Battery pack bottom guard plate and battery pack and vehicle containing the same
By applying a powder coating with appropriate thickness and roughness on the bottom protection plate of the battery pack, combined with a metal plate and an anti-corrosion layer, the problems of coating wear resistance and sliding friction of the battery pack in the power swap station are solved, and the use of the battery pack is extended. lifespan and improved circulation efficiency.
Patent Information
- Application Number
- CN202410993372.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-07-24
AI Technical Summary
During the battery swapping process of the battery pack in the battery swapping station, the coating on the bottom guard plate has insufficient wear resistance, causing friction damage and affecting the service life of the battery pack. Moreover, the battery pack containing powder coating has serious slippage during sliding friction, affecting circulation. efficiency.
A powder coating with a thickness of 50μm-400μm, a surface roughness of 15μm-60μm, and a battery pack bottom protection plate with a dynamic friction coefficient ≧0.5 is used, combined with a metal plate and anti-corrosion layer to improve the wear resistance and flow stability of the coating.
It extends the number of circulation times of the battery pack in the power swap station, improves the service life, prevents the coating from cracking and damage during the battery swap process, enhances the circulation efficiency, and avoids sliding friction and slippage.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The present application belongs to the field of battery technology, and specifically relates to a battery pack bottom guard plate and a battery pack and a vehicle containing the same. Background Art
[0002] In the past two years, the domestic new energy vehicle market has shown a rapid growth trend. With the rapid development of new energy, the energy replenishment system has become an unavoidable problem. At present, there are two ways to replenish pure electric energy in China. One is the more common construction of charging piles, and the other is the layout of battery swap stations. On the one hand, battery swapping has a crushing advantage in energy replenishment efficiency, such as being more convenient and faster. On the other hand, due to the unified management of battery swap stations, all users no longer need to worry about battery attenuation and safety issues, and can get a battery check every time they swap batteries.
[0003] At present, the warranty period of power batteries is generally 8 years. Battery companies do not have much economic motivation to extend the service life of batteries after selling batteries or vehicle manufacturers that adopt the charging and energy replenishment route after selling vehicles. However, for NIO, which adopts the battery replacement and energy replenishment route, if the battery service life can be extended, it can bring huge economic benefits. Summary of the invention
[0004] The applicant found that when the battery pack is replaced and recharged, it needs to be transported and circulated through chains or rollers at the battery swap station. During the transmission process, the bottom protective plate of the battery pack will inevitably come into contact with the chains or rollers, causing friction; if the wear resistance of the coating on the bottom protective plate of the battery pack is poor, it will cause the coating to become thinner or even expose the metal bottom plate, increasing the risk of the metal bottom plate being exposed or even corroded or punctured by external forces, affecting the service life of the battery pack.
[0005] At present, the bottom guard plate coating of the battery pack is often coated with solvent-based polyvinyl chloride (PVC) coating to achieve the effect of corrosion resistance and stone impact resistance, without considering the wear resistance of the coating. Taking the second-generation battery swap station of NIO as an example, the transmission parts used for battery swap transmission and circulation include chains and rollers. When the battery pack circulates in the battery swap station, the bottom guard plate of the battery pack will slide and rub against the nitrile rubber chain cover and the polyurethane roller. The existing battery pack with PVC coated bottom guard plate will be worn after 500-800 power swaps at the battery swap station, exposing the anti-corrosion layer underneath, thus affecting the service life of the battery pack. If the service life of the battery pack is to be increased to 15 years, according to the normal frequency of use, the battery pack ideally needs to circulate in the battery swap station 1,500 times without wearing through the bottom guard plate coating.
[0006] The applicant found that compared with battery packs with solvent-based coated bottom guard plates, battery packs with powder-coated bottom guard plates have better wear resistance and can increase the service life of the battery pack. However, when replacing batteries and replenishing energy, the battery pack bottom guard plate and the nitrile rubber chain cover and the polyurethane roller are more likely to slide and slip, thereby affecting the circulation efficiency of the battery pack, especially the sliding friction and slippage on the polyurethane roller is more serious.
[0007] In order to solve the problem of sliding friction and slipping of battery packs with powder coated bottom guard plates when circulated in battery swap stations, the present application provides a battery pack bottom guard plate that will not slide friction and slip on the nitrile rubber chain cover and polyurethane roller when circulated through the battery transfer and conveying system in the battery swap station.
[0008] The first aspect of the present application provides a battery pack bottom guard plate, comprising a metal plate and a powder coating arranged on the surface of the metal plate, the thickness of the powder coating is 50μm-400μm, the surface roughness of the powder coating is 15μm-60μm, and the dynamic friction coefficient of the powder coating and nitrile rubber is ≧0.5.
[0009] A second aspect of the present application provides a battery pack, which includes the battery pack bottom guard plate as described in the first aspect, and the powder coating is arranged on the outer surface of the battery pack.
[0010] A third aspect of the present application provides a vehicle, comprising the battery pack as described in the second aspect, wherein the battery pack is mounted on the bottom of the vehicle.
