A composite sodium ion battery material and its preparation method and application

The surface of the polyanionic precursor is coated by combining inorganic carbon particles and organic carbon, and the particle size and morphology are regulated during spray drying and vapor deposition, which solves the complex preparation of polyanionic powder materials in the prior art. Problem, the preparation of composite sodium ion battery materials with high rate performance and structural stability is suitable for mass production.

CN118495498BActive Publication Date: 2024-11-12ZONKE SENO TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410957442.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-12
Estimated Expiration
2044-07-17

AI Technical Summary

Technical Problem

The existing preparation methods for polyanionic powder materials have problems such as the use of toxic and harmful chelating agents, complex processes, large energy consumption and poor material consistency, making it difficult to prepare a composite sodium ion battery material with uniform, low cost and good rate performance.

Method used

The surface of the polyanion's precursor powder is coated by combining inorganic carbon particles and soluble organic carbon, and the particle size and morphology are regulated during spray drying and vapor deposition to form a three-dimensional network structure to prepare composite sodium ion battery materials.

Benefits of technology

It realizes the preparation of composite sodium ion battery materials that are simple to operate, low cost and environmentally friendly, improves the rate performance and structural stability of the material, and is suitable for mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118495498B_ABST
    Figure CN118495498B_ABST
Patent Text Reader

Abstract

The present invention discloses a composite sodium ion battery material and a preparation method and application thereof; wherein the preparation method of the composite sodium ion battery material comprises the following steps: S1, uniformly mixing a precursor source, a dispersant, an inorganic carbon source, an organic carbon source and a solvent to obtain a precursor mixture; the precursor source comprises a sodium source, a transition metal source and an anion source; S2, removing the solvent in the precursor mixture prepared in step S1 by spray drying to obtain a precursor intermediate; S3, pre-sintering the precursor intermediate prepared in step S2 in an inert gas, and performing secondary sintering on the pre-sintered product in a mixed gas to obtain the composite sodium ion battery material; the mixed gas comprises an inert gas and an organic small molecule gas carbon source. The present invention utilizes the combination of the inorganic carbon source and the organic carbon source in the precursor mixture to control the morphology and particle size of the powder, and further improves the rate performance of the battery material in combination with the vapor deposition method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of battery material preparation, and in particular to a composite sodium ion battery material and a preparation method and application thereof. Background Art

[0002] There are many methods for synthesizing polyanion powder materials. Common methods for preparing polyanion powder materials include sol-gel method, solvothermal method and high-temperature solid-phase method. Among them, the preparation method of sol-gel often requires the use of toxic and harmful chelating agents or initiators, and the post-processing process is very difficult, which is not in line with the green and environmentally friendly production concept. The preparation process of the solvothermal method is very complicated, the organic solvent used is expensive, the energy consumption of the preparation process is large, the phase formation process of the polyanion powder material is relatively complicated and the intermediate process is uncontrollable. The high-temperature solid-phase method has the defects of high synthesis temperature, uneven mixing of precursor raw materials, poor rate performance, and poor consistency of synthesized materials.

[0003] Therefore, at this stage, there is an urgent need for a polyanion powder material with a multidimensional structure that is uniformly carbon-coated, simple to synthesize, low cost, and has good rate performance. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a composite sodium ion battery material and its preparation method and application; the surface of the polyanion precursor powder is coated by combining inorganic carbon particles and soluble organic carbon. On the one hand, this method can ensure the uniformity of the organic carbon coating on the precursor source, and on the other hand, during the spray drying process, the inorganic carbon particles can regulate the particle size and morphology of the polyanion precursor powder, ensuring the consistency and conductivity of the polyanion powder preparation process. Finally, a three-dimensional network structure is formed between the battery materials by a vapor deposition method, thereby preparing a composite sodium ion battery material with excellent rate performance.

[0005] In order to solve the above technical problems, the first aspect of the present invention is to provide a method for preparing a composite sodium ion battery material, which specifically comprises the following steps:

[0006] S1. uniformly mixing a precursor source, a dispersant, an inorganic carbon source, an organic carbon source and a solvent to obtain a precursor mixture; the precursor source comprises a sodium source, a transition metal source and an anion source;

[0007] S2, removing the solvent in the precursor mixture prepared in step S1 by spray drying to obtain a precursor intermediate;

[0008] S3, pre-sintering the precursor intermediate prepared in step S2 in an inert gas, and performing secondary sintering on the pre-sintered product in a mixed gas to obtain the composite sodium ion battery material; the mixed gas contains an inert gas and an organic small molecule gas carbon source.

[0009] Preferably, in step S1, the precursor source, the dispersant and the solvent are firstly mixed evenly, and then the inorganic carbon source and the organic carbon source are added to form a precursor mixture.

[0010] Furthermore, in step S1, the inorganic carbon source is spherical particles and / or quasi-spherical particles. Preferably, the inorganic carbon source is selected from one or more of acetylene black, Ketjen black, graphite, activated carbon and carbon nanospheres.

[0011] Furthermore, in step S1, the organic carbon source is soluble in the solvent; preferably, the solvent is water, and the organic carbon source is selected from one or more of glucose, sucrose, polyethylene glycol, polyvinyl alcohol and citric acid.

[0012] Furthermore, in step S1, the dispersant is an inorganic alkali metal phosphate and / or an organic polymer material; preferably, the dispersant is selected from one or more of sodium tripolyphosphate, sodium hexametaphosphate, sodium pyrophosphate, polyacrylic acid, polyvinyl alcohol and polyethylene glycol; more preferably, polyacrylic acid. The mass ratio of the dispersant to the precursor source in the precursor mixture is 0.1-2:100; preferably 0.5:100.

