A method for preparing high-performance anti-sticking masterbatch

By reducing the surface energy and friction coefficient of PET materials and adding TiO2@BaSO4/MoS2 composite materials, the problems of insufficient anti-adhesion and UV aging resistance of PET materials are solved, achieving high-performance anti-sticking and wear resistance, and improving the overall performance of the material.

CN118546402BActive Publication Date: 2024-10-11湖南省升阳新材料有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411013864.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-10-11
Estimated Expiration
2044-07-26

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of anti-sticking masterbatch, and discloses a method for preparing a high-performance anti-sticking masterbatch. The masterbatch of the invention uses a modified polyester resin as a base resin, and performs a modification treatment on the synthetic polyester resin to reduce the surface free energy of the masterbatch, thereby reducing the adhesion between the masterbatch and other substances, thereby achieving an anti-sticking effect; adding a TiO2@BaSO4 / MoS2 composite material as an anti-sticking agent further improves the anti-sticking property of the masterbatch, and at the same time can also improve the ultraviolet aging resistance and wear resistance of the masterbatch; the addition of other additives synergistically plays a role, so that the masterbatch has certain high performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of anti-sticking masterbatch, and in particular to a method for preparing a high-performance anti-sticking masterbatch. Background Art

[0002] Polyethylene terephthalate (PET) is a crystalline polymer. Due to its excellent mechanical strength, electrical insulation, heat resistance and chemical resistance, it is mainly used in synthetic fibers, electrical insulation materials, films, engineering plastics and other fields. However, the friction coefficient of PET material is relatively large. When it is used in anti-adhesion materials, the anti-adhesion property of the material will decrease, and it will also affect the mechanical properties of the material, thus limiting the application of PET materials in the actual market. In addition, when PET materials are used outdoors, they need to withstand the test of environmental conditions such as sunlight, heat, oxygen, and water. Among them, the UV aging resistance is an important indicator for measuring the durability of outdoor polyester materials. Therefore, researchers need to process polyester materials according to actual application needs to improve the anti-adhesion and UV aging resistance of PET materials, so as to make them have high-performance anti-adhesion effects.

[0003] The anti-sticking property of traditional PET materials is usually achieved by adding a single filler (such as silicon dioxide, calcium carbonate, titanium dioxide, etc.) as an anti-sticking agent. However, the amount required to achieve the anti-sticking effect in this way is large, which will cause the overall performance of the PET material to decline. Studies have found that reducing the surface energy of PET materials and reducing the friction coefficient of the material can improve the anti-sticking property, thereby improving the anti-sticking property. Therefore, this application reduces the surface energy and friction coefficient of the masterbatch and adds an anti-sticking agent to synergistically improve the anti-sticking property of the material and improve the UV aging resistance to obtain a high-performance anti-sticking masterbatch. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a method for preparing a high-performance anti-sticking masterbatch.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A method for preparing a high-performance anti-sticking masterbatch comprises the following steps:

[0007] Step S1: adding 3,5-dihydroxybenzoic acid, 3-(perfluoro-n-butane)-1,2-propylene oxide and tetrabutylammonium bromide to N,N-dimethylformamide and stirring to mix evenly, introducing nitrogen and raising the system temperature to 90°C, stirring for 4-6 hours, after the reaction is completed, collecting the product by rotary evaporation, redispersing it in ethyl acetate and stirring for 10 minutes, washing, drying and rotary evaporation to obtain an intermediate product;

[0008] Step S2: adding 1 / 3 of the terephthalic acid and the intermediate product into a reactor and stirring and mixing them evenly, then adding methyl tin mercaptan and antimony trioxide, and raising the system temperature to 190-230° C., and continuing the reaction for 2-3 hours. After the reaction is completed, adding the remaining 2 / 3 of the terephthalic acid and ethylene glycol into the reactor and continuing the reaction for 4-6 hours. After the reaction is completed, cooling to room temperature and crushing to obtain a modified polyester resin;

[0009] Step S3: Weigh the raw materials by weight, add 5-15 parts of TiO 2 @BaSO 4 / MoS 2 The composite material and 0.5-2 parts of silane coupling agent are added to the reactor and stirred for 5-10 minutes, then 0.8-2 parts of antioxidant and 1-3 parts of dispersant are added and stirred for 5-10 minutes, and finally 30-80 parts of modified polyester resin are added and stirred for 10-20 minutes to obtain a mixture, and then the mixture is added to an extruder for extrusion and granulation to obtain a high-performance anti-sticking masterbatch;