[0011] The beneficial effects of this application are as follows: This application solves the problem of sliding friction and slipping of battery packs with powder-coated bottom guard plates when circulating in battery swap stations, improving the circulation efficiency of battery swap stations, and the powder coating on the bottom guard plate of this application also improves the wear resistance of the battery pack, so that the battery pack can withstand the continuous scraping and friction caused by the periodic sliding of the transmission chain or roller during the battery swap process, increasing the number of battery pack circulations in battery swap stations and improving the service life of the battery pack. Moreover, the compressive pressure of the powder coating can reach 10g / mm 2 -20g / mm 2 , and can withstand the pressure of the entire battery pack during battery replacement without any cracking, breakage, or peeling of the coating. DETAILED DESCRIPTION
[0012] For simplicity, this application only specifically discloses some numerical ranges. However, any lower limit can be combined with any upper limit to form an undefined range; and any lower limit can be combined with other lower limits to form an undefined range, and any upper limit can be combined with any other upper limit to form an undefined range. In addition, each separately disclosed point or single value can itself be combined as a lower limit or upper limit with any other point or single value or with other lower limits or upper limits to form an undefined range.
[0013] In the present application, the terms "upper", "lower", "inner", "outer" and the like indicating directions or positional relationships are only for the convenience of description, and do not indicate or imply that the device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present application. In addition, the terms "first" and "second" are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance.
[0014] In this application, unless otherwise clearly specified and limited, the terms "installation", "setting", and "connection" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a direct connection, an indirect connection through an intermediate medium, or the internal connection of two components. For those skilled in the art, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0015] Unless otherwise specified, the terms used in this application have the commonly known meanings generally understood by those skilled in the art. Unless otherwise specified, the numerical values of the parameters mentioned in this application can be measured using various measurement methods commonly used in the art (for example, they can be tested according to the methods given in the examples of this application).
[0016] The present application is further described below in conjunction with specific implementations. It should be understood that these specific implementations are only used to illustrate the present application and are not used to limit the scope of the present application.
[0017] 1. Battery pack bottom guard plate
[0018] The first aspect of the present application provides a battery pack bottom guard plate, comprising a metal plate and a powder coating disposed on the surface of the metal plate, wherein the thickness of the powder coating is 50 μm-400 μm, the surface roughness of the powder coating is 15 μm-60 μm, and the dynamic friction coefficient between the powder coating and the nitrile rubber is ≧0.5. The applicant has found that by matching the thickness, surface roughness and dynamic friction coefficient of the powder coating with the nitrile rubber, the wear resistance of the coating can be improved, the number of circulation times at the battery swap station can be increased, and the problem of sliding friction and slipping of the battery pack containing the powder coating bottom guard plate when circulating at the battery swap station can be improved.
[0019] In this application, the "dynamic friction coefficient" refers to the ratio of the friction force generated by the relative motion between the battery pack bottom guard plate and the transmission component to the pressure perpendicular to the contact surface between the battery pack bottom guard plate and the transmission component of the battery swap station.
[0020] In this application, "slipping" describes sliding friction slipping, specifically refers to the situation when the friction between the bottom guard plate of the battery pack and the transmission components of the battery swap station cannot completely offset the relative movement trend between the two, causing the battery pack to slip.
[0021] In this application, "wear resistance" refers to the ability of the coating surface to resist wear and tear, which is a kind of material durability. "Wear resistance" means that the coating is not easily worn under high-frequency friction, and the surface will not show phenomena such as thinning and peeling of the skin.
[0022] In this application, "battery swap station circulation times" refers to the number of times a battery pack completes a round trip between the battery compartment and the battery swap platform through the battery transfer and conveying system in the battery swap station. Here, the "battery transfer and conveying system" is used to transfer batteries between the battery swap station platform and the battery compartment, the "battery swap platform" is used to locate and swap batteries for the vehicle, and the "battery compartment" is used to store and charge the battery. Taking the second-generation NIO battery swap station as an example, a battery swap station circulation time refers to a battery pack going back and forth through the cache position, docking position, lifting position and battery compartment in the battery swap station.
[0023] In some embodiments, the dynamic friction coefficient of the powder coating and the nitrile rubber is exemplarily 0.50, 0.52, 0.55, 0.58, 0.60, 0.62, 0.65, 0.68, 0.70, 0.72, 0.75, 0.78, 0.80, 0.82, 0.85, 0.88, 0.9, 0.92, 0.95 or a range consisting of any two of these values. In some embodiments, the dynamic friction coefficient of the powder coating and the nitrile rubber is 0.55-0.85. If the dynamic friction coefficient is too small, the friction between the bottom guard plate of the battery pack and the upper cover of the transmission chain of the battery swap station will not be enough to provide sufficient resistance, resulting in sliding on the contact surface and unable to maintain stable movement. If the dynamic friction coefficient is too large, it will cause wear of the bottom guard plate of the battery pack and the upper cover of the transmission chain of the battery swap station, thereby reducing the service life of the battery pack and increasing the loss of parts of the battery swap station. In some embodiments, the dynamic friction coefficient between the powder coating and the nitrile rubber is 0.60-0.80. In the present application, the dynamic friction coefficient between the powder coating and the nitrile rubber can be regulated by those skilled in the art by adjusting the type of powder coating, coating thickness, coating surface roughness or adding additives.
