A reinforced self-supporting butterfly optical cable
By using a combination of modified porous hollow fillers and fibrous fillers in optical cables, combined with surface modification treatment, the tensile resistance, bending resistance and mechanical strength of the optical cables are improved, and the problems of construction difficulty and insufficient performance of traditional optical cables are solved.
Patent Information
- Application Number
- CN202410943921.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-07-15
AI Technical Summary
Traditional high-altitude optical cable transmission has safety risks and is difficult to construct. Existing self-supporting optical cables are insufficient in tensile resistance and bending resistance.
It adopts a reinforced self-supporting butterfly cable design, including self-supporting suspension wires, reinforcements and optical fibers. The sheath material is made of polyethylene, ethylene-vinyl acetate copolymer, maleic anhydride, and polybutylene succinate. It is composed of ester, modified porous hollow filler and fibrous filler. The mechanical properties and affinity of the material are improved through surface modification treatment.
It improves the tensile resistance, bending resistance and mechanical strength of the optical cable, reduces the difficulty of construction, and enhances the wear resistance of the sheath layer.
Smart Images

Figure CN118465948B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of communication optical cable manufacturing, and specifically relates to a reinforced self-supporting butterfly-shaped optical cable. Background Art
[0002] With the rapid development of communication technology, the application of optical fiber is becoming more and more extensive. During the transmission process, optical fiber is transmitted in the form of optical cable. The laying methods of optical cable during the transmission process mainly include: high-altitude erection, ground laying and underwater burial. There are many unsafe factors in the traditional high-altitude erection, and sometimes for the transmission of optical cable, it is necessary to set up steel wire rope separately, which increases the difficulty of construction. Self-supporting optical cable is the most common way to use cable high-altitude erection. The object of the present invention is to provide a reinforced self-supporting optical cable with high tensile strength and convenient construction and installation. Summary of the invention
[0003] The present invention provides a reinforced self-supporting butterfly-shaped optical cable, which comprises a self-supporting suspension line 1, a reinforcement member 2, an optical fiber 3 and a sheath 4. The suspension line 1, the reinforcement member 2 and the optical fiber 3 are all covered by the sheath 4. There are two reinforcement members 2, which are located on both sides of the optical fiber 3. The suspension line 1 is located on the side of one of the reinforcement members 2 away from the optical fiber 3. The sheath 4 comprises: a polymer, a modified porous hollow filler and a fibrous filler. After the surface of the porous hollow filler is modified, its affinity with the polymer is improved, and the polymer molecular chain can pass through the holes of the hollow filler, so that the sheath has higher mechanical properties. The optical cable has excellent supporting performance, tensile strength and bending resistance.
[0004] The specific plan is as follows:
[0005] A reinforced self-supporting butterfly optical cable comprises a self-supporting suspension wire 1, a reinforcement member 2, an optical fiber 3 and a sheath 4. The suspension wire 1, the reinforcement member 2 and the optical fiber 3 are all covered by the sheath 4. There are two reinforcement members 2, which are located on both sides of the optical fiber 3. The suspension wire 1 is located on the side of one of the reinforcement members 2 away from the optical fiber 3. The material of the sheath 4 comprises the following components by mass: 100-120 parts of polyethylene, 25-30 parts of ethylene-vinyl acetate copolymer, 10-15 parts of maleic anhydride, 10-15 parts of polybutylene succinate, 10-15 parts of modified porous hollow filler, 20-25 parts of fibrous filler, 3-6 parts of plasticizer, 3-6 parts of toughening agent and 2-3 parts of antioxidant.
[0006] Furthermore, the plasticizer is selected from one or a combination of dioctyl phthalate, butyl benzyl phthalate, dicyclohexyl phthalate, dibutyl phthalate, diisobutyl phthalate, dimethyl phthalate, and diethyl phthalate.
[0007] Furthermore, the toughening agent is selected from one or a combination of nitrile rubber and polysulfide rubber.
[0008] Furthermore, the amino silane coupling agent is selected from KH550, KH560, KH570 or KH602.
[0009] Furthermore, the antioxidant is antioxidant 1010.
[0010] Furthermore, the modified porous hollow filler is prepared by the following method:
[0011] A) dissolving silicate in dichloromethane, adding a silane coupling agent with an amino group, stirring and mixing to obtain a solution a;
[0012] B) dissolving sodium dodecyl sulfate, polyethylene glycol octyl phenyl ether, and polyether F127 dicarboxyl in deionized water to obtain solution b;
[0013] C) Mixing solution a and solution b evenly, adding NaOH solution dropwise until the pH value of the solution is 8-9, reacting completely, filtering and drying to obtain a porous hollow filler;
[0014] D) Dissolving hexadecyltrimethylammonium bromide and 1-butyl-3-methylimidazole chloride in deionized water, adding the porous hollow filler, adding chitosan, glutaraldehyde and acetic acid, performing hydrothermal reaction, filtering and drying to obtain a modified porous hollow filler.
