the novel polyphenol-type surface modifier on the surface of a PLA film, thereby achieving the technical effect of synergistically enhancing the oxygen-barrier performance of the PLA film.
[0006] A method for preparing a coated polyvinyl alcohol oxygen barrier biodegradable film comprises the following steps:
[0007] Step 1: preparing a polyphenol type surface modifier, wherein the polyphenol type surface modifier is polyphenol type surface modifier I and / or polyphenol type surface modifier II;
[0008] Step 2: modifying graphene oxide with a polyphenol-type surface modifier to prepare an oxygen barrier;
[0009] Step 3: uniformly dispersing the oxygen barrier agent in the polyvinyl alcohol matrix to prepare an oxygen barrier modified polyvinyl alcohol coating liquid;
[0010] Step 4: Prepare a PLA film by using an extrusion blow molding film-forming process, and coat the oxygen-barrier modified polyvinyl alcohol coating liquid on its surface to prepare a coated polyvinyl alcohol oxygen-barrier biodegradable film.
[0011] Preferably, the preparation method of the polyphenol surface modifier I is:
[0012] Step S2-1: utilizing a nucleophilic substitution reaction mechanism, the carboxyl functional group of gallic acid and the secondary amine group of the SCA-A86T silane coupling agent undergo an acylation reaction to generate siloxane monomer I;
[0013] Step S2-2: utilizing the nucleophilic substitution reaction mechanism, the tertiary amine group of the siloxane monomer I and the chlorine functional group of the chloroalkane undergo quaternization reaction to generate a polyphenol-type surface modifier I.
[0014] Preferably, the preparation method of the polyphenol surface modifier II is:
[0015] Step S3-1: utilizing a nucleophilic substitution reaction mechanism, the carboxyl functional group of gallic acid and the primary amine group of the SCA-A85T silane coupling agent undergo an acylation reaction to generate siloxane monomer II;
[0016] Step S3-2: utilizing the nucleophilic substitution reaction mechanism, the tertiary amine group of the siloxane monomer II undergoes a quaternization reaction with the chlorine functional group of the chloroalkane to generate a polyphenol-type surface modifier II.
[0017] Preferably, the chlorinated alkane is one of 1-chloropropane, 1-chlorobutane, 1-chloropentane and 1-chlorohexane.
[0018] Preferably, the method for preparing the oxygen-barrier modified polyvinyl alcohol coating liquid in step three is: dissolving 5 to 30 parts by weight of polyvinyl alcohol resin in deionized water at 85°C to 95°C with stirring, preparing a polyvinyl alcohol mother liquor, cooling the temperature to 55 to 65°C, adding 0.05 to 3 parts by weight of an oxygen barrier agent, mixing evenly, and preparing an oxygen-barrier modified polyvinyl alcohol coating liquid.
[0019] Preferably, the method for preparing the coated polyvinyl alcohol oxygen barrier biodegradable film in step 4 is:
[0020] Step S6-1: 5 to 50 parts by weight of polylactic acid resin are put into a twin-screw extruder for melting and extrusion, pelletized, dried, and blown by a single-screw extrusion film blowing machine using an upward blowing method to obtain a 50 to 150 μm PLA film, and the PLA film is pre-treated by washing with an ethanol aqueous solution (the volume ratio of ethanol to deionized water is 0.5 to 1.5:1) and deionized water in sequence;
[0021] Step S6-2: Use a 20-50 μm measuring rod to evenly apply the oxygen-barrier modified polyvinyl alcohol coating liquid on the surface of the PLA film, and dry it to obtain a coated polyvinyl alcohol oxygen-barrier biodegradable film.
[0022] A coated polyvinyl alcohol oxygen barrier biodegradable film is prepared according to the method.
[0023] Preferably, the oxygen permeability of the coated polyvinyl alcohol oxygen barrier biodegradable film is 0.2 to 0.5 [cm 3 / (m 2 ·24h·0.1MPa)].
