Preparation method of internally cured composite gel and its application in high performance concrete
By internally curing composite gel in high-performance concrete, the composite gel skeleton prepared by 3D printing solves the problem of autogenous shrinkage of high-performance concrete caused by low water-cement ratio, achieves higher mechanical properties and durability, and adopts Green and environmentally friendly materials.
Patent Information
- Application Number
- CN202410951146.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-10-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
High-performance concrete caused by low water-cement ratio undergoes autodrying shrinkage in the early stage of hydration, resulting in reduced internal humidity, capillary tension and autogenous shrinkage, and then micro-cracks appear, affecting its mechanical properties and durability.
Internally cured composite gel is used to prepare a composite gel skeleton through 3D printing. Sodium alginate and calcium chloride are used to cross-link to form a composite gel, which is internally cured in high-performance concrete to serve as a water storage carrier to reduce the concrete's damage. Autogenous shrinkage rate.
It effectively controls the internal humidity of the concrete, enhances the water-locking function of the gel, improves the mechanical properties of the concrete, reduces the autogenous shrinkage rate, and uses natural polymer materials, which is green and environmentally friendly and overcomes the storage problems of traditional water storage materials. Problems of poor water quality and poor pore filling ability.
Smart Images

Figure CN118479771B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building materials, in particular to a preparation method of an internally cured composite gel and application thereof in high performance concrete. Background Art
[0002] At present, concrete is the largest and most important construction material. High-performance concrete has better mechanical properties, volume stability and durability. Therefore, it is widely used in foundation engineering construction. However, due to the low water-cement ratio, high-performance concrete undergoes self-shrinkage in the early stage of hydration. Under the hydration of cement, the internal humidity is significantly reduced, which causes capillary tension and self-shrinkage of concrete. The viscosity and cohesion of the hydrated gel inside the concrete in the early stage of hydration are poor, and it cannot resist these internal stresses, resulting in microcracks. These inherent microcracks are undoubtedly hidden dangers in the concrete load-bearing process. As we all know, hardened concrete has a dense and complex pore structure and a low permeability coefficient, which makes the external high-humidity curing used in the project only increase the internal humidity to a certain extent, thereby reducing the shrinkage of high-performance concrete.
[0003] To solve this type of engineering problem, researchers proposed a new concept of internal curing of high-performance concrete, and selected inorganic porous coarse aggregate and organic water-absorbing resin (SAP) as water storage carriers, which were mixed inside high-performance concrete to delay the loss of humidity or internal water. Porous coarse aggregates are mainly porous ceramsite, hollow microspheres and zeolite, which have weak water absorption capacity and release water faster; water-absorbing resins are directly mixed into fresh concrete to absorb mixing water during mixing. However, commercial highly absorbent resins will affect the fluidity of concrete, and the voids left after complete water release will have a negative impact on the mechanical properties and durability of concrete. In addition, researchers proposed using hydrofluoric acid-corroded hollow floating beads as internal curing capsules, and using the concentration and time of the corrosive liquid to regulate the size of the water-passing channels of the floating beads, so as to control the water release rate of the capsules, more effectively balance the internal humidity of the concrete, and reduce shrinkage. However, this preparation process is complicated, has low yield, and is contrary to green environmental protection, so it is not recommended for large-scale application. In view of the current research progress, we are forced to actively develop new multifunctional composite gels to solve the engineering problems caused by the large shrinkage of high-performance concrete. Summary of the invention
[0004] Technical problems solved by the present invention:
[0005] It is used to solve the technical problem of high shrinkage of high performance concrete caused by low water-cement ratio.
[0006] The technical solution adopted by the present invention is:
[0007] In view of the above technical problems, the purpose of the present invention is to provide a method for preparing an internally cured composite gel and its application in high performance concrete. The specific contents are as follows:
[0008] First, the present invention adopts an internally cured composite gel, which is applied to high-performance concrete. The composite gel skeleton is loaded with substance A, and substance B is cross-linked with substance A to form a composite gel; substance A includes sodium alginate, and substance B includes calcium chloride.