[0013] Furthermore, in step S1, the mass ratio of the inorganic carbon source to the precursor source in the precursor mixture is 1-5:100; and the mass ratio of the organic carbon source to the precursor source in the precursor mixture is 2.5-5:100.

[0014] Furthermore, in step S1, the sodium source is selected from one or more of sodium carbonate, sodium hydroxide, sodium oxalate, sodium acetate, sodium formate and sodium citrate; the transition metal source is selected from one or more of Mn-based compounds, Fe-based compounds, Co-based compounds, Ti-based compounds and V-based compounds; the anion source is selected from one or more of phosphoric acid, phosphates and pyrophosphates.

[0015] Furthermore, the molar ratio of the anion source, the transition metal source and the sodium source in the precursor source is (1-4): (1-3): (1-4); preferably 4:1.5:2.

[0016] Furthermore, in step S2, in the spray drying process, the inlet air temperature ranges from 180-240°C, the outlet air temperature ranges from 90-120°C, and the centrifugal speed ranges from 25000-35000 r / min.

[0017] Furthermore, in step S3, in the pre-sintering process, the heating rate is 1-3 °C / min, the sintering temperature is 300-400 °C, and the sintering time is 1-5 h; in the secondary sintering process, the sintering temperature is 500-600 °C, and the sintering time is 8-12 h.

[0018] Furthermore, in step S3, the volume ratio of the inert gas and the organic small molecule gas carbon source in the mixed gas is 1:(3-5); the organic small molecule gas carbon source is selected from one or more of methane, ethane, propane, ethylene and acetylene.

[0019] The second aspect of the present invention is to provide a composite sodium ion battery material, wherein the composite sodium ion battery material is prepared by the preparation method described in the first aspect; the composite sodium ion battery material comprises a polyanion material and a carbon material; the chemical formula of the polyanion material is Na a M b X c ;

[0020] Wherein, M is selected from one or more of Mn, Fe, Co, Ti and V; X is selected from phosphate and / or pyrophosphate; 1≤a≤4, 1≤b≤3, 1≤c≤4.

[0021] Furthermore, the polyanion material is selected from one or more of Na4Fe3(PO4)2P2O7, Na3V2(PO4)3, Na3V2(PO4)3F, NaTi2(PO4)3, NaMnTi(PO4)3, Na3Fe2P2O7, Na3Co2P2O7 and Na3Mn2P2O7.

[0022] The third aspect of the present invention is to provide a battery pole piece, which includes the composite sodium ion battery material prepared by the preparation method described in the first aspect, or the composite sodium ion battery material described in the second aspect.

[0023] A fourth aspect of the present invention is to provide a sodium ion battery, wherein the sodium ion battery comprises the battery electrode sheet described in the third aspect.

[0024] Beneficial effects of the present invention:

[0025] 1. The present invention provides a method for preparing a composite sodium ion battery material, which is simple to operate, low in cost, avoids the addition of organic solvents and toxic and hazardous substances, makes the preparation process more environmentally friendly, reduces the energy consumption of the reaction process, and is suitable for mass production.

[0026] 2. The present invention prepares a precursor mixture by mixing in one step, and then obtains a composite sodium ion battery material with a multi-dimensional network structure and uniform carbon coating by a vapor deposition step. In the present invention, a water-soluble organic carbon source and a water-insoluble spherical and / or quasi-spherical carbon source are selected to modify the surface of the polyanion precursor powder; on the one hand, the water-soluble organic carbon source can form a uniform and continuous coating layer on the surface of the polyanion precursor powder; on the other hand, the inorganic carbon material in the form of spherical and / or quasi-spherical particles not only increases the specific surface area of ​​the polyanion precursor powder material, but also prevents the polyanion precursor powder from sticking and polymerizing during the spray drying process, thereby ensuring the uniform dispersion of the polyanion particles and the control of the morphology. In the process of vapor deposition, the organic small molecule gas carbon source (for example, methane will be cracked into carbon nanotubes under heating environment) will form carbon nanotubes. The presence of carbon nanotubes can construct a three-dimensional electron transmission network between battery materials; this not only enhances the structural stability of the polyanion material, but also further improves the rate performance of the polyanion material.

[0027] 3. The sodium ion battery prepared by using the composite sodium ion battery material prepared by the present invention as the positive electrode active material has excellent rate performance, and the specific capacity at a rate of 20C is 83-89% of that at a rate of 0.1C. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 is a flow chart of the preparation process of an embodiment of the present invention;

[0029] Figure 2 Schematic diagram of the structure of the carbon source and the polyanion precursor powder in the spray drying process of an embodiment of the present invention;

[0030] Figure 3 is a scanning electron microscope image (SEM) of the composite sodium ion battery material prepared in Example 1 of the present invention;

[0031] Figure 4 is a transmission electron microscope image (TEM) of the composite sodium ion battery material prepared in Example 1 of the present invention;

[0032] Figure 5 is the X-ray diffraction pattern (XRD) of the composite sodium ion battery material prepared in Example 1 of the present invention;

[0033] Figure 6 This is a scanning electron microscope image (SEM) of the composite sodium ion battery material prepared in Comparative Example 1 of the present invention;

[0034] Figure 7 The rate performance of the composite sodium ion battery materials prepared in Example 1 and Comparative Example 6 assembled into batteries;

[0035] Figure 8It is the charge and discharge curve of the battery assembled with the composite sodium ion battery materials prepared in Example 1 of the invention and Comparative Example 6 at a rate of 20C. DETAILED DESCRIPTION

[0036] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which the present invention belongs. The terms used herein in the specification of the present invention are for the purpose of describing specific embodiments only and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items. The "include" or "comprising" described in the present invention means that in addition to the components described, other components may also be included or contained. The "include" or "comprising" described in the present invention may also be replaced by the closed "for" or "consisting of...".

