Hourglass-shaped polyethersulfone membrane and preparation method and application thereof
The hourglass-type polyethersulfone membrane was prepared by thermal and humid air induction and heat carrier induction, which solved the problem of insufficient flux and contamination capacity of the filter membrane in the prior art, and realized a high-throughput and contamination capacity of the filter membrane. , suitable for infusion filtration applications of medical devices.
Patent Information
- Application Number
- CN202410970240.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-07-19
AI Technical Summary
In the prior art, hourglass-type structural filter membranes are less used in medical devices, and it is difficult to meet the high throughput and pollution absorption capacity requirements of medicinal liquid filtration during infusion, especially under the conditions of ensuring the long-term use of the filter membrane.
The cast film liquid phase separation and the heat carrier-induced cast film liquid phase separation control were prepared to prepare a polyethersulfone film with an hourglass structure. The cast film liquid was coated on the carrier and phase separation was performed in the air. , and then cured in a solidification bath, the cast membrane liquid composition and process parameters are controlled to obtain a filter membrane with high throughput and contamination capacity.
The hourglass-type polyethersulfone membrane prepared has large pore size, higher flux and dirt absorption capacity. It is suitable for the preparation of filtration products. It can effectively remove harmful particles and ensure the flow of the drug liquid during the infusion process.
Smart Images

Figure CN118496557B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of materials, and in particular to an hourglass-shaped polyethersulfone membrane and a preparation method and application thereof. Background Art
[0002] During the infusion process, the liquid medicine will directly enter the human blood, so it is necessary to ensure that there are no harmful particles in the liquid medicine. PES (polyethersulfone) material has good biocompatibility, so the filter membrane made of it is widely used in the medical device industry. In order to remove harmful particles in the liquid medicine during the infusion process and ensure the flow rate of the liquid medicine during the infusion, a large-pore PES filter membrane is usually selected, such as a PES filter membrane with a pore size of 5um. This application requires the filter membrane to have a large flux and excellent dirt holding capacity to ensure that the filter membrane can be used for a long time. Compared with the filter membrane with a symmetrical structure, the filter membrane with an asymmetric structure has a better dirt holding capacity, especially the hourglass structure. However, there are still few hourglass-shaped filter membranes used in medical devices, and further research and development is needed.
[0003] In view of this, the present invention is proposed. Summary of the invention
[0004] The first object of the present invention is to provide a method for preparing a polyethersulfone membrane with an hourglass structure. The filter membrane prepared by the preparation method has high flux and strong dirt holding capacity.
[0005] The second object of the present invention is to provide a polyethersulfone membrane with an hourglass structure.
[0006] The third object of the present invention is to provide the use of the above-mentioned hourglass-shaped polyethersulfone membrane in the preparation of filtration products.
[0007] In order to achieve the above objectives, the following technical solutions are adopted:
[0008] In a first aspect, the present invention provides a method for preparing a polyethersulfone membrane having an hourglass structure, comprising the following steps:
[0009] The casting liquid is coated on the carrier to form a liquid film, and then the carrier is exposed to air for phase separation to form a filter membrane that is completely or partially phase-separated but not solidified, and then the carrier is immersed in a coagulation bath for solidification to obtain an hourglass-shaped polyethersulfone membrane;
[0010] The casting solution comprises, by mass percentage, 8%-12% polyethersulfone, 1%-5% hydrophilic polymer, 30%-70% solvent, and the remainder is non-solvent;
[0011] The temperature of the carrier is 10-20°C higher than the cloud point of the casting solution;
[0012] The air temperature is 40-60°C, and the absolute humidity of the air is 40-100g / m3 .
[0013] As a further technical solution, the hydrophilic polymer includes at least one of PVP-K30, PVP-K45, PVP-K60, PVP-K90, sulfonated polyethersulfone or PEOX.
[0014] As a further technical solution, the solvent includes at least one of NMP, DMF, DMAC or DMSO.
