A fire-resistant and explosion-proof NBR compound for sealing systems

By introducing a self-developed crack-resistant flame retardant into nitrile rubber, the problem of poor flame resistance and heat stability of NBR under high temperature and high pressure conditions has been solved, achieving excellent fireproof and explosion-proof performance and flame retardant performance at high temperatures.

CN118440416BActive Publication Date: 2024-11-01TAICANG GUANLIAN POLYMERIC MATERIAL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410897683.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-05
Publication Date
2024-11-01
Estimated Expiration
2044-07-05

AI Technical Summary

Technical Problem

Nitrile butadiene rubber (NBR) has poor flame retardancy and heat stability under high temperature and high pressure conditions, which limits its application in such conditions.

Method used

Using chloroprene rubber as the matrix, a self-developed crack-resistant flame retardant is introduced. Through the reaction of trithiocyanate and allyl chloride to form an allyl intermediate, and then click addition with mercaptosilicone oil to form an organosilicon loading agent, which is coated on the surface of ultrafine aluminum hydroxide to form a sulfur-nitrogen structure, improving flame retardancy and dispersibility, and enhancing high-temperature explosion resistance.

Benefits of technology

It exhibits excellent fire and explosion resistance at high temperatures, with good flame retardant and fireproof properties. It avoids sealing failure caused by rubber softening and deformation at high temperatures and has good high-temperature explosion resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The present invention relates to a fireproof and explosion-proof NBR rubber compound for sealing system, belonging to the field of polymer materials. The rubber compound includes, by percentage, 22-30wt% of chloroprene rubber, 6.5-8.5wt% of anti-cracking flame retardant, 10-15wt% of reinforcing agent, 7-9wt% of plasticizer, 1.6-2.1wt% of vulcanizing agent, 3-4wt% of activating agent, 1.5-2wt% of accelerator and 1-1.5wt% of antioxidant, and the balance is nitrile rubber; the anti-cracking flame retardant uses ultrafine aluminum hydroxide as a carrier, and is loaded by chelation by an organosilicon loading agent to restrain and buffer aluminum hydroxide, inhibiting aluminum hydroxide from being decomposed in large quantities at instantaneous high temperature, while forming positive stress in rubber to resist softening deformation, resulting in a problem of decreased sealing, so that the rubber compound has excellent high-temperature explosion resistance after vulcanization, and a large number of nitrogen structures and organosilicon chains in its structure form secondary flame retardancy at high temperature, playing a good flame retardant and fireproofing effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polymer materials, and in particular relates to a fireproof and explosion-proof NBR compound rubber for a sealing system. Background Art

[0002] Sealing rubber parts are used in various industrial machinery, hydraulic pipelines, valves and other fields. From deep-sea drilling and aerospace to motorcycles, automobiles, internal combustion engines, wind power bearings, telescopic devices, etc., sealing rubber parts have also received widespread attention in the fields of vibration isolation and noise reduction.

[0003] Nitrile rubber (NBR) is a random copolymer obtained by liquid or solution polymerization of butadiene and acrylonitrile. It has good oil resistance, low cost and good physical and mechanical properties, and is an excellent material for seals. However, NBR rubber, like other rubbers, has poor flame resistance and poor heat stability. It can generally only seal stably within the range of 120°C, which greatly limits its application under high temperature and high pressure conditions. Summary of the invention

[0004] In order to solve the technical problems mentioned in the background technology, the object of the present invention is to provide a fireproof and explosion-proof NBR compound rubber for a sealing system.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A fireproof and explosion-proof NBR rubber compound for a sealing system comprises the following raw materials in percentage:

[0007] Chloroprene rubber 22-30wt%, anti-cracking flame retardant 6.5-8.5wt%, reinforcing agent 10-15wt%, plasticizer 7-9wt%, vulcanizer 1.6-2.1wt%, activator 3-4wt%, accelerator 1.5-2wt% and antioxidant 1-1.5wt%, and the balance is nitrile rubber.

