A limestone powder cement-based binder

By sieving limestone powder by particle size and optimizing its proportion, limestone powder cementitious materials were prepared, which solved the problem of underutilization of limestone powder, improved the compressive strength of concrete and reduced carbon emissions.

CN118439824BActive Publication Date: 2026-11-10CHINA RAILWAY SHANGHAI ENGINEERING GROUP NO 5 ENGINEERING CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410533608.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-30
Publication Date
2026-11-10
Estimated Expiration
2044-04-30

AI Technical Summary

Technical Problem

In existing technologies, the amount of limestone powder added to concrete is low and not fully utilized, leading to resource waste and environmental pollution. At the same time, cement production results in high carbon emissions.

Method used

Limestone powder cementitious materials were prepared by sieving limestone powder by particle size and optimizing the particle size distribution. The dosage ratio of limestone powder with different particle sizes was calculated using the modified Anderson model. With a water-cement ratio of 0.35-0.45, a high-efficiency limestone powder cementitious material was prepared.

Benefits of technology

It improves the utilization rate of limestone powder in concrete, enhances the later compressive strength of cementitious materials, reduces carbon emissions from cement production, and achieves both environmental protection and performance improvement.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118439824B_ABST
    Figure CN118439824B_ABST
Patent Text Reader

Abstract

This invention discloses a limestone powder cement-based cementitious material, relating to the field of building materials technology. The cementitious material comprises cementitious raw materials and water; the water-cement ratio of the cementitious material is 0.35-0.45; by weight percentage, the cementitious raw materials comprise (70-80):(20-30) cement and limestone powder; the limestone powder comprises coarse-grained limestone powder and fine-grained limestone powder with different particle size contents and a distribution modulus of 0.1-1. The resulting cementitious material exhibits significantly improved later-stage compressive strength, allowing the limestone powder to play a better role, enhancing the later-stage compressive strength of the cementitious material while further improving the utilization rate of the limestone powder.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of building materials technology, and more specifically, to a limestone powder cementitious material. Background Technology

[0002] Concrete, due to its abundant and inexpensive raw materials and simple production process, has become the world's most widely used building material. However, concrete is also a major source of CO2 emissions. Cement is the main binder in concrete, and its production process consumes large amounts of coal, limestone, clay, and other materials while emitting significant amounts of CO2. The most significant carbon emission from cement production comes from the CO2 produced by the decomposition of CaCO3. Producing 1 ton of cement clinker generates approximately 0.8 tons of CO2 and requires about 110 kg of coal, making the cement industry's carbon emissions relatively high. Therefore, reducing CO2 emissions from the cement industry and achieving green and sustainable development in the cement sector has attracted the attention of scholars both domestically and internationally.

[0003] Limestone powder is considered a good mineral admixture for use in the concrete industry. Due to its low cost and good grindability, the application of limestone powder in concrete has been extensively studied. However, in reality, the dosage of limestone powder is relatively low, and there are still large-scale stockpiling issues that occupy land and cause environmental pollution. In other words, this mineral resource is not being fully utilized, resulting in resource waste.

[0004] In view of this, the present invention is proposed. Summary of the Invention

[0005] The purpose of this invention is to provide a limestone powder cementitious material to solve the above-mentioned technical problems.

[0006] This invention is implemented as follows:

[0007] In a first aspect, the present invention provides a limestone powder cementitious material, which includes cementitious raw materials and water; the water-cement ratio of the cementitious material is 0.35-0.45;

[0008] By weight percentage, the cementitious materials consist of (70-80): (20-30) cement and limestone powder;

[0009] Limestone powder includes: fine-particle limestone powder with a particle size <30μm and coarse-particle limestone powder with a particle size of 30-90μm;

[0010] The particle size of the coarse-grained limestone powder includes at least one of the following: 30-54μm, 54-63μm, 63-80μm, and 80-90μm.

[0011] The distribution modulus of coarse-grained limestone powder and fine-grained limestone powder is 0.1-1.