[0037] As described in the background art, the preparation process of carbon-coated polyanion powder materials is complicated, the conductivity is poor, it is difficult to ensure the consistency of the prepared crystalline materials and uniform carbon coating, and it is currently difficult to achieve a multi-dimensional conductive network, and it is difficult to implement and produce on a large scale.

[0038] To solve the above problems, an embodiment of the present invention provides a method for preparing a composite sodium ion battery material, comprising the following steps:

[0039] S1. uniformly mixing a precursor source, a dispersant, an inorganic carbon source, an organic carbon source and a solvent to obtain a precursor mixture; the precursor source comprises a sodium source, a transition metal source and an anion source;

[0040] S2, removing the solvent in the precursor mixture prepared in step S1 by spray drying to obtain a precursor intermediate;

[0041] S3, pre-sintering the precursor intermediate prepared in step S2 in an inert gas, and performing secondary sintering on the pre-sintered product in a mixed gas to obtain the composite sodium ion battery material; the mixed gas contains an inert gas and an organic small molecule gas carbon source.

[0042] Preferably, in step S1, the precursor source, the dispersant and the solvent are firstly mixed evenly, and then the inorganic carbon source and the organic carbon source are added to form a precursor mixture.

[0043] The present invention adopts an innovative method in the mixing and drying stages, and the precursor powder is surface coated and instantaneously dried by combining organic and inorganic carbon sources. Since the organic carbon source can be completely dissolved in the solvent, a uniform and continuous coating layer can be formed on the surface of the polyanion precursor powder. At the same time, the addition of the inorganic carbon source helps to control the particle size and morphology of the polyanion precursor powder, thereby enhancing the consistency, stability and conductivity of the material in the subsequent sintering process; in addition, the present invention adopts vapor deposition technology during the sintering process, and the introduced organic small molecule gas carbon source will be cracked into carbon nanotubes, thereby forming a three-dimensional conductive network between the battery materials, which greatly improves the conductivity of the polyanion material. The entire preparation process of the present invention is not only environmentally friendly and simple to operate, but also a low-cost process preparation method with obvious commercial potential and application value.

[0044] In some preferred embodiments, the dispersant is an inorganic alkali metal phosphate and / or an organic polymer material; preferably, the dispersant is selected from one or more of sodium tripolyphosphate, sodium hexametaphosphate, sodium pyrophosphate, polyacrylic acid, polyvinyl alcohol and polyethylene glycol; more preferably, polyacrylic acid. The mass ratio of the dispersant to the precursor source in the precursor mixture is 0.1-2:100; preferably 0.5:100. Too little dispersant will cause uneven dispersion of the precursor source in the precursor mixture, resulting in the polyanion powder material formed being not uniform; too much dispersant will cause the precursor material to be excessively covered during the spray drying process, affecting the contact and reaction between the particles.

[0045] In some preferred embodiments, the inorganic carbon source is spherical particles and / or quasi-spherical particles; preferably, the inorganic carbon source is selected from one or more of acetylene black, Ketjen black, graphite, activated carbon and carbon nanospheres.

[0046] In some preferred embodiments, the organic carbon source is soluble in the solvent; preferably, the solvent is water, and the organic carbon source is selected from one or more of glucose, sucrose, polyethylene glycol, polyvinyl alcohol and citric acid. When the organic carbon source is dissolved in water, a uniform solution can be formed. Compared with solid particles, the solution can be more evenly coated on the precursor powder, thereby enhancing the conductivity between the powders. During the spray drying process, the powder particles are prone to adhesion and aggregation, which leads to the prepared polyanion powder material particles being not uniform and having poor conductivity. The present invention adds inorganic carbon spherical or quasi-spherical particles to the precursor mixture, which plays a role in isolating the polyanion precursor powder material during the spray drying process, maintains the dispersion between them, and then prepares a material of uniform size, thereby enhancing the conductive properties of the polyanion powder material.

[0047] In some preferred embodiments, in step S1, the mass ratio of the inorganic carbon source to the precursor source in the precursor mixture is 1-5:100; the mass ratio of the organic carbon source to the precursor source in the precursor mixture is 2.5-5:100.

[0048] In some preferred embodiments, in step S1, the sodium source is selected from one or more of sodium carbonate, sodium hydroxide, sodium oxalate, sodium acetate, sodium formate and sodium citrate; the transition metal source is selected from one or more of Mn-based compounds, Fe-based compounds, Co-based compounds, Ti-based compounds and V-based compounds; the anion source is selected from one or more of phosphoric acid, phosphates and pyrophosphates.

[0049] In some preferred embodiments, the molar ratio of the anion source, the transition metal source and the sodium source in the precursor source is (1-4):(1-3):(1-4); preferably 4:1.5:2.

[0050] In some preferred embodiments, in step S2, in the spray drying process:

[0051] The inlet air temperature range is 180-240 ℃, the outlet air temperature range is 90-120 ℃, and the centrifugal speed range is 25000-35000 r / min; for example, 25000 r / min, 30000 r / min, 35000 r / min, etc., including but not limited to the speeds listed above; under the premise of ensuring the specific uniformity of the prepared powder material, incomplete drying of the slurry is avoided, and the spray drying parameters need to be controlled within an appropriate range.