[0015] Furthermore, the modified porous hollow filler is prepared by the following method:
[0016] A) Dissolve 200 g of ethyl orthosilicate in 50 mL of dichloromethane, add 100 g of KH602, and stir to mix well to obtain solution a;
[0017] B) dissolving 4-6 g of sodium dodecyl sulfate, 2-4 g of polyethylene glycol octylphenyl ether, and 6-8 g of polyether F127 dicarboxyl in 200 mL of deionized water to obtain solution b;
[0018] C) Mix solution a and solution b evenly, add 1 mol / L NaOH solution until the pH value of the solution is 8-9, react completely, filter and dry to obtain a porous hollow filler;
[0019] D) Dissolve 5-8g of hexadecyltrimethylammonium bromide and 20-25g of 1-butyl-3-methylimidazole chloride in 200ml of deionized water, add 100g of porous hollow filler, add 2-4g of chitosan, 1-3g of glutaraldehyde, and 10g of acetic acid, and perform hydrothermal reaction at 70-80 degrees Celsius for complete reaction, filter, and dry to obtain a modified porous hollow filler.
[0020] Furthermore, the fibrous filler is prepared by the following method:
[0021] A) Add 10g of carbon nanofibers to 200ml of 2-3mol / L nitric acid aqueous solution, perform hydrothermal reaction at 70-80℃ for 6-10h, filter, wash and dry to obtain activated carbon nanofibers;
[0022] B) adding 10g of activated carbon nanofibers to 200ml of ethanol solution of butyl titanate with a mass fraction of 2-4wt%, adding 10g of acetic acid, hydrothermally reacting at 70-80℃ for 5-10h, filtering, washing, drying, heating to 650-700℃ and calcining for 3-5h;
[0023] C) Take 10g of the product of step B, add 5-10g of 1-butyl-3-methylimidazole bromide and 4-6g of polyethylene glycol into 100ml of N,N-dimethylformamide and mix evenly, add 1-2g of azobisisobutyronitrile and 1-2g of stannous isooctanoate, stir evenly and let stand for 10-60min, then hydrothermally react at 70-90℃ for 3-6h, filter, wash and dry to obtain the product.
[0024] Furthermore, the length of the carbon fiber is 40-60 microns.
[0025] The present invention has the following beneficial effects:
[0026] Compared with the prior art, the beneficial effects of the present invention are:
[0027] 1) Polyethylene, ethylene-vinyl acetate copolymer, maleic anhydride, polybutylene succinate can provide beneficial processing properties and good mechanical properties;
[0028] 2) The surface modification of porous silica filler by ionic liquid 1-butyl-3-methylimidazole chloride, chitosan, and cross-linking agent glutaraldehyde can greatly improve the affinity between porous filler and polymer. At the same time, the present invention uses spherical porous filler and fiber filler in combination, which not only improves the tensile strength of the material but also improves the wear resistance of the material.
[0029] 3) In the present invention, the modified fiber material, the titanium dioxide particles on the surface of the carbon fiber form protrusions on the fiber surface, and a cross-linked coating layer is formed on the surface of the carbon fiber through the polyionic liquid 1-butyl-3-methylimidazole bromide and polyethylene glycol. The coating on the carbon surface is firm and not easy to fall off, so that the carbon fiber can be anchored in the sheath, slowing down the slippage of the carbon fiber in the sheath layer, and the modified carbon fiber filler increases the mechanical strength of the sheath layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1is a cross-sectional view of the optical cable of the present invention. DETAILED DESCRIPTION
[0031] The present invention is further described below in conjunction with specific embodiments. In each embodiment and comparative example, the wall thickness of the sheath is 0.3 mm, but the protection scope of the present invention is not limited to the following embodiments. Any non-essential adjustments and modifications made to the present invention based on the above invention content still fall within the protection scope of the present invention.
[0032] Example 1
[0033] The reinforced self-supporting butterfly optical cable comprises a self-supporting suspension wire 1, a reinforcement member 2, an optical fiber 3 and a sheath 4, wherein the suspension wire 1, the reinforcement member 2 and the optical fiber 3 are all covered by the sheath 4, the reinforcement member 2 has two pieces and is located on both sides of the optical fiber 3, and the suspension wire 1 is located on the side of one of the reinforcement members 2 away from the optical fiber 3; the material of the sheath comprises the following components by mass: 100 parts of polyethylene, 25 parts of ethylene-vinyl acetate copolymer, 10 parts of maleic anhydride, 10 parts of polybutylene succinate, 10 parts of modified porous hollow filler, 20 parts of fibrous filler, 3 parts of dioctyl phthalate, 3 parts of nitrile rubber, and 2 parts of antioxidant 1010.
[0034] The modified porous hollow filler is prepared by the following method:
[0035] A) Dissolve 200 g of ethyl orthosilicate in 50 mL of dichloromethane, add 100 g of KH602, and stir to mix well to obtain solution a;
[0036] B) dissolving 4 g of sodium dodecyl sulfate, 2 g of polyethylene glycol octylphenyl ether, and 6 g of polyether F127 dicarboxyl in 200 mL of deionized water to obtain solution b;
[0037] C) Mix solution a and solution b evenly, add 1 mol / L NaOH solution until the pH value of the solution is 8, and complete the reaction, filter and dry to obtain a porous hollow filler;
[0038] D) Dissolve 5 g of hexadecyltrimethylammonium bromide and 20 g of 1-butyl-3-methylimidazole chloride in 200 ml of deionized water, add 100 g of porous hollow filler, add 2 g of chitosan, 1 g of glutaraldehyde, and 10 g of acetic acid, perform hydrothermal reaction at 80 degrees Celsius, filter, and dry to obtain a modified porous hollow filler.