[0008] The anti-cracking flame retardant is prepared by the following method:

[0009] Step A1: thiocyanuric acid, triethylamine and tetrahydrofuran are mixed and dissolved, nitrogen is introduced for protection and the pressure is increased to 3.5-4.5 bar, the temperature is raised to 70-80°C, mechanical stirring is performed at 120-180 rpm, allyl chloride is slowly and isobarically injected, and the total reaction time is controlled to be 6-8 hours. After the reaction is completed, the liquid is washed with water, the aqueous phase is removed and dried to obtain an allyl intermediate;

[0010] Furthermore, the dosage ratio of thiocyanuric acid, allyl chloride, triethylamine and tetrahydrofuran is 0.1 mol: 0.31-0.32 mol: 15-20 mL: 80-110 mL. Under the promotion of triethylamine, allyl chloride replaces the secondary amine in thiocyanuric acid to introduce terminal olefin chain modification.

[0011] Step A2: Mix the allyl intermediate, mercapto silicone oil, dimethylphenylphosphine and toluene, raise the temperature to 55-70°C, and apply 240-320W / m 2 UV irradiation, with stirring at 60-90 rpm for 1.6-2.2 h, after the reaction, toluene is removed by vacuum rotary evaporation to obtain an organosilicon support agent;

[0012] Furthermore, the usage ratio of the mercapto content of the mercapto silicone oil, the allyl intermediate, dimethylphenylphosphine and toluene is 0.1 mol: 25-30 mmol: 20-30 mg: 150-200 mL. Under the catalysis of dimethylphenylphosphine and the initiation of ultraviolet radiation, the active hydroxyl groups of the mercapto silicone oil undergo click addition with the unsaturated structure in the allyl intermediate to form a low molecular weight network compound with the allyl intermediate as a node.

[0013] Step A3: dissolving the organosilicon loading agent and dimethylacetamide, adding ultrafine aluminum hydroxide and mixing, controlling the temperature in a water bath to 40-50° C., stirring for 12 hours, then centrifuging to obtain a precipitate, washing with water, and drying to obtain an anti-cracking flame retardant;

[0014] Furthermore, the dosage ratio of ultrafine aluminum hydroxide, silicone loading agent and dimethylacetamide is 100g:2.8-3.5g:120-150mL, and the allyl intermediate in the silicone loading agent is click-added with mercapto silicone oil to form a sulfur-nitrogen structure with a strong chelating effect. During the liquid phase mixing process, the silicone loading agent is loaded onto the surface of the ultrafine aluminum hydroxide through chelation to coat the ultrafine aluminum hydroxide.

[0015] Furthermore, the median particle size of the ultrafine aluminum hydroxide is not higher than 10 μm.

[0016] A fireproof and explosion-proof NBR mixed rubber for a sealing system, the mixing process of which is as follows: adding nitrile rubber and chloroprene rubber into an open mill and plasticizing them until they are evenly rolled, adding a plasticizer and an antioxidant, adding an anti-cracking flame retardant, a reinforcing agent, an activator and a accelerator in equal amounts three times after the feeding is completed, mixing them evenly, finally adding a vulcanizer, cutting with left and right kneaders three times each, thinning through six times and then cutting off the sheets to obtain the fireproof and explosion-proof NBR mixed rubber for the sealing system.

[0017] Furthermore, during the plasticating process, the roller temperature is 45-55° C. and the roller spacing is 1-1.5 mm.

[0018] Furthermore, during the thin pass process, the roller temperature is 60-75° C. and the roller spacing is 0.6-0.8 mm.

[0019] Beneficial effects of the present invention:

