Reverse osmosis composite membrane and its preparation method and application
Through the combination technology of modified base membrane layer and polyamide separation skin layer, the problem of insufficient performance stability of reverse osmosis composite membrane under high-salt and high-pressure conditions is solved, and the effect of low salt rejection rate and average annual water flux attenuation is achieved. Extended membrane life and improved salt retention performance.
Patent Information
- Application Number
- CN202410904483.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-07-08
AI Technical Summary
It is difficult for existing reverse osmosis composite membranes to simultaneously achieve low annual average attenuation of salt rejection rate and average annual attenuation of water flux under high-salt and high-pressure conditions, resulting in insufficient performance stability.
The modified base film layer is prepared by compounding the casting liquid on the non-woven fabric through the phase inversion method. The casting liquid contains poly(p-phenylene terephthalamide), B-stage phenolic resin and triethylamine, and is passed through a specific solvent. It forms a body-shaped phenolic resin structure according to the reaction conditions, improves the compressive strength and creep resistance of the base film layer, and generates a polyamide separation skin layer on the surface of the modified base film layer.
The stable performance of the reverse osmosis composite membrane under long-term high-pressure conditions is achieved, with the average annual desalination rate attenuation <1% and the average annual water flux attenuation <3%, extending the service life of the membrane and improving the salt interception performance.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of composite membranes for separation, and in particular relates to a reverse osmosis composite membrane and a preparation method and application thereof. Background Art
[0002] Reverse osmosis is an economical and effective method for water resource utilization and liquid concentration. It uses hollow fiber reverse osmosis membranes or rolled reverse osmosis membranes. When a pressure greater than the osmotic pressure between the liquids or liquid flows on both sides of the reverse osmosis membrane is applied to the concentrated liquid (such as tap water, seawater, and wastewater), the solvent in the concentrated liquid, such as water, will pass through the reverse osmosis membrane and flow to the dilute liquid side, while the components other than the solvent in the concentrated liquid basically cannot pass through the reverse osmosis membrane, thereby achieving concentrated and dilute separation, especially the preparation of pure water. Reverse osmosis membranes are generally assembled into assemblies and operated in a cross-flow manner. Osmotic pressure reflects the binding force between solute particles and solvent in liquid, which is generally proportional to the volume molar concentration, weight concentration and absolute temperature of the solution, and is also affected by conditions such as pH value. For example, normal saline at room temperature, that is, a sodium chloride aqueous solution with a concentration of 0.9wt%, has an osmotic pressure of about 0.79MPa; a normal temperature glucose aqueous solution with a concentration of 5.0wt%, has an osmotic pressure of about 0.71MPa; the osmotic pressure of normal temperature milk is generally 0.71-0.80MPa; the osmotic pressure of normal temperature seawater with a salinity of 35 (3.5wt%) is about 2.45MPa. In applications under high salt and high pressure conditions, a rolled reverse osmosis composite membrane is generally used.
[0003] The common structure of a rolled reverse osmosis composite membrane usually includes three parts: ① The functional cortex, or selective separation layer, is the outermost layer on the high-pressure side of the reverse osmosis composite membrane. It is generally a polyamide layer formed by interfacial polymerization of polyamine monomers and acyl chloride monomers. It is about 100nm thick and has a dense structure, but contains a large number of pores with an equivalent pore diameter of less than 1nm and with charges. It is a functional layer that separates and selectively blocks macromolecules, ions and trace particles contained in the concentrated liquid; ② The base membrane layer, or porous support layer, is the middle layer of the reverse osmosis composite membrane. It is generally a polysulfone ultrafiltration layer with a thickness of about 50μm. It plays a pore transition role, provides mechanical support for the functional cortex, has good water permeability, and the surface layer combined with the functional cortex has a suitable surface flatness and pore size; ③ The non-woven fabric layer is generally made of polyester, polypropylene, polyacrylonitrile and other materials. It provides basic mechanical strength and support for the composite membrane and is also the initial carrier for the continuous production of the composite membrane. In the prior art, the improvement of the reverse osmosis composite membrane mainly focuses on the modification of the functional skin layer and the porous support layer and the composite preparation process thereof.
[0004] The porous support layer of the rolled reverse osmosis composite membrane is generally prepared by a phase inversion method, in which a non-woven fabric is coated with a polysulfone solution on one side and then placed in an aqueous coagulation bath to undergo phase change curing of the polysulfone. For example, the pressure-resistant polysulfone-based membrane disclosed in Chinese patent application CN114130216A comprises a non-woven fabric layer and a polysulfone-based layer prepared by coating a polysulfone solution on the non-woven fabric, wherein the polysulfone solution contains the following components by weight percentage: 15-25% of polysulfone (bisphenol A type polysulfone, polyethersulfone or polyarylsulfone), 4-18% of pore-forming agent (such as ethanol, propanol, ethylene glycol, glycerol, ethyl ether, ethylene glycol methyl ether, acetone, butanone, ethyl acetate, polyethylene glycol, polyvinyl alcohol or polyvinyl pyrrolidone), 0.04-0.2% of surfactant (such as sodium dodecylbenzene sulfonate, sodium dodecyl sulfate, Tween, Span, alkyl ether phosphate or phenol ether phosphate), and the rest is solvent (one of N,N-dimethylformamide, N,N-dimethylacetamide and N-methyl-2-pyrrolidone or a mixture thereof). The preparation method of the polysulfone-based membrane includes the following steps: 1) preparing a polysulfone solution by weight percentage, and dissolving it uniformly under certain dissolving conditions; 2) applying the polysulfone solution on a non-woven fabric, placing it in a coagulation bath for phase change solidification, and forming a pressure-resistant polysulfone-based membrane; the pore size of the polysulfone-based membrane is in the range of 10-50 nanometers, the water production is 800-1200L / ㎡ / h, the cross-sectional structure of the base membrane is a three-dimensional network frame structure, and it is not easy to deform when operating under a pressure of 5MPa, and can be used as a reverse osmosis membrane for treating brackish water and high-salt wastewater and a base membrane for seawater desalination reverse osmosis membrane. The polysulfone-based structure determines the pressure resistance of the reverse osmosis composite membrane; according to the order of pressure resistance from small to large, the common structures of the polysulfone-based layer are large bottom pore structure, sponge chamber structure, and three-dimensional network frame structure.
[0005] A method for preparing a polyamide skin layer by interfacial polymerization of polyamine monomers and acyl chloride monomers, such as the preparation method of a high-rejection seawater desalination composite reverse osmosis membrane disclosed in Chinese patent CN112354374A: immersing the membrane surface of a polysulfone ultrafiltration membrane on one side in an aqueous solution for 0.5-2 minutes, draining the liquid, removing the remaining liquid on the membrane surface, and then contacting the membrane surface with an oil phase solution on one side, performing interfacial polymerization at 70-100°C for 0.5-1.5 minutes, draining the liquid, and placing at 70-100°C for 2-7 minutes (heat treatment) to obtain a composite reverse osmosis membrane. The invention relates to a permeable membrane; the mass concentration of the aqueous phase solution is composed of: 3.0-5.0% m-phenylenediamine, 2.5-5.0% camphorsulfonic acid, 1.5-3.5% triethylamine, and the balance is water; the mass concentration of the oil phase solution is composed of: 0.1-0.2% trimesoyl chloride, 0.1-0.2% naphthalene trisulfonyl chloride, and the balance is a mixed solution of 80-95% isoparaffin and 5-20% xylene in a mass ratio; the naphthalene trisulfonyl chloride is preferably 1,3,6-naphthalene trisulfonyl chloride or 1,3,5-naphthalene trisulfonyl chloride; the isoparaffin is preferably Isopar G, Isopar M or Isopar L; the molecular weight cutoff of the polysulfone ultrafiltration membrane is preferably 20000-60000. In the preparation method, the naphthalene trisulfonyl chloride used has low reactivity and does not react with m-phenylenediamine, but is embedded in the polyamide network, thereby improving the salt retention and boric acid retention performance of the reverse osmosis membrane, and significantly improving the desalination and deboronization performance while ensuring a high water flux level; under the conditions of an aqueous solution of a final concentration of 35000ppm NaCl and a final concentration of 5ppm boric acid, a pressure difference of 5.5MPa, and a temperature of 25°C, the separation performance of the composite reverse osmosis membrane prepared in Examples 1-4 is: a water permeation of 37.83-47.16L / m 2 ·h, sodium chloride retention rate 99.57-99.91%, boric acid retention rate 92.54-95.34%.