[0039] The fibrous filler is prepared by the following method:
[0040] 10g of carbon nanofibers with a diameter of 40 microns were added to 200ml of nitric acid aqueous solution with a concentration of 2mol / L, and after hydrothermal reaction at 70°C for 10h, filtered, washed with deionized water, and dried at 80°C to obtain activated carbon nanofibers; 10g of activated carbon nanofibers were added to 200ml of ethanol solution of butyl titanate with a mass fraction of 2wt%, 10g of acetic acid was added, hydrothermal reaction was carried out at 70°C for 5h, filtered, washed with deionized water, dried at 80°C, and placed in a tube furnace and heated to 650°C for calcination for 3h; 10g of the product was taken, added with 5g of 1-butyl-3-methylimidazole bromide and 4g of polyethylene glycol to 100ml of N,N-dimethylformamide and mixed evenly, 1g of azobisisobutyronitrile and 1g of stannous isooctanoate were added, stirred evenly and allowed to stand for 10min, then hydrothermally reacted at 70°C for 6h, filtered, washed with deionized water, and dried at 80°C to obtain a fibrous filler.
[0041] Example 2
[0042] The reinforced self-supporting butterfly optical cable comprises a self-supporting suspension wire 1, a reinforcement member 2, an optical fiber 3 and a sheath 4, wherein the suspension wire 1, the reinforcement member 2 and the optical fiber 3 are all covered by the sheath 4, the reinforcement member 2 has two pieces and is located on both sides of the optical fiber 3, and the suspension wire 1 is located on the side of one of the reinforcement members 2 away from the optical fiber 3; the material of the sheath comprises the following components by mass: 120 parts of polyethylene, 30 parts of ethylene-vinyl acetate copolymer, 15 parts of maleic anhydride, 15 parts of polybutylene succinate, 15 parts of modified porous hollow filler, 25 parts of fibrous filler, 6 parts of dioctyl phthalate, 6 parts of nitrile rubber, and 3 parts of antioxidant 1010.
[0043] The modified porous hollow filler is prepared by the following method:
[0044] A) Dissolve 200 g of ethyl orthosilicate in 50 mL of dichloromethane, add 100 g of KH602, and stir to mix well to obtain solution a;
[0045] B) dissolving 6 g of sodium dodecyl sulfate, 4 g of polyethylene glycol octylphenyl ether, and 8 g of polyether F127 dicarboxyl in 200 mL of deionized water to obtain solution b;
[0046] C) Mix solution a and solution b evenly, add 1 mol / L NaOH solution until the pH value of the solution is 8, and complete the reaction, filter and dry to obtain a porous hollow filler;
[0047] D) 8 g of hexadecyltrimethylammonium bromide and 25 g of 1-butyl-3-methylimidazole chloride were dissolved in 200 ml of deionized water, 100 g of porous hollow filler was added, 4 g of chitosan, 3 g of glutaraldehyde, and 10 g of acetic acid were added, and the reaction was completed by hydrothermal reaction at 80 degrees Celsius, filtered, and dried to obtain a modified porous hollow filler.
[0048] The fibrous filler is prepared by the following method:
[0049] 10g of carbon nanofibers with a diameter of 40 microns were added to 200ml of 3mol / L nitric acid aqueous solution, and after hydrothermal reaction at 80°C for 6h, filtered, washed with deionized water, and dried at 80°C to obtain activated carbon nanofibers; 10g of activated carbon nanofibers were added to 200ml of 4wt% butyl titanate ethanol solution, 10g of acetic acid was added, and hydrothermal reaction was carried out at 80°C for 5h, filtered, washed with deionized water, dried at 80°C, and placed in a tube furnace and heated to 700°C for calcination for 3h; 10g of the product was taken, and 10g of 1-butyl-3-methylimidazole bromide and 6g of polyethylene glycol were added to 100ml of N, N-dimethylformamide and mixed evenly, 2g of azobisisobutyronitrile and 2g of stannous isooctanoate were added, stirred evenly and allowed to stand for 60min, and then hydrothermally reacted at 90°C for 3h, filtered, washed with deionized water, and dried at 80°C to obtain a fibrous filler.
[0050] Example 3
[0051] The reinforced self-supporting butterfly optical cable comprises a self-supporting suspension wire 1, a reinforcement member 2, an optical fiber 3 and a sheath 4, wherein the suspension wire 1, the reinforcement member 2 and the optical fiber 3 are all covered by the sheath 4, there are two reinforcement members 2, which are located on both sides of the optical fiber 3, and the suspension wire 1 is located on the side of one of the reinforcement members 2 away from the optical fiber 3; the material of the sheath comprises the following components by mass: 110 parts of polyethylene, 28 parts of ethylene-vinyl acetate copolymer, 12 parts of maleic anhydride, 13 parts of polybutylene succinate, 12 parts of modified porous hollow filler, 22 parts of fibrous filler, 5 parts of dioctyl phthalate, 5 parts of nitrile rubber, and 3 parts of antioxidant 1010.
[0052] The modified porous hollow filler is prepared by the following method:
[0053] A) Dissolve 200 g of ethyl orthosilicate in 50 mL of dichloromethane, add 100 g of KH602, and stir to mix well to obtain solution a;
[0054] B) dissolving 5 g of sodium dodecyl sulfate, 3 g of polyethylene glycol octylphenyl ether, and 7 g of polyether F127 dicarboxyl in 200 mL of deionized water to obtain solution b;
[0055] C) Mix solution a and solution b evenly, add 1 mol / L NaOH solution until the pH value of the solution is 8, and complete the reaction, filter and dry to obtain a porous hollow filler;
[0056] D) 6 g of hexadecyltrimethylammonium bromide and 22 g of 1-butyl-3-methylimidazole chloride were dissolved in 200 ml of deionized water, 100 g of porous hollow filler was added, 3 g of chitosan, 2 g of glutaraldehyde, and 10 g of acetic acid were added, and the reaction was completed by hydrothermal reaction at 80 degrees Celsius, filtered, and dried to obtain a modified porous hollow filler.