[0012] The present invention has the following beneficial effects:

[0013] The limestone powder cement-based cementitious material provided by this invention involves mixing limestone powder with cement at different distribution moduli and particle sizes as admixtures to prepare the cementitious material. The resulting cementitious material exhibits significantly improved later-stage compressive strength, allowing the limestone powder to play a better role. This not only enhances the later-stage compressive strength of the cementitious material but also further improves the utilization rate of the limestone powder, making a significant contribution to environmental protection. Attached Figure Description

[0014] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. It should be understood that the following drawings only show some embodiments of the present invention and should not be regarded as a limitation on the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.

[0015] Figure 1 This is a schematic diagram of the particle size optimization device for cementitious materials in this invention;

[0016] Figure 2 This is a schematic diagram of the screening unit in the cementitious material particle size optimization device of the present invention from a certain perspective;

[0017] Figure 3 The diagram shows the compressive strength of limestone powder cementitious materials prepared with LS20 under different distribution moduli at different times, as provided in Examples 1-10 and Comparative Example 1 of the present invention.

[0018] Figure 4 The diagram shows the compressive strength of limestone powder cementitious materials prepared by LS30 under different distribution moduli at different times according to Examples 11-20 and Comparative Example 2 of the present invention.

[0019] Figure 5 This is the particle size distribution curve of the limestone powder raw material in this invention.

[0020] Icons: 1-Base; 101-Elastic component; 2-Chassis; 201-Discharge device; 202-Vibration device; 3-Screening unit; 301-Screen; 302-Protrusion; 303-Negative pressure device; 304-Collection device; 305-Snap fastener; 306-Baffle; 4-Screen cover; 401-Inlet. Detailed Implementation

[0021] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased commercially.

[0022] Limestone powder is a fine powder of limestone with particles smaller than 0.16 mm after mechanical processing. Its chemical composition is mainly CaCO3. Limestone mines are abundant in many provinces and cities in my country, with a wide distribution range, and it can be obtained through simple production at a low cost. Limestone powder is considered an excellent mineral admixture used in the concrete industry. The addition of limestone powder can improve the fluidity, strength, and durability of concrete. Limestone powder has nucleation, filling, dilution, and chemical effects in concrete. The application of limestone powder in concrete mainly takes three forms: first, limestone powder replaces part of the fine aggregate; second, limestone powder is added externally; and third, limestone powder replaces part of the cement, either as a single or combined admixture.

[0023] Currently, the dosage of limestone powder in concrete is relatively low, generally between 5% and 20%. Excessive dosage can negatively impact the strength and durability of the concrete. The particle size of commercially available limestone powder is determined during production; industrial production rarely involves sieving the particle size or optimizing the content ratio of limestone powder with different particle sizes.

[0024] It is worth mentioning that excessively large limestone powder particles can affect the fluidity of concrete, while excessively small particles can affect its strength and durability. Therefore, there is an urgent need to find a method that can sieve limestone powder by particle size and optimize the dosage ratio of limestone powder of different particle sizes, so that the prepared cementitious material can play a better role, further increasing the amount of limestone powder while enhancing the compressive strength of the cementitious material.

[0025] In a first aspect, the present invention provides a limestone powder cementitious material, comprising cementitious raw materials and water; the water-cement ratio of the cementitious material is 0.35-0.45. By weight percentage, the cementitious raw materials comprise (70-80): (20-30) cement and limestone powder; the limestone powder comprises: fine-grained limestone powder with a particle size <30μm and coarse-grained limestone powder with a particle size of 30-90μm; wherein the particle size of the coarse-grained limestone powder includes at least one of: 30-54μm, 54-63μm, 63-80μm, and 80-90μm; the distribution modulus of the coarse-grained limestone powder and the fine-grained limestone powder is 0.1-1.

