A high insulation flame retardant epoxy resin composition and preparation method thereof
By preparing vinyl benzoxazine and nano-alumina flame retardants in epoxy resin, as well as polyurethane prepolymers and epoxy-based POSS tougheners, the problems of epoxy resin flammability and brittleness are solved, significantly Improved its flame retardancy and mechanical properties.
Patent Information
- Application Number
- CN202410841434.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-27
AI Technical Summary
The flammability and brittleness of epoxy resin limit its application in many fields. In the existing technology, molybdenum disulfide powder is not surface modified, which affects the matrix properties.
Pentaerythritol phosphate is reacted with 4,4-bis(4-hydroxyphenyl)pentanoic acid to generate a phosphate intermediate, and then combined with 3-vinylaniline and paraformaldehyde to prepare vinylbenzoxazine as a flame retardant, and Mixed with nano-alumina; simultaneously using polyurethane prepolymer and epoxy-based POSS to generate a toughening agent, which improves the flame retardancy and mechanical properties of the epoxy resin through a photoinitiated reaction.
It significantly improves the insulation, flame retardancy and mechanical properties of epoxy resin, improves the dispersion and compatibility of nano-alumina, and enhances its thermal stability and toughness.
Smart Images

Figure CN118421052B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, and in particular to a high-insulation flame-retardant epoxy resin composition and a preparation method thereof. Background Art
[0002] Thermosetting polymer materials have the advantages of high specific strength and specific stiffness, good corrosion resistance, stable structural dimensions, and good insulation. Epoxy resin is an important thermosetting resin. Its molecular structure contains epoxy groups. The epoxy groups have strong chemical activity and can generate a three-dimensional network structure after cross-linking and curing reaction, thus having good comprehensive performance. In recent years, epoxy resin compositions have been widely used in many fields because of their superior performance, stable structure, good processability, light weight and small weight. Among them, because epoxy resin has excellent electrical insulation properties, it can be used as an insulating protection material to ensure the reliable operation of high-voltage equipment, and has been widely used in electronic components, line insulation, device insulation packaging, etc.
[0003] However, epoxy resin is a flammable substance. The limiting oxygen index of epoxy cured material without flame retardant treatment is only about 20%, and its flame retardant properties usually need to be improved. In addition, the epoxy resin has poor ability to resist deformation and crack propagation after curing, is brittle, has poor toughness, and has poor impact resistance, which limits the application of epoxy resin in many fields.
[0004] Prior art, such as Chinese patent application CN104292768A, discloses an epoxy resin composition for high-voltage power insulation and a preparation method thereof, wherein bisphenol A epoxy resin is used as a matrix, molybdenum disulfide powder is used as a filler, methyltetrahydrophthalic anhydride is used as a curing agent, and aminophenol compounds are used as accelerators, and after thermal curing, an epoxy resin composition with good heat resistance and good electrical insulation is obtained. However, the molybdenum disulfide powder used as an insulating filler in the formula has not been surface modified, has poor compatibility with the matrix, and is added in a large amount, is easy to agglomerate, and affects the performance of the epoxy resin matrix. Summary of the invention
[0005] The purpose of the present invention is to overcome the deficiencies of the prior art and provide a high-insulation flame-retardant epoxy resin composition and a preparation method thereof. The epoxy resin composition has insulation and excellent flame retardancy after curing, and has good mechanical properties.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is as follows:
[0007] A method for preparing a highly insulating flame-retardant epoxy resin composition comprises the following steps:
[0008] Step 1, preparing flame retardant and toughening agent;
[0009] Wherein, the preparation of flame retardant comprises the following steps:
[0010] S11, pentaerythritol phosphate, 4,4-bis(4-hydroxyphenyl)valeric acid, p-toluenesulfonic acid and acetonitrile are mixed and reacted, and after the reaction is completed, the solvent acetonitrile is removed by rotary evaporation to obtain a reaction product, and the product is purified and dried to obtain a phosphate intermediate;
[0011] The phosphate intermediate, 3-vinylaniline, paraformaldehyde and toluene are mixed and reacted, and after the reaction is completed, the solvent toluene is removed by rotary evaporation to obtain a reaction product, which is purified and dried to obtain vinylbenzoxazine;
[0012] S12, mixing nano-alumina, γ-methacryloxypropyltrimethoxysilane and ethanol, ultrasonically dispersing, adding a regulator to adjust the pH value, reacting, and after the reaction, centrifuging, filtering, washing and drying to obtain vinyl nano-alumina; mixing vinyl benzoxazine with vinyl nano-alumina to obtain a flame retardant;
[0013] The preparation of the toughening agent comprises the following steps:
[0014] S21, 3-(2,3-epoxypropoxy)propyltrimethoxysilane, methyltriethylsilane and isopropanol are mixed, tetramethylammonium hydroxide is added, and the mixture is reacted. After the reaction is completed, the solvent is removed by rotary evaporation to obtain a crude reaction product, and the crude reaction product is mixed and dissolved with toluene, and the reaction is continued. After the reaction is completed, the mixture is cooled to room temperature to obtain a reaction product, which is purified and dried to obtain epoxy POSS;
[0015] S22, diphenylmethane diisocyanate, dibutyltin dilaurate, and ethyl acetate are mixed, and N,N-bis(2-hydroxyethyl)aminomethylenephosphonic acid diethyl ester solution is added dropwise, and after the addition is completed, the mixture is reacted, and after the reaction is completed, a phosphorus-containing polyurethane prepolymer is obtained; phosphorus-containing polyurethane prepolymer, epoxy POSS, and 2-ethyl-4-methylimidazole are mixed, and the mixture is reacted, and after the reaction is completed, a toughening agent is obtained;
[0016] Step 2: Mix epoxy resin E42 and flame retardant, stir, add photoinitiator 907, react under light, add epoxy resin E44, toughening agent and methyltetrahydrophthalic anhydride after the reaction, mix, vacuum degas, and obtain a high-insulation flame-retardant epoxy resin composition.
[0017] Preferably, when preparing the flame retardant, in S11, the mass ratio of pentaerythritol phosphate, 4,4-bis(4-hydroxyphenyl)pentanoic acid, p-toluenesulfonic acid and acetonitrile is 18-20:14-16:2.5-2.8:100-120; when preparing the phosphate intermediate, the reaction conditions are: reacting in a nitrogen atmosphere at a temperature of 60-70°C for 24-26h.
[0018] Preferably, when preparing the phosphate intermediate, the purification operation includes: mixing and dissolving the reaction product with ethyl acetate in a mass ratio of 1:5-6, adding saturated sodium bicarbonate solution and saturated sodium chloride solution 3-5 times the mass of the reaction product, washing three times respectively, separating the liquids, taking the organic phase, removing the solvent ethyl acetate by rotary evaporation at a temperature of 65-70°C, and passing through a column; the developing solvent in the column operation is prepared by mixing ethyl acetate and petroleum ether in a volume ratio of 3:1.
[0019] Preferably, when preparing the flame retardant, in S11, the mass ratio of the phosphate intermediate, 3-vinylaniline, polyformaldehyde and toluene is 4-5:2.5-3.5:4-6:120-150; when preparing vinylbenzoxazine, the reaction conditions are: reacting at a temperature of 100-110° C. for 6-8 hours.