[0020] The present invention uses chloroprene rubber and nitrile rubber as a matrix, and introduces independently developed anti-cracking flame retardants and other additives for mixing. The obtained mixed rubber exhibits excellent fireproof and explosion-resistant properties when used in sealing systems, and has far-reaching application prospects under high-temperature sealing conditions. The anti-cracking flame retardant uses aluminum hydroxide with a low decomposition temperature as a carrier, and introduces terminal olefin chains into the structure of thiocyanate through a substitution reaction between allyl chloride and thiocyanate, thereby obtaining an allyl intermediate, and then a mercaptosilicone oil is click-added to the unsaturated structure in the allyl intermediate to form a low-molecular-weight network compound with the allyl intermediate as a node, thereby obtaining an organosilicon loading agent. The sulfur-nitrogen structure formed by the click-addition of the allyl intermediate and the mercaptosilicone oil has a strong chelating effect. During the liquid phase mixing process, the organosilicon loading agent is loaded onto the surface of the ultrafine aluminum hydroxide through the chelating effect to coat the ultrafine aluminum hydroxide; the dispersibility of the organosilicon loading agent in the rubber matrix is ​​improved through coating modification, and it is more It is easy to give full play to its flame retardancy; the organosilicon loading agent is coated on the surface of aluminum hydroxide, which contains a large number of cyclic networks with the vulcanized rubber macromolecular network as the support point, which restrains and buffers the aluminum hydroxide and inhibits the large-scale decomposition of aluminum hydroxide at instantaneous high temperature, resulting in failure of rubber perforation seal. At the same time, positive stress is formed in the rubber to resist the softening and deformation of the rubber at high temperature, resulting in decreased sealing, so that the compound rubber has excellent high-temperature anti-explosion performance after vulcanization; the organosilicon loading agent contains a large number of nitrogen structures and organosilicon chains. As the temperature rises, the sulfur element promotes its decomposition to produce flame retardant substances and form secondary flame retardant in the rubber matrix. In the test, the product vulcanized from the compound rubber showed good flame retardant and fireproof properties. DETAILED DESCRIPTION

[0021] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] Example 1: This embodiment prepares fireproof and explosion-proof NBR rubber compound for sealing system, as follows:

[0023] 1) Preparation of anti-cracking flame retardant

[0024] Step A1: thiocyanuric acid, triethylamine and tetrahydrofuran are mixed and dissolved, nitrogen is introduced for protection and the pressure is increased to 3.5 bar, the temperature is raised to 70°C, and mechanical stirring is performed at 120 rpm. Allyl chloride is slowly added within 3 hours by isobaric injection. After complete injection, constant temperature stirring is continued for reaction, and the total addition reaction time is controlled to be 8 hours. In the reaction, the amount ratio of thiocyanuric acid, allyl chloride, triethylamine and tetrahydrofuran is 0.1 mol: 0.31 mol: 15 mL: 80 mL. After the reaction is completed, deionized water is added for washing, and the aqueous phase is separated and dried to obtain an allyl intermediate.

[0025] Step A2: Mix the allyl intermediate, mercapto silicone oil, dimethylphenylphosphine and toluene. In this embodiment, Shin-Etsu KF-2001 mercapto silicone oil is used. Heat to 55°C and apply a UVA light source at 240W / m 2 The reaction was carried out under ultraviolet irradiation and stirred at 60 rpm for 1.6 h. During the reaction, the mercapto content of the mercapto silicone oil, the allyl intermediate, dimethylphenylphosphine and toluene were used in a ratio of 0.1 mol: 25 mmol: 20 mg: 150 mL. After the reaction was completed, the toluene was removed by vacuum rotary evaporation to obtain the organosilicon loading agent.

[0026] Step A3: Mix the organosilicon loading agent and dimethylacetamide, and then add ultrafine aluminum hydroxide to mix. In this embodiment, the KA-2M raw material provided by Foshan Huaya Nanomaterial Technology Co., Ltd. is used, the calibrated median particle size is 7.2-8.2μm, the water bath temperature is controlled at 40°C, and the stirring is carried out at 80rpm for 12h. The amount ratio of ultrafine aluminum hydroxide, organosilicon loading agent and dimethylacetamide is 100g:2.8g:120mL. Then, the precipitate is centrifuged, washed with water and dried to obtain an anti-cracking flame retardant.