[0024] Beneficial Effects
[0025] The present invention designs and synthesizes two novel polyphenol-type surface modifiers, and uses them to modify graphene oxide to prepare an oxygen barrier agent; then the oxygen barrier agent is uniformly dispersed in a polyvinyl alcohol matrix to prepare an oxygen barrier modified polyvinyl alcohol coating liquid; finally, the oxygen barrier modified polyvinyl alcohol coating liquid is coated on the surface of a PLA film prepared by an extrusion blow molding film forming process to prepare a coated polyvinyl alcohol oxygen barrier biodegradable film;
[0026] Through experiments, it is found that: compared with polylactic acid films, the two coated polyvinyl alcohol oxygen-barrier biodegradable films prepared by the present invention can significantly reduce their oxygen permeability and show excellent oxygen-barrier performance;
[0027] It is also found that the coated polyvinyl alcohol oxygen barrier biodegradable film prepared by the present invention also has slightly improved mechanical properties, and can be used in packaging materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is the synthetic route of polyphenol type surface modifier Ⅰ;
[0029] Figure 2 This is the synthetic route of polyphenol type surface modifier II;
[0030] Figure 3 These are the experimental results of the oxygen barrier performance of the coated polyvinyl alcohol oxygen barrier biodegradable film. DETAILED DESCRIPTION
[0031] Experimental Example 1:
[0032] Synthetic polyphenol type surface modifier Ⅰ, such as Figure 1 As shown, it includes two synthesis processes, as follows:
[0033] (1) Synthesis of siloxane monomer I: Utilizing the nucleophilic substitution reaction mechanism, the carboxyl functional group of gallic acid and the secondary amine group of SCA-A86T silane coupling agent undergo acylation reaction to generate siloxane monomer I;
[0034] The specific experimental steps for synthesizing siloxane monomer I are as follows: under the protection of nitrogen, 1.7 g of gallic acid, 2.4 g of SCA-A86T silane coupling agent, 1.0 g of triethylamine and 50 mL of anhydrous dichloromethane are added to a three-necked flask with a water separator, and stirred at room temperature for 30 min. Then, 20 mL of 1-hydroxy-benzo-triazole solution (prepared with 1.3 g of 1-hydroxy-benzo-triazole and 20 mL of dichloromethane) and 30 mL of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride solution (prepared with 1.9 g of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and 30 mL of dichloromethane) are added to the three-necked flask in sequence, and stirred at room temperature for 20 h. A 1 mol / L sodium hydroxide aqueous solution is added, and the mixture is extracted with dichloromethane, dried over anhydrous magnesium sulfate, filtered, and the solvent is removed by rotary evaporation to obtain siloxane monomer I.
[0035] (2) Synthesis of polyphenolic surface modifier I: Using the nucleophilic substitution reaction mechanism, the tertiary amine group of the siloxane monomer I and the chlorine functional group of the chloroalkane undergo quaternization reaction to generate polyphenolic surface modifier I;
[0036] The chlorinated alkane is one of 1-chloropropane, 1-chlorobutane, 1-chloropentane and 1-chlorohexane; 1-chloropentane is selected in this experimental example;
[0037] The specific experimental steps for synthesizing the polyphenol surface modifier I are as follows: 2.0 g of siloxane monomer I and cyclohexane are added to a three-necked flask, and the temperature is raised to 40°C under nitrogen protection and mechanical stirring. After the temperature stabilizes, 10 mL of 1-chloropentane solution (prepared from 0.6 g of 1-chloropentane and 10 mL of cyclohexane) is added dropwise to the three-necked flask, and the reaction is maintained at 40°C with stirring for 12 h. After cooling, the polyphenol surface modifier I is obtained by rotary evaporation, washing with ethyl acetate, and vacuum drying.
[0038] The nuclear magnetic resonance hydrogen spectrum of polyphenol surface modifier I is characterized as follows: 1H NMR (CDCl3, 400MHz) δ: 0.46 (s, 3H), 0.88-0.90 (t, 3H), 1.21-1.73 (m, 10H), 3.00-3.56 (m, 18H), 3.96-4.01 (t, 2H), 7.21 (s, 2H); The active hydrogen in the phenolic hydroxyl functional group of the polyphenol-type surface modifier I does not emit a peak in the CDCl3 solvent.
