A highly flame-retardant and tensile-resistant polyamide composite material, preparation method thereof and thermal insulation nylon strip

By covering the flame retardant in the insulated nylon strip and performing graft reaction, combining the dispersion of modified glass fibers and hollow glass microbeads, the problem of insufficient flame retardant and tensile performance of the insulated nylon strip is solved, and the problem of insufficient flame retardant and tensile resistance of the insulated nylon strip is achieved. The improvement of high flame retardancy and mechanical properties meets the special fire protection requirements.

CN118421081BActive Publication Date: 2024-11-01GUANGDONG BOSHIDA NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410894832.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-11-01
Estimated Expiration
2044-07-04

AI Technical Summary

Technical Problem

The existing thermally insulated nylon strips have shortcomings in flame retardant performance and lateral tensile resistance, which cannot meet the special fire resistance requirements, and excessive addition of flame retardant will reduce the mechanical properties of the material and lead to environmental protection problems.

Method used

By coating the flame retardant on the surface of glass fiber and hollow glass microbeads and grafting reaction with PA66 resin, the dispersion of modified glass fiber and hollow glass microbeads is enhanced to improve the dispersion of flame retardant and the flame retardant area of ​​flame retardant by grafting with PA66 resin. , the flame retardant properties and mechanical properties of the reinforced materials.

Benefits of technology

It achieves high flame retardancy and excellent lateral tensile performance, ensures the mechanical properties and thermal insulation properties of composite materials, and meets the heat insulation needs of special fire-resistant glass aluminum alloy profiles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The present application relates to the field of polyamide composite materials, and specifically discloses a highly flame-retardant and tensile-resistant polyamide composite material, a preparation method thereof, and a heat-insulating nylon strip. The composite material comprises the following components in parts by weight: 100-120 parts of a modified polyamide resin, 0.2-1 parts of an antioxidant, and 0.5-2 parts of a masterbatch, wherein the modified polyamide resin is a mixture of flame-retardant glass fiber-modified PA66 and flame-retardant hollow glass microsphere-modified PA66. The composite material of the present application has excellent flame retardancy, good tensile properties, excellent heat insulation effect, and no floating fibers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of polyamide composite materials, and more specifically, to a highly flame-retardant and tensile-resistant polyamide composite material, a preparation method thereof, and a heat-insulating nylon strip. Background Art

[0002] The insulation strip is a kind of connector that connects the inner and outer profiles of aluminum alloy insulation doors and windows. Its conventional materials include nylon, ABS, etc., among which nylon 66 is the most widely used material. Nylon 66 has a high melting point and mechanical properties, but it is easy to deform and has poor dimensional stability. Glass fiber is often added to reinforce the material in applications. The interface bonding force between glass fiber and nylon 66 is poor, and the stability is not good. When the glass fiber is co-extruded, it is mostly distributed longitudinally along the insulation strip, resulting in poor transverse tensile performance and unable to meet the use requirements. In addition, the "candle wick" effect played by the addition of glass fiber reduces the combustion level of the insulation strip.

[0003] In the prior art, the flame retardant properties of nylon insulation strips are improved by adding flame retardants, but the blending of flame retardants still cannot meet the flame retardant requirements of special fire-resistant glass doors and windows, and the addition of too much flame retardant reduces the mechanical properties of the material, mechanical properties, and the thick smoke and harmful substances emitted during flame retardancy are not conducive to environmental protection. By adding a compatibilizer during blending, the interface bonding performance of glass fiber and nylon 66 can be improved to a certain extent, but there will still be problems such as poor transverse tensile strength and low impact strength, and floating fibers are prone to occur, resulting in a rough surface of the insulation strip, which affects the mechanical properties and thus shortens the service life of the insulation strip. Therefore, how to prepare an insulation strip that meets special fire protection requirements, has good flame retardant effects, and is resistant to transverse tensile stress is an urgent problem to be solved. Summary of the invention

[0004] In order to solve the problem that the thermal insulation nylon strip has both flame retardancy and transverse tensile strength, the present application provides a highly flame retardant and tensile-resistant polyamide composite material, a preparation method thereof, and a thermal insulation nylon strip.

[0005] In a first aspect, the present application provides a highly flame-retardant and tensile-resistant polyamide composite material, the preparation of which includes the following components in parts by weight:

[0006] Modified polyamide resin 100-120 parts,

[0007] Antioxidant 0.2-1 part,

[0008] Masterbatch 0.5-2 parts,

[0009] The modified polyamide resin is a mixture of flame retardant glass fiber modified PA66 and flame retardant hollow glass microsphere modified PA66.

[0010] Most of the existing polyamide composite materials improve the corresponding flame retardant effect, mechanical properties and thermal insulation effect by adding flame retardants, glass fibers, hollow glass microspheres and blending with PA66. However, the negative effects brought by the large amount of flame retardants, the incompatibility of glass fibers, floating fibers, etc. have led to the inability to obtain a thermal insulation strip that meets the requirements of special fire retardant.

[0011] Therefore, the inventors considered combining the above-mentioned additives, reinforcing agents, and fillers with PA66 resin by modification to solve the problems of insufficient compatibility and flame retardancy. Glass fiber has greatly improved the rigidity, heat resistance, and mechanical strength of PA66 resin. Glass fiber is evenly distributed in PA66 resin. When subjected to external force, the force is transmitted along the orientation direction of the glass fiber, which can disperse the force and enhance the mechanical properties. Hollow glass microspheres have a good thermal insulation effect due to their hollow structure and low thermal conductivity. The inventors coated the phosphorus-containing flame retardant component on the surface of glass fiber and hollow glass microspheres. On the one hand, it does not affect the mechanical enhancement and thermal insulation effects of glass fiber and hollow glass microspheres. On the other hand, through the dispersion of glass fiber and hollow glass microspheres, the flame retardant is well dispersed in the composite material, increasing the flame retardant area of ​​the flame retardant and further improving the flame retardancy.