[0010] Further, in step S1, the usage ratio of 3,5-dihydroxybenzoic acid, 3-(perfluoro-n-butane)-1,2-propylene oxide, tetrabutylammonium bromide, N,N-dimethylformamide and ethyl acetate is 0.05-0.15 mol: 0.05-0.15 mol: 0.0025-0.0075 mol: 100 mL: 20 mL;

[0011] Further, in step S2, the usage ratio of terephthalic acid, intermediate product, methyl tin mercaptan, antimony trioxide and ethylene glycol is 1 mol: 0.3-0.5 mol: 0.001-0.003 mol: 0.001-0.003 mol: 0.8-1.2 mol;

[0012] Furthermore, in step S3, the temperatures of the zones of the extruder are as follows: the temperature of zone 1 is 180-190°C, the temperature of zone 2 is 200-220°C, the temperatures of zones 3 to 5 are both 230-240°C, the temperatures of zones 6 to 10 are both 245-255°C, the head temperature is 255-265°C, and the screw speed is 240-280 rpm.

[0013] The TiO 2 @BaSO 4 / MoS 2 The composite material was prepared by the following steps:

[0014] Step A1: Disperse titanium dioxide in deionized water and stir to mix evenly, then add 0.05-0.1 mol / L barium chloride solution and continue stirring for 10 min, then slowly drop 0.05-0.1 mol / L sodium carbonate solution, after the dropwise addition is completed, continue to react for 2-3 h, after the reaction is completed, filter, wash, dry, collect the product, and then transfer the product to a flask, introduce sulfur dioxide to continue the reaction for 1-2 h, and then introduce air to continue the reaction for 30-60 min to obtain TiO 2 @BaSO 4 Powder (barium sulfate coated titanium dioxide powder);

[0015] Step A2: TiO 2 @BaSO 4 After the powder was ultrasonically dispersed in deionized water for 30 minutes, hexadecyltrimethylammonium bromide was added and stirred for 10 minutes, and then ultrasonically dispersed for 1-3 hours. After the reaction was completed, the powder was filtered, washed, and dried to obtain surface-modified TiO 2 @BaSO 4 powder;

[0016] Step A3: 3 g of layered molybdenum disulfide was dispersed in a mixture of 30 mL of 1,4-butanediol and 30 mL of deionized water and stirred for 30 min. After ultrasonic dispersion for 6-10 h, the mixture was centrifuged at 3000 rpm to collect the upper dispersion. The product was then centrifuged at 10000 rpm to collect the product. Then 0.2-1 g of the product was re-dispersed in 50 mL of deionized water and recorded as molybdenum disulfide solution. The surface-modified TiO 2 @BaSO 4 The powder was dispersed in deionized water, and then molybdenum disulfide solution was added and stirred. The system temperature was raised to 60-80°C, and the pH was adjusted to 11-12. After continuous stirring for 30 minutes, the mixture was transferred to a reactor and reacted at 100-130°C for 8-12 hours to obtain TiO 2 @BaSO 4 / MoS 2 Composite materials;

[0017] Further, in step A1, the dosage ratio of titanium dioxide, deionized water, barium chloride solution and sodium carbonate solution is 2-5 g: 100 mL: 20-40 mL: 20-40 mL;

[0018] Furthermore, in step A2, TiO 2 @BaSO 4 The ratio of powder, deionized water and hexadecyltrimethylammonium bromide is 2g:50mL:0.05-0.5g;

[0019] Furthermore, in step A3, the surface-modified TiO 2 @BaSO4 The dosage ratio of powder, deionized water and molybdenum disulfide solution is 0.5-1.5g:50mL:50mL.

[0020] Beneficial effects of the present invention:

[0021] The masterbatch of the present invention is based on modified polyester resin as the base resin, and is modified on the basis of synthetic polyester resin to reduce the surface free energy of the masterbatch, thereby reducing the adhesion between the masterbatch and other substances, thereby achieving an anti-sticking effect; adding TiO 2 @BaSO 4 / MoS 2 The composite material as an anti-adhesive further improves the anti-adhesive property of the masterbatch, and can also improve the UV aging resistance and wear resistance of the masterbatch; the addition of other additives works synergistically to give the masterbatch a certain high performance. In the modified polyester resin, the carboxyl group in 3,5-dihydroxybenzoic acid and the epoxy group in 3-(perfluoro-n-butane)-1,2-propylene oxide are first used to react to generate an intermediate product containing terminal hydroxyl groups; the intermediate product and the hydroxyl group in ethylene glycol are then used to react with the carboxyl group in terephthalic acid to generate a modified polyester resin; the fluorine-containing chain segment introduced into the resin can effectively reduce the surface energy of the masterbatch, making the masterbatch have excellent anti-adhesive properties, which is because the fluorine atoms in the fluorine-containing chain segment themselves have a lower surface energy. During the synthesis of the masterbatch, the fluorine atoms will migrate to the surface, thereby reducing the free energy of the masterbatch surface, making it have a certain anti-adhesive property.

[0022] TiO 2 @BaSO 4 / MoS 2 In the composite material, barium chloride and sodium carbonate are reacted to synthesize barium carbonate on the surface of titanium dioxide, and then the barium carbonate is converted into barium sulfate by air-solid conversion to synthesize TiO 2 @BaSO 4 powder; then use the surfactant hexadecyltrimethylammonium bromide to 2 @BaSO 4 The powder was surface modified to obtain TiO with positive surface charge. 2 @BaSO 4 powder; finally, electrostatic self-assembly was used to combine negatively charged MoS2 nanosheets with positively charged surface-modified TiO 2 @BaSO 4 The powder was compounded to obtain TiO 2 @BaSO 4 / MoS 2 Composite materials. TiO 2 @BaSO 4 / MoS 2The composite material is added to the matrix as a filler, which not only improves the wear resistance of the matrix, but also improves the anti-adhesion performance of the matrix, thereby making the matrix have excellent anti-adhesion properties. This is because the composite material has excellent dispersibility in the matrix and can form many tiny and hard protrusions on the surface of the matrix, thereby reducing the contact area between the matrixes and reducing the friction coefficient of the matrix surface, thereby playing an anti-adhesion role; Among them, using titanium dioxide as a base material can also improve the anti-ultraviolet performance of the masterbatch, because titanium dioxide can absorb and scatter ultraviolet light entering the inside of the matrix, convert light energy into heat energy and consume ultraviolet light, thereby avoiding polymer degradation caused by ultraviolet light; and the barium sulfate coated on the surface of titanium dioxide is a chemically inert substance, which acts as a barrier and can effectively block the electrons and holes generated by titanium dioxide under ultraviolet light from contacting with the matrix resin, inhibiting the photocatalytic activity of titanium dioxide, thereby improving the weather resistance of the masterbatch; In addition, the loading of molybdenum disulfide nanosheets also reduces the friction coefficient of the matrix and further improves the anti-adhesion property of the matrix. DETAILED DESCRIPTION

[0023] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] Example 1: TiO 2 @BaSO 4 / MoS 2 The composite material was prepared by the following steps:

[0025] Step A1: Disperse 2g of titanium dioxide in 100mL of deionized water and stir to mix evenly, then add 20mL of 0.05mol / L barium chloride solution and continue stirring for 10min, then slowly drop 20mL of 0.05mol / L sodium carbonate solution, after the dropwise addition is completed, continue to react for 2h, after the reaction is completed, filter, wash, dry, collect the product, and then transfer the product to a flask, introduce sulfur dioxide to continue the reaction for 1h, and then introduce air to continue the reaction for 30min to obtain TiO 2 @BaSO 4 powder;

[0026] Step A2: 2 g TiO 2 @BaSO 4 The powder was ultrasonically dispersed in 50 mL of deionized water for 30 min, and then 0.05 g of hexadecyltrimethylammonium bromide was added and stirred for 10 min. The powder was ultrasonically dispersed for 1 h. After the reaction was completed, the powder was filtered, washed, and dried to obtain surface-modified TiO 2 @BaSO4 powder;

[0027] Step A3: 3 g of layered molybdenum disulfide was dispersed in a mixture of 30 mL of 1,4-butanediol and 30 mL of deionized water and stirred for 30 min. After ultrasonic dispersion for 6 h, the mixture was centrifuged at 3000 rpm to collect the upper dispersion. The product was then centrifuged at 10000 rpm to collect the product. Then 0.2 g of the product was re-dispersed in 50 mL of deionized water and recorded as molybdenum disulfide solution. 0.5 g of surface-modified TiO 2 @BaSO 4 The powder was dispersed in 50 mL of deionized water, and then 50 mL of molybdenum disulfide solution was added and stirred. The system temperature was raised to 60 °C, and the pH was adjusted to 11. After continuous stirring for 30 min, it was transferred to a reactor and reacted at 100 °C for 8 h to obtain TiO 2 @BaSO 4 / MoS 2 Composite materials.

