A kind of heterogeneous adhesive hydrogel and its preparation method and application

By using a heterogeneous adhesive hydrogel double-layer structure on difficult-to-heal diabetic wounds, the inner layer of hydrogel with strong adhesive ability is combined with the outer layer of non-adhesive starch hydrogel to solve the problem of existing technology. It eliminates the problems of improper adhesion and complex preparation and achieves wound healing and improved mechanical properties.

CN118542968BActive Publication Date: 2024-10-08AFFILIATED HOSPITAL OF GUANGDONG MEDICAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410995642.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-10-08
Estimated Expiration
2044-07-24

AI Technical Summary

Technical Problem

Existing homogeneous adhesive hydrogels have the disadvantage of adhering to other objects in the repair of difficult-to-heal diabetic wounds, and the preparation method of double-layer hydrogels is complex and difficult to control, which limits its application in the field of tissue engineering.

Method used

It adopts a heterogeneous adhesive hydrogel double-layer structure. The inner layer contains double-bonded hydrophilic monomers, collagen derivatives and chitosan-grafted lipoic acid. The outer layer is natural starch hydrogel, which is riveted through multiple hydrogen bonds. To achieve strong interface bonding, the inner layer has strong adhesion for wound repair, and the outer layer is non-adhesive to prevent adhesion to other tissues or foreign objects.

Benefits of technology

It achieves simultaneous regeneration of blood vessels and nerves in the wound, accelerates wound healing, improves the overall mechanical properties of the hydrogel, expands the application scope of starch hydrogel in the field of tissue regeneration, and simplifies the preparation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118542968B_ABST
    Figure CN118542968B_ABST
Patent Text Reader

Abstract

The invention discloses a heterogeneous adhesive hydrogel and a preparation method and application thereof, and belongs to the technical field of biomedical material hydrogel. The heterogeneous adhesive hydrogel prepared by the invention is a double-layer structure, with natural starch hydrogel as the outer layer, and a hydrogel containing double bond monomers, collagen derivatives and chitosan grafted lipoic acid as the adhesive inner layer, and the inner and outer layers are riveted by multiple hydrogen bonds, and the interface bonding force is strong, and there is no delamination phenomenon; the inner layer has excellent wet tissue adhesion ability, which is used to adhere to the wound surface, and the effective ingredients act on the difficult-to-heal wound surface, so that the blood vessels and nerves around the wound are regenerated synchronously, and the wound healing is accelerated; the outer layer has no adhesion, and the inner and outer layers have different mechanical strengths, and the rigid and flexible strategy is adopted to improve the overall mechanical properties of the prepared double-layer hydrogel; the heterogeneous adhesive hydrogel prepared by the invention can realize rapid wound closure treatment, and the effective ingredients act on the wound surface for a long time, providing a new material for accelerating the treatment of difficult-to-heal wounds.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of biomedical material hydrogels, and in particular to a heterogeneous adhesive hydrogel and a preparation method and application thereof. Background Art

[0002] Diabetic wounds are a common complication in diabetic patients. In contrast to acute wounds, diabetic wounds are characterized by wound angiogenesis disorders and neuropathy caused by hyperglycemia and persistent infection, which hinder the continuous process of wound healing (Adv. Mater. 2023, 35, 2212300.). Compared with other passive protective dressings required for ordinary wounds, hydrogels have excellent advantages such as moist wound interface, ability to absorb wound exudate, good oxygen permeability and hemostasis, making functional hydrogels widely popular and of great value in the repair of difficult-to-heal wounds.

[0003] Currently, most adhesive hydrogels have a homogeneous structure, that is, the hydrogel is made of the same material as a whole, and both the inner and outer layers are adhesive. Adhesive hydrogels adhere to other objects while adhering to tissues, which is not conducive to their application in wound repair.

[0004] At present, the functional research of hydrogels used for repairing difficult-to-heal wounds in diabetes mainly focuses on antibacterial, anti-inflammatory, antioxidant and angiogenesis-promoting aspects, but ignores the fact that peripheral neuropathy of the wound is also an important factor hindering wound healing. Therefore, it is of great significance to develop a heterogeneous adhesion hydrogel with synchronous vascular-nerve regeneration ability to promote the healing of difficult-to-heal wounds and tissue regeneration in diabetic patients.

[0005] Lipoic acid has the ability to improve nervous system lesions. It is used clinically to treat paresthesia caused by diabetic peripheral neuropathy and relieve distal pain. However, the clinical use of lipoic acid injection can lead to trace element and vitamin deficiencies in patients, and more serious adverse reactions such as headaches, diarrhea, rashes, and convulsions may occur. Therefore, how to use lipoic acid safely and efficiently in clinical practice is worth pondering.

[0006] Starch is easily gelatinized, resulting in poor mechanical properties of the hydrogel produced and its inability to adapt to skin tissue, which limits its application in the field of tissue regeneration.