[0024] In some embodiments, the thickness of the powder coating is 50 μm-400 μm, exemplarily 50 μm, 60 μm, 80 μm, 100 μm, 120 μm, 140 μm, 160 μm, 180 μm, 200 μm, 220 μm, 240 μm, 260 μm, 280 μm, 300 μm, 350 μm, 400 μm or a range consisting of any two of these values. If the thickness of the powder coating is too large, it is necessary to spray the powder coating multiple times, which increases the cost and may also increase the friction coefficient, increase the risk of slipping, and cause incomplete curing of the coating, which is not conducive to improving the wear resistance of the coating. If the thickness of the powder coating is too small, it cannot effectively improve the wear resistance of the battery pack, which is not conducive to increasing the number of circulations of the battery pack in the battery swap station, thereby affecting the service life of the battery pack, and the wear of the thin coating surface is more likely to change the surface properties of the coating and increase the risk of slipping. In some embodiments, the thickness of the powder coating is 50 μm-300 μm. In some embodiments, the thickness of the powder coating is 60 μm-280 μm. In this application, the thickness of the powder coating can be regulated by those skilled in the art by adjusting spraying process parameters such as spraying pressure, spraying speed, spraying distance, nozzle size, etc. according to the type of powder coating selected.
[0025] In some embodiments, the surface roughness of the powder coating is 15μm-60μm, exemplarily 15μm, 16μm, 18μm, 20μm, 22μm, 24μm, 26μm, 28μm, 30μm, 32μm, 34μm, 36μm, 38μm, 40μm, 42μm, 45μm, 48μm, 50μm, 52μm, 55μm, 58μm, 60μm or a range consisting of any two of these values. If the surface roughness of the powder coating is too small, the friction coefficient will be reduced, causing the battery pack to slip when circulating in the battery swap station. If the surface roughness of the powder coating is too large, the coating will be more susceptible to external friction, scratches or wear, which is not conducive to improving the wear resistance of the coating. In some embodiments, the surface roughness of the powder coating is 15μm-50μm. In the present application, the surface roughness of the powder coating can be regulated by those skilled in the art by adjusting the type of powder coating, spray gun pressure and angle, coating thickness, coating curing temperature and time, adding additives, etc. Common additives include inorganic particle powder additives such as silicon dioxide, calcium carbonate, aluminum silicate, aluminum oxide, silicon carbide, etc., and foaming additives.
[0026] In some embodiments, the static friction coefficient between the powder coating and the nitrile rubber is ≧0.6, exemplarily 0.60, 0.62, 0.65, 0.68, 0.70, 0.72, 0.75, 0.78, 0.80, 0.82, 0.85, 0.88, 0.9, 0.92, 0.95, 0.98 or a range consisting of any two of these values. In some embodiments, the static friction coefficient between the powder coating and the nitrile rubber is 0.60-0.98. In some embodiments, the static friction coefficient between the powder coating and the nitrile rubber is 0.60-0.90. In some embodiments, the static friction coefficient between the powder coating and the nitrile rubber is 0.65-0.85. If the static friction coefficient is too large, it will cause wear on the bottom guard plate of the battery pack and the upper cover of the transmission chain of the battery swap station, thereby reducing the service life of the battery pack and increasing the loss of parts of the battery swap station. In the present application, the static friction coefficient between the powder coating and the nitrile rubber can be regulated by those skilled in the art by adjusting the type of powder coating, coating thickness, coating surface roughness or adding additives.
[0027] In this application, "static friction coefficient" refers to the ratio of the friction force generated when the battery pack bottom guard plate and the transmission component are in a relatively static state to the pressure perpendicular to the contact surface between the battery pack bottom guard plate and the transmission component of the battery swap station.
[0028] In some embodiments, the powder coating of the powder coating is selected from one or more of polyester powder coating, epoxy powder coating and polyamide powder coating. In some embodiments, the powder coating is polyester powder coating, epoxy powder coating or polyamide powder coating.
[0029] In some embodiments, the Shore hardness D of the powder coating is 50-95, exemplarily 50, 52, 55, 58, 60, 62, 65, 68, 70, 72, 75, 78, 80, 82, 85, 88, 90, 92, 95 or a range consisting of any two of these values. The applicant has found that the hardness of the powder coating is also related to the wear resistance of the coating. The Shore hardness D of the coating within the above range can better improve the wear resistance of the coating and increase the number of battery pack circulations in the battery swap station. If the hardness of the powder coating is too large, it will wear out the parts of the battery swap station. If the hardness is too small, it will not be conducive to further improving the wear resistance of the battery pack. In some embodiments, the Shore hardness D of the first powder coating is 70-95. In the present application, the Shore hardness D of the powder coating can be regulated by those skilled in the art by adjusting the type of powder coating, coating thickness, coating curing temperature and time, adding additives, etc. Commonly used additives include inorganic particle powder additives such as silicon dioxide, calcium carbonate, aluminum silicate, aluminum oxide, silicon carbide, etc., as well as foaming additives.