[0052] In some preferred embodiments, in step S3, in the pre-sintering process, the heating rate is 1-3°C / min, the sintering temperature is 300-400°C, and the holding time is 1-5 h.

[0053] In the treatment step of the secondary sintering, the sintering temperature is 500-600 ° C and the holding time is 8-12 h. The purpose of pre-sintering is to remove the crystal water in the precursor source and decompose the added organic carbon source; the purpose of secondary sintering is to ensure the conversion of polyanionic crystal materials and the secondary coating of organic small molecule carbon source on the crystal surface; in the process of secondary coating, the ratio of inert gas to organic small molecule gas carbon source between the mixed gas will affect the process of vapor deposition, and the excessive content of organic small molecule carbon source will cause the local temperature to rise during the heat release process, thereby activating more side reactions. If the content of inert gas is too high, the concentration of organic small molecule carbon source will be seriously diluted, the overall heat release rate of the reaction will be reduced, and the reaction will be affected, thereby reducing the degree of connection of the three-dimensional network carbon structure after cracking. Therefore, in some preferred embodiments, the volume ratio of inert gas to organic small molecule gas carbon source in the mixed gas is 1: (3-5).

[0054] Preferably, the volume ratio of the inert gas to the organic small molecule gas carbon source in the mixed gas is 1:5.

[0055] In some preferred embodiments, the organic small molecule gas carbon source is selected from one or more of methane, ethane, propane, ethylene and acetylene; preferably, the organic small molecule gas carbon source is selected from methane and / or acetylene.

[0056] In addition, an embodiment of the present invention provides a composite sodium ion battery material, including the composite sodium ion battery material prepared by the above preparation method; the composite sodium ion battery material includes a polyanion material and a carbon material; the chemical formula of the polyanion material is Na a M b X c ;

[0057] Wherein, M is selected from one or more of Mn, Fe, Co, Ti and V; X is selected from phosphate and / or pyrophosphate; 1≤a≤4, 1≤b≤3, 1≤c≤4.

[0058] An embodiment of the present invention provides a battery pole piece, which includes the composite sodium ion battery material prepared by the above preparation method, or the above composite sodium ion battery material.

[0059] An embodiment of the present invention further provides a sodium ion battery, which includes the above-mentioned battery electrode sheet.

[0060] The present invention is further described below in conjunction with specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention. Example 1

[0061] This embodiment relates to a method for preparing a composite sodium ion battery material, and its preparation process is as follows: Figure 1 As shown, the specific steps include:

[0062] S1. Preparation of mixed slurry of precursors: Dissolve the precursor sources ammonium dihydrogen phosphate, ferrous oxalate and sodium carbonate in 10 L deionized water at a molar ratio of 4:1.5:2 (calculated based on a total mass of 1 kg), and add 5 g of polyacrylic acid at 0.5 wt% of the total solid mass of the precursor sources, and mix and stir. The entire slurry preparation process uses a 20 L wet vertical external circulation ball mill, set the stirring speed to 30 Hz, and ball mill for 1 hour to obtain mixed slurry 1; add 5 wt% of the total solid mass of the precursor source carbon source to the mixed slurry 1 (25 g of 2.5 wt% acetylene black as an inorganic carbon source and 25 g of 2.5 wt% glucose as an organic carbon source), and further mix and ball mill for 2 hours to obtain mixed slurry 2 for standby use.

[0063] S2. Preparation of precursor mixed powder: The mixed slurry 2 obtained in step S1 is spray dried to remove the solvent, and the peristaltic pump feed rate is set to 120 ml / min, the atomizing disk speed is set to 30,000 r / min, the inlet air temperature is set to 230°C, and the outlet air temperature is set to 105°C; the spray-dried precursor mixed powder is obtained for standby use.

[0064] S3. Sintering synthesis and surface vapor deposition modification of polyanion materials: The precursor mixed powder obtained in step S2 is filled into a graphite sagger, and 99.99% nitrogen is introduced as a protective atmosphere. The heating rate is set at 3°C / min to 350°C and kept at this temperature for 2 hours to crack the organic-coated carbon and remove the crystal water of the precursor and the solid-phase reaction tail gas. The temperature is continued to be raised to 550°C at 5°C / min to carry out solid-phase sintering and crystal transformation of the powder. At the same time, acetylene gas is introduced during the crystal forming process to form a mixed gas. The volume ratio of nitrogen to acetylene in the mixed gas is 1:5. After keeping at 550°C for 10 hours, it is naturally cooled to obtain a composite sodium ion battery material.

[0065] The schematic diagram of the structure of the carbon source and the polyanion precursor powder during the spray drying process of step S2 of this embodiment is as follows Figure 2 As shown, the inorganic carbon particles are spherical particles. During the spray drying process, the inorganic carbon particles are isolated next to the precursor source. At the same time, the organic carbon dissolved in the solvent can form a good coating effect on the surface of the precursor source.