[0007] The preparation of double-layer hydrogels is one of the most common strategies for constructing heterogeneous adhesive hydrogels. The differential response behavior of the two layers of the hydrogel under external stimuli can cause the hydrogel to undergo anisotropic bending deformation. However, the existing methods for preparing double-layer hydrogels often require the preparation of a first layer of hydrogel first, and the preparation of a second layer of hydrogel in situ on the surface of the first layer of hydrogel before it is completely gelled. This multi-step preparation process is complex and difficult to control, and the interface bonding between the two layers is weak, which greatly limits the practical application prospects of double-layer hydrogels in the field of tissue engineering. Summary of the invention

[0008] The purpose of the present invention is to provide a heterogeneous adhesive hydrogel and a preparation method and application thereof. The prepared hydrogel is a heterogeneous two-layer structure with different adhesion properties. The inner layer hydrogel can moisten the wound surface, and the effective ingredients act on the wound surface for a long time to promote the regeneration of blood vessels and nerves around the wound, thereby accelerating the healing of the wound surface; the outer layer starch hydrogel has weak adhesion ability and will not adhere to other tissues or foreign objects during use; the interface bonding force between the two layers is strong and no debonding occurs; through the synergistic effect of the inner layer and the outer layer, not only the overall mechanical properties of the double-layer hydrogel can be improved, but also the application scope of the starch hydrogel in the field of tissue regeneration can be broadened.

[0009] To achieve the above-mentioned purpose, the present invention provides a heterogeneous adhesive hydrogel, which comprises an inner adhesive hydrogel and an outer starch hydrogel; the inner adhesive hydrogel comprises the following components in parts by weight: 30-50 parts of a double-bond hydrophilic monomer, 1-15 parts of a collagen derivative, 0.1-3 parts of a photoinitiator, 1-10 parts of chitosan grafted lipoic acid, and 50-97 parts of deionized water; the outer starch hydrogel comprises the following components in parts by weight: 10-50 parts of natural starch and 50-90 parts of deionized water.

[0010] Preferably, the inner layer adhesive hydrogel comprises the following components by weight: 50 parts of double-bond hydrophilic monomers, 3 parts of collagen derivatives, 0.1 parts of photoinitiator, 3 parts of chitosan grafted lipoic acid, and 50 parts of deionized water; the outer layer starch hydrogel comprises the following components by weight: 15 parts of natural starch and 60 parts of deionized water.

[0011] Preferably, the inner layer adhesive hydrogel comprises the following components by weight: 30 parts of double-bond hydrophilic monomers, 3 parts of collagen derivatives, 0.1 parts of photoinitiators, 1 part of chitosan grafted lipoic acid, and 50 parts of deionized water; the outer layer starch hydrogel comprises the following components by weight: 10 parts of natural starch and 50 parts of deionized water.

[0012] Preferably, the inner layer adhesive hydrogel comprises the following components by weight: 45 parts of double-bond hydrophilic monomers, 3 parts of collagen derivatives, 3 parts of photoinitiators, 10 parts of chitosan grafted lipoic acid, and 97 parts of deionized water; the outer layer starch hydrogel comprises the following components by weight: 50 parts of natural starch and 90 parts of deionized water.

[0013] Preferably, the natural starch is one of water chestnut powder, potato powder, and kudzu root powder, or a mixture of the two.

[0014] Preferably, the double-bond-containing hydrophilic monomer is one of acrylic acid, acrylamide, methacrylic acid, methacrylamide, methacrylated gelatin, or a mixture of the two.

[0015] Preferably, the collagen derivative is one of a jellyfish collagen derivative, a fish collagen derivative, a porcine collagen derivative, or a mixture of the two.

[0016] Preferably, the chitosan grafted lipoic acid is one of chitosan lipoic acid, hydroxybutyl chitosan lipoic acid, carboxymethyl chitosan lipoic acid, hydroxypropyl chitosan lipoic acid, or a mixture of the two.

[0017] A method for preparing the above-mentioned heterogeneous adhesive hydrogel comprises the following steps:

[0018] S1. Prepare the outer starch hydrogel. Accurately weigh the required amount of starch, slowly add it into deionized water under magnetic stirring, and continue stirring at room temperature at 500-1000 rpm for 5-10 h to fully disperse the starch in the water; transfer the starch dispersion to a mold, and place it in a water bath at 80-90°C for 5-10 min to obtain a transparent outer starch hydrogel;

[0019] S2. Prepare an inner layer adhesive hydrogel. Accurately weigh a double-bond hydrophilic monomer, a collagen derivative, and chitosan grafted lipoic acid, add them to deionized water, stir at 500-1000 rpm at room temperature for 2-10 h, add a photoinitiator, transfer to a dark environment and continue stirring for 10-30 min, then transfer the mixture to the starch-based hydrogel prepared in step S1, gently shake the mold to make the prepared mixture evenly distributed on the surface of the starch-based hydrogel without spilling, and cure it in a light curing machine for 5-10 min to obtain a double-layer heterogeneous adhesive hydrogel.