[0026] It should be noted that the water-cement ratio refers to the ratio of water content to the total amount of cementitious materials per cubic meter of concrete. Cementitious materials refer to the sum of cement and admixtures; admixtures include any one or more of fly ash, mineral powder, silica fume, limestone powder, and zeolite powder. In this invention, limestone powder is used as the admixture, and cementitious materials refer to both cement and limestone powder.

[0027] The water-cement ratio is related to the properties of concrete, such as strength, durability, and flowability. Generally, concrete strength increases as the water-cement ratio decreases and decreases as it increases; however, this relationship is not simple linear. When the water-cement ratio increases, the water content in the concrete increases, leading to changes in the physical properties between cement particles, thus reducing the concrete's strength. Furthermore, an excessively high water-cement ratio can also cause problems such as cracking and shrinkage. Therefore, in concrete construction, it is necessary to rationally select the water-cement ratio based on the actual conditions of the project to ensure the strength and service life of the concrete.

[0028] In a preferred embodiment of the present invention, the water-cement ratio of the cementitious material is 0.4.

[0029] In an optional embodiment of the present invention, the cementitious raw materials include cement and limestone powder in a ratio of (70-80):(20-30).

[0030] It should be noted that while an appropriate proportion of limestone powder can effectively improve the compressive strength of cementitious materials, the strength of the cementitious materials decreases more significantly with increasing limestone powder content. Conversely, as the amount of limestone powder increases, the amount of cement used decreases accordingly, leading to greater carbon reduction benefits. This has a significant impact on the effective utilization of limestone as a mineral resource and on environmental protection.

[0031] In optional embodiments of the present invention, the cement includes at least one of silicate cement, ordinary silicate cement, and mineral cement; further, the cement includes ordinary silicate cement.

[0032] Ordinary Portland cement is a hydraulic cementitious material made by grinding Portland cement clinker, 5%-20% admixtures, and an appropriate amount of gypsum. It possesses characteristics such as high strength, high heat of hydration, good frost resistance, low drying shrinkage, good abrasion resistance, good carbonation resistance, poor corrosion resistance, and poor high-temperature resistance. It is widely used in various fields, including construction, road and bridge engineering, cast-in-place concrete structures, foundations, and industry, and is an indispensable material in modern construction and infrastructure.

[0033] It should be noted that the composition of the ordinary silicate cement used in this invention is not particularly limited, and the most widely used brands and models on the market are purchased.

[0034] In an optional embodiment of the present invention, the limestone powder includes: fine-particle-size limestone powder with a particle size <30μm and coarse-particle-size limestone powder with a particle size of 30-90μm; wherein, the particle size of the coarse-particle-size limestone powder includes at least one of: 30-54μm, 54-63μm, 63-80μm and 80-90μm.

[0035] It should be noted that the classification of limestone powder particle size is not particularly limited in this invention. The specific particle size is set according to the experimental requirements of this invention. In other embodiments of this invention, the particle size can be reclassified and adjusted according to actual conditions. Furthermore, the setting of limestone powder particle size is directly related to its cumulative particle size fraction.

[0036] In an optional embodiment of the present invention, the distribution modulus of coarse-grained limestone powder and fine-grained limestone powder is 0.1-1.

[0037] It should be noted that the settings of the distribution modulus and particle size in this invention are determined by the inventors based on experimental conditions and can be reasonably adjusted according to actual circumstances. In optional embodiments of this invention, the distribution modulus values ​​are 0.1, 0.15, 0.2, 0.25, 0.3, 0.5, 0.7, 0.8, and 1.0, or other values ​​between 0.1 and 1.0.

[0038] In a preferred embodiment of the present invention, when the amount of limestone powder is 20%-23%, the distribution modulus of coarse-grained limestone powder and fine-grained limestone powder is 0.5-0.7.

[0039] When the amount of limestone powder is 23%-30%, the distribution modulus of coarse-grained limestone powder and fine-grained limestone powder is 0.2-0.8.