[0020] Preferably, when preparing vinylbenzoxazine, the purification operation includes: mixing and dissolving the reaction product with ethyl acetate in a mass ratio of 1:5-6, adding 0.1 mol / L hydrochloric acid aqueous solution and water 3-5 times the mass of the reaction product, washing three times respectively, separating the liquids, taking the organic phase, and removing the solvent ethyl acetate by rotary evaporation at a temperature of 65-70°C.
[0021] Preferably, when preparing the flame retardant, in S12: the mass ratio of nano-alumina, γ-methacryloxypropyltrimethoxysilane and ethanol is 10:5-6:340-380; the reaction conditions are: reacting at a pH value of 5-6 and a temperature of 60-70°C for 18-20h; the mass ratio of vinylbenzoxazine to vinyl nano-alumina is 2:1.
[0022] Preferably, the regulator comprises a 1 mol / L hydrochloric acid aqueous solution.
[0023] Preferably, when preparing the toughening agent, in S21: the mass ratio of 3-(2,3-epoxypropoxy)propyltrimethoxysilane, methyltriethylsilane, isopropanol, tetramethylammonium hydroxide and toluene is 18-20:13-15:110-130:8-10:80-100; the reaction conditions are: react at room temperature for 6-8h; and the continued reaction conditions are: continue the reaction at a temperature of 90-95°C for 4-5h.
[0024] Preferably, when preparing epoxy POSS, the purification operation includes: adding 3-5 times the mass of the reaction product of saturated sodium chloride aqueous solution to wash until neutral, separating the liquids, taking the organic phase, and removing the solvent toluene by rotary evaporation at a temperature of 95-100°C.
[0025] Preferably, when preparing the toughening agent, in S22: the mass ratio of diphenylmethane diisocyanate, dibutyltin dilaurate, ethyl acetate, and N,N-bis(2-hydroxyethyl)aminomethylenephosphonic acid diethyl ester solution is 18-20:0.01-0.02:18-20:50-100; the dropping conditions are: dropping for 20-30 minutes in a nitrogen atmosphere; when preparing the phosphorus-containing polyurethane prepolymer, the reaction conditions are: reacting for 2-3 hours in a nitrogen atmosphere at a temperature of 70-80°C.
[0026] Preferably, the N,N-bis(2-hydroxyethyl)aminomethylenephosphonic acid diethyl ester solution is prepared by mixing N,N-bis(2-hydroxyethyl)aminomethylenephosphonic acid diethyl ester and ethyl acetate in a mass ratio of 1:10.
[0027] Preferably, when preparing the toughening agent, in S22: the mass ratio of phosphorus-containing polyurethane prepolymer, epoxy POSS, and 2-ethyl-4-methylimidazole is 10-15:100:0.1-0.15; when preparing the toughening agent, the reaction conditions are: reacting at a temperature of 150-160°C for 2-3h.
[0028] Preferably, in step 2, the mass ratio of epoxy resin E42, epoxy resin E44, flame retardant, photoinitiator 907, toughening agent and methyltetrahydrophthalic anhydride is 60-70:30-40:30-40:1-1.5:8-10:10-12; the light reaction conditions are: at a light intensity of 3mW / cm 2 , wavelength 365nm, light reaction at 110-120℃ for 0.5-1h.
[0029] Preferably, a high-insulation flame-retardant epoxy resin composition is prepared by the method for preparing the high-insulation flame-retardant epoxy resin composition as described above.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] Bisphenol A epoxy resin is cross-linked into a network structure after curing reaction, and has good mechanical and dielectric properties. It is an important insulating material. Benzoxazine is a six-membered heterocyclic compound composed of oxygen atoms and nitrogen atoms. It can undergo ring-opening polymerization under heating or the action of a catalyst to generate a nitrogen-containing and phenolic resin-like network structure polymer with the advantages of flame retardancy, insulation, mechanical properties and thermal stability. Mixing benzoxazine with bisphenol A epoxy resin and curing it can effectively improve the thermal stability and flame retardancy of the epoxy resin.
[0032] The present invention generates a phosphate intermediate containing bisphenol hydroxyl groups by reacting pentaerythritol phosphate with 4,4-bis(4-hydroxyphenyl)pentanoic acid, and then reacts the phosphate intermediate with 3-vinylaniline and polyformaldehyde to obtain vinyl benzoxazine with better flame retardancy; vinyl benzoxazine is mixed with vinyl nano-alumina modified with γ-methacryloxypropyltrimethoxysilane to obtain a flame retardant. The vinyl nano-alumina in the flame retardant is used as a nano-filler to improve the mechanical and insulating properties of the epoxy resin matrix; the vinyl benzoxazine contains two flame retardant elements, phosphorus and nitrogen, and has a synergistic flame retardant effect; the benzoxazine structure can be copolymerized and cured with the epoxy resin to improve the thermal stability and flame retardancy of the epoxy resin.
[0033] Polyurethane has good thermal stability and insulation, and excellent toughness, and can be used as a toughening agent to toughen epoxy resin. The present invention uses N, N-bis (2-hydroxyethyl) aminomethylenephosphonic acid diethyl ester as a flame retardant monomer, adds it to the polymerization reaction of polyurethane prepolymer, obtains an isocyanate-terminated phosphorus-containing polyurethane prepolymer, and reacts the isocyanate group of the phosphorus-containing polyurethane prepolymer with the epoxy group of the epoxy group POSS under the action of an imidazole catalyst to generate a toughening agent containing an oxazolidone structure, a POSS structure, and a polyurethane segment. Wherein, the oxazolidone structure and the POSS structure both have excellent heat resistance, can effectively improve the thermal properties and mechanical properties of epoxy resin, and the POSS structure contains silicon element, has a synergistic flame retardant effect with the phosphorus element, and further improves the flame retardancy of epoxy resin; the polyurethane segment has a special soft and hard segment structure, can improve the shortcomings of epoxy resin brittleness and poor toughness to a certain extent, and further improves the mechanical properties of epoxy resin.