[0020] Preferably, the preparation method of the collagen derivative and chitosan grafted lipoic acid in step S2 is as follows:

[0021] Preparation method of collagen derivatives:

[0022] (a) At 4°C, 1 g of collagen from different sources was weighed and dissolved in a hydrochloric acid solution with a pH of 5.5. After stirring for 12 h to form a uniform mixture, 0.192 g of 1-ethyl-(3-dimethylaminopropyl)carbodiimide and 0.056 mg of N-hydroxysuccinimide were added to activate the carboxyl groups of the collagen. After activation for 1 h, 0.029 g of deferoxamine was added and reacted for 24 h.

[0023] (b) Weigh 0.15 g of 3,4-dihydroxybenzoic acid, dissolve it in water, add 0.192 g of 1-ethyl-(3-dimethylaminopropyl)carbodiimide and 0.056 g of N-hydroxysuccinimide to activate the carboxyl group, stir for 1 hour, add the mixture obtained in (b) to (a), and continue stirring for 24 hours. After the reaction is completed, dialyze and freeze-dry to obtain the collagen derivative;

[0024] Preparation method of chitosan grafted lipoic acid:

[0025] (A) Chitosan was dissolved in 2% acetic acid / deionized water and stirred at 1000 rpm for 12 h at room temperature to form a transparent and uniform mixture with a concentration of 3%;

[0026] (B) Weigh 0.206 g of lipoic acid and dissolve it in 10 mL of dimethyl sulfoxide. Add 0.192 g of 1-ethyl-(3-dimethylaminopropyl)carbodiimide and 0.056 g of N-hydroxysuccinimide to activate the carboxyl group. After stirring for 1 h, add the mixture obtained in (B) into (A) and continue stirring for 24 h. After the reaction is completed, dialyze and freeze-dry to obtain chitosan grafted with lipoic acid.

[0027] A use of the above-mentioned heterogeneous adhesive hydrogel in wound repair.

[0028] Therefore, the present invention provides a heterogeneous adhesive hydrogel and a preparation method and application thereof, and its specific technical effects are as follows:

[0029] (1) The heterogeneous adhesive hydrogel prepared by the present invention has a double-layer structure, with natural starch hydrogel as the outer layer. The two layers have different adhesive abilities. The inner layer has a strong adhesive ability and is used to adhere to the wound surface. The effective ingredients act on the difficult-to-heal wound surface, causing the blood vessels and nerves around the wound to regenerate synchronously, thereby accelerating wound healing;

[0030] (2) The heterogeneous adhesive hydrogel prepared by the present invention has a hydrogel containing double bond monomers, collagen derivatives and chitosan grafted lipoic acid as the adhesive inner layer, and the outer layer and the inner layer are riveted by multiple hydrogen bonds. The interface bonding force between the two layers is strong and delamination will not occur;

[0031] (3) The heterogeneous adhesive hydrogel prepared by the present invention adopts a "brittle and flexible" strategy. The brittle outer layer of the natural starch hydrogel is organically combined with the flexible inner layer, which can significantly improve the overall mechanical properties of the hydrogel, while not affecting the adhesive properties and making it easier to remove;

[0032] (4) The heterogeneous adhesive hydrogel prepared by the present invention utilizes the non-wetting tissue adhesion ability of starch hydrogel and creatively prepares it into an outer layer that does not require adhesion, thereby ensuring the strong adhesion of the inner layer hydrogel while preventing the entire hydrogel from adhering to other parts of the tissue or foreign objects, thereby expanding the application range of starch-based hydrogels in medicine;

[0033] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments of the present invention will be briefly introduced below. Obviously, the accompanying drawings in the following description are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative labor.

[0035] Figure 1 The results of the investigation on the toughness of the heterogeneous adhesive hydrogel interface in Example 7;

[0036] Figure 2 The results of the investigation of the mechanical properties of the heterogeneous adhesive hydrogels in Example 8, wherein A is the investigation results of Examples 1 to 3, and B is the investigation results of Examples 4 to 6;

[0037] Figure 3 The results of the investigation on the antibacterial properties of the heterogeneous adhesive hydrogel in Example 9;

[0038] Figure 4 The results of cell viability detection of the heterogeneous adhesive hydrogel extract and human umbilical vein endothelial cells co-cultured for different time periods in Example 10;

[0039] Figure 5 The results of investigating the effect of heterogeneous adhesive hydrogel on cell migration in Example 11;

[0040] Figure 6 These are the results of investigating the effect of the heterogeneous adhesive hydrogel in diabetic wound healing in Example 12. DETAILED DESCRIPTION

[0041] The technical solution of the present invention is further described below through the accompanying drawings and embodiments.