[0006] In processes such as seawater desalination and high-salt brackish water desalination that require higher reverse osmosis operating pressure (the reverse osmosis operating pressure in the seawater desalination process is generally 5-6MPa), a three-layer, rolled reverse osmosis composite membrane is usually used, but the performance and stability requirements of the functional cortex and porous support layer are relatively high. At present, the technical indicators of the reverse osmosis membrane with better performance for seawater desalination include: service life of 3-5 years, water recovery rate of 35-50%, initial water flux (water production)> 40L / m 2 ·h, initial desalination rate>99.5%, desalination rate decays by 1.2-1.5% per year, and water flux decays by 3-5% per year.
[0007] Practical experience shows that it is difficult for the rolled reverse osmosis composite membrane prepared by the existing technical methods such as Chinese patent CN112354374A to simultaneously achieve an annual average attenuation of desalination rate of less than 1% and an annual average attenuation of water flux of less than 3%, that is, there are still deficiencies in the stability of performance. Summary of the invention
[0008] The purpose of the present invention is to provide a reverse osmosis composite membrane, which has lower annual average attenuation of desalination rate and water flux and good stability performance; the present invention also provides a preparation method and application of the reverse osmosis composite membrane.
[0009] The reverse osmosis composite membrane of the present invention is a roll-type membrane which comprises, from top to bottom, a separation skin layer, a modified base membrane layer, and a non-woven fabric layer. The modified base membrane layer is prepared by compounding a casting liquid on a single surface of a non-woven fabric by a phase inversion method. The casting liquid comprises the following components in parts by weight:
[0010] 20-25 parts of base film resin with molecular weight of 30000-150000;
[0011] 1-1.5 parts of poly(p-phenylene terephthalamide) with a molecular weight of 5000-8000, added in the form of a solution of poly(p-phenylene terephthalamide) in N-methylpyrrolidone;
[0012] 1.5-2.5 parts of resol phenolic resin with a molecular weight of 1000-1500, added in the form of a solution of the resol phenolic resin in N-methylpyrrolidone;
[0013] 0.4-0.6 parts of triethylamine;
[0014] 10-15 parts of cosolvent;
[0015] The total amount of N-methylpyrrolidone (NMP) is 120-150 parts; including the amount of N-methylpyrrolidone used for preparing the N-methylpyrrolidone solution of poly(p-phenylene terephthalamide), the amount of N-methylpyrrolidone used for preparing the N-methylpyrrolidone solution of the ethyl-resin and the amount of N-methylpyrrolidone used for preparing the casting solution.
[0016] in:
[0017] The N-methylpyrrolidone solution of poly(p-phenylene terephthalamide) is prepared by the following method:
[0018] In a reactor under nitrogen protection and anhydrous conditions, N-methylpyrrolidone, lithium chloride and N-methylpyrrolidone solution of p-phenylenediamine are prepared into a mixed solution; the reactor is placed in a cold bath at -10 to -5°C, pyridine is added to the mixed solution, stirring is continued, terephthaloyl chloride is added, and the reaction is carried out for 1-2 hours to obtain an N-methylpyrrolidone solution of poly(p-phenylene terephthalamide); wherein the weight ratio of N-methylpyrrolidone, lithium chloride, p-phenylene diamine, pyridine and terephthaloyl chloride is (15-25):(0.3-0.5):1:(0.5-0.7):(1.94-2.01); the amount of N-methylpyrrolidone accounts for 21-22wt% of the total amount of N-methylpyrrolidone, and the amount of N-methylpyrrolidone in the N-methylpyrrolidone solution of p-phenylene diamine accounts for 5-6wt% of the total amount of N-methylpyrrolidone.
[0019] The N-methylpyrrolidone solution of the resol phenolic resin is prepared by the following method:
[0020] In a stirred reactor with cooling reflux and connected to a vacuum system, add a 37-40wt% formaldehyde aqueous solution, add phenol and oxalic acid, continue stirring, open reflux, reflux cooling water temperature 10-15°C, heat the feed liquid to 60-65°C and stir for 0.5-1h, then heat it to 75-80°C and react at this temperature for 5-8h, add sodium hydroxide to neutralize to pH 7.5-8, wash with water, then perform reduced pressure distillation under a vacuum condition of -0.078 to -0.083MPa, heat it to 148-152°C at a rate of 1-2°C / min until there is no distillate, close the vacuum and fill it with nitrogen to normal pressure, add N -methyl pyrrolidone, control the temperature at 148-152°C and stir for 5-10 minutes, then open the vacuum system for reduced pressure distillation at a pressure of -0.078 to -0.083 MPa, and distill until there is no distillate under the vacuum condition and the temperature of 148-152°C, and finally add N-methyl pyrrolidone to obtain a 20-50wt% N-methyl pyrrolidone solution of ethyl-resin, wherein the molar ratio of formaldehyde, phenol and oxalic acid is (0.8-1.0):1:(0.006-0.01), and the amount of N-methyl pyrrolidone added twice accounts for 12-15wt% of the total amount of N-methyl pyrrolidone.
[0021] N-methylpyrrolidone, pyridine, triethylamine and p-phenylenediamine are purified in advance, and the base film resin and lithium chloride are dried.
[0022] The purity of the NMP (normal pressure boiling point 203°C) should reach above 99.9wt%, and the water content should be less than 100mg / kg, preferably less than 50mg / kg; the recovered crude NMP with a purity of 99%, conventional NMP commercial materials, and high-purity NMP should be dehydrated and refined separately or separately after long-term storage. The refining method of the NMP solvent is: under the condition of nitrogen protection, the NMP solvent is subjected to reduced pressure distillation at a temperature of 85-90°C, and 10-20wt% of the feed weight is distilled out at a slight boiling in 1-2h, the residual liquid is cooled to room temperature, 4A molecular sieve accounting for 5-10% of the weight of the residual liquid is added, and it is placed in a sealed manner for 10-30h before use, and solid-liquid separation is performed before use.
[0023] The pyridine (normal pressure boiling point 115°C) and triethylamine (normal pressure boiling point 89°C) are also refined. Pyridine can be refined by first distilling at normal pressure and then adding 4A molecular sieve; specifically, under the condition of nitrogen protection, pyridine is distilled at normal pressure, and 10-20wt% of the feed weight is distilled out in 1-2 hours with a slight boiling, and the residual liquid is cooled to room temperature, and 4A molecular sieve accounting for 10-20% of the weight of the residual liquid is added, and it is placed in a sealed manner for 10-30 hours before use, and solid-liquid separation is performed before use. When refining triethylamine, 4A molecular sieve accounting for 20-30% of the weight of triethylamine material is directly added without distillation, and it is placed in a sealed manner for 10-30 hours before use, and solid-liquid separation is performed before use.
[0024] The p-phenylenediamine (melting point 140°C, boiling point 267°C at normal pressure) is also subjected to dehydration and refining treatment, and the specific method is: under the conditions of nitrogen protection and bubbling purging, the p-phenylenediamine is subjected to reduced pressure distillation at a temperature of 180-200°C, and 10-20wt% of the feed weight is distilled out at a slight boiling in 1-2 hours, and the remaining bottom liquid is transferred to a container protected by nitrogen, and after cooling to room temperature, it is sealed and stored for use; preferably, 3-5 times the weight of NMP solvent is added to prepare an NMP solution of p-phenylenediamine, which is sealed and stored for use.
[0025] The base film resin and lithium chloride are dehydrated and dried before use. The specific method is: the base film resin and lithium chloride are dried at a temperature of 135-150° C. and a vacuum condition of -0.08 to -0.095 MPa for 5-10 hours respectively.
[0026] The cosolvent is n-propanol, isopropanol, ethylene glycol, glycerol or ethylene glycol methyl ether. The water content of the cosolvent should be less than 250 mg / kg, and 4A molecular sieve can be used for dehydration if necessary.