[0039] Experimental Example 2:
[0040] Synthetic polyphenol type surface modifier II, such as Figure 2 As shown, it includes two synthesis processes, as follows:
[0041] (1) Synthesis of siloxane monomer II: Utilizing the nucleophilic substitution reaction mechanism, the carboxyl functional group of gallic acid and the primary amine group of SCA-A85T silane coupling agent undergo acylation reaction to generate siloxane monomer II;
[0042] The specific experimental steps for synthesizing siloxane monomer II are as follows: under nitrogen protection, 1.7 g of gallic acid, 2.8 g of SCA-A85T silane coupling agent, 1.0 g of triethylamine and 50 mL of acetonitrile are added to a three-necked flask with a water separator, and stirred at room temperature for 1 h. Then, 20 mL of N, N'-dicyclohexylcarbodiimide solution (prepared with 2.1 g of N, N'-dicyclohexylcarbodiimide and 20 mL of acetonitrile) is added to the three-necked flask, the temperature is raised to 75 ° C, stirred and reacted for 18 h, 1 mol / L sodium hydroxide aqueous solution is added, extracted with acetonitrile, dried over anhydrous magnesium sulfate, filtered, and the solvent is removed by rotary evaporation to obtain siloxane monomer II;
[0043] (2) Synthesis of polyphenolic surface modifier II: Using the nucleophilic substitution reaction mechanism, the tertiary amine group of siloxane monomer II reacts with the chlorine functional group of chloroalkane to produce polyphenolic surface modifier II;
[0044] The chlorinated alkane is one of 1-chloropropane, 1-chlorobutane, 1-chloropentane and 1-chlorohexane; 1-chloropentane is selected in this experimental example;
[0045] The specific experimental steps for preparing polyphenol type surface modifier II refer to the preparation experiment of polyphenol type surface modifier I. The difference between the preparation experiment of polyphenol type surface modifier I and the preparation experiment of polyphenol type surface modifier II is that 2.0g of siloxane monomer I is replaced by 1.1g of siloxane monomer II.
[0046] The nuclear magnetic resonance hydrogen spectrum of polyphenol surface modifier II is characterized as follows: 1H NMR (CDCl3, 400MHz)δ: 0.47 (s, 3H), 0.90-1.04 (m, 8H), 1.36-2.25 (m, 16H), 3.31-3.86 (m, 24H), 7.16 (s, 2H); The active hydrogen in the phenolic hydroxyl functional group and amide functional group of the polyphenol-type surface modifier II does not emit any peak in the CDCl3 solvent.
[0047] Embodiment 1:
[0048] (1) preparing an oxygen inhibitor I, wherein the preparation process is as follows: modifying graphene oxide with a polyphenol-type surface modifier I to obtain an oxygen inhibitor I, wherein the specific experimental steps are as follows: adding 1 g of polyphenol-type surface modifier I, 20 mL of methanol and 30 mL of deionized water into a three-necked flask, dropping glacial acetic acid to adjust the pH to 4.5, heating to 50° C. and stirring for 2 h, then heating to 70° C. under mechanical stirring, adding 5 g of graphene oxide into the three-necked flask and reflux for 3 h, cooling to room temperature, washing with methanol, precipitating, centrifuging, and drying to obtain an oxygen inhibitor I;
[0049] (2) preparing an oxygen barrier II, wherein the preparation process is as follows: modifying graphene oxide with a polyphenol-type surface modifier II to obtain an oxygen barrier II. The specific experimental steps refer to the preparation experiment of the oxygen barrier I. The difference between the preparation experiment of the oxygen barrier II and the preparation experiment of the oxygen barrier I is that the polyphenol-type surface modifier II is used to replace the polyphenol-type surface modifier I.
[0050] Among them, graphene oxide was purchased from Nanjing Xianfeng Nanomaterials Co., Ltd., and its specifications are: sheet diameter 0.5-5 μm, thickness 0.8-1.2 nm.