[0057] The fibrous filler is prepared by the following method:
[0058] 10g of carbon nanofibers with a diameter of 40 microns were added to 200ml of 2.5mol / L nitric acid aqueous solution, and after hydrothermal reaction at 75°C for 8h, filtered, washed with deionized water, and dried at 80°C to obtain activated carbon nanofibers; 10g of activated carbon nanofibers were added to 200ml of 3wt% ethanol solution of butyl titanate, 10g of acetic acid was added, hydrothermal reaction was carried out at 75°C for 6h, filtered, washed with deionized water, dried at 80°C, and heated to 670°C in a tubular furnace for calcination for 4h; 10g of the product was taken, added with 8g of 1-butyl-3-methylimidazole bromide and 5g of polyethylene glycol to 100ml of N,N-dimethylformamide, and mixed evenly, 1.5g of azobisisobutyronitrile and 1.5g of stannous isooctanoate were added, stirred evenly and allowed to stand for 30min, and then hydrothermally reacted at 80°C for 4h, filtered, washed with deionized water, and dried at 80°C to obtain a fibrous filler.
[0059] Example 4
[0060] The reinforced self-supporting butterfly optical cable comprises a self-supporting suspension wire 1, a reinforcement member 2, an optical fiber 3 and a sheath 4, wherein the suspension wire 1, the reinforcement member 2 and the optical fiber 3 are all covered by the sheath 4, there are two reinforcement members 2, which are located on both sides of the optical fiber 3, and the suspension wire 1 is located on the side of one of the reinforcement members 2 away from the optical fiber 3; the material of the sheath comprises the following components by mass: 110 parts of polyethylene, 28 parts of ethylene-vinyl acetate copolymer, 12 parts of maleic anhydride, 13 parts of polybutylene succinate, 12 parts of modified porous hollow filler, 22 parts of fibrous filler, 5 parts of dioctyl phthalate, 5 parts of nitrile rubber, and 3 parts of antioxidant 1010.
[0061] The modified porous hollow filler is prepared by the following method:
[0062] A) Dissolve 200 g of ethyl orthosilicate in 50 mL of dichloromethane, add 100 g of KH602, and stir to mix well to obtain solution a;
[0063] B) dissolving 5 g of sodium dodecyl sulfate, 4 g of polyethylene glycol octylphenyl ether, and 8 g of polyether F127 dicarboxyl in 200 mL of deionized water to obtain solution b;
[0064] C) Mix solution a and solution b evenly, add 1 mol / L NaOH solution until the pH value of the solution is 8, and complete the reaction, filter and dry to obtain a porous hollow filler;
[0065] D) Dissolve 5 g of hexadecyltrimethylammonium bromide and 25 g of 1-butyl-3-methylimidazole chloride in 200 ml of deionized water, add 100 g of porous hollow filler, add 4 g of chitosan, 1 g of glutaraldehyde, and 10 g of acetic acid, perform hydrothermal reaction at 80 degrees Celsius, filter, and dry to obtain a modified porous hollow filler.
[0066] The fibrous filler is the same as that in Example 3.
[0067] Example 5
[0068] The reinforced self-supporting butterfly optical cable comprises a self-supporting suspension wire 1, a reinforcement member 2, an optical fiber 3 and a sheath 4, wherein the suspension wire 1, the reinforcement member 2 and the optical fiber 3 are all covered by the sheath 4, there are two reinforcement members 2, which are located on both sides of the optical fiber 3, and the suspension wire 1 is located on the side of one of the reinforcement members 2 away from the optical fiber 3; the material of the sheath comprises the following components by mass: 110 parts of polyethylene, 28 parts of ethylene-vinyl acetate copolymer, 12 parts of maleic anhydride, 13 parts of polybutylene succinate, 12 parts of modified porous hollow filler, 22 parts of fibrous filler, 5 parts of dioctyl phthalate, 5 parts of nitrile rubber, and 3 parts of antioxidant 1010.
[0069] The modified porous hollow filler is prepared by the following method:
[0070] A) Dissolve 200 g of ethyl orthosilicate in 50 mL of dichloromethane, add 100 g of KH602, and stir to mix well to obtain solution a;
[0071] B) dissolving 4 g of sodium dodecyl sulfate, 4 g of polyethylene glycol octylphenyl ether, and 6 g of polyether F127 dicarboxyl in 200 mL of deionized water to obtain solution b;
[0072] C) Mix solution a and solution b evenly, add 1 mol / L NaOH solution until the pH value of the solution is 8, and complete the reaction, filter and dry to obtain a porous hollow filler;
[0073] D) 8 g of hexadecyltrimethylammonium bromide and 20 g of 1-butyl-3-methylimidazole chloride were dissolved in 200 ml of deionized water, 100 g of porous hollow filler was added, 4 g of chitosan, 3 g of glutaraldehyde, and 10 g of acetic acid were added, and the reaction was completed by hydrothermal reaction at 80 degrees Celsius, filtered, and dried to obtain a modified porous hollow filler.
[0074] The fibrous filler is the same as that in Example 3.