[0012] In addition, through the grafting reaction of flame retardant coated modified glass fiber and hollow glass microspheres with PA66 resin, the compatibility of flame retardant coated modified glass fiber and hollow glass microspheres with resin is improved, the dispersion is more uniform, the reinforcing effect of the components on PA66 is more obvious, and the dispersion of flame retardant in resin is also better. The inventor found that when flame retardant glass fiber modified PA66 and flame retardant hollow glass microsphere modified PA66 are used together, the flame retardant performance is significantly better than that of each used alone. This may be due to the continuous and irregular arrangement of the spherical structure of the hollow glass microspheres and the filamentous structure of the fibers in the system, and the irregular arrangement of the glass fibers in the gaps of the hollow glass microspheres, so that the coated flame retardant can achieve continuous flame retardant points in the resin, thereby achieving a synergistic flame retardant effect to a certain extent. In addition, the ungrafted hydrogen bonds in PA66 realize hydrogen bonding between molecules, which improves the strength of the material while making the grafted reinforcing components more stable in the material, thereby improving the reinforcing effect of the components. The flame retardant-coated stripped fibers and hollow glass microspheres are stably arranged between PA66 molecules through hydrogen bonding. The spatial effect of the hollow glass microspheres hinders the longitudinal distribution of the glass fibers during composite material blending and extrusion, and tends to be arranged irregularly in the longitudinal and transverse directions, thereby greatly improving the transverse tensile properties of the thermal insulation strip.

[0013] Preferably, the mass ratio of flame retardant glass fiber modified PA66 to flame retardant hollow glass microsphere modified PA66 is (4-6):1; preferably, the mass ratio of flame retardant glass fiber modified PA66 to flame retardant hollow glass microsphere modified PA66 is 5:1.

[0014] The reinforcing effect of glass fiber requires a certain proportion of it in the PA66 resin. Within the above ratio range, the obtained composite material has good mechanical properties, flame retardancy and thermal insulation properties. Outside the above mass ratio range, the flame retardant effect is reduced. The inventor believes that this may be because when the mass ratio of flame retardant glass fiber modified PA66 and flame retardant hollow glass microsphere modified PA66 is (4-6):1, the ratio of glass fiber and hollow glass microsphere in the system is appropriate, achieving more effective continuous flame retardant points and steric effect, thereby improving the flame retardancy and transverse tensile effect of the composite material. When the mass ratio of flame retardant glass fiber modified PA66 and flame retardant hollow glass microsphere modified PA66 is 5:1, the flame retardancy and transverse tensile properties of the composite polyamide are particularly outstanding.

[0015] Preferably, the preparation method of flame retardant glass fiber modified PA66 comprises the following steps:

[0016] S1: dissolving a phosphorus-containing silane coupling agent and an aminosilane coupling agent in an ethanol aqueous solution to prepare a mixed silane coupling agent solution;

[0017] S2: Dipping the glass fiber in the mixed silane coupling agent solution of S1, taking it out and drying and curing it to obtain the modified glass fiber;

[0018] S3: Add PA66 and initiator into solvent, raise the temperature to reaction temperature, add acrylic acid monomer, keep the temperature to react, remove impurities, separate, and dry to obtain side chain carboxyl PA66;

[0019] S4: adding the modified glass fiber prepared in S2 and the side chain carboxyl PA66 prepared in S3 into an organic solvent, heating the reaction, and removing the solvent to obtain flame-retardant glass fiber modified PA66.

[0020] The silanization step of the glass fiber can be prepared by hydrolyzing a conventional silane coupling agent. The hydrolyzed silanol group of siloxane reacts with the hydroxyl group on the surface of the glass fiber to graft the phosphorus-containing flame retardant on the surface of the glass fiber, thereby achieving the coating of the flame retardant. At the same time, an aminosilane coupling agent is added for joint modification. The aminosilane coupling agent can improve the compatibility of the glass fiber on the one hand, and can achieve better grafting with the PA66 resin on the other hand.

[0021] The inventors expect that the glass fiber, hollow glass microspheres and flame retardants can play a better role in the performance of the modified PA66 resin, and achieve better compatibility and distribution stability of the above components through grafting. In the present invention, the conventional polyamide side chain is carboxylated, and the free radical initiation of the initiator is used to achieve partial carboxyl grafting on the side chain to achieve the grafting of PA66 resin, glass fiber and hollow glass microspheres. The inventors found that compared with the grafting achieved through the PA66 end carboxyl group, the PA66 side chain grafted with the above flame retardant coated glass fiber and hollow glass microspheres, the composite material exhibits better flame retardancy and tensile properties. This may be because the modified glass microspheres and modified hollow glass microspheres are partially grafted on the side chains of the PA66 resin, and the hydrogen atoms and oxygen atoms of the ungrafted chain segments form hydrogen bonds between the two modified PA66 molecules, thereby making the modified glass microspheres and modified hollow glass microspheres more stably arranged between the resins. The surface-based flame retardant is conducive to the formation of continuous flame retardant points and increases the steric effect of the hollow glass microspheres. The side chain grafting can also meet the content requirements of the glass fiber reinforcement effect.

[0022] Preferably, the mass ratio of the phosphorus-containing silane coupling agent to the aminosilane coupling agent in S1 is (5-8): 1. The mass ratio of PA66 to the acrylic monomer in S3 is (10-20): 1.

[0023] By adjusting the mass ratio of phosphorus silane coupling agent and aminosilane coupling agent, the phosphorus-containing component can be better coated on the surface of glass fiber, improving the flame retardant performance, and the amount of aminosilane is appropriate to improve the grafting effect, so that the flame retardant and transverse tensile effects are better. The mass ratio of PA66 and acrylic monomer in the range of (10-20):1 is beneficial to the performance of the composite material. Too little grafting cannot meet the overall flame retardant, tensile and mechanical properties of the composite material. Too much grafting will affect the molecular force of PA66 and reduce the rigidity and impact resistance of the material.