[0027] 2) Preparation of rubber compound

[0028] Preparation of materials: The raw materials are taken according to the weight percentage, 37.6wt% of nitrile rubber, and the 3355F raw material provided by LANXESS Chemical Co., Ltd. is used in the implementation process; 22wt% of chloroprene rubber, and the A90 raw material provided by Shenzhen Yoshida Chemical Co., Ltd. is used in the implementation process; 8.5wt% of anti-cracking flame retardant is prepared by this implementation; 15wt% of reinforcing agent, and the N330 raw material provided by Jiangxi Black Cat Carbon Black Co., Ltd. is used in the implementation process; 8.5wt% of plasticizer, and the plasticizer trioctyl trimellitate provided by Shanghai Kunrui Chemical Co., Ltd. is used in the implementation process; 2.1wt% of vulcanizing agent, and the sulfur provided by Dongying Haijing Chemical Co., Ltd. is used in the implementation process; 3.6wt% of activator, and zinc oxide and stearic acid are used in a mass ratio of 1:1 in the implementation process; 1.5wt% of accelerator, and the accelerator TMTD and NA-22 accelerator are used in a mass ratio of 2:1 in the implementation process; 1.2wt% of antioxidant, and the antioxidant RD is used in the implementation process.

[0029] Mixing: Adjust the roller temperature of the mixing mill to 45℃ and the roller spacing to 1.5mm, add nitrile rubber and chloroprene rubber and plasticize until they are evenly wrapped around the rollers, then add plasticizer and antioxidant. After the feeding is completed, premix the anti-cracking flame retardant, reinforcing agent, activator and accelerator, add them in equal amounts three times and mix evenly, finally add the vulcanizer, cut the left and right kneaders three times each, control the roller temperature to 60℃, adjust the roller spacing to 0.8mm, and thin it six times before unrolling to obtain the fireproof and explosion-proof NBR compound rubber for sealing systems.

[0030] Example 2: This embodiment prepares a fireproof and explosion-proof NBR rubber compound for a sealing system, as follows:

[0031] 1) Preparation of anti-cracking flame retardant

[0032] Step A1: thiocyanuric acid, triethylamine and tetrahydrofuran are mixed and dissolved, nitrogen is introduced for protection and the pressure is increased to 4.0 bar, the temperature is raised to 75°C, and mechanical stirring is performed at 180 rpm. Allyl chloride is slowly added within 2.5 hours by isobaric injection. After complete injection, constant temperature stirring is continued for reaction. The total addition reaction time is controlled to be 7 hours. In the reaction, the amount ratio of thiocyanuric acid, allyl chloride, triethylamine and tetrahydrofuran is 0.1 mol: 0.31 mol: 18 mL: 100 mL. After the reaction is completed, deionized water is added for washing, and the aqueous phase is separated and dried to obtain an allyl intermediate.

[0033] Step A2: Mix the allyl intermediate, mercapto silicone oil, dimethylphenylphosphine and toluene. In this embodiment, Shin-Etsu KF-2004 mercapto silicone oil is used. Heat to 65°C and apply 300W / m 2 The reaction was carried out under ultraviolet irradiation and stirred at 90 rpm for 2.2 hours. During the reaction, the mercapto content of the mercapto silicone oil, the allyl intermediate, dimethylphenylphosphine and toluene were used in a ratio of 0.1 mol: 28 mmol: 25 mg: 180 mL. After the reaction was completed, the toluene was removed by vacuum rotary evaporation to obtain the organosilicon loading agent.

[0034] Step A3: Mix the organosilicon loading agent and dimethylacetamide, and then add ultrafine aluminum hydroxide to mix. In this embodiment, the KA-5E raw material provided by Foshan Huaya Nanomaterial Technology Co., Ltd. is used, the calibrated median particle size is 5.0-6.2μm, the water bath temperature is controlled at 50°C, and the stirring is carried out at 120rpm for 12h. The amount ratio of ultrafine aluminum hydroxide, organosilicon loading agent and dimethylacetamide is 100g:3.2g:150mL. Then, the precipitate is centrifuged, washed with water and dried to obtain an anti-cracking flame retardant.