[0051] Experimental Example 2:
[0052] (1) preparing an oxygen-barrier modified polyvinyl alcohol coating liquid I, wherein the preparation process is as follows: based on the effect of hydrogen bonding, the oxygen barrier agent I is uniformly dispersed in the polyvinyl alcohol matrix to prepare the oxygen-barrier modified polyvinyl alcohol coating liquid I, wherein the specific preparation steps are as follows: adding 5 g of polyvinyl alcohol resin and 50 mL of deionized water into a three-necked flask, heating to 90° C. and stirring and dissolving for 4 h, preparing a polyvinyl alcohol mother liquor, cooling to 60° C., adding 0.3 g of the oxygen barrier agent I into the three-necked flask, maintaining the temperature at 60° C. and stirring and reacting for 3 h, and mixing evenly to obtain the oxygen-barrier modified polyvinyl alcohol coating liquid I;
[0053] (2) preparing an oxygen-barrier modified polyvinyl alcohol coating liquid II, wherein the preparation process is as follows: based on the action of hydrogen bonding, the oxygen barrier agent II is uniformly dispersed in the polyvinyl alcohol matrix to prepare the oxygen-barrier modified polyvinyl alcohol coating liquid II. The specific preparation steps refer to the preparation experiment of the oxygen-barrier modified polyvinyl alcohol coating liquid I. The difference between the oxygen-barrier modified polyvinyl alcohol coating liquid II and the preparation experiment of the oxygen-barrier modified polyvinyl alcohol coating liquid I is that the oxygen barrier agent I is replaced by the oxygen barrier agent II.
[0054] The polyvinyl alcohol resin is Nichigo G-Polymer purchased from Mitsubishi Chemical Group. TM .
[0055] Experimental Example 3:
[0056] (1) Preparation of polyvinyl alcohol coating film I includes two preparation steps, which are as follows:
[0057] Step 1: Preparation of PLA film: PLA film is prepared by using polylactic acid resin as raw material and extrusion blow molding film forming process. The specific preparation steps are as follows:
[0058] 10 g of polylactic acid resin was put into a twin-screw extruder for melting and extrusion, and then cut with a pelletizer to obtain 1-5 mm polylactic acid resin particles, and then dried and blown with a single-screw extruder film blowing machine using an upward blowing method to obtain a 70 μm PLA film; the PLA film was fixed on a wire frame, placed in an ethanol aqueous solution (the volume ratio of ethanol to deionized water was 1:1) for washing for 2 hours, and then washed with deionized water, and placed at 45°C for drying for use;
[0059] Among them, the temperature of the 1-3 zones of the twin-screw extruder is 160°C, 180°C, and 190°C, respectively, and the speed is 100r / min; the speed of the pelletizer is 200r / min; the temperature of the 1-3 zones of the single-screw extruder film blowing machine is 180°C, 190°C, and 195°C, respectively, the speed is 50r / min, the traction speed is 6m / min, the die head diameter of the film blowing machine is 65mm, and the blow-up ratio is 3.5;
[0060] Step 2: Fix the PLA film on the coating machine, use a 30 μm metering rod to evenly apply the oxygen-barrier modified polyvinyl alcohol coating liquid I on the surface of the PLA film, put it in a 70° C. oven and dry it for 3 hours to obtain a polyvinyl alcohol coating film I;
[0061] (2) Preparation of polyvinyl alcohol coating film II: using oxygen-barrier modified polyvinyl alcohol coating solution II to replace oxygen-barrier modified polyvinyl alcohol coating solution I, referring to the preparation steps and experimental conditions of polyvinyl alcohol coating film I, to prepare polyvinyl alcohol coating film II;
[0062] The polylactic acid resin was purchased from Suzhou Jiangcangfa Plastic Chemical Co., Ltd. with the brand number of 4032D.
[0063] Performance Test:
[0064] (1) Oxygen barrier performance test: The oxygen permeability test of the sample was carried out in accordance with GB / T 1038-2000. The specific test steps are as follows: a 30 cm round sample was placed in a glass desiccator at an ambient temperature of 25°C and anhydrous calcium chloride was used as a desiccant for 72 hours. Then, the oxygen barrier performance of the sample was tested using a Y110 oxygen permeability tester.
[0065] (2) Mechanical properties test: The tensile strength of the samples was tested using an Instron 5565 universal tensile testing machine. The specific test steps are as follows: a sample of 80 mm × 15 mm was fixed on the tensile testing machine and a tensile test was performed at a tensile rate of 5 mm / min. The longitudinal and transverse tensile strengths of the samples were recorded.
[0066] The above experimental results are shown in Table 1 below.
[0067] Table 1 Performance test results of coated polyvinyl alcohol oxygen barrier biodegradable film
[0068]
[0069]
[0070] The test data in Table 1 are plotted. Figure 3 , through comprehensive analysis of the above experimental results, we can draw the following conclusions:
[0071] (1) Compared with polylactic acid films, the two polyvinyl alcohol coated films prepared by the present invention can significantly reduce their oxygen permeability and show excellent oxygen barrier properties;
[0072] (2) The polyvinyl alcohol coating film prepared by the present invention also has slightly improved mechanical properties and can be used in packaging materials.