[0040] In an optional embodiment of the present invention, the limestone powder comprises, by weight percentage: 30%-90% limestone powder with a particle size of 0-30 μm, 5%-30% limestone powder with a particle size of 30-54 μm, 1%-10% limestone powder with a particle size of 54-63 μm, 2%-20% limestone powder with a particle size of 63-80 μm, and 1%-15% limestone powder with a particle size of 80-90 μm.

[0041] In a preferred embodiment of the present invention, when the amount of limestone powder is 20%-23%, the limestone powder comprises, by weight percentage: 45%-60% limestone powder with a particle size of 0-30μm, 19%-25% limestone powder with a particle size of 30-54μm, 6%-9% limestone powder with a particle size of 54-63μm, 10%-15% limestone powder with a particle size of 63-80μm, and 5%-9% limestone powder with a particle size of 80-90μm.

[0042] When the amount of limestone powder is 23%-30%, the limestone powder comprises, by weight percentage: 41%-81% limestone powder with a particle size of 0-30μm, 10%-25% limestone powder with a particle size of 30-54μm, 2%-9% limestone powder with a particle size of 54-63μm, 4%-16% limestone powder with a particle size of 63-80μm, and 2%-9% limestone powder with a particle size of 80-90μm.

[0043] In an optional embodiment of the present invention, the allocation modulus is calculated using a modified Anderson model; the formula for the modified Anderson model is as follows:

[0044] In the formula, D i It is the particle size, P(D) i ) refers to particles smaller than D i The cumulative particle fraction (%), D max It is the maximum particle size, D min q is the minimum particle size, and q is the distribution modulus.

[0045] It should be noted that the modified Anderson model is a compressible model that considers the wall effect and relaxation effect between particles. It has the advantage of establishing the relationship between ideal packing and actual packing, and can design dense packing structures more accurately. The compressible model is established by taking individual particles as the research object and considering their interaction with particles of different sizes, rather than starting from the perspective of the overall gradation of powder materials. The modified Anderson model uses the particle size distribution rather than a single particle size to pack limestone powder of different sizes, thereby optimizing the performance of cementitious materials and improving the utilization rate of limestone mineral resources.

[0046] In an optional embodiment of the present invention, the compressive strength of the cementitious material made from limestone powder after particle size optimization is tested at 3d, 7d and 28d. When the distribution modulus is within a certain range, the compressive strength of the cementitious material after particle size optimization is higher than that of the cementitious material without particle size optimization. Moreover, the later compressive strength of the cementitious material is better than the early compressive strength.

[0047] In an optional embodiment of the present invention, the particle size optimization of the aforementioned cementitious material is achieved using a particle size optimization device, which includes a base 1, a chassis 2, and a screening unit 3; the chassis 2 is connected to the top of the base 1 via an elastic element 101; the screening unit 3 is located at one end away from the base 1 and is connected to the top of the chassis 2; the particle size optimization device also includes a screen cover 4, which is located at one end away from the chassis 2 and is connected to the top of the screening unit 3.

[0048] It should be noted that a feed inlet 401 is provided at one end of the screen cover 4; the feed inlet 401 facilitates the addition of materials.

[0049] In an optional embodiment of the present invention, the screening unit 3 includes a screen 301, a negative pressure device 303, and a collection device 304. The screen 301 is placed at an inclination inside the screening unit 3, and the screen 301 abuts against the inner wall of the screening unit 3. The feed inlet 401 is located at the higher end of the inner surface of the screen 301. The negative pressure device 303 is connected to an external negative pressure device to achieve negative pressure screening of limestone powder. Combined with the inclination of the screen 301, this allows for effective screening and grading of the limestone powder particles. The collection device 304 is located at the lower end of the inner surface of the screen 301 and is used to recycle limestone powder of the desired particle size. In other embodiments of the present invention, the position of the collection device 304 can be reasonably adjusted according to actual conditions.

[0050] It should be noted that, in an optional embodiment of the present invention, the screen 301 is detachably connected to the screening unit 3, and the screen 301 with different mesh sizes can be adjusted and replaced according to the different particle sizes of the limestone powder.

