Method for preparing polyurethane-epoxy resin composite material adhesive
By preparing a polyurethane-epoxy resin composite adhesive and utilizing the ferrocene, borate and tert-butylphenol groups in the antioxidant polyurethane prepolymer, the mechanical properties and high temperature resistance of the epoxy resin adhesive were solved. The problem of insufficient performance has been achieved by improving the toughness and heat resistance of the material.
Patent Information
- Application Number
- CN202411068182.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-08-06
AI Technical Summary
Existing epoxy resin adhesives have poor mechanical properties and insufficient high temperature resistance, making it difficult to meet the high requirements of engineering technology.
The preparation method of polyurethane-epoxy resin composite adhesive is adopted, by weighing the epoxy resin and antioxidant polyurethane prepolymer in parts by weight in the reactor, adding the curing agent and performing vacuum degassing and reaction under nitrogen protection. , forming a polyurethane-epoxy composite adhesive with ferrocene, borate ester, and tert-butylphenol groups.
Significantly improves the toughness and heat resistance of the material, enhances the mechanical properties and heat resistance, and is suitable for a wide range of bonding and high hardness applications.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of epoxy resin adhesive preparation, in particular to a method for preparing a polyurethane-epoxy resin composite adhesive. Background Art
[0002] Epoxy resin is a commonly used thermosetting resin. It is widely used in adhesives, coatings, composite matrix, etc. due to its excellent adhesion, mechanical strength, electrical insulation and good processing properties. Pure epoxy resin has a large proportion of cross-linked structure, so it has the disadvantages of brittleness, poor fatigue resistance, poor heat resistance, and poor impact resistance. It is difficult to meet higher engineering technical requirements, and its application is subject to certain restrictions. Therefore, the modification of epoxy resin is a hot topic, among which the toughening of epoxy resin is the key research direction.
[0003] A Chinese patent application with publication number CN114214019A discloses a method for preparing a one-component adhesive that can withstand high and low temperatures; the method for preparing the one-component adhesive that can withstand high and low temperatures includes epoxy resin, cyanate resin, ultra-low temperature resistant resin, toughening resin, active diluent, latent curing agent, accelerator, coupling agent, and inorganic filler.
[0004] The Chinese patent with the authorization announcement number CN103524703B discloses a method for preparing a polyurethane / epoxy resin composite material. After adding polyether polyol to the reactor for treatment, adding diisocyanate to heat up, controlling the free -NCO mass content, and vacuum degassing, component A is obtained; the diaryl amine is heated up, liquid epoxy resin is added dropwise and the temperature is raised again to react, and component B is obtained; finally, components A and B are stirred and mixed according to the metering, reacted and cured, and a polyurethane / epoxy resin composite material is obtained. The composite material has excellent bonding strength, high and low temperature resistance, impact resistance and flexibility when used as an adhesive, and has a wide range of applications. It can also be made into a high-hardness polyurethane elastomer composite material for application. Its decomposition temperature is 254°C and the peel strength is 7.6KN / m.
[0005] The epoxy resin adhesives prepared by the above patents and prior art have poor mechanical properties and poor high temperature resistance. Summary of the invention
[0006] In order to solve the above problems, the present invention provides a method for preparing a polyurethane-epoxy resin composite adhesive, and the operating steps are as follows:
[0007] S1: Weigh 80-100 parts of epoxy resin E44 and 30-40 parts of antioxidant polyurethane prepolymer in a reaction kettle by weight, stir, keep warm and degas in vacuum for 90-120 minutes under nitrogen protection;
[0008] S2: adding 1-5 parts of curing agent and stirring evenly to obtain a polyurethane-epoxy resin composite adhesive;
[0009] The preparation method of the antioxidant polyurethane prepolymer is:
[0010] A1: Add 17-34 parts of toluene diisocyanate, 2.5-6 parts of ethyl isocyanate acrylate and 200-300 parts of DMF to a reactor by mass, and stir evenly under nitrogen protection;
[0011] A2: Add 10-16 parts of trans-3-hydroxypropylene boric acid pinacol ester, 10-18 parts of polyoxypropylene ether glycol, and 2-5 parts of stannous octoate, and react at 60-70°C for 50-150 minutes;
[0012] A3: Add 0.04-0.15 parts of 4-allyl-2,6-di-tert-butylphenol, 1.4-3.5 parts of (ferrocenyl) hexanethiol, and 2-5 parts of triethylamine, the reaction temperature is 60-70°C, the time is 40-100 minutes, and DMF is removed by distillation to obtain an antioxidant polyurethane prepolymer.