[0075] Comparative Example 1
[0076] The reinforced self-supporting butterfly optical cable comprises a self-supporting suspension wire 1, a reinforcement member 2, an optical fiber 3 and a sheath 4, wherein the suspension wire 1, the reinforcement member 2 and the optical fiber 3 are all covered by the sheath 4, there are two reinforcement members 2, which are located on both sides of the optical fiber 3, and the suspension wire 1 is located on the side of one of the reinforcement members 2 away from the optical fiber 3; the material of the sheath comprises the following components by mass: 110 parts of polyethylene, 28 parts of ethylene-vinyl acetate copolymer, 12 parts of maleic anhydride, 13 parts of polybutylene succinate, 12 parts of modified porous hollow filler, 22 parts of fibrous filler, 5 parts of dioctyl phthalate, 5 parts of nitrile rubber, and 3 parts of antioxidant 1010.
[0077] The modified porous hollow filler is prepared by the following method:
[0078] A) Dissolve 200 g of ethyl orthosilicate in 50 mL of dichloromethane, add 100 g of KH602, and stir to mix well to obtain solution a;
[0079] B) dissolving 4 g of sodium dodecyl sulfate, 4 g of polyethylene glycol octylphenyl ether, and 6 g of polyether F127 dicarboxyl in 200 mL of deionized water to obtain solution b;
[0080] C) Mix solution a and solution b evenly, add 1 mol / L NaOH solution until the pH value of the solution is 8, and complete the reaction, filter and dry to obtain a porous hollow filler;
[0081] D) 8 g of hexadecyltrimethylammonium bromide was dissolved in 200 ml of deionized water, 100 g of porous hollow filler was added, 4 g of chitosan, 3 g of glutaraldehyde, and 10 g of acetic acid were added, and the reaction was completed by hydrothermal reaction at 80 degrees Celsius, filtered, and dried to obtain a modified porous hollow filler.
[0082] The fibrous filler is the same as that in Example 3.
[0083] Comparative Example 2
[0084] The reinforced self-supporting butterfly optical cable comprises a self-supporting suspension wire 1, a reinforcement member 2, an optical fiber 3 and a sheath 4, wherein the suspension wire 1, the reinforcement member 2 and the optical fiber 3 are all covered by the sheath 4, there are two reinforcement members 2, which are located on both sides of the optical fiber 3, and the suspension wire 1 is located on the side of one of the reinforcement members 2 away from the optical fiber 3; the material of the sheath comprises the following components by mass: 110 parts of polyethylene, 28 parts of ethylene-vinyl acetate copolymer, 12 parts of maleic anhydride, 13 parts of polybutylene succinate, 12 parts of modified porous hollow filler, 22 parts of fibrous filler, 5 parts of dioctyl phthalate, 5 parts of nitrile rubber, and 3 parts of antioxidant 1010.
[0085] The modified porous hollow filler is prepared by the following method:
[0086] A) Dissolve 200 g of ethyl orthosilicate in 50 mL of dichloromethane, add 100 g of KH602, and stir to mix well to obtain solution a;
[0087] B) dissolving 4 g of sodium dodecyl sulfate, 4 g of polyethylene glycol octylphenyl ether, and 6 g of polyether F127 dicarboxyl in 200 mL of deionized water to obtain solution b;
[0088] C) Mix solution a and solution b evenly, add 1 mol / L NaOH solution until the pH value of the solution is 8, and complete the reaction, filter and dry to obtain a porous hollow filler;
[0089] D) 8 g of hexadecyltrimethylammonium bromide and 20 g of 1-butyl-3-methylimidazole chloride were dissolved in 200 ml of deionized water, 100 g of porous hollow filler was added, 4 g of chitosan and 10 g of acetic acid were added, hydrothermally reacted at 80 degrees Celsius for completion, filtered and dried to obtain a modified porous hollow filler.
[0090] The fibrous filler is the same as that in Example 3.
[0091] Comparative Example 3
[0092] The reinforced self-supporting butterfly optical cable comprises a self-supporting suspension wire 1, a reinforcement member 2, an optical fiber 3 and a sheath 4, wherein the suspension wire 1, the reinforcement member 2 and the optical fiber 3 are all covered by the sheath 4, there are two reinforcement members 2, which are located on both sides of the optical fiber 3, and the suspension wire 1 is located on the side of one of the reinforcement members 2 away from the optical fiber 3; the material of the sheath comprises the following components by mass: 110 parts of polyethylene, 28 parts of ethylene-vinyl acetate copolymer, 12 parts of maleic anhydride, 13 parts of polybutylene succinate, 12 parts of modified porous hollow filler, 22 parts of fibrous filler, 5 parts of dioctyl phthalate, 5 parts of nitrile rubber, and 3 parts of antioxidant 1010.
[0093] The modified porous hollow filler is prepared by the following method:
[0094] A) Dissolve 200 g of ethyl orthosilicate in 50 mL of dichloromethane, add 100 g of KH602, and stir to mix well to obtain solution a;
[0095] B) dissolving 4 g of sodium dodecyl sulfate, 4 g of polyethylene glycol octylphenyl ether, and 6 g of polyether F127 dicarboxyl in 200 mL of deionized water to obtain solution b;
[0096] C) Mix solution a and solution b evenly, add 1 mol / L NaOH solution until the pH value of the solution is 8, and complete the reaction, filter and dry to obtain a porous hollow filler;
[0097] D) 8 g of hexadecyltrimethylammonium bromide and 20 g of 1-butyl-3-methylimidazole chloride were dissolved in 200 ml of deionized water, 100 g of porous hollow filler were added, 3 g of glutaraldehyde and 10 g of acetic acid were added, and the mixture was hydrothermally reacted at 80 degrees Celsius for completion, filtered and dried to obtain a modified porous hollow filler.