[0034] According to the present invention, after bisphenol A epoxy resin is mixed with a flame retardant, under the action of a photoinitiator, a polymerization reaction occurs between the vinyl nano-alumina in the flame retardant and the carbon-carbon double bonds of vinyl benzoxazine, thereby improving the dispersibility and compatibility of the nano-alumina in a matrix. After the reaction, a toughening agent and a curing agent are added and mixed. Since the flame retardant contains a benzoxazine structure and the toughening agent contains an unreacted epoxy group, the flame retardant and the toughening agent can be copolymerized and cured with the epoxy resin, thereby improving the dispersibility and compatibility of the flame retardant and the toughening agent in the matrix, and further improving the insulation, flame retardancy and mechanical properties of the epoxy resin. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 It is a process flow chart of preparing a high-insulation flame-retardant epoxy resin composition in the present invention;
[0036] Figure 2 It is a line graph of the impact strength of samples 1-7 in the performance test of the present invention;
[0037] Figure 3It is a line graph of the limiting oxygen index of samples 1-7 in the performance test of the present invention. DETAILED DESCRIPTION
[0038] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0039] Example 1
[0040] This embodiment discloses a method for preparing a high-insulation flame-retardant epoxy resin composition, comprising the following steps:
[0041] Step 1, preparing flame retardant and toughening agent;
[0042] Wherein, the preparation of flame retardant comprises the following steps:
[0043] S11, pentaerythritol phosphate, 4,4-bis(4-hydroxyphenyl)pentanoic acid, p-toluenesulfonic acid, and acetonitrile are mixed in a mass ratio of 19:15:2.6:110, and reacted in a nitrogen atmosphere at 65°C for 25 hours. After the reaction is completed, the solvent acetonitrile is removed by rotary evaporation at 60°C to obtain a reaction product, and the reaction product is mixed and dissolved with ethyl acetate at a mass ratio of 1:5, and a saturated sodium bicarbonate solution and a saturated sodium chloride solution of 4 times the mass of the reaction product are added and washed three times respectively, and the liquids are separated, and the organic phase is taken, and the solvent ethyl acetate is removed by rotary evaporation at 70°C, and the phase is passed through a column, and dried at 55°C for 16 hours to obtain a phosphate intermediate;
[0044] The developing solvent in the column operation is prepared by mixing ethyl acetate and petroleum ether in a volume ratio of 3:1;
[0045] The phosphate intermediate, 3-vinylaniline, polyformaldehyde, and toluene are mixed in a mass ratio of 4:2.5:4:120, and reacted at 100°C for 8 hours. After the reaction, the solvent toluene is removed by rotary evaporation at 95°C to obtain a reaction product. The reaction product is mixed and dissolved with ethyl acetate in a mass ratio of 1:5, and 0.1 mol / L hydrochloric acid aqueous solution and water are added in an amount 3 times the mass of the reaction product, respectively, and washed three times, separated, and the organic phase is taken, the solvent ethyl acetate is removed by rotary evaporation at 65°C, and dried at 50°C for 18 hours to obtain vinylbenzoxazine;
[0046] S12, nano-alumina, γ-methacryloxypropyltrimethoxysilane, and ethanol were mixed in a mass ratio of 10:5:340, ultrasonically dispersed for 0.5 h, 1 mol / L hydrochloric acid aqueous solution was added to adjust the pH value to 5, reacted at 60°C for 20 h, and after the reaction, centrifuged and filtered to obtain the filter cake, washed with 5 times the mass of ethanol, and dried at 70°C for 24 h to obtain vinyl nano-alumina;
[0047] Vinyl benzoxazine and vinyl nano-alumina are mixed in a mass ratio of 2:1 to obtain a flame retardant;
[0048] The preparation of the toughening agent comprises the following steps:
[0049] S21, 3-(2,3-epoxypropoxy)propyltrimethoxysilane, methyltriethylsilane and isopropanol were mixed, tetramethylammonium hydroxide was added, and the mixture was reacted at room temperature for 6 hours. After the reaction was completed, the solvent isopropanol was removed by rotary evaporation at 70°C to obtain a crude reaction product, the crude reaction product was mixed and dissolved with toluene, and the reaction was continued at 90°C for 5 hours. After the reaction was completed, the mixture was cooled to room temperature to obtain a reaction product, and a saturated sodium chloride aqueous solution with a mass of 3 times that of the reaction product was added to wash the mixture until it was neutral, and the mixture was separated. The organic phase was taken, the solvent toluene was removed by rotary evaporation at 95°C, and the mixture was dried at 50°C for 18 hours to obtain epoxy POSS;
[0050] The mass ratio of 3-(2,3-epoxypropoxy)propyltrimethoxysilane, methyltriethylsilane, isopropanol, tetramethylammonium hydroxide and toluene is 18:13:110:8:80;
[0051] S22, diphenylmethane diisocyanate, dibutyltin dilaurate and ethyl acetate are mixed, and N,N-bis(2-hydroxyethyl)aminomethylenephosphonic acid diethyl ester solution is added dropwise in a nitrogen atmosphere for 20 minutes. After the addition is completed, the mixture is reacted at 70° C. in a nitrogen atmosphere for 3 hours. After the reaction is completed, a phosphorus-containing polyurethane prepolymer is obtained;
[0052] The mass ratio of diphenylmethane diisocyanate, dibutyltin dilaurate, ethyl acetate and N,N-bis(2-hydroxyethyl)aminomethylenephosphonic acid diethyl ester solution is 18:0.01:18:50; the N,N-bis(2-hydroxyethyl)aminomethylenephosphonic acid diethyl ester solution is prepared by mixing N,N-bis(2-hydroxyethyl)aminomethylenephosphonic acid diethyl ester and ethyl acetate in a mass ratio of 1:10;
[0053] The phosphorus-containing polyurethane prepolymer, epoxy POSS, and 2-ethyl-4-methylimidazole were mixed in a mass ratio of 10:100:0.1, and reacted at 150° C. for 3 hours. After the reaction was completed, a toughening agent was obtained;
[0054] Step 2: Mix epoxy resin E42 and flame retardant at 110°C, stir for 1 hour, add photoinitiator 907, and heat at a light intensity of 3mW / cm 2 , irradiate with light at a wavelength of 365 nm and a temperature of 110° C. for 1 hour, and after the reaction is completed, add epoxy resin E44, a toughening agent and methyltetrahydrophthalic anhydride, mix at a temperature of 110° C., and vacuum degas, to obtain a highly insulating flame-retardant epoxy resin composition;
[0055] Among them, the mass ratio of epoxy resin E42, epoxy resin E44, flame retardant, photoinitiator 907, toughening agent and methyltetrahydrophthalic anhydride is 70:30:30:1:8:10.
[0056] Example 2
[0057] This embodiment discloses a method for preparing a high-insulation flame-retardant epoxy resin composition, comprising the following steps:
[0058] Step 1, preparing flame retardant and toughening agent;
[0059] Wherein, the preparation of flame retardant comprises the following steps:
[0060] S11, mixing a phosphate intermediate, 3-vinylaniline, polyformaldehyde, and toluene in a mass ratio of 4.2:2.8:4.5:125, reacting at 105°C for 7 hours, and after the reaction, removing the solvent toluene by rotary evaporation at 95°C to obtain a reaction product, mixing and dissolving the reaction product with ethyl acetate in a mass ratio of 1:5, adding 0.1 mol / L hydrochloric acid aqueous solution and water with a mass of 4 times the mass of the reaction product, respectively washing three times, separating the liquids, taking the organic phase, removing the solvent ethyl acetate by rotary evaporation at 65°C, and drying at 55°C for 15 hours to obtain vinylbenzoxazine; wherein the preparation of the phosphate intermediate is the same as that in Example 1;