[0035] 2) Preparation of rubber compound

[0036] Preparation of materials: The raw materials are taken according to the weight percentage, 37.6wt% of nitrile rubber, and the 3355F raw material provided by LANXESS Chemical Co., Ltd. is used in the implementation process; 26wt% of chloroprene rubber, and the A90 raw material provided by Shenzhen Yoshida Chemical Co., Ltd. is used in the implementation process; 7.5wt% of anti-cracking flame retardant is prepared by this implementation; 12wt% of reinforcing agent, and the N330 raw material provided by Jiangxi Black Cat Carbon Black Co., Ltd. is used in the implementation process; 9wt% of plasticizer, and the plasticizer trioctyl trimellitate provided by Shanghai Kunrui Chemical Co., Ltd. is used in the implementation process; 1.6wt% of vulcanizing agent, and the sulfur provided by Dongying Haijing Chemical Co., Ltd. is used in the implementation process; 3wt% of activator, and zinc oxide and stearic acid are compounded in a mass ratio of 1:1 in the implementation process; 1.8wt% of accelerator, and the accelerator TMTD and NA-22 accelerator are compounded in a mass ratio of 2:1 in the implementation process; 1.5wt% of antioxidant, and the antioxidant RD is used in the implementation process.

[0037] Mixing: Adjust the roller temperature of the mixing mill to 50℃ and the roller spacing to 1.2mm. Add nitrile rubber and chloroprene rubber and plasticize until they are evenly wrapped around the rollers. Then add plasticizer and antioxidant. After the feeding is completed, premix the anti-cracking flame retardant, reinforcing agent, activator and accelerator. Add equal amounts in three times and mix evenly. Finally, add the vulcanizer, cut the left and right kneaders three times each. Control the roller temperature to 70℃, adjust the roller spacing to 0.8mm, and thin it six times before unrolling to obtain the fireproof and explosion-proof NBR compound rubber for sealing systems.

[0038] Example 3: This embodiment prepares fireproof and explosion-proof NBR rubber compound for sealing system, as follows:

[0039] 1) Preparation of anti-cracking flame retardant

[0040] Step A1: thiocyanuric acid, triethylamine and tetrahydrofuran are mixed and dissolved, nitrogen is introduced for protection and the pressure is increased to 4.5 bar, the temperature is raised to 80°C, and mechanical stirring is performed at 180 rpm. Allyl chloride is slowly added within 2 hours by isobaric injection. After complete injection, constant temperature stirring is continued for reaction, and the total addition reaction time is controlled to be 6 hours. In the reaction, the amount ratio of thiocyanuric acid, allyl chloride, triethylamine and tetrahydrofuran is 0.1 mol: 0.32 mol: 20 mL: 110 mL. After the reaction is completed, deionized water is added for washing, and the aqueous phase is separated and dried to obtain an allyl intermediate.

[0041] Step A2: Mix the allyl intermediate, mercapto silicone oil, dimethylphenylphosphine and toluene. In this embodiment, Shin-Etsu KF-2004 mercapto silicone oil is used. Heat to 70°C and apply a UVA light source at 320W / m 2The mixture was irradiated with ultraviolet light and stirred at 90 rpm for 2.1 h. During the reaction, the mercapto content of the mercapto silicone oil, the allyl intermediate, dimethylphenylphosphine and toluene were used in a ratio of 0.1 mol: 30 mmol: 30 mg: 200 mL. After the reaction, the toluene was removed by vacuum rotary evaporation to obtain an organosilicon loading agent.

[0042] Step A3: Mix the organosilicon loading agent and dimethylacetamide, and then add ultrafine aluminum hydroxide to mix. In this embodiment, the KA-5E raw material provided by Foshan Huaya Nanomaterial Technology Co., Ltd. is used, the calibrated median particle size is 5.0-6.2μm, the water bath temperature is controlled at 50°C, and the stirring is carried out at 120rpm for 12h. The amount ratio of ultrafine aluminum hydroxide, organosilicon loading agent and dimethylacetamide is 100g:3.5g:150mL. Then, the precipitate is centrifuged, washed with water and dried to obtain an anti-cracking flame retardant.