[0098] The fibrous filler is the same as that in Example 3.
[0099] Comparative Example 4
[0100] The reinforced self-supporting butterfly optical cable comprises a self-supporting suspension wire 1, a reinforcement member 2, an optical fiber 3 and a sheath 4, wherein the suspension wire 1, the reinforcement member 2 and the optical fiber 3 are all covered by the sheath 4, there are two reinforcement members 2, which are located on both sides of the optical fiber 3, and the suspension wire 1 is located on the side of one of the reinforcement members 2 away from the optical fiber 3; the material of the sheath comprises the following components by mass: 110 parts of polyethylene, 28 parts of ethylene-vinyl acetate copolymer, 12 parts of maleic anhydride, 13 parts of polybutylene succinate, 12 parts of modified porous hollow filler, 22 parts of fibrous filler, 5 parts of dioctyl phthalate, 5 parts of nitrile rubber, and 3 parts of antioxidant 1010.
[0101] The modified porous hollow filler is prepared by the following method:
[0102] A) Dissolve 200 g of ethyl orthosilicate in 50 mL of dichloromethane, add 100 g of KH602, and stir to mix well to obtain solution a;
[0103] B) dissolving 4 g of sodium dodecyl sulfate, 4 g of polyethylene glycol octylphenyl ether, and 6 g of polyether F127 dicarboxyl in 200 mL of deionized water to obtain solution b;
[0104] C) Mix solution a and solution b evenly, add 1 mol / L NaOH solution until the pH value of the solution is 8, and complete the reaction, filter and dry to obtain a porous hollow filler;
[0105] D) 8 g of hexadecyltrimethylammonium bromide and 20 g of 1-butyl-3-methylimidazole chloride were dissolved in 200 ml of deionized water, 100 g of porous hollow filler was added, 4 g of chitosan, 3 g of glutaraldehyde, and 10 g of acetic acid were added, and the reaction was completed by hydrothermal reaction at 80 degrees Celsius, filtered, and dried to obtain a modified porous hollow filler.
[0106] The fibrous filler is prepared by the following method:
[0107] 10 g of carbon nanofibers with a diameter of 40 μm were added to 200 ml of a 2.5 mol / L nitric acid aqueous solution, subjected to hydrothermal reaction at 75° C. for 8 h, filtered, washed with deionized water, and dried at 80° C. to obtain activated carbon nanofibers; 10 g of activated carbon nanofibers were added to 200 ml of a 3 wt% ethanol solution of butyl titanate, 10 g of acetic acid was added, subjected to hydrothermal reaction at 75° C. for 6 h, filtered, washed with deionized water, dried at 80° C., and heated in a tubular furnace to 670° C. and calcined for 4 h to obtain a filler.
[0108] Comparative Example 5
[0109] The reinforced self-supporting butterfly optical cable comprises a self-supporting suspension wire 1, a reinforcement member 2, an optical fiber 3 and a sheath 4, wherein the suspension wire 1, the reinforcement member 2 and the optical fiber 3 are all covered by the sheath 4, there are two reinforcement members 2, which are located on both sides of the optical fiber 3, and the suspension wire 1 is located on the side of one of the reinforcement members 2 away from the optical fiber 3; the material of the sheath comprises the following components by mass: 110 parts of polyethylene, 28 parts of ethylene-vinyl acetate copolymer, 12 parts of maleic anhydride, 13 parts of polybutylene succinate, 12 parts of modified porous hollow filler, 22 parts of fibrous filler, 5 parts of dioctyl phthalate, 5 parts of nitrile rubber, and 3 parts of antioxidant 1010.
[0110] The modified porous hollow filler is prepared by the following method:
[0111] A) Dissolve 200 g of ethyl orthosilicate in 50 mL of dichloromethane, add 100 g of KH602, and stir to mix well to obtain solution a;
[0112] B) dissolving 4 g of sodium dodecyl sulfate, 4 g of polyethylene glycol octylphenyl ether, and 6 g of polyether F127 dicarboxyl in 200 mL of deionized water to obtain solution b;
[0113] C) Mix solution a and solution b evenly, add 1 mol / L NaOH solution until the pH value of the solution is 8, and complete the reaction, filter and dry to obtain a porous hollow filler;
[0114] D) 8 g of hexadecyltrimethylammonium bromide and 20 g of 1-butyl-3-methylimidazole chloride were dissolved in 200 ml of deionized water, 100 g of porous hollow filler was added, 4 g of chitosan, 3 g of glutaraldehyde, and 10 g of acetic acid were added, and the reaction was completed by hydrothermal reaction at 80 degrees Celsius, filtered, and dried to obtain a modified porous hollow filler.
[0115] The fibrous filler is prepared by the following method:
[0116] 10 g of carbon nanofibers with a diameter of 40 μm were added to 200 ml of a 2.5 mol / L nitric acid aqueous solution, and subjected to hydrothermal reaction at 75° C. for 8 h. The mixture was filtered, washed with deionized water, and dried at 80° C. to obtain activated carbon nanofibers. 10 g of activated carbon nanofibers, 8 g of 1-butyl-3-methylimidazole bromide, and 5 g of polyethylene glycol were added to 100 ml of N,N-dimethylformamide and mixed evenly. 1.5 g of azobisisobutyronitrile and 1.5 g of stannous isooctanoate were added, stirred evenly, and allowed to stand for 30 min. The mixture was then subjected to hydrothermal reaction at 80° C. for 4 h. The mixture was filtered, washed with deionized water, and dried at 80° C. to obtain a filler.