[0051] Specifically, the detachable connection method between the screen 301 and the screening unit 3 is selected from any one of the following: snap-fit ​​connection 305, threaded connection, and pin connection. A suitable detachable connection method can be selected based on ease of use and actual conditions. In an optional embodiment of the present invention, the direct connection method between the two is a snap-fit ​​connection 305.

[0052] Furthermore, the screening unit 3 includes at least one; in an optional embodiment of the invention, three screening units 3 are provided. Each screening unit 3 is provided with a corresponding screen 301 to facilitate the collection of limestone powder of a certain particle size.

[0053] Furthermore, the screen 301 includes protrusions 302; the protrusions 302 are evenly distributed along the inclined direction of the screen 301, and the two ends of the protrusions 302 abut against the inner sidewall of the screening unit 3; the mesh size of the screen 301 is related to the particle size to be screened, and a screen 301 with appropriate mesh size can be selected according to actual needs.

[0054] It should be noted that the protrusion 302 is designed to allow the limestone powder to pause briefly during the sieving process, facilitating complete sieving under the combined effects of vibration and negative pressure. The vibration device 202 is located on the lower side of the inner surface of the chassis 2. In other embodiments of the invention, the position of the vibration device 202 can be adjusted appropriately according to actual conditions.

[0055] Specifically, the placement direction of the protrusions 302 is perpendicular to the flow direction of limestone powder on the screen 301 from the higher side to the lower side of the screen 301. In an optional embodiment of the present invention, the protrusions 302 are evenly distributed on the screen 301, and five protrusions are provided; in other embodiments of the present invention, the specific number of protrusions 302 can be reasonably set according to the actual amount of limestone powder processed and the size of the device.

[0056] Specifically, limestone powder enters the particle size optimization device through the feed inlet 401. Under the combined action of gravity, negative pressure device 303, and the inclined setting of screen 301, limestone powder of the required particle size is sent to the corresponding collection device 304 for recycling.

[0057] In an optional embodiment of the present invention, a baffle 306 is provided at the bottom of each screen 301, that is, at the position where limestone powder particles fall on the screen 301. One end of the baffle 306 is connected to the lower end of the inner side of the screen 301, and the other end extends to the higher end near the inner side of the screen 301. This other end is in an air state and is lower than the lower end of the baffle 306 near the lower end of the inner side of the screen 301. The baffle 306 guides the material to the next screen 301, so that the material flows from the higher part of the inner side of the screen 301 to the lower part, and the screening of the material particle size is more thorough.

[0058] In an optional embodiment of the present invention, the top of the chassis 2 is connected to the bottom of the screening unit 3, and the bottom of the chassis 2 is connected to the base 1. Further, the chassis 2 includes a vibration device 202 and a discharge device 201. Specifically, the bottom of the chassis 2 is connected to the base 1 via an elastic element 101. The cooperation between the elastic element 101 and the vibration device 202 enables the material to be vibrated and screened more thoroughly. Furthermore, the vibration device 202 at the chassis 2 cooperates with the negative pressure device 303 at the screening unit 3, resulting in a more uniform particle size entering the collection device 304.

[0059] Furthermore, the inner side of the chassis 2 is inclined and abuts against the inner wall of the chassis 2; the higher side of the inner side of the chassis 2 is placed near the end of the baffle 306 that is suspended in the air, and the lower side of the inner side of the chassis 2 is placed near the end of the baffle 306 that is connected to the screen 301; this arrangement allows the material to be well screened after entering the particle size optimization device.

[0060] It should be noted that a vibration device 202 is provided on the lower side of the inner side of the chassis 2. The setting of the vibration device 202, the elastic element 101 connected to the bottom of the chassis 2, and the inclined setting of the inner side of the chassis 2 collect the finest particles in the material into the discharge device 201, making the screening more thorough and avoiding the need to clean the chassis 2.