[0061] S12, nano-alumina, γ-methacryloxypropyltrimethoxysilane, and ethanol were mixed in a mass ratio of 10:5.3:350, ultrasonically dispersed for 0.5 h, 1 mol / L hydrochloric acid aqueous solution was added to adjust the pH value to 5, and reacted at 65°C for 19 h. After the reaction, centrifuged, filtered, and the filter cake was taken, and 6 times the mass of the filter cake was added to wash it, and dried at 75°C for 21 h to obtain vinyl nano-alumina; vinyl benzoxazine and vinyl nano-alumina were mixed in a mass ratio of 2:1 to obtain a flame retardant;
[0062] The preparation of the toughening agent comprises the following steps:
[0063] S21, 3-(2,3-epoxypropoxy)propyltrimethoxysilane, methyltriethylsilane and isopropanol were mixed, tetramethylammonium hydroxide was added, and the mixture was reacted at room temperature for 6.5 hours. After the reaction was completed, the solvent isopropanol was removed by rotary evaporation at 70°C to obtain a crude reaction product, the crude reaction product was mixed and dissolved with toluene, and the reaction was continued at 90°C for 4.5 hours. After the reaction was completed, the mixture was cooled to room temperature to obtain a reaction product, and a saturated sodium chloride aqueous solution with a mass of 4 times that of the reaction product was added to wash the mixture until it was neutral, and the mixture was separated. The organic phase was taken, the solvent toluene was removed by rotary evaporation at 95°C, and the mixture was dried at 55°C for 15 hours to obtain epoxy POSS;
[0064] Among them, the mass ratio of 3-(2,3-epoxypropoxy)propyltrimethoxysilane, methyltriethylsilane, isopropanol, tetramethylammonium hydroxide, and toluene is 18.5:13.5:115:8.5:85;
[0065] S22, diphenylmethane diisocyanate, dibutyltin dilaurate and ethyl acetate were mixed, and N,N-bis(2-hydroxyethyl)aminomethylenephosphonic acid diethyl ester solution was added dropwise in a nitrogen atmosphere for 25 min. After the addition was completed, the mixture was reacted at 75° C. in a nitrogen atmosphere for 2.5 h. After the reaction was completed, a phosphorus-containing polyurethane prepolymer was obtained;
[0066] The mass ratio of diphenylmethane diisocyanate, dibutyltin dilaurate, ethyl acetate and N,N-bis(2-hydroxyethyl)aminomethylenephosphonic acid diethyl ester solution is 18.5:0.01:18.5:60; the N,N-bis(2-hydroxyethyl)aminomethylenephosphonic acid diethyl ester solution is prepared by mixing N,N-bis(2-hydroxyethyl)aminomethylenephosphonic acid diethyl ester and ethyl acetate in a mass ratio of 1:10;
[0067] The phosphorus-containing polyurethane prepolymer, epoxy POSS, and 2-ethyl-4-methylimidazole were mixed in a mass ratio of 11:100:0.1, and reacted at 155° C. for 2.5 hours. After the reaction was completed, a toughening agent was obtained;
[0068] Step 2: Mix epoxy resin E42 and flame retardant at 112°C, stir for 0.5h, add photoinitiator 907, and 2 , a wavelength of 365nm, a temperature of 115°C, and a light reaction for 0.8h. After the reaction is completed, epoxy resin E44, a toughening agent, and methyltetrahydrophthalic anhydride are added, mixed at a temperature of 115°C, and vacuum degassed to obtain a high-insulation flame-retardant epoxy resin composition;
[0069] Among them, the mass ratio of epoxy resin E42, epoxy resin E44, flame retardant, photoinitiator 907, toughening agent and methyltetrahydrophthalic anhydride is 68:32:32:1.2:8.5:10.5.
[0070] Example 3
[0071] This embodiment discloses a method for preparing a high-insulation flame-retardant epoxy resin composition, comprising the following steps:
[0072] Step 1, preparing flame retardant and toughening agent;
[0073] Wherein, the preparation of flame retardant comprises the following steps:
[0074] S11, mixing a phosphate intermediate, 3-vinylaniline, paraformaldehyde, and toluene in a mass ratio of 4.5:3:5:130, reacting at 105°C for 7h, and after the reaction, removing the solvent toluene by rotary evaporation at 98°C to obtain a reaction product, mixing and dissolving the reaction product with ethyl acetate in a mass ratio of 1:5, adding 0.1 mol / L hydrochloric acid aqueous solution and water with a mass of 4 times the mass of the reaction product, respectively washing three times, separating the liquids, taking the organic phase, removing the solvent ethyl acetate by rotary evaporation at 68°C, and drying at 55°C for 15h to obtain vinylbenzoxazine; wherein the preparation of the phosphate intermediate is the same as that in Example 1;
[0075] S12, nano-alumina, γ-methacryloxypropyltrimethoxysilane, and ethanol were mixed in a mass ratio of 10:5.5:360, ultrasonically dispersed for 0.5 h, 1 mol / L hydrochloric acid aqueous solution was added to adjust the pH value to 5.5, and reacted at 65°C for 19 h. After the reaction, centrifuged, filtered, and the filter cake was taken, and ethanol 6 times the mass of the filter cake was added for washing, and dried at 75°C for 21 h to obtain vinyl nano-alumina; vinyl benzoxazine and vinyl nano-alumina were mixed in a mass ratio of 2:1 to obtain a flame retardant;
[0076] The preparation of the toughening agent comprises the following steps:
[0077] S21, 3-(2,3-epoxypropoxy)propyltrimethoxysilane, methyltriethylsilane and isopropanol were mixed, tetramethylammonium hydroxide was added, and the mixture was reacted at room temperature for 7 hours. After the reaction was completed, the solvent isopropanol was removed by rotary evaporation at 72°C to obtain a crude reaction product, the crude reaction product was mixed and dissolved with toluene, and the reaction was continued at 92°C for 4.5 hours. After the reaction was completed, the mixture was cooled to room temperature to obtain a reaction product, and a saturated sodium chloride aqueous solution with a mass of 4 times that of the reaction product was added to wash the mixture until it was neutral, the mixture was separated, and the organic phase was taken. The solvent toluene was removed by rotary evaporation at 98°C, and the mixture was dried at 55°C for 15 hours to obtain epoxy POSS;
[0078] Among them, the mass ratio of 3-(2,3-epoxypropoxy)propyltrimethoxysilane, methyltriethylsilane, isopropanol, tetramethylammonium hydroxide, and toluene is 19:14:120:9:90;
[0079] S22, diphenylmethane diisocyanate, dibutyltin dilaurate and ethyl acetate were mixed, and N,N-bis(2-hydroxyethyl)aminomethylenephosphonic acid diethyl ester solution was added dropwise in a nitrogen atmosphere for 25 min. After the addition was completed, the mixture was reacted at 75° C. in a nitrogen atmosphere for 2.5 h. After the reaction was completed, a phosphorus-containing polyurethane prepolymer was obtained;
[0080] The mass ratio of diphenylmethane diisocyanate, dibutyltin dilaurate, ethyl acetate and N,N-bis(2-hydroxyethyl)aminomethylenephosphonic acid diethyl ester solution is 19:0.015:19:75; the N,N-bis(2-hydroxyethyl)aminomethylenephosphonic acid diethyl ester solution is prepared by mixing N,N-bis(2-hydroxyethyl)aminomethylenephosphonic acid diethyl ester and ethyl acetate in a mass ratio of 1:10;
[0081] The phosphorus-containing polyurethane prepolymer, epoxy POSS, and 2-ethyl-4-methylimidazole were mixed in a mass ratio of 12:100:0.1, and reacted at 155° C. for 2.5 hours. After the reaction was completed, a toughening agent was obtained;
[0082] Step 2: Mix epoxy resin E42 and flame retardant at 115°C, stir for 0.8h, add photoinitiator 907, and 2 , a wavelength of 365nm, a temperature of 115°C, and a light reaction for 0.8h. After the reaction is completed, epoxy resin E44, a toughening agent, and methyltetrahydrophthalic anhydride are added, mixed at a temperature of 115°C, and vacuum degassed to obtain a high-insulation flame-retardant epoxy resin composition;
[0083] Among them, the mass ratio of epoxy resin E42, epoxy resin E44, flame retardant, photoinitiator 907, toughening agent and methyltetrahydrophthalic anhydride is 65:35:35:1.3:9:11.