[0030] In some embodiments, the metal plate is a steel plate or an aluminum alloy.
[0031] In some embodiments, the metal plate is a steel plate. Compared with other metal plates, the steel plate has better tensile strength and elongation, can meet the impact resistance requirements, and is beneficial to improving the protection of the battery pack, thereby increasing the service life of the battery.
[0032] In some embodiments, an anti-corrosion layer is further provided between the metal plate and the powder coating to further improve the anti-corrosion performance of the metal plate. The anti-corrosion layer may be an electrophoretic layer or a primer layer, as long as the electrophoretic layer or the primer layer can effectively isolate the metal plate from the external environment of the battery pack as a protective layer, and protect the metal plate from environmental erosion, especially when the powder coating is damaged, the metal plate is protected from external erosion, thereby improving the service life of the battery pack.
[0033] In some embodiments, the anticorrosion layer is an epoxy electrophoretic paint layer, an acrylate electrophoretic paint layer, an acrylic electrophoretic paint layer, a polyurethane electrophoretic paint layer, a polyester electrophoretic paint layer, an epoxy primer layer, a polyacrylic primer layer or a polyester primer layer. In some preferred embodiments, the anticorrosion layer is an epoxy primer layer or an epoxy electrophoretic paint layer.
[0034] In some embodiments, the anti-corrosion layer has a thickness of 20 μm-60 μm, exemplarily 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, 55 μm, 60 μm or a range consisting of any two of these values.
[0035] In the present application, the thickness of the electrophoretic layer as the anti-corrosion layer can be controlled by adjusting the electrophoretic time, electric field strength, solution concentration, pH value, etc. The thickness of the primer layer as the anti-corrosion layer can be controlled by adjusting the spraying speed, spraying distance, nozzle size and shape, etc.
[0036] In some embodiments, the battery pack bottom guard plate includes the metal plate and a powder coating disposed on the surface of the metal plate, no anti-corrosion layer is disposed between the metal plate and the powder coating, the powder coating of the powder coating is selected from epoxy powder coating, the thickness of the powder coating is 50μm-400μm, the surface roughness of the powder coating is 15μm-60μm, the dynamic friction coefficient of the powder coating and nitrile rubber is 0.5-0.95, and the static friction coefficient of the powder coating and nitrile rubber is 0.6-0.98.
[0037] In some embodiments, the battery pack bottom guard plate includes the metal plate and a powder coating arranged on the surface of the metal plate, no anti-corrosion layer is arranged between the metal plate and the powder coating, the powder coating of the powder coating is selected from epoxy powder coating, the thickness of the powder coating is 50μm-400μm, the surface roughness of the powder coating is 15μm-60μm, the dynamic friction coefficient of the powder coating and nitrile rubber is 0.5-0.95, the static friction coefficient of the powder coating and nitrile rubber is 0.6-0.98, and the Shore hardness D of the powder coating is 50-95.
[0038] In some embodiments, the battery pack bottom guard plate includes the metal plate and a powder coating arranged on the surface of the metal plate, an anti-corrosion layer is also arranged between the metal plate and the powder coating, the powder coating of the powder coating is selected from polyester powder coating, epoxy powder coating and polyamide powder coating, the thickness of the powder coating is 50μm-400μm, the surface roughness of the powder coating is 15μm-60μm, the dynamic friction coefficient of the powder coating and nitrile rubber is 0.5-0.95, the static friction coefficient of the powder coating and nitrile rubber is 0.6-0.98, the anti-corrosion layer is an epoxy primer layer or an epoxy electrophoretic paint layer, and the thickness of the anti-corrosion layer is 20μm-60μm.
[0039] In some embodiments, the battery pack bottom guard plate includes the metal plate and a powder coating arranged on the surface of the metal plate, an anti-corrosion layer is also arranged between the metal plate and the powder coating, the powder coating of the powder coating is selected from polyester powder coating, epoxy powder coating and polyamide powder coating, the thickness of the powder coating is 50μm-400μm, the surface roughness of the powder coating is 15μm-60μm, the dynamic friction coefficient of the powder coating and nitrile rubber is 0.5-0.95, the static friction coefficient of the powder coating and nitrile rubber is 0.6-0.98, the Shore hardness D of the powder coating is 50-95, the anti-corrosion layer is an epoxy primer layer or an epoxy electrophoretic paint layer, and the thickness of the anti-corrosion layer is 20μm-60μm.
[0040] In some embodiments, the thickness of the metal plate is 0.7 mm-1.5 mm, exemplarily 0.7 mm, 0.9 mm, 1.1 mm, 1.3 mm, 1.5 mm or a range consisting of any two of these values. In some embodiments, the thickness of the metal plate is 0.8 mm-1 mm.
[0041] In some embodiments, the thickness of the battery pack bottom guard plate is 0.7 mm-1.5 mm, exemplarily 0.7 mm, 0.9 mm, 1.1 mm, 1.3 mm, 1.5 mm, or a range consisting of any two of these values. In some embodiments, the thickness of the battery pack bottom guard plate is 0.8 mm-1 mm.