[0024] Preferably, the preparation method of flame retardant hollow glass microspheres modified PA66 comprises the following steps:

[0025] S11: dissolving a phosphorus-containing silane coupling agent and an aminosilane coupling agent in an ethanol aqueous solution to prepare a mixed silane coupling agent solution;

[0026] S12: After the hollow glass microspheres are hydroxylated, they are added to the mixed silane coupling agent solution of S11 for heating reaction, and then filtered, washed, and dried to obtain modified hollow glass microspheres;

[0027] S13: adding PA66 and an initiator into a solvent, heating to a reaction temperature, adding an acrylic acid monomer, keeping the temperature for reaction, removing impurities, separating, and drying to obtain a side chain carboxyl PA66;

[0028] S14: adding the modified hollow glass microspheres prepared in S12 and the side chain carboxyl PA66 prepared in S13 into an organic solvent, heating the reaction, and removing the solvent to obtain flame-retardant hollow glass microsphere modified PA66.

[0029] The mass ratio of the phosphorus-containing silane coupling agent to the aminosilane coupling agent in S11 is (5-8):1; the mass ratio of PA66 to the acrylic monomer in S13 is (10-20):1.

[0030] Hollow glass microspheres are first pretreated by hydroxylation to increase the number of hydroxyl groups on the surface of hollow glass microspheres, improve the modification effect of silane coupling agents, improve the flame retardant effect by modification of phosphorus-containing flame retardants, and improve grafting by aminosilane modification to obtain flame-retardant hollow glass microspheres modified PA66. The mass ratio of phosphorus silane coupling agent and aminosilane coupling agent is adjusted to achieve better coating of the phosphorus-containing component on the surface of hollow glass microspheres, improve flame retardant properties, and the amount of aminosilane is appropriate to improve the grafting effect. The overall flame retardancy and thermal insulation properties of the composite material are good when the mass ratio of PA66 to acrylic monomer is within the range of (10-20):1. Excessive grafting will affect the molecular force of PA66 and reduce the rigidity and impact resistance of the material.

[0031] In addition, the present application provides a method for preparing a highly flame-retardant and tensile-resistant polyamide composite material, comprising the following steps: mixing the components in proportion, melt-extruding, and shaping to obtain the composite material.

[0032] By modifying the PA66 resin, two different modified PA66 blends are obtained, and a small amount of masterbatch and antioxidant are added as needed for melt extrusion. The formula is simple, the process is simple, and multiple feeding processes are not required. The process equipment is simplified, and excellent flame retardancy, heat insulation, and tensile properties can be achieved by adding several components.

[0033] The present application also provides a heat-insulating nylon strip, which is prepared by the above-mentioned highly flame-retardant and tensile-resistant polyamide composite material. The composite material of the present application has excellent mechanical strength, good tensile properties, excellent flame-retardant effect, and good thermal insulation. The prepared heat-insulating strip can be used for special fireproof glass aluminum alloy profile insulation parts.

[0034] In summary, this application has at least the following beneficial effects:

[0035] 1. This application prepares a composite material by modifying PA66 resin with flame retardant-coated glass fiber and flame retardant-coated hollow glass microspheres to solve the problems of component compatibility, material flame retardancy, and insufficient transverse tensile properties. The phosphorus-containing flame retardant component is coated on the surface of glass fiber and hollow glass microspheres. On the one hand, it does not affect the mechanical reinforcement and heat insulation effects of glass fiber and hollow glass microspheres. On the other hand, the flame retardancy is improved by the dispersion of glass fiber and hollow glass microspheres. The flame retardant-coated modified glass fiber and hollow glass microspheres are grafted with PA66 resin to improve compatibility. Flame-retardant glass fiber modified PA66 and flame-retardant hollow glass microsphere modified PA66 are used together. The spherical structure of the hollow glass microspheres and the filamentous structure of the fibers are arranged continuously and irregularly in the system. The glass fibers are arranged irregularly in the gaps between the hollow glass microspheres, so that the coated flame retardant achieves continuous flame retardant points, thereby achieving a synergistic flame retardant effect to a certain extent. The flame retardant-coated glass fibers and hollow glass microspheres are arranged between PA66 molecules through hydrogen bonds. The spatial effect of the hollow glass microspheres hinders the longitudinal distribution of the glass fibers during the blending and extrusion of the composite materials to prepare the thermal insulation strips, and tends to be arranged irregularly in the longitudinal and transverse directions, thereby greatly improving the transverse tensile properties of the thermal insulation strips.

[0036] 2. This application adjusts the mass ratio of flame-retardant glass fiber modified PA66 and flame-retardant hollow glass microsphere modified PA66, and uses an appropriate ratio of glass fiber and hollow glass microsphere in the system to achieve more effective continuous flame retardant points, thereby improving the flame retardancy of the composite material. At the same time, it ensures that the mechanical properties, tensile properties, and thermal insulation effects of the composite material are excellent.

[0037] 3. This application realizes the grafting of PA66 resin and glass fiber and hollow glass microspheres by carboxylation of conventional polyamide side chains and free radical initiation of initiator to realize partial carboxyl grafting on the side chains. Compared with the grafting realized by the end carboxyl groups of PA66, the PA66 side chains grafted with flame retardant coated glass fiber and hollow glass microspheres, the composite material exhibits better flame retardancy and transverse tensile properties.

[0038] 4. This application achieves better flame retardant coating, improves flame retardant performance and grafting effect by adjusting the mass ratio of phosphorus silane coupling agent and amino silane coupling agent. Reasonable control of the mass ratio of PA66 and acrylic monomer improves the overall flame retardancy, tensile strength, rigidity, impact resistance and other properties of the composite material. DETAILED DESCRIPTION

[0039] The present application is further described in detail below in conjunction with the examples. Nylon 66 is Shenma Nylon Chemical EPR27; glass fiber chopped length is 4.5 mm; hollow glass microspheres are 3M hollow glass microspheres S32HS; The experimental reagents in the examples or comparative examples, unless otherwise specified, are conventional commercial brands or obtained through conventional preparation processes.

[0040] Flame retardant glass fiber modified PA66:

[0041] S1: dissolving a phosphorus-containing silane coupling agent and an aminosilane coupling agent in an ethanol aqueous solution to prepare a mixed silane coupling agent solution. The ethanol aqueous solution can be prepared at a volume ratio of ethanol to water of 1:1, 1:0.8, or 1:0.6. The aminosilane can be any conventional amino-containing silane coupling agent, γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, or N-(β-aminoethyl)-γ-aminopropyltriethoxysilane; preferably γ-aminopropyltriethoxysilane.