[0027] In the refining process of NMP solvent, pyridine, triethylamine and the dehydration process of cosolvent, it is more preferred to use a more efficient 4A molecular sieve fixed bed continuous treatment method. The 4A molecular sieve should be activated before use, and the activation method is: the charging tray containing the 4A molecular sieve is placed in a muffle furnace, warmed to 350-400 ° C, and moved into a closed material box or dryer after a constant temperature of 4-8h, and used after cooling. The 4A molecular sieve after refining or dehydration can be air-dried or placed in an oven, pre-baked at 80-120 ° C for 3-10h, most of the liquid components are removed, and then activated in a muffle furnace. During the solid-liquid separation, the supernatant can be directly poured out, preferably filtered under nitrogen protection conditions.
[0028] The base film resin is bisphenol A type polysulfone, polyethersulfone or polyarylsulfone, and the molecular weight of the base film resin is preferably 50,000-80,000.
[0029] The non-woven fabric layer has a thickness of 80-120 μm and is made of polyester, polypropylene or polyacrylonitrile.
[0030] The method for preparing the reverse osmosis composite membrane of the present invention comprises the following steps:
[0031] (1) Preparation of casting solution:
[0032] Subtract the amount of N-methylpyrrolidone consumed in preparing the N-methylpyrrolidone solution of poly(p-phenylene terephthalamide) and the N-methylpyrrolidone solution of the resol phenolic resin from the total amount of N-methylpyrrolidone, and place the remaining N-methylpyrrolidone as a solvent in a reactor under nitrogen protection and anhydrous conditions, add a cosolvent and a base film resin, continue stirring, raise the temperature and control it at 50-60° C., after the base film resin is completely dissolved, add the N-methylpyrrolidone solution of poly(p-phenylene terephthalamide) and the N-methylpyrrolidone solution of the resol phenolic resin, control the temperature at 50-60° C., add triethylamine after 5-10 minutes, cool the feed liquid to 20-30° C. within 10 minutes after 20-30 minutes, stop stirring, degas under reduced pressure for 10-30 minutes, and then place it in a sealed container for more than 10 hours to obtain a casting liquid;
[0033] The casting solution does not generate suspended matter during preparation, and the suspended matter introduced by the raw materials can be removed by high-speed centrifugal sedimentation. The co-solvent also has the function of adjusting the pore size and water flux of the modified base membrane layer;
[0034] (2) Preparation of ultrafiltration membrane composed of modified base membrane layer and non-woven fabric layer:
[0035] Under air conditions of 20-30°C and 30-40% relative humidity, coating the non-woven fabric with a casting liquid on one side, with a coating thickness of 60-120 μm; immersing the non-woven fabric in a coagulation bath with a temperature of 15-20°C and containing 20-30wt% N-methylpyrrolidone for a residence time of 1-10 minutes; then immersing the non-woven fabric in water with a temperature of 20-30°C and a residence time of 3-10 minutes; then immersing the non-woven fabric in an aqueous solution with a temperature of 50-60°C and containing 3-5g / L HCl for 10-30 hours, and then washing the non-woven fabric with water to a pH value of more than 6 to obtain an ultrafiltration membrane composed of a modified base membrane layer and a non-woven fabric layer;
[0036] (3) Forming a polyamide separation layer on the surface of the modified base membrane layer of the ultrafiltration membrane:
[0037] In step (2), the surface of the modified base membrane layer of the ultrafiltration membrane is first coated with an aqueous solution containing polyamine monomers, and then coated with an oily solution containing acyl chloride monomers. After heat treatment, a polyamide separation layer is generated to obtain a reverse osmosis composite membrane.
[0038] in:
[0039] In step (3), the aqueous phase solution containing polyamine monomers is an aqueous solution containing 3-5wt% of m-phenylenediamine, 2-4wt% of camphorsulfonic acid, and 1.5-3wt% of triethylamine, and the oil phase solution containing acyl chloride monomers is a solution of n-hexane, cyclohexane, n-heptane, ethylcyclohexane or a mixture thereof containing 0.1-0.2wt% of trimesoyl chloride.
[0040] Furthermore, the operation process of step (3) is as follows:
[0041] Under air or nitrogen conditions at a temperature of 20-30°C and a relative humidity of 30-40%, an aqueous solution containing polyamine monomers at a temperature of 20-30°C is coated on the surface of the modified base membrane layer of the ultrafiltration membrane in step (2) and maintained for 1-2 minutes; excess aqueous solution on the surface is removed, and then an oil solution containing acyl chloride monomers at a temperature of 20-30°C is coated and maintained for 1-3 minutes; excess oil solution on the surface is removed, and heat treatment is performed under air conditions at a temperature of 75-90°C for 2-10 minutes to obtain a reverse osmosis composite membrane.
[0042] The application of the reverse osmosis composite membrane of the present invention is as follows:
[0043] The reverse osmosis composite membrane is used in processes such as seawater desalination and high-salt brackish water desalination that require higher reverse osmosis operating pressure.
[0044] Compared with the prior art, the present invention has the following beneficial effects:
[0045] 1. The modified base membrane layer of the present invention has high compressive strength, creep resistance and hydrophilicity, so that the reverse osmosis composite membrane can be used at an operating pressure of 5-7 MPa for a long time and maintain relatively stable performance.
[0046] 2. In the application of seawater desalination, the reverse osmosis composite membrane of the present invention can achieve the following technical indicators: service life 3-5 years, water recovery rate 35-50%, initial water flux, i.e. water production> 40L / m 2 ·h, initial desalination rate>99.5%, annual average desalination rate attenuation<1%, annual average water flux attenuation<3%; the annual average desalination rate attenuation and water flux attenuation are better than the existing technology, and have good application prospects.
[0047] According to the effects of the embodiments and comparative examples, the main principles of the present invention include the following aspects:
[0048] A. The poly(p-phenylene terephthalamide) (hereinafter referred to as polymer A) prepared by the present invention is a straight chain with high rigidity and monodispersity, and its molecular length is 30-50nm; since terephthaloyl chloride is excessive by 3-7% during preparation, both ends of its molecular straight chain are acyl chloride groups; the prepared ethyl-resin is a linear oligomer with high monodispersity, and its molecular chain length is about 10nm. During the preparation of the casting solution, poly(p-phenylene terephthalamide) is added in the form of an NMP solution of poly(p-phenylene terephthalamide), and phenolic resin is added in the form of an NMP solution of phenolic resin. Within 20-30 minutes after the addition of triethylamine, the acyl chloride groups at both ends of the straight chain of the polymer A molecule react with the phenolic hydroxyl groups in the phenolic resin molecules, and a linear phenolic resin oligomer molecule with a length of about 10 nm is grafted on both ends of the straight chain of the poly(p-phenylene terephthalamide) molecule through the generated ester group to generate polymer B. The introduced poly(p-phenylene terephthalamide) is converted to generate polymer B. At the same time, a small amount of residual terephthaloyl chloride introduced by the NMP solution of poly(p-phenylene terephthalamide) also reacts with the phenolic hydroxyl groups. HCl released by these two reactions is combined and removed by triethylamine.
[0049] B. In step (2) of the method for preparing a reverse osmosis composite membrane of the present invention, after the non-woven fabric is coated with the casting liquid on one side, it is immersed in the coagulation bath at a temperature of 15-20° C. and containing 20-30wt% NMP for 1-10 minutes, polymer B and the remaining phenolic resin molecules will basically solidify into a film with the base film resin (bisphenol A type polysulfone, polyethersulfone or polyarylsulfone); immersed in water at a temperature of 20-30° C. for 3-10 minutes, polymer B and the remaining phenolic resin molecules will completely solidify into a film with the base film resin; during the process of soaking in an aqueous solution at a temperature of 50-60° C. and containing 3-5g / L HCl for 10-30 hours, the phenolic resin molecular segments in polymer B and the remaining phenolic resin molecules will undergo mutual indirect grafting and polymerization reactions under the action of the acidic conditions of the aqueous solution, and the phenolic resin will be converted into the C-type phenolic resin, further forming a three-dimensional phenolic resin structure.
[0050] C. In the modified base membrane layer obtained by the present invention, polymer B has a high rigidity due to the poly(p-phenylene terephthalamide) straight chain segment in its molecule, which plays a major reinforcing role on the base membrane resin. The phenolic resin segment structure at both ends of the molecule also contributes to the reinforcing effect of polymer B to a certain extent, because the uniform distribution of polymer B in the base membrane layer is improved; the added ethyl-resin has an auxiliary reinforcing effect after forming a bulk phenolic resin structure; the combined effect of polymer B and the bulk phenolic resin finally formed significantly improves the compressive strength and creep resistance of the modified base membrane layer under long-term pressure conditions, so that the irreversible compression of the base membrane layer in the thickness direction and the uneven compression degree in each microscopic region in the plane direction are significantly lighter and slower, thereby reducing and delaying the adverse deformation of the polyamide separation skin layer and the microscopic bonding layer between it and the surface layer of the modified base membrane in the thickness direction and the plane direction, and finally reducing the annual average attenuation of the desalination rate of the reverse osmosis composite membrane and the annual average attenuation rate of the water flux.