[0042] In some embodiments, the powder coating has a compressive pressure of 10 g / mm 2 -20g / mm 2 , exemplarily 10 g / mm 2 , 12g / mm 2 , 14g / mm 2 , 16g / mm 2 , 18g / mm 2 , 20g / mm 2 Or a range consisting of any two of these values. When the battery pack is replaced, the bottom guard plate needs to withstand the pressure of the entire battery pack, and accordingly the powder coating on the bottom guard plate also needs to withstand the pressure of the entire battery pack, otherwise it will cause cracking, damage, peeling, etc. of the coating.
[0043] 2. Battery Pack
[0044] The second aspect of the present application provides a battery pack, which includes the battery pack bottom guard plate as described in the first aspect, and the powder coating is arranged on the outer surface of the battery pack. The powder coating is arranged on the outer surface of the battery pack to solve the problem that the battery pack is easy to slip when it is circulated in the battery swap station, and can also improve the wear resistance of the battery pack.
[0045] 3. Vehicles
[0046] A third aspect of the present application provides a vehicle, comprising a battery pack as described in the second aspect, wherein the battery pack is installed on the vehicle. In some embodiments, the battery pack is installed on the bottom of the vehicle. When the battery pack is installed, the bottom guard plate of the battery pack is arranged toward the ground.
[0047] In some embodiments, the battery pack is mounted on a chassis of the vehicle, and the battery pack bottom guard plate is disposed away from the chassis.
[0048] In some embodiments, the vehicle is a battery-swappable vehicle. In this application, a battery-swappable vehicle generally refers to all vehicles that support a battery-swappable function. In some embodiments, the vehicle has a structure for replacing the battery pack.
[0049] In some embodiments, the vehicle includes, but is not limited to, an electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. Example
[0050] In the present application, the methods in the examples, unless otherwise specified, are all conventional methods in the art; the raw materials, materials, and reagents in the examples, unless otherwise specified, are all commercially available conventional raw materials, materials, or reagents.
[0051] 1. Determination of dynamic friction coefficient
[0052] The dynamic friction coefficient of powder coating and nitrile rubber was measured with reference to the national standard GB / T 10006-2021 Determination of friction coefficient of plastic films and sheets.
[0053] 2. Determination of static friction coefficient
[0054] The static friction coefficient of powder coating and nitrile rubber was measured with reference to the national standard GB / T 10006-2021 Determination of the friction coefficient of plastic films and sheets.
[0055] 3. Thickness measurement
[0056] The film thickness gauge is used to measure the thickness of powder coating, electrophoretic coating, primer layer and solvent-based coating.
[0057] Use a vernier caliper to measure the thickness of the battery pack bottom guard plate.
[0058] 4. Coating hardness measurement
[0059] The Shore D hardness of powder coatings and solvent-based coatings was measured using an LX-D Shore Hardness Tester.
[0060] 5. Determination of coating surface roughness
[0061] The surface roughness of the powder coating and solvent-based coating was measured by a 3D profiler VR-6000 at a magnification of 50 times, and the arithmetic mean height Sa was taken as the surface roughness value. The measurement accuracy in the Z direction was 0.4 μm, and the measurement accuracy in the X and Y directions was 0.5 μm.
[0062] 6. Coating rotation wear test (Taber test)
[0063] The battery pack bottom guard plate of each embodiment and comparative example was cut into a rectangular sample of 100mm×100mm, and the wear resistance of the powder coating and solvent-based coating was tested with an abrasion tester at room temperature of 23℃±2℃ and relative humidity of 50%±5%. At least 3 samples of each embodiment and comparative example were prepared for testing, and the test results were averaged. The test method refers to GB / T 1768 Determination of the wear resistance of paints and varnishes - Rotating rubber grinding wheel method.
[0064] The parameters of the grinding wheel and wear machine used in the test simulate the actual situation of the NIO battery swap station. The grinding wheel is a polyurethane grinding wheel, the grinding wheel rotation radius is set to 28.25mm, the grinding wheel speed is set to 72r / min, the grinding wheel thickness is set to 8mm, the single wheel load is set to 2kg, and the Shore hardness D of the grinding wheel is 28-38. Every 1000 revolutions of the grinding wheel, check the wear of the powder coating or solvent-based coating in a standard light source color light box. If it is not worn through, use a dry film thickness gauge to measure the film thickness at three points of the friction mark and record it, and use an electronic balance to weigh the film weight before continuing the test.
[0065] Stop the test after the grinding wheel runs 30,000 revolutions or the coating is worn through (whichever comes first), and record the reduction in layer thickness and layer weight of the powder coating or solvent-based coating, with the thickness accurate to 1μm and the weight accurate to 0.001g. If the coating is not worn through after the grinding wheel runs 30,000 revolutions, record the layer thickness and layer weight loss of the coating after running 30,000 revolutions. If the coating is worn through after the grinding wheel runs 6,000 revolutions, record the layer thickness and layer weight loss of the coating after running 6,000 revolutions. "Wear through" here refers to the exposure of the anti-corrosion layer (when an anti-corrosion layer exists) or metal plate (when an anti-corrosion layer does not exist) under the powder coating or solvent-based coating.