[0042] The phosphorus-containing silane coupling agent is any phosphorus-containing flame retardant silane coupling agent, preferably having the following structure:

[0043]

[0044] The phosphorus-containing silane coupling agent of the above structure is a conventional phosphorus-containing flame retardant with good flame retardancy. It is more conducive to grafting when used for the modification of PA66, and the nitrogen and hydrogen atoms contained in it can enhance the hydrogen bonding effect with the PA66 resin. All embodiments and comparative examples of the present application select the phosphorus-containing silane coupling agent of the above structure.

[0045] The present application has no restrictions on the concentration of the mixed silane coupling agent solution, and surface silanization modification to achieve better flame retardant-coated glass fibers is preferred. The solute mass fraction of the mixed silane coupling agent solution is preferably 15-40%. The mass ratio of the phosphorus-containing silane coupling agent to the aminosilane coupling agent is preferably (5-8):1. More preferably, 6:1.

[0046] S2: Dipping the glass fiber in the mixed silane coupling agent solution of S1, taking it out and drying and curing it to obtain the modified glass fiber;

[0047] The glass fiber is preferably contacted with the silane coupling agent by dipping, which is more conducive to surface modification. The drying temperature is 90-150° C., the drying time is 10-20 min, the curing temperature is 120-200° C., and the curing time is 10-20 min.

[0048] S3: Add PA66 and initiator into solvent, raise the temperature to reaction temperature, add acrylic acid monomer, keep the temperature to react, remove impurities, separate, and dry to obtain side chain carboxyl PA66;

[0049] The side chain carboxylation of PA66 is a conventional modification process, and any process for side chain carboxylation can be used to prepare the side chain carboxyl PA66 of this application. In the scheme of this application, the solvent is preferably a mixture of alkane, ether, ester solvent and water, and more preferably a mixture of alkane solvent and water; the initiator is preferably a free radical initiator, and more preferably benzoyl peroxide; the reaction temperature is 80-100°C, the reaction time is 2-4h, and the impurities of the homopolymer are removed by washing with a mixed aqueous solution of sodium chloride and sodium hydroxide, and the drying temperature is 50-80°C. The mass ratio of PA66 and acrylic monomer is preferably (10-20):1.

[0050] S4: adding the modified glass fiber prepared in S2 and the side chain carboxyl PA66 prepared in S3 into an organic solvent, heating the reaction, and removing the solvent to obtain flame-retardant glass fiber modified PA66.

[0051] The mass ratio of modified glass fiber to side chain carboxyl PA66 is preferably 1:(6-10), the reaction temperature is 90-100° C., and the reaction time is 2-4 h; the organic solvent is preferably DMF.

[0052] Flame retardant hollow glass microsphere modified PA66:

[0053] S11: dissolving the phosphorus-containing silane coupling agent and the aminosilane coupling agent in an ethanol aqueous solution to prepare a mixed silane coupling agent solution. The mixed silane coupling agent solution can be prepared in the same manner as the mixed silane coupling agent solution in the step of modifying PA66 with flame-retardant glass fiber.

[0054] The ethanol aqueous solution can be prepared with a volume ratio of ethanol to water of 1:1, 1:0.8, or 1:0.6. The aminosilane can be any conventional amino-containing silane coupling agent, such as γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, or N-(β-aminoethyl)-γ-aminopropyltriethoxysilane; preferably γ-aminopropyltriethoxysilane.

[0055] The phosphorus-containing silane coupling agent is any phosphorus-containing flame retardant silane coupling agent, preferably having the following structure:

[0056]

[0057] The present application has no restrictions on the concentration of the mixed silane coupling agent solution, and surface silanization modification to complete the hollow glass microspheres coated with better flame retardants is preferred. All embodiments and comparative examples of the present application select the above-mentioned phosphorus-containing silane coupling agent. The mass fraction of the mixed silane coupling agent solution is preferably 15-40%. The mass ratio of the phosphorus-containing silane coupling agent to the aminosilane coupling agent is preferably (5-8):1. More preferably 6:1.

[0058] S12: After the hollow glass microspheres are hydroxylated, they are added to the mixed silane coupling agent solution of S11 for heating reaction, and then filtered, washed, and dried to obtain modified hollow glass microspheres;

[0059] Conventional hydroxylation treatment processes can be used to increase the number of hydroxyl groups on the surface of hollow glass microspheres. The hollow glass microspheres are added to a sodium hydroxide solution and refluxed at 80-90°C for 1-2 hours, filtered, washed, and dried to achieve surface hydroxylation. The concentration of the sodium hydroxide solution is preferably 0.2-0.5 mol / L. The hollow glass microspheres are modified in the solution, heated to a reaction temperature of 120-150°C, a reaction time of 30-50 minutes, and a drying temperature of 80-100°C.

[0060] S13: adding PA66 and an initiator into a solvent, heating to a reaction temperature, adding an acrylic acid monomer, keeping the temperature for reaction, removing impurities, separating, and drying to obtain a side chain carboxyl PA66;

[0061] The side chain carboxylation process of PA66 can be the same as or different from the process for preparing glass fiber modified PA66. Any process for grafting carboxyl groups on the side chain can be used to prepare the side chain carboxyl PA66 of this application. In the scheme of this application, the solvent is preferably an alkane, ether, ester solvent and water, more preferably an alkane solvent and water; the initiator is preferably a free radical initiator, more preferably benzoyl peroxide; the reaction temperature is 80-100°C, the reaction time is 2-4h, and the impurities of the homopolymer are removed by washing with a mixed aqueous solution of sodium chloride and sodium hydroxide, and the drying temperature is 50-80°C. The mass ratio of PA66 and acrylic monomer is preferably (10-20):1.

[0062] S14: adding the modified hollow glass microspheres prepared in S12 and the side chain carboxyl PA66 prepared in S13 into an organic solvent, heating the reaction, and removing the solvent to obtain flame-retardant hollow glass microsphere modified PA66.

[0063] The mass ratio of the modified hollow glass microspheres to the side chain carboxyl PA66 is preferably 1:(4-6), the reaction temperature is 90-100° C., and the reaction time is 2-4 h; the organic solvent is preferably DMF.