[0028] Example 2: TiO 2 @BaSO 4 / MoS 2 The composite material was prepared by the following steps:

[0029] Step A1: Disperse 3g of titanium dioxide in 100mL of deionized water and stir to mix evenly, then add 30mL of 0.07mol / L barium chloride solution and continue stirring for 10min, then slowly drop 30mL of 0.07mol / L sodium carbonate solution, after the dropwise addition is completed, continue to react for 2.5h, after the reaction is completed, filter, wash, dry, collect the product, and then transfer the product to a flask, introduce sulfur dioxide to continue the reaction for 1.5h, then introduce air to continue the reaction for 45min, and obtain TiO 2 @BaSO 4 powder;

[0030] Step A2: 2 g TiO 2 @BaSO 4 The powder was ultrasonically dispersed in 50 mL of deionized water for 30 min, and then 0.2 g of hexadecyltrimethylammonium bromide was added and stirred for 10 min. The powder was ultrasonically dispersed for 2 h. After the reaction was completed, the powder was filtered, washed, and dried to obtain surface-modified TiO 2 @BaSO 4 powder;

[0031] Step A3: 3 g of layered molybdenum disulfide was dispersed in a mixture of 30 mL of 1,4-butanediol and 30 mL of deionized water and stirred for 30 min. After ultrasonic dispersion for 8 h, the mixture was centrifuged at 3000 rpm to collect the upper dispersion. The product was then centrifuged at 10000 rpm to collect the product. Then 0.5 g of the product was re-dispersed in 50 mL of deionized water and recorded as molybdenum disulfide solution. 1 g of surface-modified TiO 2 @BaSO 4 The powder was dispersed in 50 mL of deionized water, and then 50 mL of molybdenum disulfide solution was added and stirred. The system temperature was raised to 70 °C, and the pH was adjusted to 11.5. After continuous stirring for 30 min, it was transferred to a reactor and reacted at 120 °C for 10 h to obtain TiO 2 @BaSO 4 / MoS 2 Composite materials.

[0032] Example 3: TiO 2 @BaSO 4 / MoS 2 The composite material was prepared by the following steps:

[0033] Step A1: Disperse 5g of titanium dioxide in 100mL of deionized water and stir to mix evenly, then add 40mL of 0.1mol / L barium chloride solution and continue stirring for 10min, then slowly drop 40mL of 0.1mol / L sodium carbonate solution, after the dropwise addition is completed, continue to react for 3h, after the reaction is completed, filter, wash, dry, collect the product, and then transfer the product to a flask, introduce sulfur dioxide to continue the reaction for 2h, then introduce air to continue the reaction for 60min, and TiO 2 @BaSO 4 powder;

[0034] Step A2: 2 g TiO 2 @BaSO4 powder was ultrasonically dispersed in 50 mL of deionized water for 30 min, 0.5 g of hexadecyltrimethylammonium bromide was added and stirred for 10 min, and then ultrasonically dispersed for 3 h. After the reaction was completed, the powder was filtered, washed, and dried to obtain surface-modified TiO 2 @BaSO4 powder;

[0035] Step A3: 3 g of layered molybdenum disulfide was dispersed in a mixture of 30 mL of 1,4-butanediol and 30 mL of deionized water and stirred for 30 min. After ultrasonic dispersion for 10 h, the mixture was centrifuged at 3000 rpm to collect the upper dispersion. The product was then centrifuged at 10000 rpm to collect the product. Then 1 g of the product was dispersed in 50 mL of deionized water and recorded as molybdenum disulfide solution. 1.5 g of surface-modified TiO 2@BaSO4 powder was dispersed in 50mL deionized water, and then 50mL molybdenum disulfide solution was added and stirred. The system temperature was raised to 80℃, and the pH was adjusted to 12. After continuous stirring for 30min, it was transferred to a reactor and reacted at 130℃ for 12h to obtain TiO 2 @BaSO4 / MoS 2 Composite materials.