[0066] Since the above-mentioned wear test simulates the actual situation of a battery swap station, if the powder coating on the bottom guard plate is not worn through after running 30,000 revolutions, it can be roughly assumed that the powder coating of the battery pack containing this bottom guard plate is not worn through after 1,500 circulations in the battery swap station, which is equivalent to the service life of the battery pack being increased to 15 years.
[0067] 7. Slip test
[0068] The battery pack bottom guard plates of each embodiment and comparative example were cut into rectangular specimens of 100 mm × 100 mm, and the sliding friction and slip of the coating were tested using an abrasion tester at room temperature of 23°C ± 2°C and relative humidity of 50% ± 5%. The test conditions and the grinding wheel used in the test were consistent with those described in the Taber test in the previous section.
[0069] Since the battery pack with a powder-coated bottom guard is more prone to sliding friction and slipping at the polyurethane roller than at the nitrile rubber chain cover, a polyurethane grinding wheel is used here to simulate the polyurethane roller of the NIO battery swap station to test the sliding friction and slipping of the bottom guard.
[0070] If the polyurethane grinding wheel is not observed to idle during its operation of 30,000 revolutions, and there is no abnormal noise or poor positioning of the bottom guard plate, it is considered that there is no sliding friction and slippage. It can also be approximately considered that the battery pack containing this bottom guard plate will not experience sliding friction and slippage on the nitrile rubber chain cover and the polyurethane roller when it is actually circulated in the battery swap station.
[0071] Example 1
[0072] The battery pack bottom guard plate of this embodiment includes a metal plate as a bottom plate and a powder coating disposed on the surface of the metal plate, and an anti-corrosion layer is also disposed between the powder coating and the metal plate. Among them, the metal plate is a steel plate, the anti-corrosion layer is an epoxy primer layer, and the powder coating is a polyester powder coating. The thickness of the anti-corrosion layer and the thickness of the powder coating, Shore hardness D, surface roughness, static friction coefficient and dynamic friction coefficient with nitrile rubber are detailed in Table 1. The overall thickness of the battery pack bottom guard plate is 0.8mm-1mm.
[0073] When preparing the bottom guard plate of the battery pack, first spray epoxy primer on the surface of the steel plate, and after baking, obtain the bottom guard plate substrate, that is, the steel plate with epoxy primer on the surface, and the dry film thickness of the epoxy primer layer is 53μm. The back of the bottom guard plate substrate is masked with masking tape, and polyester powder coating is sprayed on the front of the bottom guard plate substrate. After drying, remove the back masking tape to obtain the bottom guard plate of the battery pack, wherein the thickness of the polyester powder coating is 257μm, the Shore hardness D is 84.4, the surface roughness Sa is 20.2μm, the static friction coefficient with nitrile rubber is 0.78, and the dynamic friction coefficient with nitrile rubber is 0.70.
[0074] Example 2
[0075] The battery pack bottom guard plate of this embodiment includes a metal plate as a bottom plate and a powder coating disposed on the surface of the metal plate. The metal plate is a steel plate and the powder coating is an epoxy powder coating. The thickness, Shore hardness D, surface roughness, static friction coefficient and dynamic friction coefficient of the powder coating with nitrile rubber are shown in Table 1. The overall thickness of the battery pack bottom guard plate is 0.8mm-1mm.
[0076] When preparing the battery pack bottom guard plate, first mask the back of the steel plate with masking tape, spray epoxy powder coating on the surface of the steel plate, and remove the masking tape after drying to obtain the battery pack bottom guard plate, wherein the thickness of the epoxy powder coating is 138μm, the Shore hardness D is 72.8, the surface roughness Sa is 46.3μm, the static friction coefficient with nitrile rubber is 0.66, and the dynamic friction coefficient with nitrile rubber is 0.65.
[0077] Example 3
[0078] The battery pack bottom guard plate of Example 3 is based on Example 2 by changing the spraying process parameters or adding 0.1wt%-5wt% of texture additive to the powder coating to adjust the thickness, Shore hardness D, surface roughness, static friction coefficient and dynamic friction coefficient of the epoxy powder coating. The specific adjusted data are shown in Table 1.
[0079] Example 4
[0080] The battery pack bottom guard plate of Example 4 is based on Example 2 by changing the spraying process parameters or adding 0.1wt%-5wt% of silicon additives to the powder coating to adjust the thickness, Shore hardness D, surface roughness, static friction coefficient and dynamic friction coefficient of the epoxy powder coating. The specific adjusted data are shown in Table 1.
[0081] Example 5
[0082] The battery pack bottom guard plate of this embodiment includes a metal plate as a bottom plate and a powder coating disposed on the surface of the metal plate, and an anti-corrosion layer is also disposed between the powder coating and the metal plate. Among them, the metal plate is a steel plate, the anti-corrosion layer is an epoxy electrophoretic paint layer, and the powder coating is a polyamide (PA11) powder coating. The thickness of the anti-corrosion layer and the thickness of the powder coating, Shore hardness D, surface roughness, static friction coefficient and dynamic friction coefficient with nitrile rubber are detailed in Table 1. The overall thickness of the battery pack bottom guard plate is 0.8mm-1mm.