[0051] D. In step (3), the surface of the modified base membrane layer of the ultrafiltration membrane serves as the basis for the growth of the polyamide separation cortex. The structure and properties of the surface layer have a significant impact on the generation and performance of the polyamide separation cortex, while ensuring a high water flux level. The desalination performance is significantly improved; the reason is that the molecular structure of polymer B and the final phenolic resin contains more phenolic hydroxyl groups, which improves the hydrophilicity of the base membrane layer, thereby improving the bonding strength between the polyamide cortex with high hydrophilicity and the surface of the base membrane layer, and to a certain extent improves the performance stability of the bonding layer between the polyamide cortex and the surface of the base membrane layer, thereby making the salt retention performance of the reverse osmosis composite membrane more stable, and also plays a significant role in reducing the annual average decay rate of the desalination rate of the reverse osmosis composite membrane.
[0052] E. NMP solution of poly(p-phenylene terephthalamide), wherein the method of using 3-7% excess of terephthaloyl chloride and changing the ratio of reactants in its preparation process controls the molecular weight or polymerization degree of polymer A, and the characteristic is that when other conditions remain unchanged, the molecular weight of polymer A is lower when terephthaloyl chloride is excessively high, and the molecular weight of polymer A is higher when the excess is less, and the repeatability is good, indicating that the method has operability. Two-step reaction occurs in the preparation process, the first step is the block polymerization reaction between p-phenylenediamine and terephthaloyl chloride, generating a block molecule straight chain with mainly acyl chloride groups at both ends, and the reaction basically occurs in the early stage of the preparation process; the second step is the block molecule straight chain with acyl chloride groups at both ends (the product of the first step reaction), and then further connected by the reaction of terminal acyl chloride groups with p-phenylenediamine, generating polymer A, and the reaction mainly occurs in the middle and late stages of the preparation process; after the p-phenylenediamine is consumed, the polymerization reaction automatically terminates, and the two ends of the polymer A molecule straight chain in the obtained solution are basically acyl chloride groups, i.e., acyl chloride end-capping. DETAILED DESCRIPTION
[0053] The present invention is specifically described and illustrated below in conjunction with embodiments.
[0054] Example 1
[0055] The reverse osmosis composite membrane of this embodiment is a roll-type membrane which comprises a separation skin layer, a modified base membrane layer, and a non-woven fabric layer from top to bottom; the modified base membrane layer is prepared by compounding a casting liquid on a single side of the non-woven fabric by a phase inversion method;
[0056] The casting solution comprises the following components in parts by weight:
[0057] 250 g of base film resin, bisphenol A type polysulfone (Solvay P-3500) with a molecular weight of 80,000;
[0058] 12.5 g of poly(p-phenylene terephthalamide) with a molecular weight of 5060 was added in the form of a NMP solution of poly(p-phenylene terephthalamide);
[0059] 25 g of resol phenolic resin with a molecular weight of 1270 was added in the form of NMP solution of resol phenolic resin;
[0060] Triethylamine 6g;
[0061] Co-solvent isopropanol 120g;
[0062] The total amount of NMP is 1500g.
[0063] The NMP solution of poly(p-phenylene terephthalamide) (polymer A) was prepared by the following method, and 118.1 g (containing 12.5 g of poly(p-phenylene terephthalamide) and 98.3 g of NMP) was weighed and set aside:
[0064] In a glass reaction flask (pre-weighed) under nitrogen protection and anhydrous conditions, 325 g of NMP, 8.0 g of lithium chloride, and 100.0 g of NMP solution containing 20.00 g of p-phenylenediamine were added, and the mixture was stirred for 12 minutes to prepare a mixed solution; the reactor was placed in a cold bath at -10°C, 12.0 g of pyridine was added to the mixed solution, and stirring was continued. 40.24 g of terephthaloyl chloride (200 mesh powder, purity 99.9%) was added and the timing was started. After 21 minutes, the solid matter was completely dissolved, and the reaction was carried out for 1.5 hours to obtain 478.2 g of NMP solution containing poly(p-phenylene terephthalamide) (obtained from the total weight of the flask and the solution, minus the weight of the flask), and the molecular weight of polymer A in the solution was measured by sampling, which was 5060; it was calculated that the solution contained approximately 50.6 g of polymer A and 398 g of NMP solvent; in the ingredients, the molar ratio of p-phenylene diamine to terephthaloyl chloride was 1:1.07.
[0065] The NMP solution of resol phenolic resin is prepared by the following method. 50 g (containing 25 g of resol phenolic resin and 25 g of NMP solvent) is weighed and set aside:
[0066] In a glass reaction flask (pre-weighed) with cooling reflux and connected to a vacuum system, add 138.5 g of formaldehyde aqueous solution (concentration 39wt%), 189.0 g of phenol (purity 99.6wt%) and 1.44 g of oxalic acid (the molar ratio of formaldehyde aqueous solution, phenol and oxalic acid is 0.9:1:0.008), continue stirring, turn on reflux (reflux cooling water temperature 10°C), heat the liquid to 60°C and stir for 1h, then heat it to 80°C and react at this temperature for 5h, then add 5wt% sodium hydroxide to neutralize to pH 7.5-8, add 100mL of water to wash three times (each time washing, add water and stir for 10min, then stop stirring, let it stand for 20min, and pour off the upper aqueous phase), then connect the flask to the vacuum system and maintain a vacuum of -0.080MPa. The flask was once distilled under vacuum conditions, the temperature was increased to 152°C at a rate of 2°C / min and the temperature was maintained, distilled until there was no distillate, the vacuum was turned off and nitrogen was filled to normal pressure, 30g of NMP was added to the residual liquid, the temperature was controlled at 152°C, stirred and placed for 10min, the flask was connected to the vacuum system again, and the vacuum condition of -0.080MPa was maintained for secondary distillation, the temperature was increased to 152°C at a rate of 2°C / min and the temperature was maintained, distilled until there was no distillate, the vacuum was turned off and nitrogen was filled to normal pressure to obtain a residual liquid containing 187g of resol phenolic resin (the total weight of the flask and the resin, minus the weight of the flask), 187g of NMP was added, the mixture was stirred and cooled to normal temperature to obtain an NMP solution containing 50wt% of resol phenolic resin, and the molecular weight of the resol phenolic resin in the solution was measured by sampling and 1270.
[0067] The reverse osmosis composite membrane 0.5 m was prepared according to the following steps. 2 , wherein step (2) prepares an ultrafiltration membrane 2m 2 :
[0068] (1) Subtracting the amount of NMP solvent consumed in preparing the NMP solution of poly(p-phenylene terephthalamide) and the NMP solution of ethylene-based phenolic resin from the total amount of NMP, and placing the remaining NMP in a reactor under nitrogen protection and anhydrous conditions, adding a co-solvent and a base film resin, stirring continuously, raising the temperature and controlling it at 60° C. After the base film resin is completely dissolved, adding the NMP solution of poly(p-phenylene terephthalamide) and the NMP solution of ethylene-based phenolic resin, controlling the temperature at 60° C., adding triethylamine after 10 minutes, cooling the feed liquid to 30° C. within 10 minutes after 30 minutes, stopping stirring, degassing under reduced pressure and slight boiling for 20 minutes, and then placing it in a sealed container for 10 hours to obtain a casting solution; under strong light conditions, no visible suspended matter is observed in the casting solution by naked eye;
[0069] (2) Under air conditions of 20°C and 35% relative humidity, a non-woven fabric (thickness 80 μm) made of polyacrylonitrile is coated with the casting solution of step (1) on one side with a coating thickness of 120 μm; the non-woven fabric is immersed in a coagulation bath (4 L) at a temperature of 20°C and containing 20 wt% NMP for a residence time of 2 min; the non-woven fabric is then immersed in a sufficient amount of water at a temperature of 30°C for a residence time of 5 min; the non-woven fabric is then immersed in an aqueous solution at a temperature of 55°C and containing 4 g / L HCl for 20 h, and then washed with water to a pH value of 6-6.5, to obtain an ultrafiltration membrane composed of a modified base membrane layer and a non-woven fabric layer;
[0070] (3) Under nitrogen conditions at a temperature of 25°C and a relative humidity of 35%, the surface of the modified base membrane layer of the ultrafiltration membrane in step (2) is purged with a nitrogen stream to remove excess water, firstly coated with an aqueous solution containing 4wt% of m-phenylenediamine, 3wt% of camphorsulfonic acid and 2wt% of triethylamine at a temperature of 25°C and maintained for 1 min, and then purged with a nitrogen stream to remove excess solution, and then coated with an n-heptane solution (oil phase) containing 0.15wt% of trimesoyl chloride at a temperature of 25°C and maintained for 2 min, and then excess solution is removed, and heat-treated under air conditions at a temperature of 80°C for 6 min, cooled to room temperature, washed with water, and a reverse osmosis composite membrane is obtained and stored in a sealed and moisturizing manner.