[0042] In order to make the purpose, technical scheme and advantages of the present application clearer, more thorough and more complete, the technical scheme of the present invention is clearly and completely described below through the accompanying drawings and examples. The following detailed descriptions are all descriptions of the embodiments, and are intended to provide further detailed descriptions of the present invention. Unless otherwise specified, all technical terms used in the present invention have the same meaning as those generally understood by those skilled in the art to which the present application belongs.

[0043] The instruments, equipment, reagents and materials used in the examples were all obtained through commercial channels.

[0044] Method for preparing collagen derivatives:

[0045] (a) At 4°C, 1 g of jellyfish collagen was weighed and dissolved in a hydrochloric acid solution with a pH of 5.5. After stirring for 12 h to form a uniform mixture, 0.192 g of 1-ethyl-(3-dimethylaminopropyl)carbodiimide (EDC) and 0.056 mg of N-hydroxysuccinimide (NHS) were added to activate the carboxyl groups of the collagen. After activation for 1 h, 0.029 g of deferoxamine was added and reacted for 24 h.

[0046] (b) Weigh 0.15 g of 3,4-dihydroxybenzoic acid, dissolve it in water, add 0.192 g of EDC and 0.056 g of NHS to activate the carboxyl group, stir for 1 hour, add the mixture obtained in (b) to (a), and continue stirring for 24 hours. After the reaction is completed, dialyze and freeze-dry to obtain the collagen derivative.

[0047] Method for preparing chitosan grafted lipoic acid:

[0048] (A) Chitosan was dissolved in 2% acetic acid / water and stirred at 1000 rpm for 12 h at room temperature to form a transparent and uniform mixture with a concentration of 3%;

[0049] (B) Weigh 0.206 g of lipoic acid and dissolve it in 10 mL of dimethyl sulfoxide, add 0.192 g of EDC and 0.056 g of NHS to activate the carboxyl group, stir for 1 h, then add the mixture obtained in (B) to (A), and continue stirring for 24 h. After the reaction is completed, dialyze and freeze-dry to obtain chitosan grafted with lipoic acid.

[0050] Embodiment 1

[0051] A heterogeneous adhesive hydrogel is prepared by the following steps:

[0052] S1. Prepare the outer starch hydrogel. Add 60 mL of deionized water to a 100 mL beaker placed on a magnetic stirrer. Turn on the magnetic stirrer and set the speed to 500 rpm. Accurately weigh 15 g of water chestnut powder and slowly add the water chestnut powder to the deionized water. Continue stirring at room temperature for 5 h to fully disperse the starch in the water. After the time is up, extract 10 mL of the water chestnut powder dispersion and transfer it to a mold (5.0×5.0×3.2 cm 3 ) and placed in a water bath at 80 °C for 10 min to obtain the outer starch hydrogel.

[0053] S2. Prepare the inner layer adhesion hydrogel. Accurately weigh 5 mL of acrylic acid, 0.3 g of jellyfish collagen, deferoxamine protocatechuic acid, and 0.1 g of chitosan lipoic acid, add them to 5 mL of deionized water, turn on the magnetic stirrer, set the speed to 500 rpm, stir at room temperature for 2 h, add 0.01 g of photoinitiator, continue stirring for 10 min, and then transfer the mixture to the starch-based hydrogel prepared in step S1. Gently shake the mold to make the prepared mixture evenly distributed on the surface of the starch-based hydrogel without spilling. Cure it in a light curing machine for 5 min to obtain a double-layer heterogeneous adhesion hydrogel.

[0054] Embodiment 2

[0055] A heterogeneous adhesive hydrogel is prepared by the following steps:

[0056] S1. Prepare the outer starch hydrogel. Add 60 mL of deionized water to a 100 mL beaker placed on a magnetic stirrer. Turn on the magnetic stirrer and set the speed to 500 rpm. Accurately weigh 15 g of water chestnut powder and slowly add the water chestnut powder to the deionized water. Continue stirring at room temperature for 5 h to fully disperse the starch in the water. After the time is up, extract 10 mL of the water chestnut powder dispersion and transfer it to a mold (5.0×5.0×3.2 cm 3 ) and placed in a water bath at 80 °C for 10 min to obtain the outer starch hydrogel.

[0057] S2. Prepare the inner layer adhesion hydrogel. Accurately weigh 5 mL of acrylic acid, 0.3 g of jellyfish collagen, deferoxamine protocatechuic acid, and 0.2 g of chitosan lipoic acid, add them to 5 mL of deionized water, turn on the magnetic stirrer, set the speed to 500 rpm, stir at room temperature for 2 h, add 0.01 g of photoinitiator, continue stirring for 10 min, and then transfer the mixture to the starch-based hydrogel prepared in step S1. Gently shake the mold to make the prepared mixture evenly distributed on the surface of the starch-based hydrogel without spilling. Cure it in a light curing machine for 5 min to obtain a double-layer heterogeneous adhesion hydrogel.