[0064] An antioxidant is added to the composite material to improve the antioxidant effect. Preferably, the antioxidant is a hindered phenol antioxidant, such as antioxidant 1010.

[0065] Masterbatch can also be added to the composite material according to the process requirements, preferably, black masterbatch is selected. Example 1

[0066] Preparation of flame retardant glass fiber modified PA66:

[0067] 1 kg of ethanol aqueous solution was prepared with a volume ratio of ethanol to water of 1:0.6, 180 g of phosphorus-containing silane coupling agent and 30 g of γ-aminopropyltriethoxysilane were dissolved in the ethanol aqueous solution, and stirred for 1-2 h to prepare a mixed silane coupling agent solution for standby use;

[0068] 20 g of glass fiber was added to the above solution and allowed to stand for 30 min. After being taken out, it was dried at 100° C. for 15 min, and then cured at 160° C. for 15 min to obtain the modified glass fiber for use;

[0069] Prepare a mixed solvent with 600 mL of water and 400 mL of hexane, add 15 g of PA66 resin and 0.15 g of benzoyl peroxide into the mixed solvent, heat to 90°C, add 1 g of acrylic acid monomer, keep warm and react for 3 hours, add 20 g of sodium chloride and 5 g of sodium hydroxide into water to form 500 mL of mixed aqueous solution for washing to remove impurities, separate and remove the solvent, put into a 60°C oven to dry to obtain PA66 with side chain carboxylation for use;

[0070] Take 2 g of the above-mentioned modified glass fiber and 16 g of PA66 with side chain carboxylation, add them into 200 mL of DMF, stir and react at 95° C. for 3 h, remove the solvent, and obtain glass fiber modified PA66.

[0071] Preparation of flame retardant hollow glass microspheres modified PA66:

[0072] 1 kg of ethanol aqueous solution was prepared with a volume ratio of ethanol to water of 1:0.6, 180 g of phosphorus-containing silane coupling agent and 30 g of γ-aminopropyltriethoxysilane were dissolved in the ethanol aqueous solution, and stirred for 1-2 h to prepare a mixed silane coupling agent solution for standby use;

[0073] Weigh 10 g of hollow glass microspheres, add 300 mL of 0.3 mol / L sodium hydroxide solution, reflux at 85° C. for 1.5 h, filter, wash with water 3 times, and dry in an oven to obtain hydroxylated hollow glass microspheres, then add the mixed silane coupling agent solution, heat to 135° C. for reflux reaction for 40 min, filter, wash with water 3 times, and place in a 90° C. oven to obtain modified hollow glass microspheres for standby use;

[0074] Prepare a mixed solvent with 600 mL of water and 400 mL of hexane, add 15 g of PA66 resin and 0.15 g of benzoyl peroxide into the mixed solvent, heat to 90°C, add 1 g of acrylic acid monomer, keep warm and react for 3 hours, add 500 mL of a mixed aqueous solution of 20 g of sodium chloride and 5 g of sodium hydroxide to wash and remove impurities, separate and remove the solvent, put into a 60°C oven to dry to obtain side chain carboxylated PA66 for use;

[0075] 2 g of the modified hollow glass microspheres and 10 g of PA66 with side chain carboxylation were added to 200 mL of DMF, stirred and reacted at 95° C. for 3 h, and the solvent was removed to obtain hollow glass microsphere-modified PA66.

[0076] Preparation of composite material: 8 kg of flame-retardant glass fiber modified PA66 prepared in the above manner, 2.8 kg of flame-retardant hollow glass microsphere modified PA66, 50 g of antioxidant 1010, and 100 g of black masterbatch were melt-blended for 10 min and extruded to obtain a composite material. The temperature of the feeding zone was 180°C, the temperature of the compression zone was 260°C, and the temperature of the homogenization zone was 280°C. Example 2

[0077] 8.7 kg of flame-retardant glass fiber modified PA66 prepared in the manner of Example 1, 2.1 kg of flame-retardant hollow glass microsphere modified PA66 prepared in the manner of Example 1, 50 g of antioxidant 1010, and 100 g of black masterbatch were melt-blended for 10 min and extruded to obtain a composite material. The temperature of the feeding zone was 180° C., the temperature of the compression zone was 260° C., and the temperature of the homogenization zone was 280° C. Example 3

[0078] 9 kg of flame-retardant glass fiber modified PA66 prepared in the manner of Example 1, 1.8 kg of flame-retardant hollow glass microsphere modified PA66 prepared in the manner of Example 1, 50 g of antioxidant 1010, and 100 g of black masterbatch were melt-blended for 10 min and extruded to obtain a composite material. The temperature of the feeding zone was 180°C, the temperature of the compression zone was 260°C, and the temperature of the homogenization zone was 280°C. Example 4

[0079] 9.2 kg of flame-retardant glass fiber modified PA66 prepared in the manner of Example 1, 1.6 kg of flame-retardant hollow glass microsphere modified PA66 prepared in the manner of Example 1, 50 g of antioxidant 1010, and 100 g of black masterbatch were melt-blended for 10 min and extruded to obtain a composite material. The temperature of the feeding zone was 180° C., the temperature of the compression zone was 260° C., and the temperature of the homogenization zone was 280° C. Example 5

[0080] 9.6 kg of flame-retardant glass fiber modified PA66 prepared in the manner of Example 1, 1.2 kg of flame-retardant hollow glass microsphere modified PA66 prepared in the manner of Example 1, 50 g of antioxidant 1010, and 100 g of black masterbatch were melt-blended for 10 min and extruded to obtain a composite material. The temperature of the feeding zone was 180° C., the temperature of the compression zone was 260° C., and the temperature of the homogenization zone was 280° C. Example 6

[0081] Preparation of flame retardant glass fiber modified PA66:

[0082] 1 kg of ethanol aqueous solution was prepared with a volume ratio of ethanol to water of 1:0.6, 160 g of phosphorus-containing silane coupling agent and 50 g of γ-aminopropyltriethoxysilane were dissolved in the ethanol aqueous solution, and stirred for 1-2 h to prepare a mixed silane coupling agent solution for standby use;