[0015] As a further technical solution, the non-solvent includes at least one of ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, ethanol, isopropanol or water.
[0016] As a further technical solution, the carrier includes a steel belt.
[0017] As a further technical solution, the flow rate of the air is 0-1m / s;
[0018] As a further technical solution, the exposure time is 2-10s.
[0019] As a further technical solution, the coagulation bath comprises water.
[0020] In a second aspect, the present invention provides a polyethersulfone membrane with an hourglass-shaped structure, which is prepared by the above-mentioned preparation method.
[0021] As a further technical solution, the pore size of the hourglass-shaped polyethersulfone membrane is 1-10 um, the thickness is 70-140 um, the flow rate is 1,500,000-5,000,000 LMH / Bar, and the initial bubble pressure is 0.015-0.04 MPa.
[0022] In a third aspect, the present invention provides the use of the above-mentioned hourglass-shaped polyethersulfone membrane in the preparation of filtration products.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] The invention provides a method for preparing a polyethersulfone membrane with an hourglass structure, which simultaneously uses hot and humid air to induce phase separation of the casting liquid and a heat carrier to induce phase separation of the casting liquid to regulate the structure of the filter membrane, so as to obtain a polyethersulfone membrane with an hourglass structure. The preparation method is simple and efficient, and the prepared polyethersulfone membrane with an hourglass structure has a large pore size, higher flux and dirt holding capacity, and can be used for the preparation of filtration products. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0026] Figure 1 The electron microscopy result of the filter membrane of Example 1 is shown;
[0027] Figure 2 The electron microscopy result of the filter membrane of Example 2 is shown;
[0028] Figure 3 The electron microscopy result of the filter membrane of Comparative Example 1 is shown;
[0029] Figure 4 The electron microscopy results of the filter membrane of Comparative Example 2 are shown;
[0030] Figure 5 This is the electron microscopy result of the filter membrane in comparative example 3. DETAILED DESCRIPTION
[0031] The embodiments of the present invention will be described in detail below in conjunction with the embodiments and examples, but it will be appreciated by those skilled in the art that the following embodiments and examples are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. If specific conditions are not specified, proceed according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0032] In a first aspect, the present invention provides a method for preparing a polyethersulfone membrane having an hourglass structure, comprising the following steps:
[0033] The casting liquid is coated on the carrier to form a liquid film, and then the carrier is exposed to air for phase separation to form a filter membrane that is completely or partially phase-separated but not solidified, and then the carrier is immersed in a coagulation bath for solidification to obtain an hourglass-shaped polyethersulfone membrane;
[0034] The casting solution is mainly composed of polyethersulfone, a hydrophilic polymer, a solvent and a non-solvent. In terms of mass percentage, in the casting solution, the mass percentage of polyethersulfone can be, for example, but not limited to 8%, 9%, 10%, 11% or 12%; the mass percentage of the hydrophilic polymer can be, for example, but not limited to 1%, 2%, 3%, 4% or 5%; the mass percentage of the solvent can be, for example, but not limited to 30%, 40%, 50%, 60% or 70%; the balance is the non-solvent;
[0035] The temperature of the carrier is 10-20° C. higher than the cloud point of the casting solution.
[0036] The temperature of the air may be, for example, but not limited to, 40°C, 45°C, 50°C, 55°C or 60°C, and the absolute humidity of the air may be, for example, but not limited to, 40 g / m 3 , 50g / m 3 , 60g / m 3 , 70g / m 3 , 80g / m 3 , 90g / m 3 or 100g / m 3 .
[0037] The invention provides a method for preparing a polyethersulfone membrane with an hourglass structure, which simultaneously uses hot and humid air to induce phase separation of the casting liquid and a heat carrier to induce phase separation of the casting liquid to regulate the structure of the filter membrane, so as to obtain a polyethersulfone membrane with an hourglass structure. The preparation method is simple and efficient, and the prepared polyethersulfone membrane with an hourglass structure has a large pore size, higher flux and dirt holding capacity, and can be used for the preparation of filtration products.