[0058] Embodiment 3

[0059] A heterogeneous adhesive hydrogel is prepared by the following steps:

[0060] S1. Prepare the outer starch hydrogel. Add 60 mL of deionized water to a 100 mL beaker placed on a magnetic stirrer. Turn on the magnetic stirrer and set the speed to 500 rpm. Accurately weigh 15 g of water chestnut powder and slowly add the water chestnut powder to the deionized water. Continue stirring at room temperature for 5 h to fully disperse the starch in the water. After the time is up, extract 10 mL of the water chestnut powder dispersion and transfer it to a mold (5.0×5.0×3.2 cm 3 ) and placed in a water bath at 80 °C for 10 min to obtain the outer starch hydrogel.

[0061] S2. Prepare the inner layer adhesion hydrogel. Accurately weigh 5 mL of acrylic acid, 0.3 g of jellyfish collagen, deferoxamine protocatechuic acid, and 0.3 g of chitosan lipoic acid, add them to 5 mL of deionized water, turn on the magnetic stirrer, set the speed to 500 rpm, stir at room temperature for 2 h, add 0.01 g of photoinitiator, continue stirring for 10 min, and then transfer the mixture to the starch-based hydrogel prepared in step S1. Gently shake the mold to make the prepared mixture evenly distributed on the surface of the starch-based hydrogel without spilling. Cure it in a light curing machine for 5 min to obtain a double-layer heterogeneous adhesion hydrogel.

[0062] Embodiment 4

[0063] A heterogeneous adhesive hydrogel is prepared by the following steps:

[0064] S1. Prepare the outer starch hydrogel. Add 60 mL of deionized water to a 100 mL beaker placed on a magnetic stirrer. Turn on the magnetic stirrer and set the speed to 500 rpm. Accurately weigh 15 g of water chestnut powder and slowly add the water chestnut powder to the deionized water. Continue stirring at room temperature for 5 h to fully disperse the starch in the water. After the time is up, extract 10 mL of the water chestnut powder dispersion and transfer it to a mold (5.0×5.0×3.2 cm 3 ) and placed in a water bath at 80 °C for 10 min to obtain the outer starch hydrogel.

[0065] S2. Prepare the inner layer adhesion hydrogel. Accurately weigh 5 mL of acrylic acid, 0.3 g of jellyfish collagen deferoxamine protocatechuic acid, and 0.1 g of hydroxybutyl chitosan lipoic acid, add them to 5 mL of deionized water, turn on the magnetic stirrer, set the speed to 500 rpm, stir at room temperature for 2 h, add 0.01 g of photoinitiator, continue stirring for 10 min, and then transfer the mixture to the starch-based hydrogel prepared in step S1. Gently shake the mold to make the prepared mixture evenly distributed on the surface of the starch-based hydrogel without spilling. Cure it in a light curing machine for 5 min to obtain a double-layer heterogeneous adhesion hydrogel.

[0066] Embodiment 5

[0067] A heterogeneous adhesive hydrogel is prepared by the following steps:

[0068] S1. Prepare the outer starch hydrogel. Add 60 mL of deionized water to a 100 mL beaker placed on a magnetic stirrer. Turn on the magnetic stirrer and set the speed to 500 rpm. Accurately weigh 15 g of water chestnut powder and slowly add the water chestnut powder to the deionized water. Continue stirring at room temperature for 5 h to fully disperse the starch in the water. After the time is up, extract 10 mL of the water chestnut powder dispersion and transfer it to a mold (5.0×5.0×3.2 cm 3 ) and placed in a water bath at 80 °C for 10 min to obtain the outer starch hydrogel.

[0069] S2. Prepare the inner layer adhesion hydrogel. Accurately weigh 5 mL of acrylic acid, 0.3 g of jellyfish collagen deferoxamine protocatechuic acid, and 0.2 g of hydroxybutyl chitosan lipoic acid, add them to 5 mL of deionized water, turn on the magnetic stirrer, set the speed to 500 rpm, stir at room temperature for 2 h, add 0.01 g of photoinitiator, continue stirring for 10 min, and then transfer the mixture to the starch-based hydrogel prepared in step S1. Gently shake the mold to make the prepared mixture evenly distributed on the surface of the starch-based hydrogel without spilling. Cure it in a light curing machine for 5 min to obtain a double-layer heterogeneous adhesion hydrogel.