Claims
1. A method for preparing a coated polyvinyl alcohol oxygen barrier biodegradable film, characterized in that: The following steps are involved: Step 1: preparing a polyphenol type surface modifier, wherein the polyphenol type surface modifier is polyphenol type surface modifier I and / or polyphenol type surface modifier II; The preparation method of the polyphenol surface modifier I is: By using the nucleophilic substitution reaction mechanism, the carboxyl functional group of gallic acid and the secondary amine group of SCA-A86T silane coupling agent undergo acylation reaction to generate siloxane monomer Ⅰ; By utilizing the nucleophilic substitution reaction mechanism, the tertiary amine group of the siloxane monomer Ⅰ and the chlorine functional group of the chloroalkane undergo quaternization reaction to generate the polyphenol type surface modifier Ⅰ; The preparation method of the polyphenol surface modifier II is: By using the nucleophilic substitution reaction mechanism, the carboxyl functional group of gallic acid and the primary amine group of SCA-A85T silane coupling agent undergo acylation reaction to generate siloxane monomer II. By utilizing the nucleophilic substitution reaction mechanism, the tertiary amine group of the siloxane monomer II reacts with the chlorine functional group of the chloroalkane to form a polyphenol-type surface modifier II. Step 2: modifying graphene oxide with a polyphenol-type surface modifier to prepare an oxygen barrier; Step 3: uniformly dispersing the oxygen barrier agent in the polyvinyl alcohol matrix to prepare an oxygen barrier modified polyvinyl alcohol coating liquid; Step 4: Prepare a PLA film by using an extrusion blow molding film-forming process, and coat the oxygen-barrier modified polyvinyl alcohol coating liquid on its surface to prepare a coated polyvinyl alcohol oxygen-barrier biodegradable film.
2. The method for preparing a coated polyvinyl alcohol oxygen-barrier biodegradable film according to claim 1, characterized in that the chlorinated alkane is one of 1-chloropropane, 1-chlorobutane, 1-chloropentane and 1-chlorohexane.
3. The method for preparing a coated polyvinyl alcohol oxygen barrier biodegradable film according to claim 1, characterized in that: The preparation method of the oxygen-barrier modified polyvinyl alcohol coating liquid in step three is: dissolving 5 to 30 parts by weight of polyvinyl alcohol resin in deionized water at 85° C. to 95° C. with stirring, preparing a polyvinyl alcohol mother liquor, cooling the temperature to 55 to 65° C., adding 0.05 to 3 parts by weight of an oxygen barrier agent, mixing evenly, and preparing an oxygen-barrier modified polyvinyl alcohol coating liquid.
4. The method for preparing a coated polyvinyl alcohol oxygen barrier biodegradable film according to claim 1, characterized in that: The preparation method of the coated polyvinyl alcohol oxygen barrier biodegradable film in step 4 is as follows: 5-50 parts by weight of polylactic acid resin are put into a twin-screw extruder for melting and extrusion, pelletized, dried, and blown by a single-screw extrusion film blowing machine using an upward blowing method to obtain a 50-150 μm PLA film, and the PLA film is pretreated, specifically, washing with a mixed solution consisting of 0.5-1.5 parts by volume of ethanol and 1 part by volume of deionized water and deionized water in sequence; The oxygen-barrier modified polyvinyl alcohol coating liquid was evenly applied on the surface of the PLA film using a 20-50 μm measuring rod, and then dried to obtain a coated polyvinyl alcohol oxygen-barrier biodegradable film.
5. A coated polyvinyl alcohol oxygen barrier biodegradable film prepared according to the method according to any one of claims 1 to 4.
6. A coated polyvinyl alcohol oxygen barrier biodegradable film according to claim 5, characterized in that: The oxygen permeability of the coated polyvinyl alcohol oxygen barrier biodegradable film is (0.2~0.5) cm 3 / (m 2 •24h•0.1MPa).
7. Use of the coated polyvinyl alcohol oxygen barrier biodegradable film prepared by the method according to any one of claims 1 to 4 in packaging materials.