[0038] In some optional embodiments, the hydrophilic polymer includes but is not limited to at least one of PVP-K30, PVP-K45, PVP-K60, PVP-K90, sulfonated polyethersulfone or PEOX (poly(2-ethyl-2-oxazoline)).
[0039] In some optional embodiments, the solvent includes but is not limited to at least one of NMP (N-methylpyrrolidone), DMF (dimethylformamide), DMAC (dimethylacetamide) or DMSO (dimethyl sulfoxide).
[0040] In some optional embodiments, the non-solvent includes but is not limited to at least one of ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, ethanol, isopropanol or water.
[0041] In some optional embodiments, the carrier includes but is not limited to a steel belt, or other carriers well known in the art.
[0042] In some optional embodiments, the air flow rate may be, for example, but not limited to, 0 m / s, 0.2 m / s, 0.4 m / s, 0.6 m / s, 0.8 m / s or 1 m / s; the membrane structure may be controlled by controlling parameters such as the air flow rate.
[0043] In some optional embodiments, the exposure time may be, for example, but not limited to, 2s, 4s, 6s, 8s or 10s.
[0044] By controlling the exposure time, the membrane liquid can form a filter membrane that is completely or partially phase-separated but not solidified.
[0045] In some optional embodiments, the coagulation bath is water, and the filter membrane is solidified by immersing the carrier in water.
[0046] In a second aspect, the present invention provides a polyethersulfone membrane with an hourglass-shaped structure, which is prepared by the above-mentioned preparation method.
[0047] The hourglass-shaped polyethersulfone membrane has a large pore size, higher flux and dirt holding capacity, and can be used for the preparation of filtration products.
[0048] In some optional embodiments, the pore size of the hourglass-shaped polyethersulfone membrane is 1-10 um, the thickness is 70-140 um, the flow rate is 1,500,000-5,000,000 LMH / Bar, and the initial bubble pressure is 0.015-0.04 MPa.
[0049] In a third aspect, the present invention provides the use of the above-mentioned hourglass-shaped polyethersulfone membrane in the preparation of filtration products.
[0050] The hourglass-shaped polyethersulfone membrane provided by the invention has a large pore size, higher flux and dirt holding capacity, and can be used for the preparation of filtering products.
[0051] The present invention is further described below by means of specific examples and comparative examples. However, it should be understood that these examples are only used for more detailed description and should not be construed as limiting the present invention in any form.
[0052] Example 1
[0053] A method for preparing a polyethersulfone membrane with an hourglass structure comprises the following steps:
[0054] 1) Prepare casting solution.
[0055] 2) Use a scraper or die head to apply the casting liquid on a stainless steel belt at a certain temperature.
[0056] 3) The stainless steel strip is exposed to an environment of certain temperature, absolute humidity and air flow rate to form a filter membrane that has been completely or partially phase-separated but not solidified.
[0057] 4) Immerse the stainless steel strip in a coagulation bath to solidify the filter membrane, and the coagulation bath is pure water.
[0058] 5) Rinse the filter membrane with pure water to remove all residual organic solvents.
[0059] 6) Dry the filter membrane at a temperature of 60-100°C.
[0060] 7) Roll up the filter membrane.
[0061] The composition and process conditions of the casting solution are shown in Table 1.
[0062] Example 2
[0063] A method for preparing a polyethersulfone membrane with an hourglass structure, which is different from Example 1 in that the casting solution or process conditions are different. The casting solution or process conditions are shown in Table 1.
[0064] Example 3
[0065] A method for preparing a polyethersulfone membrane with an hourglass structure, which is different from Example 1 in that the casting solution or process conditions are different. The casting solution or process conditions are shown in Table 1.
[0066] Example 4
[0067] A method for preparing a polyethersulfone membrane with an hourglass structure, which is different from Example 1 in that the casting solution or process conditions are different. The casting solution or process conditions are shown in Table 1.