[0036] Embodiment 4: A method for preparing a high-performance anti-sticking masterbatch, comprising the following steps:

[0037] Step S1: 0.05 mol 3,5-dihydroxybenzoic acid, 0.05 mol 3-(perfluoro-n-butane)-1,2-epoxypropane and 0.0025 mol tetrabutylammonium bromide are added to 100 mL N,N-dimethylformamide and stirred to mix evenly, nitrogen is introduced and the system temperature is increased to 90° C., and stirred for 4 hours. After the reaction is completed, the product is collected by rotary evaporation, redispersed in 20 mL ethyl acetate, stirred for 10 minutes, washed, dried, and rotary evaporated to obtain an intermediate product;

[0038] Step S2: 0.333 mol of terephthalic acid and 0.3 mol of the intermediate product are added into a reactor and stirred to mix evenly, and then 0.001 mol of methyl tin mercaptan and 0.001 mol of antimony trioxide are added, and the system temperature is increased to 190° C. and the reaction is continued for 2 hours. After the reaction is completed, 0.666 mol of terephthalic acid and 0.8 mol of ethylene glycol are added into the reactor and the reaction is continued for 4 hours. After the reaction is completed, the mixture is cooled to room temperature and crushed to obtain a modified polyester resin;

[0039] Step S3: Weigh the raw materials by weight, and mix 5 parts of TiO 2 @BaSO 4 / MoS 2 The composite material and 0.5 parts of KH550 were added to the reactor and stirred for 5 minutes, and then 0.8 parts of antioxidant 1010 and 1 part of TAS-2A dispersant were added and stirred for 5 minutes. Finally, 30 parts of modified polyester resin were added and stirred for 10 minutes to obtain a mixture. The mixture was then added to an extruder for extrusion and granulation to obtain a high-performance anti-sticking masterbatch. In step S3, the temperatures of the zones of the extruder were as follows: the temperature of zone 1 was 180°C, the temperature of zone 2 was 200°C, the temperatures of zones 3 to 5 were all 230°C, the temperatures of zones 6 to 10 were all 245°C, the head temperature was 255°C, and the screw speed was 240 rpm.

[0040] Embodiment 5: A method for preparing a high-performance anti-sticking masterbatch, comprising the following steps:

[0041] Step S1: 0.1 mol 3,5-dihydroxybenzoic acid, 0.1 mol 3-(perfluoro-n-butane)-1,2-epoxypropane and 0.005 mol tetrabutylammonium bromide are added to 100 mL N,N-dimethylformamide and stirred to mix evenly, nitrogen is introduced and the system temperature is increased to 90° C., and stirred for 5 h. After the reaction is completed, the product is collected by rotary evaporation, redispersed in 20 mL ethyl acetate, stirred for 10 min, washed, dried, and rotary evaporated to obtain an intermediate product;

[0042] Step S2: 0.333 mol of terephthalic acid and 0.4 mol of the intermediate product are added into a reactor and stirred to mix evenly, and then 0.002 mol of methyl tin mercaptan and 0.002 mol of antimony trioxide are added, and the system temperature is increased to 210° C., and the reaction is continued for 2.5 hours. After the reaction is completed, 0.666 mol of terephthalic acid and 1 mol of ethylene glycol are added into the reactor and the reaction is continued for 5 hours. After the reaction is completed, the mixture is cooled to room temperature and crushed to obtain a modified polyester resin;

[0043] Step S3: Weigh the raw materials by weight, and mix 10 parts of TiO prepared in Example 2 2 @BaSO 4 / MoS 2 The composite material and 1 part of KH550 were added to the reactor and stirred for 10 minutes, and then 1.3 parts of antioxidant 1010 and 2 parts of TAS-2A dispersant were added and stirred for 10 minutes. Finally, 50 parts of modified polyester resin were added and stirred for 15 minutes to obtain a mixture. The mixture was then added to an extruder for extrusion and granulation to obtain a high-performance anti-sticking masterbatch. In step S3, the temperatures of the zones of the extruder were as follows: the temperature of zone 1 was 185°C, the temperature of zone 2 was 210°C, the temperatures of zones 3 to 5 were all 235°C, the temperatures of zones 6 to 10 were all 250°C, the head temperature was 260°C, and the screw speed was 260 rpm.