[0084] Example 4
[0085] This embodiment discloses a method for preparing a high-insulation flame-retardant epoxy resin composition, comprising the following steps:
[0086] Step 1, preparing flame retardant and toughening agent;
[0087] Wherein, the preparation of flame retardant comprises the following steps:
[0088] S11, mixing a phosphate intermediate, 3-vinylaniline, paraformaldehyde, and toluene in a mass ratio of 4.8:3.2:5.5:140, reacting at 110°C for 6 hours, and after the reaction, removing the solvent toluene by rotary evaporation at 100°C to obtain a reaction product, mixing and dissolving the reaction product with ethyl acetate in a mass ratio of 1:5, adding 0.1 mol / L hydrochloric acid aqueous solution and water with a mass of 4 times the mass of the reaction product, respectively washing three times, separating the liquids, taking the organic phase, removing the solvent ethyl acetate by rotary evaporation at 65°C, and drying at 55°C for 15 hours to obtain vinylbenzoxazine; wherein the preparation of the phosphate intermediate is the same as that in Example 1;
[0089] S12, nano-alumina, γ-methacryloxypropyltrimethoxysilane, and ethanol were mixed in a mass ratio of 10:5.8:370, ultrasonically dispersed for 0.5 h, 1 mol / L hydrochloric acid aqueous solution was added to adjust the pH value to 6, and reacted at 65°C for 19 h. After the reaction, centrifuged, filtered, and the filter cake was taken, and 6 times the mass of the filter cake was added to wash it, and dried at 75°C for 21 h to obtain vinyl nano-alumina; vinyl benzoxazine and vinyl nano-alumina were mixed in a mass ratio of 2:1 to obtain a flame retardant;
[0090] The preparation of the toughening agent comprises the following steps:
[0091] S21, 3-(2,3-epoxypropoxy)propyltrimethoxysilane, methyltriethylsilane and isopropanol were mixed, tetramethylammonium hydroxide was added, and the mixture was reacted at room temperature for 8 hours. After the reaction was completed, the solvent isopropanol was removed by rotary evaporation at 75°C to obtain a crude reaction product, the crude reaction product was mixed and dissolved with toluene, and the reaction was continued at 95°C for 4.5 hours. After the reaction was completed, the mixture was cooled to room temperature to obtain a reaction product, and a saturated sodium chloride aqueous solution with a mass of 5 times that of the reaction product was added to wash the mixture until it was neutral, and the mixture was separated. The organic phase was taken, the solvent toluene was removed by rotary evaporation at 100°C, and the mixture was dried at 55°C for 15 hours to obtain epoxy POSS;
[0092] Among them, the mass ratio of 3-(2,3-epoxypropoxy)propyltrimethoxysilane, methyltriethylsilane, isopropanol, tetramethylammonium hydroxide, and toluene is 19.5:14.5:125:9.5:95;
[0093] S22, diphenylmethane diisocyanate, dibutyltin dilaurate and ethyl acetate are mixed, and N,N-bis(2-hydroxyethyl)aminomethylenephosphonic acid diethyl ester solution is added dropwise in a nitrogen atmosphere for 30 minutes. After the addition is completed, the mixture is reacted at 75° C. in a nitrogen atmosphere for 3 hours. After the reaction is completed, a phosphorus-containing polyurethane prepolymer is obtained;
[0094] The mass ratio of diphenylmethane diisocyanate, dibutyltin dilaurate, ethyl acetate and N,N-bis(2-hydroxyethyl)aminomethylenephosphonic acid diethyl ester solution is 19.5:0.02:19.5:90; the N,N-bis(2-hydroxyethyl)aminomethylenephosphonic acid diethyl ester solution is prepared by mixing N,N-bis(2-hydroxyethyl)aminomethylenephosphonic acid diethyl ester and ethyl acetate in a mass ratio of 1:10;
[0095] The phosphorus-containing polyurethane prepolymer, epoxy POSS, and 2-ethyl-4-methylimidazole were mixed in a mass ratio of 14:100:0.15, and reacted at a temperature of 155° C. for 2.5 hours. After the reaction was completed, a toughening agent was obtained;
[0096] Step 2: Mix epoxy resin E42 and flame retardant at 120°C, stir for 0.5h, add photoinitiator 907, and 2 , a wavelength of 365nm, a temperature of 120°C, and a light reaction for 0.5h. After the reaction is completed, epoxy resin E44, a toughening agent, and methyltetrahydrophthalic anhydride are added, mixed at a temperature of 115°C, and vacuum degassed to obtain a high-insulation flame-retardant epoxy resin composition;
[0097] Among them, the mass ratio of epoxy resin E42, epoxy resin E44, flame retardant, photoinitiator 907, toughening agent and methyltetrahydrophthalic anhydride is 63:37:37:1.4:9.5:11.5.
[0098] Example 5
[0099] This embodiment discloses a method for preparing a high-insulation flame-retardant epoxy resin composition, comprising the following steps:
[0100] Step 1, preparing flame retardant and toughening agent;
[0101] Wherein, the preparation of flame retardant comprises the following steps:
[0102] S11, mixing a phosphate intermediate, 3-vinylaniline, paraformaldehyde, and toluene in a mass ratio of 5:3.5:6:150, reacting at 110°C for 6 hours, and after the reaction, removing the solvent toluene by rotary evaporation at 100°C to obtain a reaction product, mixing and dissolving the reaction product with ethyl acetate in a mass ratio of 1:6, adding 0.1 mol / L hydrochloric acid aqueous solution and water with a mass of 5 times the mass of the reaction product, respectively washing three times, separating the liquids, taking the organic phase, removing the solvent ethyl acetate by rotary evaporation at 70°C, and drying at 60°C for 12 hours to obtain vinylbenzoxazine; wherein the preparation of the phosphate intermediate is the same as that in Example 1;
[0103] S12, nano-alumina, γ-methacryloxypropyltrimethoxysilane, and ethanol were mixed in a mass ratio of 10:6:380, ultrasonically dispersed for 1 hour, 1 mol / L hydrochloric acid aqueous solution was added to adjust the pH value to 6, and reacted at 70°C for 18 hours. After the reaction, centrifuged, filtered, and the filter cake was taken, and ethanol 8 times the mass of the filter cake was added for washing, and dried at 80°C for 18 hours to obtain vinyl nano-alumina; vinyl benzoxazine and vinyl nano-alumina were mixed in a mass ratio of 2:1 to obtain a flame retardant;
[0104] The preparation of the toughening agent comprises the following steps:
[0105] S21, 3-(2,3-epoxypropoxy)propyltrimethoxysilane, methyltriethylsilane and isopropanol were mixed, tetramethylammonium hydroxide was added, and the mixture was reacted at room temperature for 8 hours. After the reaction was completed, the solvent isopropanol was removed by rotary evaporation at 75°C to obtain a crude reaction product, the crude reaction product was mixed and dissolved with toluene, and the reaction was continued at 95°C for 4 hours. After the reaction was completed, the mixture was cooled to room temperature to obtain a reaction product, and a saturated sodium chloride aqueous solution with a mass of 5 times that of the reaction product was added to wash the mixture until it was neutral, and the mixture was separated. The organic phase was taken, the solvent toluene was removed by rotary evaporation at 100°C, and the mixture was dried at 60°C for 12 hours to obtain epoxy POSS;
[0106] Wherein, the mass ratio of 3-(2,3-epoxypropoxy)propyltrimethoxysilane, methyltriethylsilane, isopropanol, tetramethylammonium hydroxide, and toluene is 20:15:130:10:100;
[0107] S22, diphenylmethane diisocyanate, dibutyltin dilaurate and ethyl acetate are mixed, and N,N-bis(2-hydroxyethyl)aminomethylenephosphonic acid diethyl ester solution is added dropwise in a nitrogen atmosphere for 30 minutes. After the addition is completed, the mixture is reacted at 80° C. in a nitrogen atmosphere for 2 hours. After the reaction is completed, a phosphorus-containing polyurethane prepolymer is obtained;
[0108] The mass ratio of diphenylmethane diisocyanate, dibutyltin dilaurate, ethyl acetate and N,N-bis(2-hydroxyethyl)aminomethylenephosphonic acid diethyl ester solution is 20:0.02:20:100; the N,N-bis(2-hydroxyethyl)aminomethylenephosphonic acid diethyl ester solution is prepared by mixing N,N-bis(2-hydroxyethyl)aminomethylenephosphonic acid diethyl ester and ethyl acetate in a mass ratio of 1:10;
[0109] The phosphorus-containing polyurethane prepolymer, epoxy POSS, and 2-ethyl-4-methylimidazole were mixed in a mass ratio of 15:100:0.15, and reacted at 160° C. for 2 hours. After the reaction was completed, a toughening agent was obtained;
[0110] Step 2: Mix epoxy resin E42 and flame retardant at 120°C, stir for 0.5h, add photoinitiator 907, and 2 , a wavelength of 365nm, a temperature of 120°C, and a light reaction for 0.5h. After the reaction is completed, epoxy resin E44, a toughening agent and methyltetrahydrophthalic anhydride are added, mixed at a temperature of 120°C, and vacuum degassed to obtain a high-insulation flame-retardant epoxy resin composition;
[0111] Among them, the mass ratio of epoxy resin E42, epoxy resin E44, flame retardant, photoinitiator 907, toughening agent and methyltetrahydrophthalic anhydride is 60:40:40:1.5:10:12.