[0043] 2) Preparation of rubber compound

[0044] Preparation of materials: The raw materials are taken according to the weight percentage, 37.6wt% of nitrile rubber, and the 3355F raw material provided by LANXESS Chemical Co., Ltd. is used in the implementation process; 30wt% of chloroprene rubber, and the A90 raw material provided by Shenzhen Yoshida Chemical Co., Ltd. is used in the implementation process; 6.5wt% of anti-cracking flame retardant is prepared by this implementation; 10wt% of reinforcing agent, and the N330 raw material provided by Jiangxi Black Cat Carbon Black Co., Ltd. is used in the implementation process; 7wt% of plasticizer, and the plasticizer trioctyl trimellitate provided by Shanghai Kunrui Chemical Co., Ltd. is used in the implementation process; 1.9wt% of vulcanizing agent, and the sulfur provided by Dongying Haijing Chemical Co., Ltd. is used in the implementation process; 4wt% of activator, and zinc oxide and stearic acid are compounded in a mass ratio of 1:1 in the implementation process; 2wt% of accelerator, and the accelerator TMTD and NA-22 accelerator are compounded in a mass ratio of 2:1 in the implementation process; 1wt% of antioxidant, and the antioxidant RD is used in the implementation process.

[0045] Mixing: Adjust the roller temperature of the mixing mill to 55℃ and the roller spacing to 1mm, add nitrile rubber and chloroprene rubber and plasticize until they are evenly wrapped around the rollers, then add plasticizer and antioxidant. After the feeding is completed, premix the anti-cracking flame retardant, reinforcing agent, activator and accelerator, add them in equal amounts three times and mix evenly, finally add the vulcanizer, cut the left and right kneaders three times each, control the roller temperature to 75℃, adjust the roller spacing to 0.6mm, thin it six times and then take off the sheet to obtain the fireproof and explosion-proof NBR compound rubber for sealing system.

[0046] Comparative Example 1

[0047] This comparative example is a control test of Example 2, except that the anti-cracking flame retardant is replaced by 6.5% KA-5E ultrafine aluminum hydroxide and 1% silane coupling agent KH570, and both are premixed with the reinforcing agent, activator and promoter, and the rest are exactly the same.

[0048] Comparative Example 2

[0049] This comparative example is selected from commercially available explosion-proof sealing rings, which are provided by Yueqing Hongyun Electrical Appliance Parts Factory.

[0050] In order to verify the performance of the rubber mix prepared above in sealing materials, the rubber mix was cut and loaded into a rubber vulcanizer, the temperature was controlled at 160±5℃, the vulcanization time was 25min, and it was left to stand for 12h after demoulding, and sheet specimens and ring specimens were made respectively;

[0051] Take the sheet specimens for mechanical property tests, including: hardness test according to GB / T 531.1-2008 standard; tensile test according to GB / T 528-2009 standard, tensile rate is 100mm / min; tear test according to GB / T 529-2008 standard, right-angle tear specimen, tensile rate is 100mm / min; specific test results are shown in Table 1:

[0052] Table 1

[0053]

[0054] From the test results in Table 1, it can be seen that the Shore A hardness of the mixed gel prepared in Example and Comparative Example 1 after vulcanization is about 80, which has moderate hardness. The tensile and tear properties of the example are slightly higher than those of Comparative Example 1. After analysis, it may be related to the compatibility of the anti-cracking flame retardant with the base rubber, and has little effect on the mechanical properties of the base rubber.

[0055] Take the annular sample prepared above, refer to the NORSOK-M710 standard rubber sealing material instantaneous decompression test method and requirements, and conduct explosion resistance test on the epoxy sample. The test temperatures are 100℃, 200℃ and 300℃ respectively. The pressure when the rating of the annular sample reaches level 4 and is unacceptable after the test is recorded as the explosion resistance strength; take a sheet with a thickness of 1mm from the above sheet sample and conduct UL94 combustion test. The specific test data are shown in Table 2:

[0056] Table 2

[0057]