[0117] Comparative Example 6
[0118] The reinforced self-supporting butterfly optical cable comprises a self-supporting suspension wire 1, a reinforcement member 2, an optical fiber 3 and a sheath 4, wherein the suspension wire 1, the reinforcement member 2 and the optical fiber 3 are all covered by the sheath 4, there are two reinforcement members 2, which are located on both sides of the optical fiber 3, and the suspension wire 1 is located on the side of one of the reinforcement members 2 away from the optical fiber 3; the material of the sheath comprises the following components by mass: 110 parts of polyethylene, 28 parts of ethylene-vinyl acetate copolymer, 12 parts of maleic anhydride, 13 parts of polybutylene succinate, 12 parts of modified porous hollow filler, 22 parts of fibrous filler, 5 parts of dioctyl phthalate, 5 parts of nitrile rubber, and 3 parts of antioxidant 1010.
[0119] The modified porous hollow filler is prepared by the following method:
[0120] A) Dissolve 200 g of ethyl orthosilicate in 50 mL of dichloromethane, add 100 g of KH602, and stir to mix well to obtain solution a;
[0121] B) dissolving 4 g of sodium dodecyl sulfate, 4 g of polyethylene glycol octylphenyl ether, and 6 g of polyether F127 dicarboxyl in 200 mL of deionized water to obtain solution b;
[0122] C) Mix solution a and solution b evenly, add 1 mol / L NaOH solution until the pH value of the solution is 8, and complete the reaction, filter and dry to obtain a porous hollow filler;
[0123] D) 8 g of hexadecyltrimethylammonium bromide and 20 g of 1-butyl-3-methylimidazole chloride were dissolved in 200 ml of deionized water, 100 g of porous hollow filler was added, 4 g of chitosan, 3 g of glutaraldehyde, and 10 g of acetic acid were added, and the reaction was completed by hydrothermal reaction at 80 degrees Celsius, filtered, and dried to obtain a modified porous hollow filler.
[0124] The fibrous filler is prepared by the following method:
[0125] 10g of carbon nanofibers with a diameter of 40 microns were added to 200ml of 2.5mol / L nitric acid aqueous solution, and after hydrothermal reaction at 75°C for 8h, filtered, washed with deionized water, and dried at 80°C to obtain activated carbon nanofibers; 10g of activated carbon nanofibers were added to 200ml of 3wt% butyl titanate ethanol solution, 10g of acetic acid was added, hydrothermal reaction was carried out at 75°C for 6h, filtered, washed with deionized water, dried at 80°C, and heated to 670°C in a tubular furnace for calcination for 4h; 10g of the product was taken, added to 8g of 1-butyl-3-methylimidazole bromide in 100ml of N,N-dimethylformamide and mixed evenly, 1.5g of azobisisobutyronitrile and 1.5g of stannous isooctanoate were added, stirred evenly and allowed to stand for 30min, then hydrothermally reacted at 80°C for 4h, filtered, washed with deionized water, and dried at 80°C to obtain filler.
[0126] Comparative Example 7
[0127] The reinforced self-supporting butterfly optical cable comprises a self-supporting suspension wire 1, a reinforcement member 2, an optical fiber 3 and a sheath 4, wherein the suspension wire 1, the reinforcement member 2 and the optical fiber 3 are all covered by the sheath 4, there are two reinforcement members 2, which are located on both sides of the optical fiber 3, and the suspension wire 1 is located on the side of one of the reinforcement members 2 away from the optical fiber 3; the material of the sheath comprises the following components by mass: 110 parts of polyethylene, 28 parts of ethylene-vinyl acetate copolymer, 12 parts of maleic anhydride, 13 parts of polybutylene succinate, 12 parts of modified porous hollow filler, 22 parts of fibrous filler, 5 parts of dioctyl phthalate, 5 parts of nitrile rubber, and 3 parts of antioxidant 1010.
[0128] The modified porous hollow filler is prepared by the following method:
[0129] A) Dissolve 200 g of ethyl orthosilicate in 50 mL of dichloromethane, add 100 g of KH602, and stir to mix well to obtain solution a;
[0130] B) dissolving 4 g of sodium dodecyl sulfate, 4 g of polyethylene glycol octylphenyl ether, and 6 g of polyether F127 dicarboxyl in 200 mL of deionized water to obtain solution b;
[0131] C) Mix solution a and solution b evenly, add 1 mol / L NaOH solution until the pH value of the solution is 8, and complete the reaction, filter and dry to obtain a porous hollow filler;
[0132] D) 8 g of hexadecyltrimethylammonium bromide and 20 g of 1-butyl-3-methylimidazole chloride were dissolved in 200 ml of deionized water, 100 g of porous hollow filler was added, 4 g of chitosan, 3 g of glutaraldehyde, and 10 g of acetic acid were added, and the reaction was completed by hydrothermal reaction at 80 degrees Celsius, filtered, and dried to obtain a modified porous hollow filler.