[0112] Comparative Example 1
[0113] This comparative example discloses a method for preparing an epoxy resin composition, comprising the following steps:
[0114] Step 1, preparing vinyl nano-alumina and toughening agent;
[0115] Wherein, the preparation of vinyl nano-alumina comprises the following steps:
[0116] S11, nano-alumina, γ-methacryloxypropyltrimethoxysilane, and ethanol were mixed in a mass ratio of 10:5:340, ultrasonically dispersed for 0.5 h, 1 mol / L hydrochloric acid aqueous solution was added to adjust the pH value to 5, reacted at 60°C for 20 h, and after the reaction, centrifuged and filtered to obtain a filter cake, washed with 5 times the mass of ethanol, and dried at 70°C for 24 h to obtain vinyl nano-alumina;
[0117] The preparation of the toughening agent comprises the following steps:
[0118] S11, 3-(2,3-epoxypropoxy)propyltrimethoxysilane, methyltriethylsilane and isopropanol were mixed, tetramethylammonium hydroxide was added, and the mixture was reacted at room temperature for 6 hours. After the reaction was completed, the solvent isopropanol was removed by rotary evaporation at 70°C to obtain a crude reaction product, the crude reaction product was mixed and dissolved with toluene, and the reaction was continued at 90°C for 5 hours. After the reaction was completed, the mixture was cooled to room temperature to obtain a reaction product, and a saturated sodium chloride aqueous solution with a mass of 3 times that of the reaction product was added to wash the mixture until it was neutral, and the mixture was separated. The organic phase was taken, the solvent toluene was removed by rotary evaporation at 95°C, and the mixture was dried at 50°C for 18 hours to obtain epoxy POSS;
[0119] The mass ratio of 3-(2,3-epoxypropoxy)propyltrimethoxysilane, methyltriethylsilane, isopropanol, tetramethylammonium hydroxide and toluene is 18:13:110:8:80;
[0120] S12, diphenylmethane diisocyanate, dibutyltin dilaurate and ethyl acetate were mixed, and N,N-bis(2-hydroxyethyl)aminomethylenephosphonic acid diethyl ester solution was added dropwise in a nitrogen atmosphere for 20 min. After the addition was completed, the mixture was reacted at 70° C. in a nitrogen atmosphere for 3 h. After the reaction was completed, a phosphorus-containing polyurethane prepolymer was obtained;
[0121] The mass ratio of diphenylmethane diisocyanate, dibutyltin dilaurate, ethyl acetate and N,N-bis(2-hydroxyethyl)aminomethylenephosphonic acid diethyl ester solution is 18:0.01:18:50; the N,N-bis(2-hydroxyethyl)aminomethylenephosphonic acid diethyl ester solution is prepared by mixing N,N-bis(2-hydroxyethyl)aminomethylenephosphonic acid diethyl ester and ethyl acetate in a mass ratio of 1:10;
[0122] The phosphorus-containing polyurethane prepolymer, epoxy POSS, and 2-ethyl-4-methylimidazole were mixed in a mass ratio of 10:100:0.1, and reacted at 150° C. for 3 hours. After the reaction was completed, a toughening agent was obtained;
[0123] Step 2: Mix epoxy resin E42 and vinyl nano-alumina at 110° C., stir for 1 hour, add epoxy resin E44, toughening agent and methyltetrahydrophthalic anhydride, mix at 110° C., and vacuum degas to obtain an epoxy resin composition;
[0124] Among them, the mass ratio of epoxy resin E42, epoxy resin E44, vinyl nano-alumina, photoinitiator 907, toughening agent and methyltetrahydrophthalic anhydride is 70:30:10:1:8:10.
[0125] Comparative Example 2
[0126] This comparative example discloses a method for preparing an epoxy resin composition, comprising the following steps:
[0127] Step 1, preparing a flame retardant;
[0128] S11, mixing a phosphate intermediate, 3-vinylaniline, paraformaldehyde, and toluene in a mass ratio of 4:2.5:4:120, reacting at 100°C for 8 hours, and after the reaction, removing the solvent toluene by rotary evaporation at 95°C to obtain a reaction product, mixing and dissolving the reaction product with ethyl acetate in a mass ratio of 1:5, adding 0.1 mol / L hydrochloric acid aqueous solution and water in an amount 3 times the mass of the reaction product, washing three times respectively, separating the liquids, taking the organic phase, removing the solvent ethyl acetate by rotary evaporation at 65°C, and drying at 50°C for 18 hours to obtain vinylbenzoxazine; wherein the preparation of the phosphate intermediate is the same as that in Example 1;
[0129] S12, nano-alumina, γ-methacryloxypropyltrimethoxysilane, and ethanol were mixed in a mass ratio of 10:5:340, ultrasonically dispersed for 0.5 h, 1 mol / L hydrochloric acid aqueous solution was added to adjust the pH value to 5, and reacted at 60°C for 20 h. After the reaction, centrifuged, filtered, and the filter cake was taken, and 5 times the mass of the filter cake was added to wash it, and dried at 70°C for 24 h to obtain vinyl nano-alumina; vinyl benzoxazine and vinyl nano-alumina were mixed in a mass ratio of 2:1 to obtain a flame retardant;
[0130] Step 2: Mix epoxy resin E42 and flame retardant at 110°C, stir for 1 hour, add photoinitiator 907, and heat at a light intensity of 3mW / cm 2 , irradiate with light at a wavelength of 365 nm and a temperature of 110° C. for 1 hour, and after the reaction is completed, add epoxy resin E44 and methyltetrahydrophthalic anhydride, mix at a temperature of 110° C., and perform vacuum degassing to obtain an epoxy resin composition;
[0131] Among them, the mass ratio of epoxy resin E42, epoxy resin E44, flame retardant, photoinitiator 907 and methyltetrahydrophthalic anhydride is 70:38:30:1:8:10.