[0071] Before each of the above preparation operations, the NMP solvent was refined in advance by the following method from the NMP commercial material: the NMP commercial material was subjected to reduced pressure distillation at 85°C under the condition of nitrogen protection, and about 15wt% of the feed weight was distilled out in 1h with a slight boiling, and the remaining liquid was cooled to room temperature, and a 4A molecular sieve accounting for about 10% of the weight of the remaining liquid was added, and it was placed in a closed manner for 20h before use, and the water content was sampled and tested at 28mg / kg, and the upper and middle layers of the liquid were directly poured out before use. Pyridine was refined by the same method, and the water content was sampled and tested at 43mg / kg. The 4A molecular sieve was activated before use, and the activation method was as follows: a loading tray containing a 4A molecular sieve was placed in a muffle furnace, heated to 400°C, and moved into a dryer after a constant temperature of 6h, and used after cooling.
[0072] The triethylamine was refined in advance from commercial materials by the following method: 4A molecular sieve accounting for 30% of the weight of the triethylamine material was directly added, and the mixture was placed in a sealed container for 20 hours before use. The water content was 32 mg / kg after sampling and detection, and the middle and upper layers of the liquid were directly poured out before use. The isopropanol and n-heptane were refined in the same way. The water content of the isopropanol after sampling and detection was 45 mg / kg, and the water content of the n-heptane after the refining treatment was 7 mg / kg.
[0073] The p-phenylenediamine is purified in advance from commercial materials according to the following method: under the conditions of nitrogen protection and nitrogen bubble purging, the p-phenylenediamine material is subjected to reduced pressure distillation at a temperature of 180° C., and about 20wt% of the feed weight is distilled out at a slight boiling point in 1 hour, and the remaining bottom liquid is transferred into a container protected by nitrogen, and is sealed and stored after cooling to room temperature; a certain amount of the purified p-phenylenediamine is weighed, and 4 times the weight of NMP solvent is added to prepare an NMP solution containing 20wt% of p-phenylenediamine, which is sealed and stored and used.
[0074] The base film resin and lithium chloride are also dehydrated and dried before use. The specific method is: the base film resin commercial material and the lithium chloride commercial material are dried for 8 hours at 140°C and -0.095MPa vacuum conditions, filled with nitrogen to normal pressure, transferred into a dryer, and cooled to obtain the base film resin and lithium chloride.
[0075] In the preparation process of the following examples and comparative examples, unless otherwise specified, the same raw materials and equipment conditions as in Example 1 are used, or the reagents after various purification treatments or drying and dehydration treatments in Example 1 are directly used, and re-prepared when the quantity is insufficient.
[0076] Example 2
[0077] The composition and specific preparation process of the reverse osmosis composite membrane and ultrafiltration membrane of this embodiment are basically the same as those in Example 1, except that 10 g of poly(p-phenylene terephthalamide) with a molecular weight of 5060 is used, and the NMP solution of poly(p-phenylene terephthalamide) is added, specifically, 94.5 g (containing 10 g of poly(p-phenylene terephthalamide) and 78.7 g of NMP solvent) is taken from the prepared NMP solution of poly(p-phenylene terephthalamide) (polymer A) for use; the NMP solution of the ethyl-resin prepared in Example 1 is directly used.
[0078] Example 3
[0079] The composition and specific preparation process of the reverse osmosis composite membrane and ultrafiltration membrane of this embodiment are basically the same as those in Example 1, except that 15 g of poly(p-phenylene terephthalamide) with a molecular weight of 7800 is added in the form of an NMP solution of poly(p-phenylene terephthalamide); the NMP solution of the ethyl-resin prepared in Example 1 is directly used; and in step (2) of preparing the reverse osmosis composite membrane, a non-woven fabric with a thickness of 120 μm and made of polyester is used.
[0080] The NMP solution of poly(p-phenylene terephthalamide) (polymer A) is prepared by taking 147.5 g (containing 15 g of poly(p-phenylene terephthalamide) and 123.2 g of NMP solvent) from a solution prepared by the following method:
[0081] In a glass reaction flask (pre-weighed) under nitrogen protection and anhydrous conditions, 325 g of NMP solvent, 8.0 g of lithium chloride, and 100.0 g of NMP solution containing 20.00 g of p-phenylenediamine were added, and the mixture was stirred for 12 minutes to prepare a mixed solution; the reactor was placed in a cold bath at -10°C, 12.0 g of pyridine was added to the mixed solution, and stirring was continued. 38.84 g of terephthaloyl chloride (200 mesh powder, purity 99.9%) was added and the timing was started. After 20 minutes, the solid matter was completely dissolved, and the reaction was carried out for 1.5 hours to obtain 478.9 g of NMP solution containing poly(p-phenylene terephthalamide) (obtained from the total weight of the flask and the solution, minus the weight of the flask), and the molecular weight of polymer A in the solution was measured by sampling, which was 7800; it was calculated that the solution contained approximately 48.7 g of polymer A and 400 g of NMP solvent; in the ingredients, the molar ratio of p-phenylene diamine to terephthaloyl chloride was 1:1.03.
[0082] Example 4
[0083] The reverse osmosis composite membrane and ultrafiltration membrane of the present embodiment, their composition and specific preparation process are basically the same as those in Example 1, except that 12.5 g of poly(p-phenylene terephthalamide) with a molecular weight of 6550 is added in the form of an NMP solution of poly(p-phenylene terephthalamide); and the NMP solution of the resol prepared in Example 1 is directly used.
[0084] The NMP solution of poly(p-phenylene terephthalamide) (polymer A) is prepared by taking 120.8 g (containing 12.5 g of poly(p-phenylene terephthalamide) and 100.8 g of NMP solvent) from a solution prepared by the following method:
[0085] In a glass reaction flask (pre-weighed) under nitrogen protection and anhydrous conditions, 325 g of NMP solvent, 8.0 g of lithium chloride, and 100.0 g of NMP solution containing 20.00 g of p-phenylenediamine were added, and the mixture was stirred for 12 minutes to prepare a mixed solution; the reactor was placed in a cold bath at -7°C, 12.0 g of pyridine was added to the mixed solution, and stirring was continued. 39.54 g of terephthaloyl chloride (200 mesh powder, purity 99.9%) was added and the timing was started. After 20 minutes, the solid matter was completely dissolved, and the reaction was carried out for 1.5 hours to obtain 479.3 g of NMP solution containing poly(p-phenylene terephthalamide) (obtained from the total weight of the flask and the solution, minus the weight of the flask), and the molecular weight of polymer A in the solution was measured by sampling, which was 6550; it was calculated that the solution contained approximately 49.6 g of polymer A and 400 g of NMP solvent; in the ingredients, the molar ratio of p-phenylene diamine to terephthaloyl chloride was 1:1.05.
[0086] Example 5
[0087] The composition and specific preparation process of the reverse osmosis composite membrane and ultrafiltration membrane of this embodiment are basically the same as those of Example 4, except that 200 g of another base membrane resin, polyethersulfone (BASF E6020) with a molecular weight of 50,000, is used; in step (3) of preparing the reverse osmosis composite membrane, an oil phase solution containing 0.20 wt % of trimesoyl chloride is used, and the oil phase solvent is a mixture of 40 wt % cyclohexane and 60 wt % n-heptane; when preparing the casting solution, the NMP solution of the ethyl-resin prepared in Example 1 is directly used.