[0070] Embodiment 6

[0071] A heterogeneous adhesive hydrogel is prepared by the following steps:

[0072] S1. Prepare the outer starch hydrogel. Add 60 mL of deionized water to a 100 mL beaker placed on a magnetic stirrer. Turn on the magnetic stirrer and set the speed to 500 rpm. Accurately weigh 15 g of water chestnut powder and slowly add the water chestnut powder to the deionized water. Continue stirring at room temperature for 5 h to fully disperse the starch in the water. After the time is up, extract 10 mL of the water chestnut powder dispersion and transfer it to a mold (5.0×5.0×3.2 cm3 ) and placed in a water bath at 80°C for 10 min to obtain the outer starch hydrogel.

[0073] S2. Prepare the inner layer adhesion hydrogel. Accurately weigh 5 mL of acrylic acid, 0.3 g of jellyfish collagen deferoxamine protocatechuic acid, and 0.3 g of hydroxybutyl chitosan lipoic acid, add them to 5 mL of deionized water, turn on the magnetic stirrer, set the speed to 500 rpm, stir at room temperature for 2 h, add 0.01 g of photoinitiator, continue stirring for 10 min, and then transfer the mixture to the starch-based hydrogel prepared in step S1. Gently shake the mold to make the prepared mixture evenly distributed on the surface of the starch-based hydrogel without spilling. Cure it in a light curing machine for 5 min to obtain a double-layer heterogeneous adhesion hydrogel.

[0074] Embodiment 7

[0075] The interfacial toughness of the heterogeneous adhesive hydrogels prepared in Examples 1 to 6 on pig skin was investigated, and the specific steps were as follows:

[0076] Use detergent to clean the surface fat of fresh pigs, cut the hydrogel into 80×10×4 mm 3 The inner layer of hydrogel was placed in contact with the surface of fresh pig skin at 37 °C for 30 min, and then the interface toughness was tested. The tensile speed was 100 mm / min. Each sample was repeated 5 times. The results are shown in Figure 1 .

[0077] from Figure 1 It can be concluded that the prepared double-layer hydrogel has excellent adhesion properties on pig skin tissue.

[0078] Embodiment 8

[0079] The mechanical properties of the heterogeneous adhesive hydrogels prepared in Examples 1 to 6 were investigated, and the specific steps were as follows:

[0080] The double-layer hydrogel was cut into dumbbell shape and the tensile properties of the hydrogel were evaluated using a universal tensile machine. The tensile speed was set at 5 mm / min and each sample was repeated 5 times. The results are shown in Figure 2 Same as Table 1.

[0081] Table 1 Tensile strength of heterogeneous adhesive hydrogels prepared in Examples 1 to 6

[0082] ;

[0083] from Figure 2As can be seen from Table 1, the tensile strength of the heterogeneous adhesive hydrogels prepared in Examples 1 to 6 is between 0.17 and 0.33 MPa, and the mechanical strength of the hydrogel can be controlled by adjusting the proportion of the components of the inner layer of the hydrogel to obtain a hydrogel compatible with skin tissue.

[0084] Embodiment 9

[0085] The antibacterial properties of the hydrogels prepared in Examples 1 to 6 were investigated, and the specific steps were as follows;

[0086] Prepare liquid culture medium: weigh 2.5 g of tryptone powder, 1.25 g of yeast extract powder, and 2.5 g of sodium chloride into a 500-mL conical flask, and add 250 mL of deionized water to dissolve. Seal the flask with a sterile breathable sealing film and tie it tightly with a rubber band. Autoclave at 120 °C for 20 min and cool to room temperature before use.

[0087] Prepare solid culture medium: weigh 2.5 g of tryptone, 1.25 g of yeast extract, 2.5 g of sodium chloride, 3.7 g of agar, and 250 mL of deionized water, heat to 40 °C, adjust the pH to 7.0 after all components are completely dissolved, then seal with a high-temperature sterilization breathable sealing film, sterilize at 120 °C and high pressure for 20 min, wait for it to cool naturally, and then plate it in a culture dish, 10 mL per dish, and use it after it is completely cooled and solidified.

[0088] Prepare bacterial suspension: activate Escherichia coli and Staphylococcus aureus. When the OD values ​​of Escherichia coli and Staphylococcus aureus tested at 600 nm by a microplate reader are between 0.3 and 0.5, inoculate them into 4 mL of sterile liquid culture medium and 0.3 g of hydrogel, respectively. Place the inoculated culture medium and hydrogel in a constant temperature shaker at 37°C for 3 h.

[0089] After the culture was completed, 10 μL of bacterial suspension was taken from each culture and diluted with 1 mL of PBS. Then, 100 μL of the dilution was spread on an agar plate and cultured in an incubator for 12 h before taking photos.

[0090] The results are as follows Figure 3 As shown, the heterogeneous adhesive hydrogels prepared in Examples 1 to 6 have excellent antibacterial ability.