[0009] According to some embodiments, the material of the skeleton is thermoplastic PLA.
[0010] According to some embodiments, the mass concentration of substance A is 0.5-3%, and more preferably 2%.
[0011] According to some embodiments, the mass concentration of substance B is 6-14%, more preferably 10%.
[0012] According to some embodiments, the skeleton comprises the following features:
[0013] (1) The skeleton is formed by 3D printing. The composite gel skeleton is designed using 3D modeling software (such as Shapr3D). After setting the internal filling rate of the skeleton on the 3D printer, printing is performed. Here, the internal filling rate can be selected from 30% to 70%, or 30%, 50% and 70%.
[0014] (2) The shape of the skeleton is C60, and the diameter is 3~5mm;
[0015] (3) The shape of the skeleton is filled fiber; when the filling material is steel fiber, the slenderness ratio is 5:1, the fiber length is 5 mm, and the bottom diameter is 1 mm;
[0016] (4) The shape of the skeleton is aggregate, which can be designed to mimic the size of river sand aggregate with a particle size of ≤5 mm.
[0017] In the above, the skeleton is preferably filled fiber, the filled fiber is a rod-shaped structure, and the filling rate is preferably 50%.
[0018] Second, the present invention provides a method for preparing the internally cured composite gel as described above, comprising the following steps:
[0019] After the skeleton material is immersed in solution A, it is immersed in solution B and cured to obtain an internally cured composite gel. To expand, that is to say: the printed composite gel skeleton is completely immersed in solution A, then placed in a vacuum dryer for vacuuming, and then the excess liquid on the surface is removed by a cement negative pressure sieve analyzer; the saturated composite gel skeleton is taken out and placed in solution B for curing, and then lightly stirred and taken out. The internally cured composite gel is subjected to negative pressure degassing treatment and stored in a moisturizing box for later use.
[0020] If substance A is sodium alginate, place the sodium alginate powder in warm deionized water, fully dissolve it with a magnetic stirrer, and let it stand until there are no bubbles in the liquid medium.
[0021] Third, the present invention provides an application of the internally cured composite gel as described above in high performance concrete.
[0022] Fourthly, the present invention provides a micro-expansive high-performance concrete, comprising the internally cured composite gel as described above. Specifically, it is:
[0023] The components of micro-expansive high-performance concrete include: cement, aggregate, water, internal curing composite gel, water reducing agent = 500~650:1200~1700:150~350:50~75:1~8. Portland cement is used for cement; river sand is used for aggregate; polycarboxylic acid water reducing agent is used for water reducing agent, and the water reducing rate is ≥40%. The amount of internal curing composite gel added = m (cement hydration water requirement) - m (mixing water), where the cement hydration water requirement refers to the water required for the cement to be fully hydrated.
[0024] The technical mechanism and beneficial effects adopted by the present invention are as follows:
[0025] (1) The internally cured composite gel provided by the present invention can realize the flexible design of the gel skeleton, and improve its water locking function by enriching the skeleton network space; and remove the interstitial water retained between the gel skeletons, which is beneficial to quantitatively control the effective water content of the internally cured composite gel of high-performance concrete.
[0026] (2) The internally cured composite gel provided by the present invention overcomes the shortcomings of low mechanical strength and easy deformation of bio-type hydrogels; it plays a role in supporting the hydrogel inside the concrete, solving the key problem that the holes left after the hydrogel releases water lead to the degradation of concrete performance.
[0027] (3) The internally solidified composite gel provided by the present invention is a natural polymer material that is cheap, green and environmentally friendly and has sustainable performance characteristics. In addition, the alginate gel can cross-link and seal free water, has the function of retaining moisture and releasing water in cement paste, and has a certain regulating function on cement hydration, so as to promote the internally solidified composite gel to not only retain moisture and release water, but also has the function of regulating cement hydration and hardening.