[0061] In an optional embodiment of the present invention, the discharge device 201 is disposed at one end near the base 1, and the discharge device 201 is installed directly below the chassis 2. In other embodiments of the present invention, the position of the discharge device 201 can be reasonably adjusted according to the actual situation.

[0062] In an optional embodiment of the present invention, the chassis 2 is connected to the top of the base 1 via an elastic element 101; specifically, the elastic element 101 is evenly arranged around the discharge device 201 and the chassis 2 is fixedly connected to the base 1. The cooperation between the elastic element 101 and the vibration device 202 will make the material screening more thorough.

[0063] In an optional embodiment of the present invention, support members (not shown in the figure) can be evenly arranged at the end of the base 1 near the ground to protect the stability of the device during operation and prevent water stains on the ground from corroding the base 1 and shortening the service life of the device.

[0064] Specifically, the support members of the base 1 are arranged on the outer periphery of the base 1, and their specific positions are related to the shape of the base 1. If the base 1 is circular, they can be evenly arranged along the circular edge; if the base 1 is rectangular, the support members are arranged at the intersection of every two edges and at the midpoint of the edge. The specific number of support members is reasonably determined according to the size of the base 1, and this invention does not impose any particular limitation.

[0065] It should be noted that the shape and specifications of the base 1, chassis 2, screening unit 3, screen 301, baffle 306, and screen cover 4 of the particle size optimization device in this invention can be reasonably set according to actual needs. For example, their shape can be cylindrical or prismatic. This particle size optimization device can screen multiple particle size ranges of limestone powder in one go. The screening of limestone powder is achieved by the vibration device 202 and the negative pressure device 303, which greatly improves the screening efficiency.

[0066] The features and performance of the present invention will be further described in detail below with reference to embodiments.

[0067] Examples 1-10

[0068] Examples 1-10 of this invention provide a limestone powder cementitious material, the preparation steps of which are as follows:

[0069] S1. The limestone powder raw material is screened using a particle size optimization device, and the screening particle size is set to 0-30μm, 30-54μm, 54-63μm, 63-80μm and 80-90μm;

[0070] It should be noted that in other embodiments of the present invention, limestone powder with other particle sizes can be set according to actual needs; the limestone powder raw material is purchased from commercially available products.

[0071] S2. The dosage of limestone powder with different particle sizes was optimized using a modified Anderson model. The distribution modulus was set to values ​​between 0.1 and 1.0. The specific dosage of limestone powder with different particle sizes corresponding to different distribution moduli is shown in Table 1.

[0072] Mix limestone powder of different particle sizes and stir evenly for later use.

[0073] S3. Use the limestone powder that was mixed evenly in step S2 as an admixture, and purchase commercially available ordinary Portland cement;

[0074] Weigh out 80:20 (g / g) of cement and limestone powder as cementitious raw materials by weight percentage;

[0075] Add 40g of water at a water-to-gel ratio of 0.4.

[0076] S4. Weigh the cement, limestone powder and water from step S3, mix them, stir evenly, place them in the corresponding molds, and prepare the cementitious materials, which are respectively recorded as LS20-0.1 to LS20-1.0.

[0077] S5. The compressive strength of the cementitious material prepared in step S4 was tested. The compressive strength of the cementitious material at 3d, 7d and 28d was tested. The specific results are shown in Table 2.

[0078] Examples 11-20

[0079] Examples 11-20 provide a limestone powder cementitious material, which differs from Example 1 only in that:

[0080] In step S3, cement and limestone powder in a weight ratio of 70:30 (g / g) were weighed as cementitious raw materials to prepare cementitious materials. The prepared cementitious materials were denoted as LS30-0.1 to LS30-1.0, and the compressive strength of the cementitious materials at 3d, 7d and 28d was tested. The specific results are shown in Table 2.

[0081] Comparative Example 1

[0082] This embodiment provides a limestone powder cementitious material, which differs from Embodiments 1-10 only in that steps S1 and S2 are missing.