[0091] Embodiment 10

[0092] The cell compatibility of the heterogeneous adhesive hydrogels prepared in Examples 3 and 6 was investigated, and the specific steps were as follows:

[0093] After irradiating the hydrogel with UV light for 1 h, turn the back side over and irradiate for another 1 h. 3000 human umbilical vein endothelial cells (HUVECs) were inoculated into each well and co-cultured with 50 mg / mL hydrogel extract at 37 °C. According to the instructions attached to the CCK8 kit, the absorbance (OD) at 450 nm was measured at 24 h, 48 h, and 72 h of co-culture using a microplate reader. The control group was treated with only culture medium without hydrogel. The results are shown in Table 1. Figure 4 .

[0094] from Figure 4 It can be seen that the relative cell viability of the two double-layer hydrogels prepared in Examples 3 and 6 after co-culture with HUVECs for different time periods is above 100%, indicating that the hydrogels have excellent cell compatibility and can be used in wound repair.

[0095] Embodiment 11

[0096] The effects of the heterogeneous adhesive hydrogels prepared in Example 3 and Example 6 on cell migration were investigated, and the specific steps were as follows:

[0097] 800 μL of DMEM medium (containing 50 mg / mL hydrogel extract) was added to the bottom of the 24-well plate, and 3×10 4 After 24 h of culture, the original culture medium was removed and the cells were rinsed twice with PBS. The PBS was removed and the cells were fixed with fixative at room temperature for 20 min. The cells were incubated with crystal violet stain at room temperature in the dark for 15 min and washed twice with washing solution, each for 15 s. The residual water was aspirated and images were collected with a microscope.

[0098] Results Figure 5 The heterogeneous adhesive hydrogels prepared in Example 3 and Example 6 are beneficial to the migration of HUVECs cells.

[0099] Embodiment 12

[0100] The effects of the heterogeneous adhesive hydrogels prepared in Example 3 and Example 6 on diabetic wound healing were investigated, and the specific steps were as follows:

[0101] (1) Fifteen 8-week-old mice (blood glucose levels > 16.7 mmol / L) were selected and randomly divided into three groups: an experimental group (groups of Example 3 and Example 6) and a control group (ordinary medical gauze group), with 5 mice in each group.

[0102] (2) Under deep anesthesia, remove hair from the back of the mouse using a razor and depilatory cream;

[0103] (3) A wound with a diameter of approximately 10 mm was created on the back of the mouse and photographed (recorded as day 0). Sterile hydrogel and medical gauze were applied to the wound, respectively. The hydrogel and gauze were replaced every 3 days and photographs were taken to record the wound healing status.

[0104] The results of some mice are as follows Figure 6 As shown, compared with the control group, the double-layer adhesive hydrogels prepared in Example 3 and Example 6 can accelerate the healing of diabetic wounds.

[0105] Therefore, the heterogeneous adhesive hydrogel prepared by the present invention has a double-layer structure, with natural starch hydrogel as the outer layer and hydrogel containing double bond monomers, collagen derivatives and chitosan grafted lipoic acid as the adhesive inner layer, the inner and outer layers are riveted by multiple hydrogen bonds, the interface bonding force is strong, and there is no delamination phenomenon; the inner layer has excellent moist tissue adhesion ability, is used to adhere to the wound surface, and the effective ingredients act on the difficult-to-heal wound surface, so that the blood vessels and nerves around the wound are regenerated synchronously, and the wound healing is accelerated; the outer layer has no adhesion, and the different mechanical strengths of the inner and outer layers are used to improve the overall mechanical properties of the prepared double-layer hydrogel by adopting a rigid-flexible strategy; the heterogeneous adhesive hydrogel prepared by the present invention can realize rapid wound sealing treatment, and the effective ingredients act on the wound surface for a long time, thereby providing a new material for accelerating the treatment of difficult-to-heal wounds; the preparation method is simple and easy to operate, the equipment requirements are simple, the preparation of the two layers of the hydrogel is carried out simultaneously, the efficiency is high, and the effect is good.

[0106] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.

Claims

1. A heterogeneous adhesive hydrogel, characterized in that: The heterogeneous adhesive hydrogel comprises an inner adhesive hydrogel and an outer starch hydrogel; the inner adhesive hydrogel comprises the following components in parts by weight: 30-50 parts of a double-bond hydrophilic monomer, 1-15 parts of a collagen derivative, 0.1-3 parts of a photoinitiator, 1-10 parts of chitosan grafted lipoic acid, and 50-97 parts of deionized water; the outer starch hydrogel comprises the following components in parts by weight: 10-50 parts of natural starch and 50-90 parts of deionized water.

2. The heterogeneous adhesive hydrogel according to claim 1, characterized in that: The inner layer adhesive hydrogel comprises the following components by weight: 50 parts of double-bond hydrophilic monomers, 3 parts of collagen derivatives, 0.1 parts of photoinitiators, 3 parts of chitosan grafted lipoic acid, and 50 parts of deionized water; the outer layer starch hydrogel comprises the following components by weight: 15 parts of natural starch and 60 parts of deionized water.