[0083] 20 g of glass fiber was added to the above solution and allowed to stand for 30 min. After being taken out, it was dried at 100° C. for 15 min, and then cured at 160° C. for 15 min to obtain the modified glass fiber for use;

[0084] Prepare a mixed solvent with 600 mL of water and 400 mL of hexane, add 15 g of PA66 resin and 0.15 g of benzoyl peroxide into the mixed solvent, heat to 90°C, add 1 g of acrylic acid monomer, keep warm and react for 3 hours, add 500 mL of a mixed aqueous solution of 20 g of sodium chloride and 5 g of sodium hydroxide to wash and remove impurities, separate and remove the solvent, put into a 60°C oven to dry to obtain side chain carboxylated PA66 for use;

[0085] 2 g of the modified glass fiber and 16 g of PA66 with side chain carboxylation were added to 200 mL of DMF, stirred and reacted at 95 °C for 3 h, and the solvent was removed to obtain glass fiber modified PA66;

[0086] 9.6 kg of flame-retardant glass fiber modified PA66 prepared in the above manner, 1.2 kg of flame-retardant hollow glass microsphere modified PA66 prepared in the manner of Example 1, 50 g of antioxidant 1010, and 100 g of black masterbatch were melt-blended for 10 min and extruded to obtain a composite material. The temperature of the feeding zone was 180°C, the temperature of the compression zone was 260°C, and the temperature of the homogenization zone was 280°C. Example 7

[0087] Preparation of flame retardant glass fiber modified PA66:

[0088] 1 kg of ethanol aqueous solution was prepared with a volume ratio of ethanol to water of 1:0.6, 190 g of phosphorus-containing silane coupling agent and 20 g of γ-aminopropyltriethoxysilane were dissolved in the ethanol aqueous solution, and stirred for 1-2 h to prepare a mixed silane coupling agent solution for standby use;

[0089] 20 g of glass fiber was added to the above solution and allowed to stand for 30 min. After being taken out, it was dried at 100° C. for 15 min, and then cured at 160° C. for 15 min to obtain the modified glass fiber for use;

[0090] Prepare a mixed solvent with 600 mL of water and 400 mL of hexane, add 15 g of PA66 resin and 0.15 g of benzoyl peroxide into the mixed solvent, heat to 90°C, add 1 g of acrylic acid monomer, keep warm and react for 3 hours, add 500 mL of a mixed aqueous solution of 20 g of sodium chloride and 5 g of sodium hydroxide to wash and remove impurities, separate and remove the solvent, put into a 60°C oven to dry to obtain side chain carboxylated PA66 for use;

[0091] Take 2 g of the above-mentioned modified glass fiber and 16 g of PA66 with side chain carboxylation, add them into 200 mL of DMF, stir and react at 95° C. for 3 h, remove the solvent, and obtain glass fiber modified PA66.

[0092] 9.6 kg of flame-retardant glass fiber modified PA66 prepared in the above manner, 1.2 kg of flame-retardant hollow glass microsphere modified PA66 prepared in the manner of Example 1, 50 g of antioxidant 1010, and 100 g of black masterbatch were melt-blended for 10 min and extruded to obtain a composite material. The temperature of the feeding zone was 180°C, the temperature of the compression zone was 260°C, and the temperature of the homogenization zone was 280°C. Example 8

[0093] Preparation of flame retardant hollow glass microspheres modified PA66:

[0094] 1 kg of ethanol aqueous solution was prepared with a volume ratio of ethanol to water of 1:0.6, 160 g of phosphorus-containing silane coupling agent and 50 g of γ-aminopropyltriethoxysilane were dissolved in the ethanol aqueous solution, and stirred for 1-2 h to prepare a mixed silane coupling agent solution for standby use;

[0095] Weigh 10 g of hollow glass microspheres, add 300 mL of 0.3 mol / L sodium hydroxide solution, reflux at 85° C. for 1.5 h, filter, wash with water 3 times, and dry in an oven to obtain hydroxylated hollow glass microspheres, then add the mixed silane coupling agent solution, heat to 135° C. for reflux reaction for 40 min, filter, wash with water 3 times, and place in a 90° C. oven to obtain modified hollow glass microspheres for standby use;

[0096] Prepare a mixed solvent with 600 mL of water and 400 mL of hexane, add 15 g of PA66 resin and 0.15 g of benzoyl peroxide into the mixed solvent, heat to 90°C, add 1 g of acrylic acid monomer, keep warm and react for 3 hours, add 500 mL of a mixed aqueous solution of 20 g of sodium chloride and 5 g of sodium hydroxide to wash and remove impurities, separate and remove the solvent, put into a 60°C oven to dry to obtain PA66 with side chain carboxylation for use;

[0097] 2 g of the modified hollow glass microspheres and 10 g of PA66 with side chain carboxylation were added to 200 mL of DMF, stirred and reacted at 95° C. for 3 h, and the solvent was removed to obtain hollow glass microsphere-modified PA66.

[0098] 9.6 kg of flame-retardant glass fiber modified PA66 prepared in the manner of Example 1, 1.2 kg of flame-retardant hollow glass microsphere modified PA66 prepared in the above manner, 50 g of antioxidant 1010, and 100 g of black masterbatch were melt-blended for 10 min and extruded to obtain a composite material. The temperature of the feeding zone was 180°C, the temperature of the compression zone was 260°C, and the temperature of the homogenization zone was 280°C. Example 9

[0099] Preparation of flame retardant hollow glass microspheres modified PA66:

[0100] 1 kg of ethanol aqueous solution was prepared with a volume ratio of ethanol to water of 1:0.6, 190 g of phosphorus-containing silane coupling agent and 20 g of γ-aminopropyltriethoxysilane were dissolved in the ethanol aqueous solution, and stirred for 1-2 h to prepare a mixed silane coupling agent solution for standby use;

[0101] Weigh 10 g of hollow glass microspheres, add 300 mL of 0.3 mol / L sodium hydroxide solution, reflux at 85° C. for 1.5 h, filter, wash with water 3 times, and dry in an oven to obtain hydroxylated hollow glass microspheres, then add the mixed silane coupling agent solution, heat to 135° C. for reflux reaction for 40 min, filter, wash with water 3 times, and place in a 90° C. oven to obtain modified hollow glass microspheres for standby use;

[0102] Prepare a mixed solvent with 600 mL of water and 400 mL of hexane, add 15 g of PA66 resin and 0.15 g of benzoyl peroxide into the mixed solvent, heat to 90°C, add 1 g of acrylic acid monomer, keep warm and react for 3 hours, add 500 mL of a mixed aqueous solution of 20 g of sodium chloride and 5 g of sodium hydroxide to wash and remove impurities, separate and remove the solvent, put into a 60°C oven to dry to obtain side chain carboxylated PA66 for use;

[0103] 2 g of the modified hollow glass microspheres and 10 g of PA66 with side chain carboxylation were added to 200 mL of DMF, stirred and reacted at 95° C. for 3 h, and the solvent was removed to obtain hollow glass microsphere-modified PA66.