[0083] S3. Commercially available limestone powder (without particle size optimization treatment) is used as an admixture.

[0084] S4. Weigh the cement, limestone powder and water from step S3, mix them, stir evenly, place them in the corresponding mold, and prepare the cementitious material, denoted as LS20.

[0085] Comparative Example 2

[0086] This embodiment provides a limestone powder cementitious material, which differs from embodiments 11-20 only in that steps S1 and S2 are missing.

[0087] S3. Commercially available limestone powder (without particle size optimization treatment) is used as an admixture.

[0088] S4. Weigh the cement, limestone powder and water from step S3, mix them, stir evenly, place them in the corresponding mold, and prepare the cementitious material, denoted as LS30.

[0089] Experimental Example 1

[0090] This experiment tested the compressive strength of the cementitious materials prepared in Examples 1-20 and Comparative Examples 1-2. The testing instrument used was a hydraulic universal testing machine, and the specific parameters were as follows: the compressive strength loading rate was 0.3 mm / min. The test results are shown in Table 2.

[0091] Experimental Example 2

[0092] This experiment tested the particle size distribution of commercially available limestone powder using a Mastersizer 2000 laser particle size analyzer. Specific parameters were as follows: the test range was set to 0.01-3000 μm. Test results are shown below. Figure 5 .

[0093] Laser particle size analysis results show that: D(10) = 1.904 μm, D(50) = 9.067 μm, D(90) = 66.938 μm; where D(10) = 1.904 μm represents the particle size corresponding to a cumulative content of 10% in the particle size distribution curve.

[0094] Table 1 Content of each particle size under different distribution moduli

[0095]

[0096] It should be noted that the calculation of the content of limestone powder of different particle sizes under different distribution moduli, taking q=0.1 as an example, is as follows:

[0097]

[0098]

[0099]

[0100] Based on the above calculations, the limestone powder content is 89.60% for particles with a diameter of 0-30μm, 5.42% for particles with a diameter of 30-54μm, 1.48% for particles with a diameter of 54-63μm, 2.33% for particles with a diameter of 63-80μm, and 1.17% for particles with a diameter of 80-90μm.

[0101] Table 2 Compressive Strength of Limestone Powder Cement-Based Cementitious Materials

[0102]

[0103]

[0104] The compressive strength results of limestone powder cementitious materials in Table 2 show that the compressive strength decreases with the increase of limestone powder content.

[0105] When the limestone powder content is 20%, the overall compressive strength of the cementitious material is significantly improved when the distribution modulus of coarse and fine limestone powder is between 0.5 and 0.7. Specifically, for the early compressive strength at 3 days, the distribution modulus of 0.1 is 12.8% higher than that of Comparative Example 1; for the later compressive strength at 7 days, the distribution modulus of 0.7 is 7.05% higher than that of Comparative Example 1; and for the later compressive strength at 28 days, the distribution modulus of 0.6 is 13.3% higher than that of Comparative Example 1. In terms of long-term performance, when the limestone powder content is 20%, the limestone powder particle size distribution corresponding to a distribution modulus of 0.6 is superior.

[0106] When the limestone powder content is 30%, the overall compressive strength of the cementitious material is significantly improved when the distribution modulus of coarse and fine limestone powder is between 0.2 and 0.8. Specifically, for the early compressive strength at 3 days, the improvement in Examples 11-20 compared to Comparative Example 2 is small, and even lower than that in Comparative Example 1; for the later compressive strength at 7 days, the improvement is 17.2% when the distribution modulus is 0.6 compared to the comparative example; and for the later compressive strength at 28 days, the improvement is 21.8% when the distribution modulus is 0.8 compared to the comparative example. In terms of long-term performance, when the limestone powder content is 30%, the limestone powder particle size distribution corresponding to a distribution modulus of 0.8 is superior.