[0083] When preparing the bottom guard plate of the battery pack, firstly, electrophoresis epoxy is applied on the surface of the steel plate, and after baking, the bottom guard plate substrate is obtained, that is, the steel plate with epoxy electrophoretic paint on the surface, and the dry film thickness of the epoxy electrophoretic paint layer is 31μm. The back of the bottom guard plate substrate is masked with masking tape, and polyamide (PA11) powder coating is sprayed on the front of the bottom guard plate substrate. After drying, the back masking tape is removed to obtain the bottom guard plate of the battery pack, wherein the thickness of the epoxy powder coating is 120μm, the Shore hardness D is 94.7, the surface roughness Sa is 46.7μm, the static friction coefficient with nitrile rubber is 0.73, and the dynamic friction coefficient with nitrile rubber is 0.65.
[0084] Comparative Example 1
[0085] The battery pack bottom guard plate of this comparative example includes a metal plate as a bottom plate and a solvent-based coating arranged on the surface of the metal plate, and an anti-corrosion layer is also arranged between the solvent-based coating and the metal plate. Among them, the metal plate is a steel plate, the anti-corrosion layer is an epoxy electrophoretic paint layer, and the solvent-based coating is a polyvinyl chloride (PVC) coating. The thickness of the anti-corrosion layer and the thickness of the solvent-based coating, Shore hardness D, surface roughness, static friction coefficient and dynamic friction coefficient with nitrile rubber are shown in Table 1. The overall thickness of the battery pack bottom guard plate is 0.8mm-1mm.
[0086] When preparing the bottom guard plate of the battery pack, first electrophoresis epoxy is applied on the surface of the steel plate, and after baking, the bottom guard plate substrate is obtained, that is, the steel plate with epoxy electrophoretic paint on the surface, and the dry film thickness of the epoxy electrophoretic paint layer is 28μm. The back of the bottom guard plate substrate is masked with masking tape, and PVC solvent-based paint is sprayed on the front of the bottom guard plate substrate. After drying, the back masking tape is removed to obtain the battery pack bottom guard plate, wherein the thickness of the PVC solvent-based coating is 995μm, the Shore hardness D is 56.2, the surface roughness Sa is 56.4μm, the static friction coefficient with nitrile rubber is 0.84, and the dynamic friction coefficient with nitrile rubber is 0.75.
[0087] Comparative Example 2
[0088] The battery pack bottom guard plate of Comparative Example 2 is prepared by changing the spraying process parameters of Comparative Example 1 to adjust the thickness, Shore D hardness, surface roughness, static friction coefficient and dynamic friction coefficient of the PVC solvent-based coating. The specific adjusted data are shown in Table 1.
[0089] Comparative Example 3
[0090] The battery pack bottom guard plate of this comparative example includes a metal plate as a bottom plate and a powder coating arranged on the surface of the metal plate, and an anti-corrosion layer is also arranged between the powder coating and the metal plate. Among them, the metal plate is a steel plate, the anti-corrosion layer is an epoxy electrophoretic paint layer, and the powder coating is a PA11 powder coating. The thickness of the anti-corrosion layer and the thickness of the powder coating, Shore hardness D, surface roughness, static friction coefficient and dynamic friction coefficient with nitrile rubber are detailed in Table 1. The overall thickness of the battery pack bottom guard plate is 0.8mm-1mm.
[0091] When preparing the bottom guard plate of the battery pack, first electrophoresis epoxy is applied on the surface of the steel plate, and after baking, the bottom guard plate substrate is obtained, that is, the steel plate with epoxy electrophoretic paint on the surface, and the dry film thickness of the epoxy electrophoretic paint is 24μm. The back of the bottom guard plate substrate is masked with masking tape, and PA11 powder coating is sprayed on the front of the bottom guard plate substrate. After drying, the back masking tape is removed to obtain the battery pack bottom guard plate, wherein the thickness of the PA11 powder coating is 82μm, the Shore hardness D is 90.9, the surface roughness Sa is 16.2μm, the static friction coefficient with nitrile rubber is 0.42, and the dynamic friction coefficient with nitrile rubber is 0.32.
[0092] Comparative Example 4
[0093] The battery pack bottom guard plate of Comparative Example 4 is obtained by adjusting the thickness of the anti-corrosion layer by changing the electrophoresis process parameters based on Comparative Example 1, and adjusting the thickness, Shore hardness D, surface roughness, static friction coefficient and dynamic friction coefficient of the PA11 powder coating by changing the spraying process parameters. The specific adjusted data are shown in Table 1.
[0094] Comparative Example 5
[0095] The battery pack bottom guard plate of Comparative Example 5 is based on Comparative Example 1, by changing the electrophoresis process parameters to adjust the thickness of the anti-corrosion layer, and by changing the spraying process parameters or adding 5wt%-8wt% of inorganic particle powder to the powder coating to adjust the thickness, Shore hardness D, surface roughness, static friction coefficient and dynamic friction coefficient of the PA11 powder coating. The specific adjusted data are shown in Table 1.