[0044] Embodiment 6: A method for preparing a high-performance anti-sticking masterbatch, comprising the following steps:

[0045] Step S1: adding 0.15 mol 3,5-dihydroxybenzoic acid, 0.15 mol 3-(perfluoro-n-butane)-1,2-epoxypropane and 0.0075 mol tetrabutylammonium bromide into 100 mL N,N-dimethylformamide and stirring to mix evenly, introducing nitrogen and raising the system temperature to 90° C., stirring for 6 h. After the reaction is completed, collecting the product by rotary evaporation, redispersing it in 20 mL ethyl acetate and stirring for 10 min, washing, drying and rotary evaporation to obtain an intermediate product;

[0046] Step S2: 0.333 mol of terephthalic acid and 0.5 mol of the intermediate product are added into a reactor and stirred to mix evenly, and then 0.003 mol of methyl tin mercaptan and 0.003 mol of antimony trioxide are added, and the system temperature is increased to 230° C. and the reaction is continued for 3 hours. After the reaction is completed, 0.666 mol of terephthalic acid and 1.2 mol of ethylene glycol are added into the reactor and the reaction is continued for 6 hours. After the reaction is completed, the mixture is cooled to room temperature and crushed to obtain a modified polyester resin;

[0047] Step S3: Weigh the raw materials by weight, and mix 15 parts of TiO prepared in Example 3 2 @BaSO 4 / MoS 2 The composite material and 2 parts of silane coupling agent are added to the reactor and stirred for 10 minutes, then 2 parts of antioxidant 1010 and 3 parts of TAS-2A dispersant are added and stirred for 10 minutes, and finally 30-80 parts of modified polyester resin are added and stirred for 20 minutes to obtain a mixture, and then the mixture is added to the extruder for extrusion and granulation to obtain a high-performance anti-sticking masterbatch. In step S3, the temperatures of the zones of the extruder are as follows: the temperature of zone 1 is 190° C., the temperature of zone 2 is 220° C., the temperatures of zones 3 to 5 are all 240° C., the temperatures of zones 6 to 10 are all 255° C., the head temperature is 265° C., and the screw speed is 280 rpm.

[0048] Comparative Example 1: This comparative example is an anti-sticking masterbatch, which differs from Example 6 in that an equal amount of polyester resin is used to replace the modified polyester resin, and the rest are the same.

[0049] Comparative Example 2: This comparative example is an anti-sticking masterbatch. The difference from Example 6 is that the TiO prepared in Example 3 is replaced by an equal amount of titanium dioxide. 2 @BaSO 4 / MoS 2 Composite material, all other aspects are the same.

[0050] The anti-sticking masterbatches prepared in Examples 4-6 and Comparative Examples 1-2 were added to PET resin at 2% by weight to prepare 25 μm PET sheets, and the performance tests were performed:

[0051] Friction coefficient test: Tested in accordance with GB 10006-1988 standard;

[0052] UV resistance test: Use a UV lamp with a wavelength of 350nm to irradiate each PET sheet sample for 48 hours at room temperature, where the sample is 10cm away from the UV light source. The retention rate of tensile strength is used to measure the UV aging resistance. The tensile strength is tested according to GB / T 1040.1-2018;

[0053] The test results are shown in the following table:

[0054]

[0055] As can be seen from the above table, the masterbatch prepared by the present invention exhibits lower static friction coefficient and dynamic friction coefficient after the friction test, indicating that the masterbatch has excellent wear resistance and anti-sticking properties; after the UV aging resistance test, it still has a higher tensile strength retention rate, indicating that the masterbatch also has excellent UV aging effect.

[0056] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the scope defined by the concept of the invention, they should all fall within the protection scope of the present invention.