[0066] Figure 3 and Figure 4The scanning electron microscope image and transmission electron microscope image of the battery material prepared in Example 1 are respectively. The scanning electron microscope image results show that the prepared composite sodium ion battery material has a three-dimensional conductive network, and the interface between the amorphous and crystalline structures can be observed from the transmission electron microscope image, wherein the amorphous is coated on the surface of the crystal, the thickness of the amorphous carbon coating layer ranges from 80 to 120 nm, and the lattice fringes of the polyanion material can be clearly seen inside the coating layer. Figure 5 It can be seen that the diffraction peak belonging to the polyanion crystalline material can be observed in the XRD pattern of the composite sodium ion battery material prepared in this embodiment. Therefore, it can be seen that the crystals observed in the transmission electron microscope image are polyanion crystalline materials. The composite sodium ion battery material prepared in this embodiment includes a polyanion crystalline material and an amorphous carbon material coated on the surface of the polyanion crystalline material. Example 2

[0067] This embodiment relates to a method for preparing a composite sodium ion battery material, which specifically includes the following steps:

[0068] S1. Preparation of mixed slurry of precursor: ammonium dihydrogen phosphate, ferrous oxalate and sodium carbonate are weighed in a molar ratio of 4:1.5:2 (calculated based on a total mass of 1 kg) and dissolved in 10 L of deionized water. At the same time, 5 g of polyacrylic acid is added at 0.5 wt% of the total solid mass of the precursor source, and mixed and stirred. The entire slurry preparation process uses a 20 L wet vertical external circulation ball mill, and the stirring speed is set to 30 Hz for ball milling for 1 hour to obtain mixed slurry 1; then add 5 wt% of the total solid mass of the precursor source. Carbon source (25 g of 2.5 wt% acetylene black as an inorganic carbon source, and 25 g of 2.5 wt% glucose as an organic carbon source) is added and further mixed and ball milled for 2 hours to obtain mixed slurry 2 for standby use.

[0069] S2. Preparation of precursor mixed powder: The mixed slurry 2 obtained in step S1 is spray dried to remove the solvent, and the peristaltic pump feed rate is set to 120 ml / min, the atomizing disk speed is set to 30,000 r / min, the inlet air temperature is set to 230°C, and the outlet air temperature is set to 105°C; the spray-dried precursor mixed powder is obtained for standby use.

[0070] S3. Sintering synthesis and surface vapor deposition modification of polyanion materials: The precursor mixed powder obtained in step S2 is filled into a graphite sagger, and 99.99% nitrogen is introduced as a protective atmosphere. The heating rate is set to 3°C / min to 350°C and kept warm for 2 hours to crack the organic-coated carbon and remove the crystal water of the precursor and the solid-phase reaction tail gas. The temperature is continued to be raised to 550°C at 5°C / min to carry out solid-phase sintering and crystal transformation of the powder. At the same time, methane gas is introduced during the crystal forming process to form a mixed gas. The volume ratio of nitrogen to methane in the mixed gas is 1:5. After keeping warm at 550°C for 10 hours, it is naturally cooled to obtain a composite sodium ion battery material. Example 3

[0071] This embodiment relates to a method for preparing a composite sodium ion battery material. The difference between this embodiment and embodiment 1 is only that the mass of the organic carbon source and the inorganic carbon source added in step S1 is different; specifically, the following steps are included:

[0072] Dissolve ammonium dihydrogen phosphate, ferrous oxalate and sodium carbonate in 10 L deionized water at a molar ratio of 4:1.5:2 (calculated based on a total mass of 1 kg), and add 5 g of polyacrylic acid at 0.5 wt% of the total solid mass of the precursor source, and mix and stir. The entire slurry preparation process uses a 20 L wet vertical external circulation ball mill, set the stirring speed to 30 Hz, and ball mill for 1 hour to obtain mixed slurry 1; add 10 wt% of the total solid mass of the precursor source as a carbon source to the mixed slurry 1 (50 g of 5 wt% acetylene black as an inorganic carbon source and 50 g of 5 wt% glucose as an organic carbon source), and further mix and ball mill for 2 hours to prepare mixed slurry 2 for standby use. Example 4

[0073] This embodiment relates to a method for preparing a composite sodium ion battery material. The difference between this embodiment and embodiment 1 is only that the mass of the organic carbon source and the inorganic carbon source added in step S1 is different; specifically, the following steps are included:

[0074] Dissolve ammonium dihydrogen phosphate, ferrous oxalate and sodium carbonate in 10 L deionized water at a molar ratio of 4:1.5:2 (calculated based on a total mass of 1 kg), and add 5 g of polyacrylic acid at 0.5 wt% of the total solid mass of the precursor source, and mix and stir. The entire slurry preparation process uses a 20 L wet vertical external circulation ball mill, set the stirring speed to 30 Hz, and ball mill for 1 hour to obtain mixed slurry 1; add 5 wt% of the total solid mass of the precursor source as a carbon source to the mixed slurry 1 (20 g of 2wt% acetylene black as an inorganic carbon source, and 30 g of 3wt% glucose as an organic carbon source), and further mix and ball mill for 2 hours to prepare mixed slurry 2 for standby use. Example 5

[0075] This embodiment relates to a method for preparing a composite sodium ion battery material. The difference between this embodiment and embodiment 1 is only that the mass of the organic carbon source and the inorganic carbon source added in step S1 is different; specifically, the following steps are included:

[0076] Dissolve ammonium dihydrogen phosphate, ferrous oxalate and sodium carbonate in 10 L deionized water at a molar ratio of 4:1.5:2 (calculated based on a total mass of 1 kg), and add 5 g of polyacrylic acid at 0.5 wt% of the total solid mass of the precursor source, and mix and stir. The entire slurry preparation process uses a 20 L wet vertical external circulation ball mill, set the stirring speed to 30 Hz, and ball mill for 1 hour to obtain mixed slurry 1; add 5 wt% of the total solid mass of the precursor source as a carbon source to the mixed slurry 1 (10 g of 1 wt% acetylene black as an inorganic carbon source, and 40 g of 4 wt% glucose as an organic carbon source), and further mix and ball mill for 2 hours to prepare mixed slurry 2 for standby use. Comparative Example 1