[0104] 9.6 kg of flame-retardant glass fiber modified PA66 prepared in the manner of Example 1, 1.2 kg of flame-retardant hollow glass microsphere modified PA66 prepared in the above manner, 50 g of antioxidant 1010, and 100 g of black masterbatch were melt-blended for 10 min and extruded to obtain a composite material. The temperature of the feeding zone was 180°C, the temperature of the compression zone was 260°C, and the temperature of the homogenization zone was 280°C. Example 10

[0105] Preparation of flame retardant glass fiber modified PA66:

[0106] 1 kg of ethanol aqueous solution was prepared with a volume ratio of ethanol to water of 1:0.6, 180 g of phosphorus-containing silane coupling agent and 30 g of γ-aminopropyltriethoxysilane were dissolved in the ethanol aqueous solution, and stirred for 1-2 h to prepare a mixed silane coupling agent solution for standby use;

[0107] 20 g of glass fiber was added to the above solution and allowed to stand for 30 min. After being taken out, it was dried at 100° C. for 15 min, and then cured at 160° C. for 15 min to obtain the modified glass fiber for use;

[0108] Take 2 g of the above modified glass fiber and 16 g of PA66, add them into 200 mL of DMF, stir and react at 95° C. for 3 h, remove the solvent, and obtain glass fiber modified PA66.

[0109] Preparation of flame retardant hollow glass microspheres modified PA66:

[0110] 1 kg of ethanol aqueous solution was prepared with a volume ratio of ethanol to water of 1:0.6, 180 g of phosphorus-containing silane coupling agent and 30 g of γ-aminopropyltriethoxysilane were dissolved in the ethanol aqueous solution, and stirred for 1-2 h to prepare a mixed silane coupling agent solution for standby use;

[0111] Weigh 10 g of hollow glass microspheres, add 300 mL of 0.3 mol / L sodium hydroxide solution, reflux at 85° C. for 1.5 h, filter, wash with water 3 times, and dry in an oven to obtain hydroxylated hollow glass microspheres, then add the mixed silane coupling agent solution, heat to 135° C. for reflux reaction for 40 min, filter, wash with water 3 times, and place in a 90° C. oven to obtain modified hollow glass microspheres for standby use;

[0112] Take 2 g of the above-mentioned modified hollow glass microspheres and 10 g of PA66, add them into 200 mL of DMF, stir and react at 95° C. for 3 h, remove the solvent, and obtain hollow glass microsphere-modified PA66.

[0113] 9.6 kg of flame-retardant glass fiber modified PA66 prepared in the above manner, 1.2 kg of flame-retardant hollow glass microsphere modified PA66 prepared in the above manner, 50 g of antioxidant 1010, and 100 g of black masterbatch were melt-blended for 10 min and extruded to obtain a composite material. The temperature of the feeding zone was 180°C, the temperature of the compression zone was 260°C, and the temperature of the homogenization zone was 280°C.

[0114] Comparative Example 1

[0115] 10.8 kg of flame-retardant glass fiber modified PA66 prepared in the manner of Example 1, 50 g of antioxidant 1010, and 100 g of black masterbatch were melt-blended for 10 min and extruded to obtain a composite material. The temperature of the feeding zone was 180°C, the temperature of the compression zone was 260°C, and the temperature of the homogenization zone was 280°C.

[0116] Comparative Example 2

[0117] 10.8 kg of flame-retardant hollow glass microsphere modified PA66 prepared in the manner of Example 1, 50 g of antioxidant 1010, and 100 g of black masterbatch were melt-blended for 10 min and extruded to obtain a composite material. The temperature of the feeding zone was 180°C, the temperature of the compression zone was 260°C, and the temperature of the homogenization zone was 280°C.

[0118] Comparative Example 3

[0119] 1kg of glass fiber, 9.5kg of PA66, 0.3kg of hollow glass microspheres, 50g of antioxidant 1010, and 100g of black masterbatch were melt-blended for 10 minutes and extruded to obtain a composite material. The temperature of the feeding zone was 180°C, the temperature of the compression zone was 260°C, and the temperature of the homogenization zone was 280°C.

[0120] Comparative Example 4

[0121] 1 kg of modified glass fiber of Example 1, 9.5 kg of PA66, 0.3 kg of modified hollow glass microspheres of Example 1, 50 g of antioxidant 1010, and 100 g of black masterbatch were melt-blended for 10 min and extruded to obtain a composite material. The temperature of the feeding zone was 180°C, the temperature of the compression zone was 260°C, and the temperature of the homogenization zone was 280°C.

[0122] Comparative Example 5

[0123] 9 kg of flame-retardant glass fiber modified PA66 prepared in the manner of Example 1, 0.3 kg of modified hollow glass microspheres of Example 1, 1.5 kg of PA66, 50 g of antioxidant 1010, and 100 g of black masterbatch were melt-blended for 10 min and extruded to obtain a composite material. The temperature of the feeding zone was 180°C, the temperature of the compression zone was 260°C, and the temperature of the homogenization zone was 280°C.

[0124] Comparative Example 6

[0125] 1 kg of modified glass fiber of Example 1, 8 kg of PA66, 1.8 kg of flame-retardant hollow glass microspheres modified PA66 prepared in the manner of Example 1, 50 g of antioxidant 1010, and 100 g of black masterbatch were melt-blended for 10 min and extruded to obtain a composite material. The temperature of the feeding zone was 180°C, the temperature of the compression zone was 260°C, and the temperature of the homogenization zone was 280°C.