Claims

1. A method for preparing a high-performance anti-sticking masterbatch, It is characterized in that The following steps are involved: Step S1: adding 3,5-dihydroxybenzoic acid, 3-(perfluoro-n-butane)-1,2-propylene oxide and tetrabutylammonium bromide to N,N-dimethylformamide and stirring to mix evenly, introducing nitrogen and raising the system temperature to 90°C, stirring for 4-6 hours, after the reaction is completed, collecting the product by rotary evaporation, redispersing it in ethyl acetate and stirring for 10 minutes, washing, drying and rotary evaporation to obtain an intermediate product; Step S2: adding 1 / 3 of the weight of terephthalic acid and the intermediate product into a reactor and stirring and mixing them evenly, then adding methyl tin mercaptan and antimony trioxide, and raising the system temperature to 190-230° C., and continuing the reaction for 2-3 hours. After the reaction is completed, adding the remaining terephthalic acid and ethylene glycol into the reactor and continuing the reaction for 4-6 hours. After the reaction is completed, cooling to room temperature and crushing to obtain a modified polyester resin; Step S3: Weigh the raw materials by weight, add 5-15 parts of TiO 2 @BaSO4 / MoS 2 The composite material and 0.5-2 parts of silane coupling agent are added to the reactor and stirred for 5-10 minutes, then 0.8-2 parts of antioxidant and 1-3 parts of dispersant are added and stirred for 5-10 minutes, and finally 30-80 parts of modified polyester resin are added and stirred for 10-20 minutes to obtain a mixture, and then the mixture is added to an extruder for extrusion and granulation to obtain a high-performance anti-sticking masterbatch; The TiO 2 @BaSO4 / MoS 2 The composite material was prepared by the following steps: Step A1: Disperse titanium dioxide in deionized water and stir to mix evenly, then add 0.05-0.1 mol / L barium chloride solution and continue stirring for 10 min, then slowly drop 0.05-0.1 mol / L sodium carbonate solution, after the dropwise addition is completed, continue to react for 2-3 h, after the reaction is completed, filter, wash, dry, collect the product, and then transfer the product to a flask, introduce sulfur dioxide to continue the reaction for 1-2 h, and then introduce air to continue the reaction for 30-60 min to obtain TiO 2 @BaSO4 powder; Step A2: TiO 2 @BaSO4 powder was ultrasonically dispersed in deionized water for 30 minutes, and then hexadecyl trimethyl ammonium bromide was added and stirred for 10 minutes, and then ultrasonically dispersed for 1-3 hours. After the reaction was completed, the powder was filtered, washed, and dried to obtain surface-modified TiO 2 @BaSO4 powder; Step A3: dispersing layered molybdenum disulfide in a mixture of 1,4-butanediol and deionized water and stirring for 30 minutes, then ultrasonically dispersing for 6-10 hours, centrifuging at a speed of 3000 rpm, collecting the upper dispersion, and then centrifuging at a speed of 10000 rpm to collect the product, and then re-dispersing the product in deionized water, which is recorded as a molybdenum disulfide solution; Surface modified TiO 2 @BaSO4 powder is dispersed in deionized water, and then molybdenum disulfide solution is added and stirred. The system temperature is raised to 60-80℃, and the pH is adjusted to 11-12. After continuous stirring for 30 minutes, it is transferred to a reactor and reacted at 100-130℃ for 8-12 hours to obtain TiO 2 @BaSO4 / MoS 2 Composite materials.

2. A method for preparing a high-performance anti-sticking masterbatch according to claim 1, It is characterized in that In step S1, the usage ratio of 3,5-dihydroxybenzoic acid, 3-(perfluoro-n-butane)-1,2-propylene oxide, tetrabutylammonium bromide, N,N-dimethylformamide and ethyl acetate is 0.05-0.15 mol: 0.05-0.15 mol: 0.0025-0.0075 mol: 100 mL: 20 mL.

3. A method for preparing a high-performance anti-sticking masterbatch according to claim 1, It is characterized in that In step S2, the usage ratio of terephthalic acid, intermediate product, methyl tin mercaptan, antimony trioxide and ethylene glycol is 1 mol: 0.3-0.5 mol: 0.001-0.003 mol: 0.001-0.003 mol: 0.8-1.2 mol.

4. A method for preparing a high-performance anti-sticking masterbatch according to claim 1, It is characterized in that In step S3, the temperatures of the zones of the extruder are as follows: the temperature of zone 1 is 180-190°C, the temperature of zone 2 is 200-220°C, the temperatures of zones 3 to 5 are 230-240°C, the temperatures of zones 6 to 10 are 245-255°C, the die temperature is 255-265°C, and the screw speed is 240-280 rpm.

5. The method for preparing a high-performance anti-sticking masterbatch according to claim 1, It is characterized in that In step A1, the usage ratio of titanium dioxide, deionized water, barium chloride solution and sodium carbonate solution is 2-5 g: 100 mL: 20-40 mL: 20-40 mL.

6. A method for preparing a high-performance anti-sticking masterbatch according to claim 1, It is characterized in that Step A2 TiO 2 @The dosage ratio of BaSO4 powder, deionized water and hexadecyltrimethylammonium bromide is 2g:50mL:0.05-0.5g.

7. The method for preparing a high-performance anti-sticking masterbatch according to claim 1, It is characterized in that Surface modified TiO in step A3 2 @The dosage ratio of BaSO4 powder, deionized water and molybdenum disulfide solution is 0.5-1.5g:50mL:50mL.