[0058] It can be seen from the test results in Table 2 that the explosion resistance of the embodiment and comparative example 1 is about 90 MPa within the range of 100°C, which is slightly lower than that of comparative example 2. After analysis, it is possible that at this temperature, the rubber matrix maintains good stability, thereby maintaining good sealing. The hard aluminum hydroxide in the introduced anti-cracking flame retardant is hardened by the rubber matrix, resulting in a relatively decreased sealing; as the temperature rises to 200-300°C, the rubber matrix softens, resulting in a decrease in the ability to support the seal, and the explosion resistance decreases to a certain extent, among which comparative example 2 shows a significant decrease. In the embodiments and comparative examples, a small amount of primary decomposition of aluminum hydroxide occurs, forming positive stress in the material, resisting deformation of the sealing material, thereby preventing leakage, showing excellent explosion resistance. In the combustion test, the UL94 grade of the 1mm sheet reaches V-1, and it has good flame retardant and fireproof capabilities.

[0059] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0060] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A fireproof and explosion-proof NBR rubber compound for a sealing system, characterized in that: The following raw materials are included in percentage: 22-30wt% chloroprene rubber, 6.5-8.5wt% anti-cracking flame retardant, 10-15wt% reinforcing agent, 7-9wt% plasticizer, 1.6-2.1wt% vulcanizing agent, 3-4wt% activator, 1.5-2wt% accelerator and 1-1.5wt% antioxidant, and the balance is nitrile rubber; The anti-cracking flame retardant is prepared by the following method: Step A1: thiocyanuric acid, triethylamine and tetrahydrofuran are mixed, nitrogen is introduced for protection and the pressure is increased to 3.5-4.5 bar, the temperature is raised to 70-80° C., allyl chloride is slowly and isobarically injected with stirring, and the total reaction time is controlled to be 6-8 hours. After the reaction is completed, the liquid is washed with water, the aqueous phase is removed and dried to obtain an allyl intermediate, wherein the amount ratio of thiocyanuric acid, allyl chloride, triethylamine and tetrahydrofuran is 0.1 mol: 0.31-0.32 mol: 15-20 mL: 80-110 mL; Step A2: Mix the allyl intermediate, mercapto silicone oil, dimethylphenylphosphine and toluene, raise the temperature to 55-70°C, and apply 240-320W / m 2 UV irradiation, stirring and reacting for 1.6-2.2h, after the reaction, toluene is removed by vacuum rotary evaporation to obtain an organosilicon support agent, wherein the amount ratio of the mercapto content of the mercapto silicone oil, the allyl intermediate, dimethylphenylphosphine and toluene is 0.1mol: 25-30mmol: 20-30mg: 150-200mL; Step A3: Mix the organosilicon loading agent and dimethylacetamide, then add ultrafine aluminum hydroxide and mix, control the temperature in a water bath to 40-50°C, stir for 12 hours, then centrifuge to obtain the precipitate, wash with water and dry to obtain an anti-cracking flame retardant, wherein the dosage ratio of ultrafine aluminum hydroxide, organosilicon loading agent and dimethylacetamide is 100g:2.8-3.5g:120-150mL.

2. The fireproof and explosion-proof NBR rubber compound for sealing system according to claim 1, characterized in that: The median particle size of ultrafine aluminum hydroxide is not higher than 10μm.

3. The fireproof and explosion-proof NBR rubber compound for sealing system according to claim 1, characterized in that: The mixing process is as follows: add nitrile rubber and chloroprene rubber into an open mixing mill and plasticize until they are evenly coated on the rollers; add plasticizer and antioxidant; after the feeding is completed, add anti-cracking flame retardant, reinforcing agent, activator and accelerator in equal amounts three times and mix evenly; finally add vulcanizer, cut with left and right kneaders three times each, and after six thin passes, remove the sheet to obtain fireproof and explosion-proof NBR mixed rubber for sealing systems.

4. The fireproof and explosion-proof NBR rubber compound for sealing system according to claim 3, characterized in that: During the plasticating process, the roller temperature is 45-55°C and the roller spacing is 1-1.5mm.

5. The fireproof and explosion-proof NBR rubber compound for sealing system according to claim 3, characterized in that: During the thin pass process, the roller temperature is 60-75°C and the roller spacing is 0.6-0.8mm.