[0096] Comparative Example 6
[0097] The battery pack bottom guard plate of this comparative example includes a metal plate as a bottom plate and a powder coating disposed on the surface of the metal plate. The metal plate is a steel plate and the powder coating is an epoxy powder coating. The thickness, Shore hardness D, surface roughness, static friction coefficient and dynamic friction coefficient of the powder coating with nitrile rubber are shown in Table 1. The overall thickness of the battery pack bottom guard plate is 0.8mm-1mm.
[0098] When preparing the battery pack bottom guard plate, first mask the back of the steel plate with masking tape, spray epoxy powder coating on the surface of the steel plate, and remove the masking tape after drying to obtain the battery pack bottom guard plate, wherein the thickness of the epoxy powder coating is 130 μm, the Shore hardness D is 91.8, the surface roughness Sa is 17.5 μm, the static friction coefficient with nitrile rubber is 0.45, and the dynamic friction coefficient with nitrile rubber is 0.40.
[0099] Comparative Example 7
[0100] The battery pack bottom guard plate of Comparative Example 7 is obtained by changing the spraying process parameters or adding 0.5wt%-3wt% of foaming aid to the powder coating to adjust the thickness, Shore hardness D, surface roughness, static friction coefficient and dynamic friction coefficient of the epoxy powder coating on the basis of Comparative Example 6. The specific adjusted data are shown in Table 1.
[0101] Comparative Example 8
[0102] The battery pack bottom guard plate of Comparative Example 8 is obtained by changing the spraying process parameters or adding 0.5wt%-3wt% of foaming aid to the powder coating to adjust the thickness, Shore hardness D, surface roughness, static friction coefficient and dynamic friction coefficient of the epoxy powder coating on the basis of Comparative Example 6. The specific adjusted data are shown in Table 1.
[0103] Comparative Example 9
[0104] The battery pack bottom guard plate of Comparative Example 9 is adjusted by changing the spraying process parameters on the basis of Comparative Example 6 to adjust the thickness, Shore D hardness, surface roughness, static friction coefficient and dynamic friction coefficient of the epoxy powder coating with nitrile rubber. The specific adjusted data are shown in Table 1.
[0105] Table 1
[0106]
[0107] Table 2 records the wear test results of the rotational wear @30,000 revolutions of the bottom guard plates of each embodiment and comparative example, as well as the results of whether there was slippage observed during the test. It can be seen that the bottom guard plates of Examples 1-6 of the present application do not have any sliding friction and slippage with the polyurethane grinding wheel during the entire test process of rotational wear @30,000 revolutions compared to the bottom guard plates of Comparative Examples 1-9, and also have excellent wear resistance, indicating that when they are actually circulated in battery swap stations, they can not only increase the number of battery pack circulations and improve the service life of the battery pack, but also will not cause sliding friction and slippage at the polyurethane roller and the upper cover of the nitrile rubber chain. In addition, the powder coatings of the bottom guard plates of Examples 1-6 of the present application can withstand 10g / mm 2 -20g / mm 2 The compressive pressure will not cause cracking, damage or peeling of the coating.
[0108] Table 2
[0109]
[0110] Although some exemplary embodiments of the present application have been illustrated and described, the present application is not limited to the disclosed embodiments. On the contrary, those skilled in the art will recognize that some modifications and changes may be made to the described embodiments without departing from the spirit and scope of the present application as described in the appended claims.
Claims
1. A battery pack bottom guard plate, characterized in that: It comprises a metal plate and a powder coating arranged on the surface of the metal plate, wherein the thickness of the powder coating is 50 μm-400 μm, the surface roughness of the powder coating is 15 μm-60 μm, and the dynamic friction coefficient between the powder coating and the nitrile rubber is ≧0.5; The dynamic friction coefficient between the powder coating and the nitrile rubber is 0.5-0.95; The static friction coefficient between the powder coating and the nitrile rubber is 0.6-0.98; The powder coating of the powder coating is selected from polyester powder coating, epoxy powder coating and polyamide powder coating.
2. The battery pack bottom guard plate according to claim 1, characterized in that: The powder coating has a Shore D hardness of 50-95.
3. The battery pack bottom guard plate according to claim 1 or 2, characterized in that: An anti-corrosion layer is also provided between the metal plate and the powder coating, and the thickness of the anti-corrosion layer is 20 μm-60 μm.
4. The battery pack bottom guard plate according to claim 3, characterized in that: The anti-corrosion layer is an epoxy primer layer or an epoxy electrophoretic paint layer.
5. A battery pack, characterized in that: It comprises a battery pack bottom guard plate as described in any one of claims 1 to 4, wherein the powder coating is arranged on the outer surface of the battery pack.
6. The battery pack according to claim 5, characterized in that: The compressive pressure of the powder coating is 10g / mm 2 -20g / mm 2 .
7. A vehicle, characterized in that: Comprising a battery pack as claimed in claim 5 or 6, wherein the battery pack is installed in the vehicle.
8. The vehicle according to claim 7, characterized in that The vehicle has a structure for replacing the battery pack.
Citation Information
Patent Citations
Coating composition, cured product and laminate, and manufacturing process for cured product
JP2002302645A
Corrosion resistant coating and method for forming the same
JP2020157689A