3. The heterogeneous adhesive hydrogel according to claim 1, characterized in that: The inner layer adhesive hydrogel comprises the following components by weight: 30 parts of double-bond hydrophilic monomers, 3 parts of collagen derivatives, 0.1 parts of photoinitiators, 1 part of chitosan grafted lipoic acid, and 50 parts of deionized water; the outer layer starch hydrogel comprises the following components by weight: 10 parts of natural starch and 50 parts of deionized water.

4. The heterogeneous adhesive hydrogel according to claim 1, characterized in that: The inner layer adhesive hydrogel comprises the following components by weight: 45 parts of double-bond hydrophilic monomers, 3 parts of collagen derivatives, 3 parts of photoinitiators, 10 parts of chitosan grafted lipoic acid, and 97 parts of deionized water; the outer layer starch hydrogel comprises the following components by weight: 50 parts of natural starch and 90 parts of deionized water.

5. The heterogeneous adhesive hydrogel according to claim 1, characterized in that: The natural starch is one of water chestnut powder, potato powder and kudzu root powder or a mixture of the two; the double-bond-containing hydrophilic monomer is one of acrylic acid, acrylamide, methacrylic acid, methacrylamide and methacrylated gelatin or a mixture of the two.

6. The heterogeneous adhesive hydrogel according to claim 1, characterized in that: The collagen derivative is one of jellyfish collagen derivative, fish collagen derivative, pig collagen derivative or a mixture of the two.

7. The heterogeneous adhesive hydrogel according to claim 1, characterized in that: The chitosan grafted lipoic acid is one of chitosan lipoic acid, hydroxybutyl chitosan lipoic acid, carboxymethyl chitosan lipoic acid, hydroxypropyl chitosan lipoic acid or a mixture of the two.

8. A method for preparing a heterogeneous adhesive hydrogel according to any one of claims 1 to 7, characterized in that: Here are the steps: S1. Prepare the outer starch hydrogel. Accurately weigh the required amount of starch, slowly add it into deionized water under magnetic stirring, and continue stirring at room temperature at 500-1000 rpm for 5-10 h to fully disperse the starch in the water. Transfer the starch dispersion into a mold and place it in a water bath at 80-90 °C for 5-10 min to obtain a transparent outer starch hydrogel. S2. Prepare an inner layer adhesive hydrogel. Accurately weigh a double-bond hydrophilic monomer, a collagen derivative, and chitosan grafted lipoic acid, add them to deionized water, stir at 500-1000 rpm at room temperature for 2-10 h, add a photoinitiator, transfer to a dark environment and continue stirring for 10-30 min, then transfer the mixture to the starch-based hydrogel prepared in step S1, gently shake the mold to make the prepared mixture evenly distributed on the surface of the starch-based hydrogel without spilling, and cure it in a light curing machine for 5-10 min to obtain a double-layer heterogeneous adhesive hydrogel.

9. The method for preparing a heterogeneous adhesive hydrogel according to claim 8, characterized in that: The preparation method of the collagen derivative and chitosan grafted lipoic acid in step S2 is as follows: Preparation method of collagen derivatives: (a) At 4°C, 1 g of collagen from different sources was dissolved in a hydrochloric acid solution with a pH of 5.

5. After stirring for 12 h to form a uniform mixture, 0.192 g of 1-ethyl-(3-dimethylaminopropyl)carbodiimide and 0.056 mg of N-hydroxysuccinimide were added to activate the carboxyl groups of the collagen. After activation for 1 h, 0.029 g of deferoxamine was added and the mixture was reacted for 24 h. (b) Weigh 0.15 g of 3,4-dihydroxybenzoic acid, dissolve it in water, add 0.192 g of 1-ethyl-(3-dimethylaminopropyl)carbodiimide and 0.056 g of N-hydroxysuccinimide to activate the carboxyl group, stir for 1 h, add the mixture obtained in (b) into (a), continue stirring for 24 h, and after the reaction is completed, dialyze and freeze-dry to obtain a collagen derivative; Preparation method of chitosan grafted lipoic acid: (A) Chitosan was dissolved in 2% acetic acid / deionized water and stirred at 1000 rpm for 12 h at room temperature to form a transparent and uniform mixture with a concentration of 3%; (B) Weigh 0.206 g of lipoic acid and dissolve it in 10 mL of dimethyl sulfoxide. Add 0.192 g of 1-ethyl-(3-dimethylaminopropyl)carbodiimide and 0.056 g of N-hydroxysuccinimide to activate the carboxyl group. After stirring for 1 hour, add the mixture obtained in (B) into (A) and continue stirring for 24 hours. After the reaction is completed, dialyze and freeze-dry to obtain chitosan grafted with lipoic acid.