[0068] Example 5
[0069] A method for preparing a polyethersulfone membrane with an hourglass structure, which is different from Example 1 in that the casting solution or process conditions are different. The casting solution or process conditions are shown in Table 1.
[0070] Example 6
[0071] A method for preparing a polyethersulfone membrane with an hourglass structure, which is different from Example 1 in that the casting solution or process conditions are different. The casting solution or process conditions are shown in Table 1.
[0072] Comparative Example 1
[0073] A method for preparing a polyethersulfone membrane, which is different from Example 1 in that the casting solution or process conditions are different. The casting solution or process conditions are shown in Table 1.
[0074] Comparative Example 2
[0075] A method for preparing a polyethersulfone membrane, which is different from Example 1 in that the casting solution or process conditions are different. The casting solution or process conditions are shown in Table 1.
[0076] Comparative Example 3
[0077] A method for preparing a polyethersulfone membrane, which is different from Example 1 in that the casting solution or process conditions are different. The casting solution or process conditions are shown in Table 1.
[0078] Table 1
[0079] .
[0080] The filter membranes prepared in the above examples and comparative examples were tested, and the electron microscopy results were as follows: Figure 1-4 The performance test results are shown in Table 1. Figure 1-2 It can be seen that the method of the present invention successfully prepared a filter membrane with an hourglass structure. In addition, Examples 3-5 also successfully prepared a filter membrane with an hourglass structure. However, using a preparation method other than the process parameters of the present invention, such as Comparative Examples 1-3, the filter membranes prepared did not have an hourglass structure ( Figure 3-Figure 5 ). In Comparative Example 1, air at room temperature was used as the phase separation medium, resulting in the inability of the membrane liquid to effectively separate phases in the VIPS stage, and eventually a dense structure with a very small pore size was formed on the surface. In Comparative Example 2, a steel strip at room temperature was used as the medium, resulting in the inability of the lower layer of the membrane liquid to effectively separate phases, and eventually a double-layer structure was formed instead of an hourglass-shaped structure. In Comparative Example 3, a steel strip with a temperature lower than the cloud point temperature of the casting liquid was used as the medium, resulting in the inability of the lower layer of the membrane liquid to effectively separate phases, and the prepared membrane did not have an hourglass-shaped structure.
[0081] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing an hourglass-shaped polyethersulfone membrane, characterized in that: The following steps are involved: The casting liquid is coated on the carrier to form a liquid film, and then the carrier is exposed to air for phase separation to form a filter membrane that is completely or partially phase-separated but not solidified, and then the carrier is immersed in a coagulation bath for solidification to obtain an hourglass-shaped polyethersulfone membrane; The casting solution comprises, by mass percentage, 8%-12% polyethersulfone, 1%-5% hydrophilic polymer, 30%-70% solvent, and the remainder is non-solvent; The temperature of the carrier is 10-20°C higher than the cloud point of the casting solution; The air temperature is 40-60°C, and the absolute humidity of the air is 40-100g / m 3 ; The air flow rate is 0-1m / s; the exposure time is 2-10s; The pore size of the hourglass-shaped polyethersulfone membrane is 1-10 um, the thickness is 70-140 um, the flow rate is 1,500,000-5,000,000 LMH / Bar, and the initial bubble pressure is 0.015-0.04 MPa.
2. The preparation method according to claim 1, characterized in that The hydrophilic polymer includes at least one of PVP-K30, PVP-K45, PVP-K60, PVP-K90, sulfonated polyethersulfone or PEOX.
3. The preparation method according to claim 1, characterized in that: The solvent includes at least one of NMP, DMF, DMAC or DMSO.
4. The preparation method according to claim 1, characterized in that: The non-solvent includes at least one of ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, ethanol, isopropanol or water.
5. The preparation method according to claim 1, characterized in that: The carrier comprises a steel belt.
6. The preparation method according to claim 1, characterized in that: The coagulation bath includes water.