[0028] (4) The internally cured composite gel provided by the present invention overcomes the practical problems of poor water storage and poor in-situ pore filling capacity of traditional water storage materials, and achieves the shrinkage reduction goal of low water-cement ratio concrete, providing a new idea and solution for the successful preparation of micro-expansive high-performance concrete. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1Schematic diagram of the design of the internally cured composite gel. DETAILED DESCRIPTION
[0030] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0031] Examples 1-9
[0032] A 3D printed lightweight and high-strength skeleton is used as the gel skeleton (PLA), with 3 shapes and 3 filling rates. Rods, spheres and particle sizes are similar to river sand, about 3-5mm. The water carrying capacity of the gel is determined by the filling rate of the internally cured composite gel, which is about 30%-70%. The water-cement ratio of high-performance concrete is 0.35, and the cement selected is silicate cement PO 42.5. The specific steps are as follows:
[0033] Step 1: According to Figure 1 The design is output in stl. file format; a light and high-strength skeleton is made by a digital display micro 3D printer. The gel skeleton of river sand morphology is not given. This is because the shape of the actual aggregate in practical applications is uncertain and unknown;
[0034] Step 2: Place the gel skeleton in a 2% sodium alginate solution, use a vacuum filter to filter to a negative pressure state and maintain for 4 hours; immediately pick it up, invert it in a 10% calcium chloride solution, and stir it slowly clockwise with a glass rod for 1 minute. Pick up the internally solidified composite gel and drain it;
[0035] Step 3: Use the cement negative pressure sieving instrument to remove the adhering water and put it into a moisturizing bag for later use. For long-term storage of the internally cured composite gel, the moisturizing bag should be placed in a temperature and humidity box with a humidity of 95%, and it can be stored for one week to half a month.
[0036] Step 4: According to the formulation of high performance concrete as shown in Table 1 (gel core material refers to calcium alginate gel, and internally cured composite gel refers to calcium alginate composite gel with a PLA skeleton), refer to GB / T 1346-2011 to prepare Examples 1-9, and mix the internally cured composite gel with domestic water for use as mixing water.
[0037] Examples 10-18
[0038] A 3D printed lightweight and high-strength skeleton is used as the gel skeleton (PLA), with 3 shapes and 3 filling rates. Rod-shaped, spherical and particle sizes are similar to river sand, about 3-5mm. The water carrying capacity of the gel is determined by the filling rate of the internally cured composite gel, which is about 30%-70%. The water-cement ratio of high-performance concrete is 0.35, and the cement used is sulphoaluminate cement. The specific steps are as follows:
[0039] Step 1: According to Figure 1 The design is exported in stl. file format; a light and high-strength skeleton is made using a digital display micro 3D printer. The gel skeleton of river sand morphology is not given because the shape of the actual aggregate in practical applications is uncertain and unknown;
[0040] Step 2: Place the gel skeleton in a 2% sodium alginate solution, use a vacuum filter to filter to a negative pressure state and maintain for 4 hours; immediately pick it up, invert it in a 10% calcium chloride solution, and stir it slowly clockwise with a glass rod for 1 minute. Pick up the internally solidified composite gel and drain it;
[0041] Step 3: Use the cement negative pressure sieving instrument to remove the adhering water and put it into a moisturizing bag for later use. For long-term storage of the internally cured composite gel, the moisturizing bag should be placed in a temperature and humidity box with a humidity of 95%, and it can be stored for one week to half a month.
[0042] Step 4: According to the formulation of high performance concrete as shown in Table 2 (gel core material refers to calcium alginate gel, and internally cured composite gel refers to calcium alginate composite gel with a PLA skeleton), refer to GB / T 1346-2011 to prepare Examples 1-9, and mix the internally cured composite gel with domestic water for use as mixing water.