[0077] This comparative example relates to a method for preparing a composite sodium ion battery material. The difference between this comparative example and Example 1 is that no carbon source is added in step S1, and there is no vapor deposition step in step S3; specifically, the following steps are included:

[0078] S1. Preparation of mixed slurry of precursors: Dissolve the precursor sources of ammonium dihydrogen phosphate, ferrous oxalate and sodium carbonate in 10 L of deionized water at a molar ratio of 4:1.5:2 (calculated based on a total mass of 1 kg), and add 5 g of polyacrylic acid at 0.5 wt% of the total solid mass of the precursor sources, and mix and stir. The entire slurry preparation process uses a 20 L wet vertical external circulation ball mill, set the stirring speed to 30 Hz, and ball mill for 1 hour to obtain mixed slurry 1.

[0079] S2. Preparation of precursor mixed powder: The mixed slurry obtained in step S1 is spray dried to remove the solvent, and the peristaltic pump feed rate is set to 120 ml / min, the atomizing disk speed is set to 30,000 r / min, the inlet air temperature is set to 230°C, and the outlet air temperature is set to 105°C; the spray-dried precursor mixed powder is obtained for standby use.

[0080] S3. Sintering of composite sodium ion battery materials: The precursor powder obtained in step S2 is loaded into a graphite sagger, and 99.99% nitrogen is introduced as a protective atmosphere. The heating rate is set at 3 °C / min to 350 °C and kept for 2 hours to crack the organic coated carbon and remove the crystal water of the precursor and the solid phase reaction tail gas. The temperature is continued to be raised to 550 °C at 5 °C / min and maintained for 10 hours to obtain a composite sodium ion battery material.

[0081] like Figure 6 As shown, the composite sodium ion battery materials prepared without inorganic carbon and organic carbon coating are severely aggregated, and the absence of inorganic carbon source leads to the spray drying process not being able to play a good insulation role; and no carbon nanotubes are formed on its surface, and a three-dimensional conductive network cannot be formed. This is because the organic small molecule carbon source will form a carbon nanotube structure during the vapor deposition process, and then establish a three-dimensional conductive network between the battery materials. Comparative Example 2

[0082] This comparative example relates to a method for preparing a composite sodium ion battery material. The difference between this comparative example and Example 1 is that organic carbon is not added in step S1. The specific operation is as follows:

[0083] Ammonium dihydrogen phosphate, ferrous oxalate and sodium carbonate were weighed in a molar ratio of 4:1.5:2 (calculated based on a total amount of 1 kg) and dissolved in 10 L of deionized water. At the same time, 5 g of polyacrylic acid was added at 0.5 wt% of the solid mass of the precursor source, and mixed and stirred. The entire slurry preparation process used a 20 L wet vertical external circulation ball mill, set the stirring speed to 30 Hz, and ball milled for 1 h to obtain mixed slurry 1; then, 50 g of inorganic carbon source (acetylene black) at 5 wt% of the total solid mass of the precursor source was added, and further mixed and ball milled for 2 h to obtain mixed slurry 2 for standby use. Comparative Example 3

[0084] This comparative example relates to a method for preparing a composite sodium ion battery material. The difference between this comparative example and Example 1 is that inorganic carbon is not added in step S1. The specific operation is as follows:

[0085] Ammonium dihydrogen phosphate, ferrous oxalate and sodium carbonate were weighed in a molar ratio of 4:1.5:2 (calculated based on a total mass of 1 kg) and dissolved in 10 L of deionized water. At the same time, 5 g of polyacrylic acid was added at 0.5 wt% of the total solid mass of the precursor source, and mixed and stirred. The entire slurry preparation process used a 20 L wet vertical external circulation ball mill, set the stirring speed to 30 Hz, and ball milled for 1 h to obtain mixed slurry 1; then, 50 g of an organic carbon source (glucose) of 5 wt% of the total solid mass of the precursor source was added and further mixed and ball milled for 2 h to obtain mixed slurry 2 for standby use. Comparative Example 4

[0086] This comparative example relates to a method for preparing a composite sodium ion battery material. The difference between this comparative example and Example 1 is that no organic carbon is added in step S1 and there is no vapor deposition process in step S3. The specific operation is as follows:

[0087] S1. Preparation of mixed slurry of precursor: ammonium dihydrogen phosphate, ferrous oxalate and sodium carbonate are weighed in a molar ratio of 4:1.5:2 (calculated based on a total mass of 1 kg) and dissolved in 10 L of deionized water. At the same time, 5 g of polyacrylic acid is added at 0.5 wt% of the total solid mass of the precursor source, and mixed and stirred. The entire slurry preparation process uses a 20 L wet vertical external circulation ball mill, set the stirring speed to 30 Hz, and ball mill for 1 hour to obtain mixed slurry 1; then add 5 wt% of the total solid mass of the precursor source as a carbon source: 50 g of 5 wt% acetylene black is used as an inorganic carbon source, and further mixed and ball milled for 2 hours to obtain mixed slurry 2 for standby use.