[0126] Performance testing:

[0127] Limiting oxygen index: The composite materials of Examples 1-10 and Comparative Examples 1-6 were injection molded into test standard specimens, and the limiting oxygen index was tested using an oxygen index tester according to GB / T 2406.2-2009 standard.

[0128] Transverse tensile strength: The composite materials of Examples 1-10 and Comparative Examples 1-6 were injection molded into test standard specimens, and the room temperature transverse tensile strength was tested according to GB / T 23615.1-2009 standard.

[0129] The test results are shown in Table 1:

[0130] Limiting oxygen index (%) Transverse tensile strength (Mpa) Example 1 38.7 117 Example 2 40.4 121 Example 3 41.1 122 Example 4 39.5 123 Example 5 38.2 120 Example 6 35.1 116 Example 7 36.4 115 Example 8 36.9 118 Example 9 37.3 117 Example 10 33.8 119 Comparative Example 1 30.7 110 Comparative Example 2 31.5 65 Comparative Example 3 21.5 98 Comparative Example 4 28.2 102 Comparative Example 5 32.6 112 Comparative Example 6 32.2 104

[0131] It can be seen from Examples 1-10 and Comparative Examples 1-6 that the present application replaces conventional PA66 with modified flame-retardant glass fiber modified PA66 and flame-retardant hollow glass microsphere modified PA66 to prepare a composite material, thereby achieving excellent flame retardancy and transverse tensile properties of PA66 polyamide material. At the same time, it can be seen from Examples 1-5 that the flame retardant effect is better when the mass ratio of modified flame-retardant glass fiber modified PA66 and flame-retardant hollow glass microsphere modified PA66 is (4-6):1, and the flame retardant effect is best when the mass ratio is 5:1, and it also has excellent transverse tensile strength.

[0132] Combining Examples 5-9, it can be seen that the flame retardancy and transverse tensile properties are good when the ratio of phosphorus-containing silane coupling agent to aminosilane coupling agent is within an appropriate range, and the performance of Example 5 is slightly better than that of Examples 6-9 when the ratio of phosphorus-containing silane coupling agent to aminosilane coupling agent is 6:1. It can be seen from Examples 5 and 10 that the flame retardancy and transverse tensile properties of Example 10 are inferior to those of Example 5, and the modified PA66 obtained by the modification step of the present application can further improve the performance of the composite material.

[0133] Combining Example 3 and Comparative Examples 1-5, it can be seen that by co-coating the flame retardant with glass fiber and hollow glass microspheres and then grafting PA66, the performance of the composite material is greatly improved.

[0134] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A highly flame-retardant and tensile-resistant polyamide composite material, It is characterized in that The composition comprises the following components in parts by weight: Modified polyamide resin 100-120 parts, Antioxidant 0.2-1 part, Masterbatch 0.5-2 parts, The modified polyamide resin is a mixture of flame retardant glass fiber modified PA66 and flame retardant hollow glass microsphere modified PA66; The preparation method of the flame-retardant glass fiber modified PA66 comprises the following steps: S1: dissolving a phosphorus-containing silane coupling agent and an aminosilane coupling agent in an ethanol aqueous solution to prepare a mixed silane coupling agent solution; S2: Dipping the glass fiber in the mixed silane coupling agent solution of S1, taking it out and drying and curing it to obtain the modified glass fiber; S3: Add PA66 and initiator into solvent, raise the temperature to reaction temperature, add acrylic acid monomer, keep the temperature to react, remove impurities, separate, and dry to obtain side chain carboxyl PA66; S4: adding the modified glass fiber prepared in S2 and the side chain carboxyl PA66 prepared in S3 into an organic solvent, heating the reaction, and removing the solvent to obtain flame-retardant glass fiber modified PA66; The preparation method of flame retardant hollow glass microsphere modified PA66 comprises the following steps: S11: dissolving a phosphorus-containing silane coupling agent and an aminosilane coupling agent in an ethanol aqueous solution to prepare a mixed silane coupling agent solution; S12: After the hollow glass microspheres are hydroxylated, they are added to the mixed silane coupling agent solution of S11 for heating reaction, and then filtered, washed, and dried to obtain modified hollow glass microspheres; S13: adding PA66 and an initiator into a solvent, heating to a reaction temperature, adding an acrylic acid monomer, keeping the temperature for reaction, removing impurities, separating, and drying to obtain a side chain carboxyl PA66; S14: adding the modified hollow glass microspheres prepared in S12 and the side chain carboxyl PA66 prepared in S13 into an organic solvent, heating the mixture for reaction, and removing the solvent to obtain flame-retardant hollow glass microspheres modified PA66; The mass ratio of the flame retardant glass fiber modified PA66 to the flame retardant hollow glass microsphere modified PA66 is (4-6):1; The mass ratio of the phosphorus-containing silane coupling agent to the aminosilane coupling agent in S1 is (5-8):

1.

2. The highly flame-retardant and tensile-resistant polyamide composite material according to claim 1, It is characterized in that The mass ratio of the flame retardant glass fiber modified PA66 to the flame retardant hollow glass microsphere modified PA66 is 5:

1.

3. The highly flame-retardant and tensile-resistant polyamide composite material according to claim 1, It is characterized in that The mass ratio of PA66 to acrylic acid monomer in S3 is (10-20):

1.

4. The highly flame-retardant and tensile-resistant polyamide composite material according to claim 1, It is characterized in that The mass ratio of the phosphorus-containing silane coupling agent to the aminosilane coupling agent in the S11 is (5-8):1; the mass ratio of PA66 to the acrylic monomer in the S13 is (10-20):

1.

5. A method for preparing the highly flame-retardant and tensile-resistant polyamide composite material according to any one of claims 1 to 4, It is characterized in that The method comprises the following steps: mixing the components in proportion, melting and extruding, and shaping to obtain the composite material.

6. A heat-insulating nylon strip, It is characterized in that The composite material is prepared from the highly flame-retardant and tensile-resistant polyamide composite material according to any one of claims 1 to 4.