[0043] Comparative Examples 1-3
[0044] The water-cement ratio of high-performance concrete is selected as 0.35, the cement is silicate cement PO 42.5, and the gel core material is biological calcium alginate gel. The specific steps are as follows:
[0045] (1) Steps of Comparative Examples 1 and 3
[0046] Step 1: According to the high performance concrete formulation as shown in Table 1, comparative examples 1 and 3 were prepared with reference to the specification GB / T 1346-2011.
[0047] (2) Steps of Comparative Example 2:
[0048] Step 1: Inject 2% sodium alginate solution into a medical syringe, and inject it into 10% calcium chloride solution using a micro-medical syringe. Stir slowly clockwise for 1 minute with a glass rod. Then use a colander to scoop up the gel core and drain.
[0049] Step 2: Use a cement negative pressure sieving instrument to filter the solution in the gaps of the gel core material and put it into a moisturizing bag for later use. For long-term storage of the gel core material, the moisturizing bag should be placed in a temperature and humidity box with a humidity of 95%, which can be stored for one week to half a month.
[0050] Step 3: According to the formulation of high performance concrete as shown in Table 3 (gel core material refers to calcium alginate gel), reference is made to the specification GB / T 1346-2011 to prepare comparative example 2. The gel core material and domestic water are mixed together and used as mixing water.
[0051] Comparative Examples 4-6
[0052] The water-cement ratio of high-performance concrete is selected as 0.35, the cement is aluminate cement, and the gel core material is biological calcium alginate gel. The specific steps are as follows:
[0053] (1) Steps of Comparative Examples 4 and 6:
[0054] Step 1: According to the high performance concrete formulation as shown in Table 1, comparative examples 4 and 6 were prepared with reference to the specification GB / T 1346-2011.
[0055] (2) Steps of Comparative Example 5:
[0056] Step 1: Inject 2% sodium alginate solution into a medical syringe, and inject it into 10% calcium chloride solution using a micro medical syringe. Stir slowly clockwise for 1 minute with a glass rod. Then use a colander to scoop up the solidified gel core and drain.
[0057] Step 2: Use a cement negative pressure sieving instrument to filter the solution in the gaps of the gel core material and put it into a moisturizing bag for later use. For long-term storage of the gel core material, the moisturizing bag should be placed in a temperature and humidity box with a humidity of 95%, which can be stored for one week to half a month.
[0058] Step 3: According to the formulation of high performance concrete as shown in Table 4 (gel core material refers to calcium alginate gel), comparative example 5 was prepared with reference to specification GB / T 1346-2011, and the gel core material and domestic water were mixed together and used as mixing water.
[0059] Test example
[0060] The samples prepared in Examples 1-18 and Comparative Examples 1-9 were measured.
[0061] Determination indicators:
[0062] (1) Prepare concrete according to GB / T 1346-2011 and measure the compressive strength using a press;
[0063] (2) Prepare cement mortar autogenous shrinkage specimens according to ASTM C1698-09 and measure the autogenous shrinkage.
[0064] The measurement results are shown in Table 5.
[0065] Table 1 Allocation ratio of each group in Examples 1-9
[0066]
[0067] Table 2 Allocation ratio of each group in Examples 10-18
[0068]
[0069] Table 3 Allocation ratio of each group of comparative examples 1-3
[0070]
[0071] Table 4 Allocation ratio of each group of comparative examples 4-6
[0072]
[0073] Table 5 Measurement results (Comparative example is represented by D, and Example is represented by E)
[0074]
[0075] From the results in Table 5, we can see that:
[0076] In the research system of silicate cement, adding gel core material can effectively adjust the internal humidity of high-performance concrete and cause micro-expansion, solving the problem of high shrinkage caused by low water-cement ratio. Using 3D printed composite gel skeleton as supporting gel core material is conducive to improving the mechanical strength of gel core material and maximally compensating for the strength loss caused by water release voids.