[0088] S2, preparation of precursor mixed powder: remove the solvent from the mixed slurry 2 obtained in step S1 by spray drying, set the peristaltic pump feed rate to 120 ml / min, the atomizing disk speed to 30000 r / min, the air inlet temperature to 230°C, and the air outlet temperature to 105°C. The spray-dried precursor mixed powder is obtained for standby use.

[0089] S3, sintering step of polyanion material: the precursor mixed powder obtained in step S2 is filled into a graphite sagger, 99.99% nitrogen is introduced as a protective atmosphere, the heating rate is set to 3 ℃ / min to 350 ℃ and kept warm for 2 hours to remove the crystallization water and solid phase reaction tail gas of the precursor, and the temperature is continued to be raised to 550 ℃ at 5 ℃ / min to perform solid phase sintering and crystal transformation of the powder, and after keeping warm at 550 ℃ for 10 hours, it is naturally cooled to obtain a composite sodium ion battery material. Comparative Example 5

[0090] This comparative example relates to a method for preparing a composite sodium ion battery material. The difference between this comparative example and Example 1 is that no inorganic carbon is added in step S1 and there is no vapor deposition process in step S3. The specific operation is as follows:

[0091] S1. Preparation of mixed slurry of precursor: ammonium dihydrogen phosphate, ferrous oxalate and sodium carbonate are weighed in a molar ratio of 4:1.5:2 (calculated based on a total mass of 1 kg) and dissolved in 10 L of deionized water. At the same time, 5 g of polyacrylic acid is added at 0.5 wt% of the total solid mass of the precursor source, and mixed and stirred. The entire slurry preparation process uses a 20 L wet vertical external circulation ball mill, set the stirring speed to 30 Hz, and ball mill for 1 hour to obtain mixed slurry 1; then add 5 wt% of the total solid mass of the precursor source. Carbon source: 50 g of 5 wt% glucose is used as the organic carbon source, and further mixed and ball milled for 2 hours to obtain mixed slurry 2 for standby use.

[0092] S2, preparation of precursor mixed powder: remove the solvent from the mixed slurry 2 obtained in step S1 by spray drying, set the peristaltic pump feed rate to 120 ml / min, the atomizing disk speed to 30000 r / min, the air inlet temperature to 230°C, and the air outlet temperature to 105°C. The spray-dried precursor mixed powder is obtained for standby use.

[0093] S3, sintering step of polyanion material: the precursor mixed powder obtained in step S2 is filled into a graphite sagger, 99.99% nitrogen is introduced as a protective atmosphere, the heating rate is set to 3 ℃ / min to 350 ℃ and kept warm for 2 hours to crack the organic coated carbon and remove the crystal water of the precursor and the solid phase reaction tail gas, and then the temperature is continued to be raised to 550 ℃ at 5 ℃ / min to carry out solid phase sintering and crystal transformation of the powder, and the mixture is kept warm at 550 ℃ for 10 hours and then naturally cooled to obtain a composite sodium ion battery material. Comparative Example 6

[0094] This comparative example relates to a method for preparing a composite sodium ion battery material. The difference between this comparative example and Example 1 is that there is no vapor deposition process in step S3. The specific operation is as follows:

[0095] The precursor powder obtained in step S2 is loaded into a graphite crucible, and 99.99% nitrogen is introduced as a protective atmosphere. The heating rate is set to 3 °C / min to 350 °C and kept warm for 2 hours to crack the organic-coated carbon and remove the crystal water of the precursor and the solid-phase reaction tail gas. The temperature is continued to be raised to 550 °C at 5 °C / min to perform solid-phase sintering and crystal transformation of the powder. At the same time, it is kept warm at 550 °C for 10 hours and then naturally cooled to obtain a composite sodium ion battery material.

[0096] like Figure 7 and 8 As shown: Compared with Example 1, the battery assembled with the composite sodium ion battery material prepared without the vapor deposition process as the active material in Comparative Example 6 exhibited poor rate performance.

[0097] Application of composite sodium ion battery materials

[0098] The composite sodium ion battery materials prepared in the above examples and comparative examples are respectively used as positive electrode active materials to prepare sodium ion batteries, and the specific operations are as follows:

[0099] Preparation of positive electrode sheets: The prepared composite sodium ion battery material, super P, and polyvinylidene fluoride are mixed in a mass ratio of 8:1:1, and NMP is added and stirred to obtain a positive electrode active slurry. The positive electrode active slurry is evenly coated on the surface of the aluminum foil current collector, and a 200um blade coating is performed to prepare a sheet. After drying at 100°C for 10 h, the electrode film is punched into a sheet with a diameter of 14 mm for standby use.

[0100] Battery assembly: The positive electrode, electrolyte, polypropylene separator (manufacturer: Celgard) and metal sodium negative electrode are assembled into a button half-cell. The electrolyte is 1 mol / L NaPF6, and the electrolyte solvent is a mixed solvent with a volume ratio of EC:DMC:EMC=1:1:1.

[0101] Test conditions: The composite sodium ion battery materials prepared in the embodiment and the comparative example were assembled into a battery and charged and discharged at 1.5 V ~ 4.2 V, charged to 4.2 V by constant current charging, and then discharged to 1.5 V by constant current discharging. The charge and discharge current was cycled for 5 cycles at 0.1C, 1C, 5C, 10C and 20C rates, and the average specific capacity of 5 cycles was tested. The test results are shown in Table 1.