[0088] Example 6
[0089] The reverse osmosis composite membrane of this embodiment is prepared by using part of the ultrafiltration membrane prepared in step (2) of Example 1, except that in step (3), an aqueous solution containing 5wt% of m-phenylenediamine, 4wt% of camphorsulfonic acid and 3wt% of triethylamine and an n-heptane solution containing 0.20wt% of trimesoyl chloride (oil phase) are used, and the membrane is heat treated for 10 minutes in air at a temperature of 90°C, cooled to room temperature, washed with water, and the reverse osmosis composite membrane is obtained and stored in a sealed and moisturizing manner.
[0090] Comparative Example 1
[0091] The composition and specific preparation process of the reverse osmosis composite membrane and ultrafiltration membrane of this comparative example are basically the same as those in Example 1, except that the NMP solution of poly(p-phenylene terephthalamide) (polymer A) is not added to the casting solution in step (1); the NMP solution of ethyl-resin prepared by the method in Example 1 is directly used.
[0092] Comparative Example 2
[0093] The composition and specific preparation process of the reverse osmosis composite membrane and ultrafiltration membrane of this comparative example are basically the same as those in Example 1, except that the NMP solution of ethyl-resin is not added to the casting solution in step (1); instead, the NMP solution of poly(p-phenylene terephthalamide) (polymer A) prepared by the method in Example 1 is directly used.
[0094] Comparative Example 3
[0095] The composition and specific preparation process of the reverse osmosis composite membrane and ultrafiltration membrane of this comparative example are basically the same as those in Example 1, except that no triethylamine is added to the casting solution in step (1); the NMP solution of poly(p-phenylene terephthalamide) (polymer A) and the NMP solution of ethylene-resin prepared by the method in Example 1 are directly used.
[0096] Comparative Example 4
[0097] The reverse osmosis composite membrane and ultrafiltration membrane of this comparative example were prepared according to the other compositions and processes in Example 1 without using the NMP solution of poly(p-phenylene terephthalamide) (polymer A), the NMP solution of ethyl-resin and triethylamine described in Example 1.
[0098] The reverse osmosis composite membrane of this comparative example is a roll-type membrane which comprises a separation skin layer, a base membrane layer, and a non-woven fabric layer from top to bottom; the base membrane layer is obtained by compounding a casting liquid on a single surface of the non-woven fabric by a phase inversion method;
[0099] The casting solution comprises the following components in parts by weight:
[0100] 250g of base film resin, bisphenol A polysulfone (Solvay P-3500) with a molecular weight of 80,000,
[0101] Solvent isopropanol 120g,
[0102] NMP1500g;
[0103] The reverse osmosis composite membrane 0.5 m was prepared according to the following steps. 2 , wherein step (2) prepares an ultrafiltration membrane 2m 2 :
[0104] (1) placing NMP in a reactor under nitrogen protection and anhydrous conditions, adding a co-solvent and a base film resin, stirring continuously, raising the temperature and controlling it at 60°C, and after the base film resin is completely dissolved, stopping stirring, degassing under reduced pressure and slight boiling for 20 minutes, and then sealing and placing for 10 hours to obtain a casting solution; under strong light conditions, the casting solution is observed by naked eyes to have no visible suspended matter;
[0105] (2) Under air conditions of 15°C (using a slightly lower casting liquid temperature to obtain a suitable viscosity) and 35% relative humidity, a non-woven fabric (thickness 80 μm) made of polyacrylonitrile is coated with the casting liquid of step (1) on one side with a coating thickness of 120 μm; immersed in a coagulation bath containing 20 wt% NMP at a temperature of 20°C for a residence time of 2 min; then immersed in a sufficient amount of water at a temperature of 30°C for a residence time of 5 min; and an ultrafiltration membrane composed of a base membrane layer and a non-woven fabric layer is obtained;
[0106] (3) Under nitrogen conditions at a temperature of 25°C and a relative humidity of 35%, the surface of the modified base membrane layer of the ultrafiltration membrane in step (2) is purged with a nitrogen stream to remove excess water, firstly coated with an aqueous solution containing 4wt% of m-phenylenediamine, 3wt% of camphorsulfonic acid and 2wt% of triethylamine at a temperature of 25°C and maintained for 1 min, and then purged with a nitrogen stream to remove excess solution, and then coated with an n-heptane solution (oil phase) containing 0.15wt% of trimesoyl chloride at a temperature of 25°C and maintained for 2 min, and then excess solution is removed, and heat-treated under air conditions at a temperature of 80°C for 6 min, cooled to room temperature, washed with water, and a reverse osmosis composite membrane is obtained and stored in a sealed and moisturizing manner.
[0107] Comparative Example 5
[0108] The reverse osmosis composite membrane and ultrafiltration membrane of this comparative example have the same composition and specific preparation process as those in Example 1, except that an NMP solution of poly(p-phenylene terephthalamide) with a molecular weight of 13,400 is added to the casting solution; the preparation method of the NMP solution of poly(p-phenylene terephthalamide) used is basically the same as that in Example 1, except that the molar ratio of p-phenylene diamine (20.00 g) to terephthaloyl chloride (37.61 g) is 1:1, and the molecular weight of the poly(p-phenylene terephthalamide) in the obtained solution is 13,400 when sampled; the NMP solution of the ethyl-resin prepared by the method in Example 1 is directly used.
[0109] Comparative Example 6
[0110] The reverse osmosis composite membrane and ultrafiltration membrane of this comparative example have the same composition and specific preparation process as those in Example 1, except that an NMP solution of poly(p-phenylene terephthalamide) with a molecular weight of 23,600 is added to the casting solution, and the amount of poly(p-phenylene terephthalamide) used is 37.5 g (three times the amount used in Example 1); the preparation method of the NMP solution of poly(p-phenylene terephthalamide) used is basically the same as that in Example 1, except that lithium chloride is not used in the ingredients. As a result, the molecular weight of the poly(p-phenylene terephthalamide) measured in the obtained solution is 23,600; the NMP solution of the ethyl-resin prepared by the method in Example 1 is directly used.
[0111] During the operation of the above Examples 1-6 and Comparative Examples 1-6, the 4 L coagulation bath containing 20 wt% NMP used in step (2) of Example 1 was not replaced but used sequentially in the operation of Examples 2-6 and Comparative Examples 1-6; the solution in Comparative Example 6 was still clear after use, and was still clear after sampling and diluting it 1 times with water, indicating that the ethyl-resin in the casting solution did not enter the coagulation bath containing 20 wt% NMP at a temperature of 20°C.
[0112] Example 1 and Comparative Example 6 verify that in the known preparation technology of low molecular weight poly(p-phenylene terephthalamide), the polymer obtained without adding lithium chloride is a parallel bundle-like aggregate of multiple poly(p-phenylene terephthalamide) molecular straight chains, not a single molecular straight chain, and thus has a low enhancement efficiency for the base film layer.
[0113] Comparative Example 7
[0114] The composition and specific preparation process of the reverse osmosis composite membrane and ultrafiltration membrane of this comparative example are basically the same as those in Example 1, except that in step (2), no immersion treatment in an aqueous solution containing 4 g / L HCl at a temperature of 55°C is carried out (polymerization reaction of the phenolic resin is not carried out); and the NMP solution of poly(p-phenylene terephthalamide) (polymer A) and the NMP solution of the phenolic resin prepared by the method in Example 1 are directly used.
[0115] Comparative Example 8
[0116] The ultrafiltration membrane and reverse osmosis composite membrane of this comparative example were prepared using the casting solution prepared according to step (1) in Example 1 and basically according to steps (2) to (3) in Example 1, except that 0.7 L of a coagulation bath solution having an NMP concentration of 60 wt% was used in step (2).
[0117] Take a sample of the coagulation bath solution after use in step (2) and add 5 times the weight of water. A large amount of suspended matter is produced in the dilution solution, indicating that a part of the ethyl-resin has entered the coagulation bath solution, making the compressive strength of the obtained ultrafiltration membrane and reverse osmosis composite membrane lower.