[0132] In the above embodiments and comparative examples: pentaerythritol phosphate is from Shanghai Aladdin Biochemical Technology Co., Ltd., model cage pentaerythritol phosphate PEPA, item number H138950, CAS number: 5301-78-0; 4,4-bis(4-hydroxyphenyl)pentanoic acid is from Wuhan Kemik Biopharmaceutical Technology Co., Ltd., CAS number: 126-00-1; p-toluenesulfonic acid is from Guangdong Wengjiang Chemical Reagent Co., Ltd., CAS number: 104-15-4; acetonitrile is from Anhui Jinyueguan New Material Technology Co., Ltd., CAS number: 75-05-8; ethyl acetate is from Tianjin Fuyu Fine Chemical Co., Ltd., CA S number: 141-78-6; sodium bicarbonate from Shandong Haihua Supply Chain Co., Ltd., specification 1000 mesh, CAS number: 144-55-8; sodium chloride from Wuxi Jingke Chemical Co., Ltd., CAS number: 7647-14-5; petroleum ether from Guangdong Xiaoda Chemical Co., Ltd., CAS number: 8032-32-4; 3-vinylaniline from Shanghai Aladdin Biochemical Technology Co., Ltd., CAS number: 15411-43-5; polyformaldehyde from Shanghai Aladdin Biochemical Technology Co., Ltd., product number C104190, CAS number: 30525-89-4; toluene from Alfa Aesar Company, CAS No.: 108-88-3; Nano-alumina comes from Zhejiang Zhitai Nano-Micro New Materials Co., Ltd., model ZT-L30JY, particle size 30nm, CAS No.: 1344-28-1; γ-methacryloxypropyltrimethoxysilane comes from Wuhan Kemik Biomedical Technology Co., Ltd., model KH570, CAS No.: 2530-85-0; Photoinitiator 907 comes from BASF, Germany, model Irgacure907, CAS No.: 71868-10-5; 3-(2,3-epoxypropoxy)propyltrimethoxysilane comes from Wuhan Kemik Biomedical Technology Co., Ltd., CAS No.: 2530-83-8; Methyltriethylsilane comes from Anhui Silicon Innovation Materials Technology Co., Ltd., CAS No.: 757-21-1; Isopropanol comes from Wuxi City Jingke Chemical Co., Ltd., CAS No.: 67-63-0; Tetramethylammonium hydroxide comes from Hubei Xinghengye Technology Co., Ltd., CAS No.: 75-59-2; Diphenylmethane diisocyanate comes from Mitsui Chemicals Co., Ltd., CAS No.: 101-68-8; Dibutyltin dilaurate comes from Maoming Xiongda Chemical Co., Ltd., CAS No.: 77-58-7; N,N-bis(2-hydroxyethyl)aminomethylenephosphonic acid diethyl ester comes from Shanghai Yuanye Biotechnology Co., Ltd., model flame retardant FRC-6, CAS No.: 2781-11-5; 2-ethyl-4-methylimidazole comes from Shandong Duoju Chemical Co., Ltd., CAS No.: 931-36-2; Epoxy resin E42 and epoxy resin E44 are both from Baling Petrochemical Company, model bisphenol A epoxy resin E-42, bisphenol A epoxy resin E-44;Methyltetrahydrophthalic anhydride comes from Jiangsu Runfeng Synthetic Technology Co., Ltd., CAS No.: 11070-44-3. ;
[0133] Test example
[0134] The epoxy resin compositions prepared in Examples 1-5 and Comparative Examples 1-2 were cured to obtain Samples 1-7, and comprehensive performance tests were performed on Samples 1-7, wherein the curing operation included: a first curing at 120° C. for 6 h, a second curing at 130° C. for 5 h, and a third curing at 180° C. for 1 h. The specific test results are shown in Table 1:
[0135] Table 1
[0136] Bending strength (MPa) <![CDATA[Impact strength (KJ / m 2 )]]> Glass transition temperature (℃) Volume resistivity (Ω·cm) Limiting oxygen index (%) Flame retardant grade (grade) Sample 1 >70 29.7 >130 <![CDATA[>1×10 13 ]]> 35.1 V-0 Sample 2 >70 30.1 >130 <![CDATA[>1×10 13 ]]> 35.6 V-0 Sample 3 >70 30.6 >130 <![CDATA[>1×10 13 ]]> 36.2 V-0 Sample 4 >70 31.0 >130 <![CDATA[>1×10 13 ]]> 36.5 V-0 Sample 5 >70 31.4 >130 <![CDATA[>1×10 13 ]]> 36.9 V-0 Sample 6 >70 25.8 >130 <![CDATA[>1×10 13 ]]> 27.1 V-1 Sample 7 >70 23.1 >130 <![CDATA[>1×10 13 ]]> 33.3 V-0
[0137] The tests of various indicators in Table 1 are based on the following standards: flexural strength is measured by ASTM D790-03 "Standard Test Method for Flexural Properties of Unreinforced and Reinforced Plastics and Electrical Insulating Materials"; impact strength is measured by ASTM D256-1997 "Standard Test Method for Izod Impact Properties of Plastics"; glass transition temperature is measured by GB / T22567-2008 "Test Method for Determining Glass Transition Temperature of Electrical Insulating Materials"; volume resistivity is measured by GB / T1410 "Test Method for Volume Resistivity and Surface Resistivity of Solid Insulating Materials"; limiting oxygen index is measured by ISO4589-1981 "Determination of Flammability by Oxygen Index Method for Plastics"; and flame retardancy grade is measured by ANSI / UL94 "UL-94 Combustion Standard".
[0138] It can be seen from the test results in Table 1 that the epoxy resin composition prepared by the present invention has insulation and excellent flame retardancy after curing, and has good mechanical properties.
[0139] The present invention mixes vinyl benzoxazine with vinyl nano-alumina modified by γ-methacryloxypropyltrimethoxysilane to obtain a flame retardant. The vinyl nano-alumina in the flame retardant acts as a nanofiller and can improve the mechanical and insulating properties of an epoxy resin matrix; the vinyl benzoxazine contains two flame retardant elements, phosphorus and nitrogen, and has a synergistic flame retardant effect; the benzoxazine structure can be copolymerized and cured with the epoxy resin to improve the thermal stability and flame retardancy of the epoxy resin. After the bisphenol A epoxy resin is mixed with the flame retardant, under the action of a photoinitiator, the vinyl nano-alumina in the flame retardant and the carbon-carbon double bond of the vinyl benzoxazine undergo a polymerization reaction, thereby improving the dispersibility and compatibility of the nano-alumina in the matrix and improving the insulation, flame retardancy and mechanical properties of the epoxy resin. In Comparative Example 1, no vinylbenzoxazine is added to the flame retardant, and the flame retardant and volume-increasing effects of vinylbenzoxazine are lacking. The compatibility of nano-alumina in the matrix is reduced, which affects the mechanical properties of the epoxy resin. Therefore, the mechanical properties and flame retardancy of Sample 6 prepared in Comparative Example 1 are lower than those in the embodiment.