[0102] Table 1

[0103]

[0104] As shown in Table 1, the battery assembled with the composite sodium ion battery material prepared in Examples 1-5 has good rate performance, and the specific capacity at 20C rate is 83-89% of that at 0.1C rate. This is because the simultaneous introduction of inorganic carbon material and organic carbon material into the mixed slurry can promote the particles to form a more complete electron transport network during the spray drying process; in this embodiment, the organic carbon selects water-soluble organic carbon, so that the organic carbon material can form a uniform and continuous coating layer on the surface of the polyanion precursor material. The inorganic carbon material exists in the form of particles, which not only increases the specific surface area of ​​the powder, but also prevents the powder from sticking and polymerizing during the spray drying process, thereby ensuring the uniform dispersion and morphology control of the powder particles, and significantly improving the rate performance of the material. In the subsequent vapor deposition process, the secondary carbon coating of the organic small molecule carbon source will form carbon nanotubes, which further construct a three-dimensional electron transport network structure between the battery materials. The vapor deposition step enhances the structural stability of the material while further improving the rate performance of the composite sodium ion battery material.

[0105] It can be seen from Example 1 and Comparative Examples 1-3 that when inorganic carbon and organic carbon cannot exist at the same time, the rate performance of the composite sodium ion battery is very poor, which indicates that the inorganic carbon source and the organic carbon source in the mixed slurry have a synergistic effect in the spray drying step.

[0106] By comparing Example 1 and Comparative Example 6, Comparative Example 2 and Comparative Example 4, and Comparative Example 3 and Comparative Example 5, it can be seen that the vapor deposition process can greatly improve the specific capacity of the material at a high rate. This is because the carbon nanotubes formed during the sintering process can form a network of conductive connections on the surface of the material.

[0107] It can be seen from the above embodiments and comparative examples that the addition of organic carbon source and inorganic carbon source in the mixing stage and the introduction of cracked carbon source during sintering can greatly improve the rate performance of the material through the synergistic effect of the three.

[0108] The above-described embodiments are only preferred embodiments for fully illustrating the present invention, and the protection scope of the present invention is not limited thereto. Equivalent substitutions or changes made by those skilled in the art based on the present invention are within the protection scope of the present invention. The protection scope of the present invention shall be subject to the claims.

Claims

1. A method for preparing a composite sodium ion battery material, characterized in that: The following steps are involved: S1. uniformly mixing a precursor source, a dispersant, an inorganic carbon source, an organic carbon source and a solvent to obtain a precursor mixture; the precursor source comprises a sodium source, a transition metal source and an anion source; the inorganic carbon source is a spherical particle and / or a spherical-like particle; S2, removing the solvent in the precursor mixture prepared in step S1 by spray drying to obtain a precursor intermediate; S3. Pre-sintering the precursor intermediate prepared in step S2 in an inert gas, and performing secondary sintering on the pre-sintered product in a mixed gas to obtain the composite sodium ion battery material; the mixed gas contains an inert gas and an organic small molecule gas carbon source, and the volume ratio of the inert gas to the organic small molecule gas carbon source in the mixed gas is 1: (3-5); the pre-sintering temperature is 300-400°C, and the time is 1-5 h; the secondary sintering temperature is 500-600°C, and the time is 8-12 h.

2. The preparation method according to claim 1, characterized in that In step S1, the inorganic carbon source is selected from one or more of acetylene black, Ketjen black, graphite, activated carbon and carbon nanospheres; The organic carbon source is soluble in the solvent; the solvent is water, and the organic carbon source is selected from one or more of glucose, sucrose, polyethylene glycol, polyvinyl alcohol and citric acid.

3. The preparation method according to claim 1, characterized in that: In step S1, the mass ratio of the inorganic carbon source to the precursor source in the precursor mixture is 1-5:100; The mass ratio of the organic carbon source to the precursor source in the precursor mixture is 2.5-5:

100.

4. The preparation method according to claim 1, characterized in that: In step S1, the sodium source is selected from one or more of sodium carbonate, sodium hydroxide, sodium oxalate, sodium acetate, sodium formate and sodium citrate; The transition metal source is selected from one or more of Mn-based compounds, Fe-based compounds, Co-based compounds, Ti-based compounds and V-based compounds; The anion source is selected from one or more of phosphoric acid, phosphate and pyrophosphate; The molar ratio of the anion source, the transition metal source and the sodium source in the precursor source is (1-4): (1-3): (1-4).

5. The preparation method according to claim 1, characterized in that: In step S2, in the spray drying process: The inlet air temperature range is 180-240 ℃, the outlet air temperature range is 90-120 ℃, and the centrifugal speed range is 25000-35000 r / min.

6. The preparation method according to claim 1, characterized in that: In step S3, in the pre-sintering process, the heating rate is 1-3°C / min.

7. The preparation method according to claim 1, characterized in that: In step S3, the organic small molecule gas carbon source is selected from one or more of methane, ethane, propane, ethylene and acetylene.

8. A composite sodium ion battery material, characterized in that: Prepared by the preparation method according to any one of claims 1 to 7; the composite sodium ion battery material comprises a polyanion material and a carbon material; the chemical formula of the polyanion material is Na a M b X c ; Wherein, M is selected from one or more of Mn, Fe, Co, Ti and V; X is selected from phosphate and / or pyrophosphate; 1≤a≤4, 1≤b≤3, 1≤c≤4.

9. A battery pole piece, characterized in that: The battery pole piece includes the composite sodium ion battery material prepared by the preparation method according to any one of claims 1 to 7, or includes the composite sodium ion battery material according to claim 8.

10. A sodium ion battery, characterized in that: The sodium ion battery comprises the battery pole piece according to claim 9.