[0118] Test Example 1
[0119] The ultrafiltration membranes prepared in the above embodiments and comparative examples were cut and sampled, stacked into 60 layers, and cut to obtain test blocks of 30x30 mm. Pressures of 1 MPa, 6 MPa, and 9 MPa were applied in a direction perpendicular to the plane of the stacking and maintained for 10 min respectively. The compression rate at 6 MPa and 9 MPa pressures in the thickness direction of the stacking was measured based on the thickness of the stacking after compression at 1 MPa.
[0120] The results show that the 6MPa compression rate and 9MPa compression rate of the ultrafiltration membrane test blocks of Examples 1-6 are lower than 3% and 5%, respectively. The 6MPa compression rate of the ultrafiltration membrane test blocks of Comparative Examples 1-8 are higher than 8%, and the 9MPa compression rate is higher than 14%. The overall order of compression rate from low to high is Comparative Examples 5, 6, 3, 7, 2, 1, 8, 4.
[0121] Test Example 2
[0122] The ultrafiltration membranes prepared in the above examples were cut and sampled, and the water flux of pure water (pure water obtained by reverse osmosis and then distillation) was measured using a cross-flow evaluation device. The effective membrane area was 38.2 cm 2 , water temperature 25℃, pressure difference 0.2MPa, start metering after stabilization for 10min, metering time 60min.
[0123] As a result, the water flux of each pure water is higher than 800L / m 2 ·h.
[0124] Test Example 3
[0125] The reverse osmosis composite membranes prepared in the above embodiments and comparative examples were cut and sampled respectively. The initial water flux and initial desalination rate at a temperature of 25°C were measured in three sets of cross-flow evaluation devices with the same configuration. The first condition was that the inlet concentration of the sodium chloride aqueous solution was 5.3wt%, the outlet concentration was 5.5wt% and the pressure difference was 5.5MPa. The second condition was that the inlet concentration of the sodium chloride aqueous solution was 8.3wt%, the outlet concentration was 8.6wt% and the pressure difference was 8.0MPa. The effective membrane area was 38.2cm 2 , start metering after stabilization for 10 minutes, metering time is 60 minutes; the sodium chloride aqueous solution used is made of pure water (pure water obtained by distillation after reverse osmosis) and recrystallized sodium chloride, and then purified by ultrafiltration device before use. The concentration of sodium chloride aqueous solution is determined by conductivity method, and water is first added to dilute it according to a fixed multiple during the determination.
[0126] The result is that the initial water flux of the reverse osmosis composite membrane of each embodiment is greater than 40L / m 2 ·h, the initial desalination rate is >99.7%; among them, the overall effect of the reverse osmosis composite membrane of Example 4 is the best, and the initial water flux is >42L / m 2 ·h. The initial water flux of the reverse osmosis composite membranes of each comparative example is less than 32L / m 2 ·h; Among them, the overall effect of the reverse osmosis composite membranes of Comparative Examples 2 and 4 is the worst, and the overall effect of the reverse osmosis composite membrane of Comparative Example 5 is the best.
[0127] Test Example 4
[0128] The reverse osmosis composite membranes prepared in the above Example 4 and Comparative Example 5 were re-cut and sampled, and the desalination rate attenuation and water flux attenuation at 25°C were measured in the cross-flow evaluation device used in Test Example 3. The inlet concentration of the sodium chloride aqueous solution was 8.3wt%, the outlet concentration was 8.6wt% and the pressure difference was 8.0MPa under Condition 2; the effective membrane area was 38.2cm 2 , start measuring after stabilization for 10 minutes, and the test time is 300 hours each; the discharged sodium chloride aqueous solution and desalted water are continuously mixed and recycled.
[0129] The result is that the initial water flux of the reverse osmosis composite membrane of Example 4 is 42.6 L / m 2 ·h, the initial desalination rate was 99.78%, and after 300h of continuous operation, the desalination rate decayed by 0.03%, and the water flux decay did not decrease. The initial water flux of the reverse osmosis composite membrane of Comparative Example 5 was 31.5L / m 2 ·h, the initial desalination rate was 99.62%. After 300h of continuous operation, the desalination rate decayed by 0.16%, and the water flux decayed by 0.13%.
[0130] According to the effects of the above embodiments, comparative examples and test examples, combined with the relevant known technologies in the art, the main principles and features of the present invention include:
[0131] 1. During the preparation of the casting solution in step (1), poly(p-phenylene terephthalamide) and phenolic resin undergo a grafting reaction between the terminal acyl chloride group and the phenolic hydroxyl group under the catalytic action of triethylamine. In step (2), after the non-woven fabric is coated with the casting liquid on one side, the polymer component is completely solidified into a film during the phase conversion process; during the process of soaking in an aqueous solution containing 3-5 g / L HCl at a temperature of 50-60° C. for 10-30 hours, the molecular chain segments of the ethyl-resin and the remaining ethyl-resin molecules undergo a mutual grafting and polymerization reaction, where the ethyl-resin is converted into the propyl-resin, and further form a bulk phenolic resin structure; in the obtained modified base membrane layer, the conversion product of poly(p-phenylene terephthalamide) (polymer B) plays a major reinforcing role, and the bulk phenolic resin structure formed by the ethyl-resin has an auxiliary reinforcing effect, thereby significantly improving the compressive strength and creep resistance of the modified base membrane layer under long-term pressure conditions, and ultimately reducing the annual average attenuation rate of the desalination rate and the annual average attenuation rate of the water flux of the reverse osmosis composite membrane.
[0132] 2. In step (3), the surface of the modified base membrane layer of the ultrafiltration membrane serves as the basis for the growth of the polyamide cortex, and the structure and properties of the surface layer have a significant impact on the generation and performance of the polyamide cortex, thereby significantly improving the desalination performance while ensuring a high water flux level; the reason is that the molecular structure of polymer B and the final phenolic resin contains more phenolic hydroxyl groups, which improves the hydrophilicity of the base membrane layer, thereby improving the bonding strength between the polyamide cortex with high hydrophilicity and the surface of the base membrane layer, and to a certain extent improves the performance stability of the bonding layer between the polyamide cortex and the surface of the base membrane layer, thereby making the salt retention performance of the reverse osmosis composite membrane more stable, and also plays a significant role in reducing the annual average decay rate of the desalination rate of the reverse osmosis composite membrane.
[0133] 3. The NMP solution of poly(p-phenylene terephthalamide) (polymer A) is prepared by using a method in which terephthaloyl chloride is excessively added by 3-7% and the ratio of reactants is changed to control the molecular weight or degree of polymerization of polymer A. The method has good repeatability, operability and usability.
[0134] Industrial Application Example 1
[0135] The reverse osmosis composite membrane of Example 4 was scaled up and made into a membrane with an effective membrane area of 61m 2 The reverse osmosis module was tested in a seawater desalination project and was specially equipped with a pressurized water pump and a control system for flow, pressure, etc.
[0136] The reverse osmosis module uses normal temperature seawater after pre-purification and ultrafiltration. The initial water flux is 43.7L / m at a water recovery rate of 50% and a pressure difference of 5.52MPa. 2 h, with an initial desalination rate of 99.75%; during the subsequent three and a half years of long-term operation, the flow rate, pressure, etc. were controlled according to conventional reverse osmosis operation methods, and routine cleaning was carried out when necessary.
[0137] During the three and a half years of application tests, under the conditions of normal temperature and water recovery rate of 35-50%, a pressure difference of 5-7MPa can be used for a long time, with an average annual attenuation of desalination rate of 0.7% and an average annual attenuation of water flux of 1.6%, maintaining relatively stable performance.
[0138] Based on the results of the above test examples and industrial application examples, combined with the accumulated experience in this field, the modified base membrane layer in the reverse osmosis composite membrane of the present invention has high compressive strength, creep resistance and hydrophilicity, so that the reverse osmosis composite membrane can be used for a long time at an operating pressure of 5-7MPa while maintaining relatively stable performance; in the application of seawater desalination, the following technical indicators can be achieved: service life of 3-5 years, water recovery rate of 35-50%, initial water flux> 40L / m 2 ·h, initial desalination rate>99.7%, annual average desalination rate attenuation<1%, annual average water flux attenuation<3%; the annual average desalination rate attenuation and water flux attenuation are better than the existing technology, and have good application prospects.
[0139] In the present invention, the molecular weights of the resin and polymer are both viscosity average molecular weights; and the solvent of the coagulation bath is water.