[0133] The fibrous filler is prepared by the following method:
[0134] 10g of carbon nanofibers with a diameter of 40 microns were added to 200ml of 2.5mol / L nitric acid aqueous solution, and after hydrothermal reaction at 75°C for 8h, filtered, washed with deionized water, and dried at 80°C to obtain activated carbon nanofibers; 10g of activated carbon nanofibers were added to 200ml of 3wt% ethanol solution of butyl titanate, 10g of acetic acid was added, hydrothermal reaction was carried out at 75°C for 6h, filtered, washed with deionized water, dried at 80°C, and heated to 670°C in a tubular furnace and calcined for 4h; 10g of the product was taken, added with 5g of polyethylene glycol to 100ml of N,N-dimethylformamide and mixed evenly, 1.5g of azobisisobutyronitrile and 1.5g of stannous isooctanoate were added, stirred evenly and allowed to stand for 30min, then hydrothermally reacted at 80°C for 4h, filtered, washed with deionized water, and dried at 80°C to obtain filler.
[0135] Experiments and Data
[0136] The tensile strength and environmental stress cracking time of the sheath material are tested in accordance with the national standard GB / T2951.
[0137] The wear resistance performance refers to the standard GB / T17737.324-2018 "Mechanical test methods for coaxial communication cables - Cable wear resistance test" to measure the loss mass of the specimen after 500 cycles.
[0138] The results are shown in Table 1.
[0139] Table 1
[0140]
[0141] Tests and Results
[0142] Table 1 shows the corresponding effects of the components in the preparation process. The surface modification of the porous silica filler by the ionic liquid 1-butyl-3-methylimidazole chloride, chitosan, and the crosslinking agent glutaraldehyde can greatly improve the affinity between the porous filler and the polymer. At the same time, the present invention uses the spherical porous filler and the fiber filler in combination, which not only improves the tensile strength of the material but also improves the wear resistance of the material.
[0143] Modified fiber material, titanium dioxide particles are modified on the surface of carbon fiber, and a cross-linked coating is formed on the surface of carbon fiber by polyionic liquid 1-butyl-3-methylimidazole bromide and polyethylene glycol. The coating is firm on the carbon surface and not easy to fall off, so that bulges can be formed on the surface of the carbon fiber, which produces an anchoring effect in the sheath, slows down the slippage of carbon fiber in the sheath layer, and the modified carbon fiber filler increases the mechanical strength of the sheath layer.
[0144] Although the content of the present invention has been described in detail through the above preferred embodiments, the above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A reinforced self-supporting butterfly optical cable, comprising a self-supporting suspension wire, a reinforcement member, an optical fiber and a sheath, wherein the suspension wire, the reinforcement member and the optical fiber are all covered by the sheath, the reinforcement member has two pieces and is located on both sides of the optical fiber, the suspension wire is located on the side of one of the reinforcement members away from the optical fiber, and is characterized in that: The material of the sheath includes the following components by mass: 100-120 parts of polyethylene, 25-30 parts of ethylene-vinyl acetate copolymer, 10-15 parts of maleic anhydride, 10-15 parts of polybutylene succinate, 10-15 parts of modified porous hollow filler, 20-25 parts of fibrous filler, 3-6 parts of plasticizer, 3-6 parts of toughening agent, and 2-3 parts of antioxidant; The modified porous hollow filler is prepared by the following method: A) Dissolve 200 g of ethyl orthosilicate in 50 mL of dichloromethane, add 100 g of KH602, and stir to mix well to obtain solution a; B) dissolving 4-6 g of sodium dodecyl sulfate, 2-4 g of polyethylene glycol octylphenyl ether, and 6-8 g of polyether F127 dicarboxyl in 200 mL of deionized water to obtain solution b; C) Mix solution a and solution b evenly, add 1 mol / L NaOH solution until the pH value of the solution is 8-9, react completely, filter and dry to obtain a porous hollow filler; D) dissolving 5-8g of hexadecyltrimethylammonium bromide and 20-25g of 1-butyl-3-methylimidazole chloride in 200ml of deionized water, adding 100g of porous hollow filler, adding 2-4g of chitosan, 1-3g of glutaraldehyde, and 10g of acetic acid, hydrothermally reacting at 70-80 degrees Celsius to complete, filtering, and drying to obtain a modified porous hollow filler; The fibrous filler is prepared by the following method: A) Add 10g of carbon nanofibers to 200ml of 2-3mol / L nitric acid aqueous solution, perform hydrothermal reaction at 70-80℃ for 6-10h, filter, wash and dry to obtain activated carbon nanofibers; B) adding 10g of activated carbon nanofibers to 200ml of ethanol solution of butyl titanate with a mass fraction of 2-4wt%, adding 10g of acetic acid, hydrothermally reacting at 70-80℃ for 5-10h, filtering, washing, drying, heating to 650-700℃ and calcining for 3-5h; C) Take 10g of the product of step B, add 5-10g of 1-butyl-3-methylimidazole bromide and 4-6g of polyethylene glycol into 100ml of N,N-dimethylformamide and mix evenly, add 1-2g of azobisisobutyronitrile and 1-2g of stannous isooctanoate, stir evenly and let stand for 10-60min, then hydrothermally react at 70-90℃ for 3-6h, filter, wash and dry to obtain the product.
2. A reinforced self-supporting butterfly optical cable as claimed in claim 1, characterized in that: The plasticizer is selected from one or a combination of dioctyl phthalate, butyl benzyl phthalate, dicyclohexyl phthalate, dibutyl phthalate, diisobutyl phthalate, dimethyl phthalate, and diethyl phthalate.
3. A reinforced self-supporting butterfly optical cable as claimed in claim 1, characterized in that: The toughening agent is selected from one or a combination of nitrile rubber and polysulfide rubber.
4. A reinforced self-supporting butterfly optical cable as claimed in claim 1, characterized in that: The antioxidant is antioxidant 1010.