[0140] The present invention uses N, N-bis (2-hydroxyethyl) aminomethylenephosphonic acid diethyl ester as a flame retardant monomer, adds it to the polymerization reaction of a polyurethane prepolymer, obtains an isocyanate-terminated phosphorus-containing polyurethane prepolymer, and reacts the isocyanate group of the phosphorus-containing polyurethane prepolymer with the epoxy group of the epoxy group POSS under the action of an imidazole catalyst to generate a toughening agent containing an oxazolidone structure, a POSS structure, and a polyurethane segment. Among them, the oxazolidone structure and the POSS structure both have excellent heat resistance, can effectively improve the thermal properties and mechanical properties of epoxy resin, and the POSS structure contains silicon elements, which have a synergistic flame retardant effect with phosphorus elements, and further improves the flame retardancy of the epoxy resin; the polyurethane segment has a special soft and hard segment structure, can improve the shortcomings of large brittleness and poor toughness of the epoxy resin to a certain extent, and further improves the mechanical properties of the epoxy resin. No toughening agent was added in Comparative Example 2, and the synergistic flame retardant effect of the POSS silicon element in the toughening agent and the phosphorus element in the flame retardant was lacking, the flame retardant properties of the matrix were reduced, and the toughening effect of the oxazolidinone structure, POSS structure, and polyurethane chain segment on the epoxy resin was lacking, and the impact strength of the matrix was reduced. Therefore, the mechanical properties and flame retardancy of Sample 7 prepared by Comparative Example 2 were lower than those in the embodiment.
[0141] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a highly insulating flame-retardant epoxy resin composition, characterized in that: The following steps are involved: Step 1, preparing flame retardant and toughening agent; Wherein, the preparation of flame retardant comprises the following steps: S11, mixing the phosphate intermediate, 3-vinylaniline, paraformaldehyde and toluene, reacting, and after the reaction, removing the solvent toluene by rotary evaporation to obtain a reaction product, purifying and drying to obtain vinylbenzoxazine; Wherein, the phosphate intermediate comprises the following steps to prepare: Pentaerythritol phosphate, 4,4-bis(4-hydroxyphenyl)valeric acid, p-toluenesulfonic acid and acetonitrile are mixed and reacted, and after the reaction is completed, the solvent acetonitrile is removed by rotary evaporation to obtain a reaction product, which is purified and dried to obtain a phosphate intermediate; The mass ratio of pentaerythritol phosphate, 4,4-bis(4-hydroxyphenyl)pentanoic acid, p-toluenesulfonic acid and acetonitrile is 18-20:14-16:2.5-2.8:100-120; when preparing the phosphate intermediate, the reaction conditions are: reacting in a nitrogen atmosphere at a temperature of 60-70°C for 24-26 hours; S12, mixing nano-alumina, γ-methacryloxypropyltrimethoxysilane and ethanol, ultrasonically dispersing, adding a regulator to adjust the pH value, reacting, and after the reaction, centrifuging, filtering, washing and drying to obtain vinyl nano-alumina; mixing vinyl benzoxazine with vinyl nano-alumina to obtain a flame retardant; Wherein, the preparation of toughening agent comprises the following steps: S21, 3-(2,3-epoxypropoxy)propyltrimethoxysilane, methyltriethylsilane and isopropanol are mixed, tetramethylammonium hydroxide is added, and the mixture is reacted. After the reaction is completed, the solvent is removed by rotary evaporation to obtain a crude reaction product, and the crude reaction product is mixed and dissolved with toluene, and the reaction is continued. After the reaction is completed, the mixture is cooled to room temperature to obtain a reaction product, which is purified and dried to obtain epoxy POSS; S22, mixing the phosphorus-containing polyurethane prepolymer, epoxy POSS, and 2-ethyl-4-methylimidazole, and reacting them, and obtaining a toughening agent after the reaction is completed; Wherein, the phosphorus-containing polyurethane prepolymer is prepared by the following steps: Mix diphenylmethane diisocyanate, dibutyltin dilaurate and ethyl acetate, add N,N-bis(2-hydroxyethyl)aminomethylenephosphonic acid diethyl ester solution dropwise, react after the addition is complete, and obtain a phosphorus-containing polyurethane prepolymer after the reaction is complete; The mass ratio of diphenylmethane diisocyanate, dibutyltin dilaurate, ethyl acetate, and N,N-bis(2-hydroxyethyl)aminomethylenephosphonic acid diethyl ester solution is 18-20:0.01-0.02:18-20:50-100; the dropping condition is: dropping for 20-30 minutes in a nitrogen atmosphere; the reaction condition is: reacting for 2-3 hours at a temperature of 70-80°C in a nitrogen atmosphere; Step 2: Mix epoxy resin E42 and flame retardant, stir, add photoinitiator 907, react under light, add epoxy resin E44, toughening agent and methyltetrahydrophthalic anhydride after the reaction, mix, vacuum degas, and obtain a high-insulation flame-retardant epoxy resin composition.
2. The method for preparing a highly insulating flame-retardant epoxy resin composition according to claim 1, characterized in that: When preparing the flame retardant in step 1, in S11, the mass ratio of the phosphate intermediate, 3-vinylaniline, polyformaldehyde and toluene is 4-5:2.5-3.5:4-6:120-150; when preparing vinylbenzoxazine, the reaction conditions are: reacting at a temperature of 100-110° C. for 6-8 hours.
3. The method for preparing a highly insulating flame-retardant epoxy resin composition according to claim 1, characterized in that: When preparing the flame retardant in step 1, in S12: the mass ratio of nano-alumina, γ-methacryloxypropyltrimethoxysilane and ethanol is 10:5-6:340-380; the reaction conditions are: reacting at a pH value of 5-6 and a temperature of 60-70° C. for 18-20 hours; and the mass ratio of vinylbenzoxazine to vinyl nano-alumina is 2:
1.
4. The method for preparing a highly insulating flame-retardant epoxy resin composition according to claim 1, characterized in that: When preparing the toughening agent in step 1, in S21: the mass ratio of 3-(2,3-epoxypropoxy)propyltrimethoxysilane, methyltriethylsilane, isopropanol, tetramethylammonium hydroxide and toluene is 18-20:13-15:110-130:8-10:80-100; the reaction conditions are: react at room temperature for 6-8h; the continued reaction conditions are: continue to react at a temperature of 90-95°C for 4-5h.
5. The method for preparing a highly insulating flame-retardant epoxy resin composition according to claim 1, characterized in that: When preparing the toughening agent in step 1, in S22: the mass ratio of phosphorus-containing polyurethane prepolymer, epoxy POSS, and 2-ethyl-4-methylimidazole is 10-15:100:0.1-0.15; when preparing the toughening agent, the reaction conditions are: reacting at a temperature of 150-160° C. for 2-3 hours.
6. The method for preparing a highly insulating flame-retardant epoxy resin composition according to claim 1, characterized in that: In the step 2, the mass ratio of epoxy resin E42, epoxy resin E44, flame retardant, photoinitiator 907, toughening agent and methyltetrahydrophthalic anhydride is 60-70:30-40:30-40:1-1.5:8-10:10-12.
7. The method for preparing a highly insulating flame-retardant epoxy resin composition according to claim 1, characterized in that: In step 2: the light reaction conditions are: at a light intensity of 3mW / cm 2 , wavelength 365nm, light reaction at 110-120℃ for 0.5-1h.
8. A high-insulation flame-retardant epoxy resin composition prepared by the method for preparing a high-insulation flame-retardant epoxy resin composition as claimed in any one of claims 1 to 7.
Citation Information
Cited By
Low-volatility high-performance environment-friendly insulating resin and preparation method thereof