Claims
1. A reverse osmosis composite membrane is a roll-type membrane which comprises, from top to bottom, a separation skin layer, a modified base membrane layer, and a non-woven fabric layer, wherein the modified base membrane layer is prepared by compounding a casting liquid on a single surface of a non-woven fabric by a phase inversion method, and is characterized in that: The casting solution comprises the following components in parts by weight: 20-25 parts of base film resin with molecular weight of 30000-150000; 1-1.5 parts of poly(p-phenylene terephthalamide) with a molecular weight of 5000-8000, added in the form of a solution of poly(p-phenylene terephthalamide) in N-methylpyrrolidone; 1.5-2.5 parts of resol phenolic resin with a molecular weight of 1000-1500, added in the form of a solution of the resol phenolic resin in N-methylpyrrolidone; 0.4-0.6 parts of triethylamine; 10-15 parts of cosolvent; The total amount of N-methylpyrrolidone is 120-150 parts, including the amount of N-methylpyrrolidone used to prepare the N-methylpyrrolidone solution of poly(p-phenylene terephthalamide), the amount of N-methylpyrrolidone used to prepare the N-methylpyrrolidone solution of the resol phenolic resin, and the amount of N-methylpyrrolidone used to prepare the casting solution; The N-methylpyrrolidone solution of poly(p-phenylene terephthalamide) was prepared by the following method: In a reactor under nitrogen protection and anhydrous conditions, N-methylpyrrolidone, lithium chloride and N-methylpyrrolidone solution of p-phenylenediamine are prepared into a mixed solution; the reactor is placed in a cold bath at -10 to -5°C, pyridine is added to the mixed solution, stirring is continued, terephthaloyl chloride is added, and the reaction is carried out for 1-2 hours to obtain an N-methylpyrrolidone solution of poly(p-phenylene terephthalamide); wherein the weight ratio of N-methylpyrrolidone, lithium chloride, p-phenylene diamine, pyridine and terephthaloyl chloride is (15-25):(0.3-0.5):1:(0.5-0.7):(1.94-2.01); the amount of N-methylpyrrolidone accounts for 21-22wt% of the total amount of N-methylpyrrolidone, and the amount of N-methylpyrrolidone in the N-methylpyrrolidone solution of p-phenylene diamine accounts for 5-6wt% of the total amount of N-methylpyrrolidone.
2. The reverse osmosis composite membrane according to claim 1, characterized in that: The N-methylpyrrolidone solution of resol phenolic resin was prepared by the following method: In a stirred reactor with cooling reflux and connected to a vacuum system, add a 37-40wt% formaldehyde aqueous solution, add phenol and oxalic acid, continue stirring, open reflux, reflux cooling water temperature 10-15°C, heat the feed liquid to 60-65°C and stir for 0.5-1h, then heat it to 75-80°C and react at this temperature for 5-8h, add sodium hydroxide to neutralize to pH 7.5-8, wash with water, then perform reduced pressure distillation under a vacuum condition of -0.078 to -0.083MPa, heat it to 148-152°C at a rate of 1-2°C / min until there is no distillate, close the vacuum and fill it with nitrogen to normal pressure, add N -methyl pyrrolidone, control the temperature at 148-152°C and stir for 5-10 minutes, then open the vacuum system for reduced pressure distillation at a pressure of -0.078 to -0.083 MPa, and distill until there is no distillate under the vacuum condition and the temperature of 148-152°C, and finally add N-methyl pyrrolidone to obtain a 20-50wt% N-methyl pyrrolidone solution of ethyl-resin, wherein the molar ratio of formaldehyde, phenol and oxalic acid is (0.8-1.0):1:(0.006-0.01), and the amount of N-methyl pyrrolidone added twice accounts for 12-15wt% of the total amount of N-methyl pyrrolidone.
3. The reverse osmosis composite membrane according to claim 1, characterized in that: N-methylpyrrolidone, pyridine, triethylamine and p-phenylenediamine are purified in advance, and the base film resin and lithium chloride are dried.
4. The reverse osmosis composite membrane according to claim 1, characterized in that: The base film resin is bisphenol A type polysulfone, polyethersulfone or polyarylsulfone, and the molecular weight of the base film resin is 50000-80000.
5. The reverse osmosis composite membrane according to claim 1, characterized in that: The thickness of the non-woven fabric layer is 80-120 μm, and the material is polyester, polypropylene or polyacrylonitrile; the co-solvent is n-propanol, isopropanol, ethylene glycol, glycerol or ethylene glycol methyl ether.
6. A method for preparing a reverse osmosis composite membrane according to any one of claims 1 to 5, characterized in that: The steps include: (1) Subtracting the amount of N-methylpyrrolidone consumed in preparing the N-methylpyrrolidone solution of poly(p-phenylene terephthalamide) and the N-methylpyrrolidone solution of ethylene-based phenolic resin from the total amount of N-methylpyrrolidone, and placing the remaining N-methylpyrrolidone as a solvent in a reactor under nitrogen protection and anhydrous conditions, adding a co-solvent and a base film resin, stirring continuously, raising the temperature and controlling it at 50-60° C., after the base film resin is completely dissolved, adding the N-methylpyrrolidone solution of poly(p-phenylene terephthalamide) and the N-methylpyrrolidone solution of ethylene-based phenolic resin, controlling the temperature at 50-60° C., adding triethylamine after 5-10 minutes, cooling the feed liquid to 20-30° C. within 10 minutes after 20-30 minutes, stopping stirring, degassing under reduced pressure for 10-30 minutes, and then sealing and placing for more than 10 hours to obtain a casting liquid; (2) Under air conditions of 20-30°C and relative humidity of 30-40%, coating the non-woven fabric with a casting liquid on one side to a coating thickness of 60-120 μm; immersing the non-woven fabric in a coagulation bath having a temperature of 15-20°C and containing 20-30 wt% of N-methylpyrrolidone for a residence time of 1-10 min; then immersing the non-woven fabric in water having a temperature of 20-30°C and a residence time of 3-10 min; then immersing the non-woven fabric in an aqueous solution having a temperature of 50-60°C and containing 3-5 g / L of HCl for 10-30 h, and then washing the non-woven fabric with water to a pH value of more than 6 to obtain an ultrafiltration membrane composed of a modified base membrane layer and a non-woven fabric layer; (3) The surface of the modified base membrane layer of the ultrafiltration membrane in step (2) is first coated with an aqueous solution containing polyamine monomers, and then coated with an oily solution containing acyl chloride monomers, and a polyamide separation layer is generated after heat treatment to obtain a reverse osmosis composite membrane.
7. The method for preparing a reverse osmosis composite membrane according to claim 6, characterized in that: In step (3), the aqueous phase solution containing the polyamine monomer is an aqueous solution containing 3-5wt% of m-phenylenediamine, 2-4wt% of camphorsulfonic acid, and 1.5-3wt% of triethylamine; the oil phase solution containing the acyl chloride monomer is a solution of n-hexane, cyclohexane, n-heptane, ethylcyclohexane or a mixture thereof containing 0.1-0.2wt% of trimesoyl chloride.
8. The method for preparing a reverse osmosis composite membrane according to claim 6, characterized in that: The operation process of step (3) is: Under air or nitrogen conditions at a temperature of 20-30°C and a relative humidity of 30-40%, an aqueous solution containing polyamine monomers at a temperature of 20-30°C is coated on the surface of the modified base membrane layer of the ultrafiltration membrane in step (2) and maintained for 1-2 minutes; excess aqueous solution on the surface is removed, and then an oil solution containing acyl chloride monomers at a temperature of 20-30°C is coated and maintained for 1-3 minutes; excess oil solution on the surface is removed, and heat treatment is performed under air conditions at a temperature of 75-90°C for 2-10 minutes to obtain a reverse osmosis composite membrane.
9. An application of the reverse osmosis composite membrane according to any one of claims 1 to 5, characterized in that: The reverse osmosis composite membrane is used in seawater desalination and brackish water desalination.
Citation Information
Patent Citations
High-interception seawater desalination composite reverse osmosis membrane and preparation method and application
CN112354374A
Pressure-resistant polysulfone-based membrane and preparation method thereof
CN114130216A
Phenolic resin containing vinyl ether side chain
CN108084380A
Membrane casting solution, ultrafiltration membrane and preparation method of ultrafiltration membrane
CN109012236A
Composite reverse osmosis membrane and preparation method thereof
CN112619443A