[0077] Based on this, the present invention uses the filling rate and shape of the internally cured composite gel as dual variables to study the intrinsic relationship between its autogenous shrinkage performance and strength. A higher filling rate is beneficial to improving the mechanical properties of the gel skeleton and enhancing the reinforcing effect of the skeleton; at the same time, a higher filling rate reduces the space for storing the gel core material, increases the river sand replacement rate, reduces the utilization rate of river sand, and increases the cost. In terms of shape, the shape of the 3D printed internally cured composite gel has no obvious effect on the compressive strength, and the rod-shaped structure is more conducive to improving the toughness and bending resistance of concrete. In the preferred case, the water-cement ratio is 0.35, the filling rate of the internally cured composite gel is 50%, and compared with no curing agent, the flexural strength of the rod-shaped internally cured composite gel is reduced by 1.97%, the compressive strength is reduced by 7.27%, and the autogenous shrinkage rate is reduced by 132.36%; compared with the curing agent with only the gel core material, the flexural strength of the rod-shaped internally cured composite gel is increased by 35.20%, the compressive strength is increased by 10.69%, and the autogenous shrinkage rate is reduced by 8.98%.
[0078] In the sulphoaluminate cement system, the addition of gel core material can effectively adjust the internal humidity of high-performance concrete and cause micro-expansion, thus avoiding the high self-shrinkage problem of rapid-hardening cement. Using 3D-printed internally cured composite gel to support the gel core material is beneficial to improving the mechanical strength of the internally cured composite gel and maximally compensating for the strength loss caused by water release voids. Based on this, the present invention uses the filling rate and shape of the internally cured composite gel as dual variables to study the intrinsic connection between its self-shrinkage performance and strength. A higher filling rate is beneficial to improving the mechanical properties of the internally cured capsule and optimizing the skeleton effect of the composite gel; at the same time, a higher filling rate reduces the space for storing the gel core material, increases the river sand replacement rate, reduces the utilization rate of river sand, and increases costs. In terms of shape, the shape of the 3D-printed internally cured composite gel has no obvious effect on the compressive strength, and the rod-like structure is more conducive to improving the toughness and bending resistance of concrete. In the preferred case, the water-cement ratio is 0.35, the filling rate of the internal curing capsule is 50%, and compared with the curing agent without curing agent, the flexural strength of the rod-shaped internal curing composite gel is reduced by 1.97%, the compressive strength is reduced by 7.27%, and the autogenous shrinkage rate is reduced by 90.17%; compared with the curing agent with only gel core material, the flexural strength of the rod-shaped internal curing composite gel is increased by 20.01%, the compressive strength is reduced by 1.16%, and the autogenous shrinkage rate is increased by 0.96%.
[0079] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. An internally cured composite gel for concrete, characterized in that: The composite gel skeleton is loaded with substance A, and substance B is used to cross-link substance A to form a composite gel; substance A includes sodium alginate, and substance B includes calcium chloride; The skeleton is formed by 3D printing, and the skeleton includes any one of the features (1) to (3): (1) The shape of the skeleton is C60, and the diameter is 3~5mm; (2) The shape of the skeleton is steel fiber, the slenderness ratio of the steel fiber is 5:1, the fiber length is 5 mm, and the bottom diameter is 1 mm; (3) The shape of the skeleton is aggregate, with a particle size of ≤5 mm; The material of the skeleton is thermoplastic PLA; the internal filling rate of the skeleton is 30~70%.
2. The internally cured composite gel for concrete according to claim 1, characterized in that: The mass concentration of substance A is 0.5~3%.
3. The internally cured composite gel for concrete according to claim 1, characterized in that: The mass concentration of substance B is 6~14%.
4. The method for preparing an internally cured composite gel for concrete according to any one of claims 1 to 3, characterized in that: The steps include: The skeleton material is immersed in solution A and dried to obtain an intermediate, which is then immersed in solution B for solidification and then subjected to negative pressure evacuation to obtain an internally solidified composite gel.
5. Use of the internally cured composite gel for concrete as claimed in any one of claims 1 to 3 in high performance concrete.
6. A micro-expansive high-performance concrete, characterized in that: The invention comprises the internally-cured composite gel for concrete as claimed in any one of claims 1 to 3.