[0107] In summary, the limestone powder cement-based cementitious material provided by this invention uses a particle size optimization device to screen the limestone powder, and then a modified Anderson model is used to optimize and determine the dosage ratio for each particle size range. When the amount of limestone powder in the cement is different, the compressive strength of the prepared cementitious material will also be greatly affected. Different amounts of limestone powder will also result in significant differences in the distribution modulus. It is evident that particle size screening of limestone powder and optimization of the dosage ratio of limestone powder with different particle sizes are of great significance.

[0108] Furthermore, limestone powder cementitious materials are prepared by mixing limestone powder of different particle sizes in appropriate proportions, as well as combinations of limestone powder of different particle sizes, with cement as admixtures. The resulting cementitious materials exhibit significantly improved later-stage compressive strength, allowing limestone powder to play a better role. This not only enhances the later-stage compressive strength of the cementitious materials but also further improves the utilization rate of limestone powder and makes an important contribution to environmental protection.

[0109] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A limestone powder cementitious material, characterized in that, The cementitious material comprises cementitious raw materials and water; the water-cement ratio of the cementitious material is 0.35-0.45; The cementitious raw materials comprise (70-80): (20-30) cement and limestone powder by weight percentage; The limestone powder includes: fine-grained limestone powder with a particle size <30μm and coarse-grained limestone powder with a particle size of 30-90μm. The particle size of the coarse-grained limestone powder includes at least one of the following: 30-54μm, 54-63μm, 63-80μm, and 80-90μm; The distribution modulus of the coarse-grained limestone powder and the fine-grained limestone powder is 0.1-1; when the amount of limestone powder is 20%-23%, the distribution modulus of the coarse-grained limestone powder and the fine-grained limestone powder is 0.5-0.7; when the amount of limestone powder is 23%-30%, the distribution modulus of the coarse-grained limestone powder and the fine-grained limestone powder is 0.2-0.

8. The allocation modulus is calculated using a modified Anderson model; the formula for the modified Anderson model is as follows: ; In the formula, It refers to the particle size. It refers to particles smaller than The cumulative percentage of particles (%) It is the maximum particle size. q is the minimum particle size, and q is the distribution modulus.

2. The cementitious material according to claim 1, characterized in that, By weight percentage, the limestone powder comprises: 30%-90% limestone powder with a particle size of 0-30μm, 5%-30% limestone powder with a particle size of 30-54μm, 1%-10% limestone powder with a particle size of 54-63μm, 2%-20% limestone powder with a particle size of 63-80μm, and 1%-15% limestone powder with a particle size of 80-90μm.

3. The cementitious material according to claim 2, characterized in that, When the amount of limestone powder is 20%-23%, the limestone powder comprises, by weight percentage: 45%-60% limestone powder with a particle size of 0-30μm, 19%-25% limestone powder with a particle size of 30-54μm, 6%-9% limestone powder with a particle size of 54-63μm, 10%-15% limestone powder with a particle size of 63-80μm, and 5%-9% limestone powder with a particle size of 80-90μm.

4. The cementitious material according to claim 3, characterized in that, When the amount of limestone powder is 23%-30%, the limestone powder comprises, by weight percentage: 41%-81% limestone powder with a particle size of 0-30μm, 10%-25% limestone powder with a particle size of 30-54μm, 2%-9% limestone powder with a particle size of 54-63μm, 4%-16% limestone powder with a particle size of 63-80μm, and 2%-9% limestone powder with a particle size of 80-90μm.

5. The cementitious material according to claim 1, characterized in that, The water-cement ratio of the cementitious material is 0.

4.

6. The cementitious material according to claim 1, characterized in that, The cement includes at least one of silicate cement, ordinary silicate cement, and mineral cement.

7. The cementitious material according to claim 6, characterized in that, The cement includes ordinary Portland cement.

Citation Information

Patent Citations

  • Micro-grading type high-performance limestone powder admixture capable of being applied to cement concrete

    CN106007431A

  • Admixture, concrete prepared therefrom and preparation methods for admixture and concrete prepared therefrom

    CN108911544A