[0013] The stirring speed is 200-300r / min.
[0014] The reaction temperature of S1 is 50-60°C.
[0015] The curing agent is one of triethylamine, tripropylamine, tributylamine, maleic anhydride and N-benzyldimethylamine.
[0016] The molecular weight of the polyoxypropylene ether glycol is 400, 600, 800 or 1000.
[0017] The reaction temperature of S2 is 75-90°C and the reaction time is 85-130min.
[0018] Reaction mechanism: Formation of polyurethane: Toluene diisocyanate and ethyl isocyanate acrylate react with trans-3-hydroxypropylene pinacol borate and polypropylene oxide ether diol to form a polyurethane with pinacol borate and ethyl acrylate groups; the introduction of these groups provides the necessary functional groups for the subsequent thiol-allyl reaction, and also provides additional functionality to the final polymer, enhancing the mechanical properties of the material.
[0019] The thiol-allyl reaction of 4-allyl-2,6-di-tert-butylphenol and (ferrocenyl)hexanethiol further introduced the two structures of ferrocene and tert-butylphenol; ferrocene worked together with borate and tert-butylphenol to significantly improve the heat resistance of the material.
[0020] The method for preparing a polyurethane-epoxy resin composite material adhesive of the present invention has the following beneficial effects:
[0021] 1. The polyurethane-epoxy resin composite material adhesive prepared by the present invention can play a good role in dispersing stress and effectively improve the toughness of the material;
[0022] 2. The present invention obtains an antioxidant polyurethane prepolymer by modifying epoxy resin with polyurethane. The polyurethane prepolymer contains key groups such as ferrocene, borate and tert-butylphenol. The combined effect of these groups makes the polyurethane-epoxy resin composite adhesive not only have good mechanical properties, but also have improved heat resistance. DETAILED DESCRIPTION
[0023] In order to further explain the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the following is a detailed description in combination with embodiments and comparative examples:
[0024] Peel strength test, bonding strength test: refer to GB / T39289-2020 for testing.
[0025] Heat resistance test: The test was conducted using a thermogravimetric analyzer (TA Instruments TGAQ50, USA); heating rate: 10°C / min; test atmosphere: air.
[0026] Example 1: A method for preparing a polyurethane-epoxy resin composite adhesive, the operating steps of which are:
[0027] S1: Weigh 80g of epoxy resin E44 and 30g of antioxidant polyurethane prepolymer into a reaction kettle, stir under nitrogen protection, and keep warm and vacuum degas for 90min;
[0028] S2: Add 1 g of curing agent and stir evenly to obtain a polyurethane-epoxy resin composite adhesive;
[0029] The preparation method of the antioxidant polyurethane prepolymer is:
[0030] A1: Add 17g toluene diisocyanate, 2.5g ethyl isocyanate acrylate and 200g DMF into a reaction kettle and stir evenly under nitrogen protection;
[0031] A2: Add 10g of trans-3-hydroxypropylene pinacol borate, 10g of polyoxypropylene ether glycol, and 2g of stannous octoate, and react at 60°C for 50min;
[0032] A3: 0.04 g of 4-allyl-2,6-di-tert-butylphenol, 1.4 g of (ferrocenyl) hexanethiol, and 2 g of triethylamine were added, the reaction temperature was 60° C., the reaction time was 40 min, and DMF was removed by distillation to obtain an antioxidant polyurethane prepolymer.
[0033] The stirring speed is 200r / min.
[0034] The reaction temperature of S1 is 50°C.
[0035] The curing agent is triethylamine.
[0036] The molecular weight of the polyoxypropylene ether glycol is 400.
[0037] The reaction temperature of S2 is 75°C and the reaction time is 85 minutes.
[0038] Example 2: A method for preparing a polyurethane-epoxy resin composite adhesive, the operating steps of which are as follows:
[0039] S1: Weigh 85g of epoxy resin E44 and 33g of antioxidant polyurethane prepolymer into a reaction kettle, stir under nitrogen protection, and keep warm and vacuum degas for 100min;
[0040] S2: adding 2 g of curing agent and stirring evenly to obtain a polyurethane-epoxy resin composite adhesive;
[0041] The preparation method of the antioxidant polyurethane prepolymer is:
[0042] A1: Add 22g toluene diisocyanate, 3.7g ethyl isocyanate acrylate and 240g DMF into a reaction kettle and stir evenly under nitrogen protection;
[0043] A2: Add 12g of trans-3-hydroxypropylene boric acid pinacol, 14g of polyoxypropylene ether glycol, and 3g of stannous octoate, and react at 65°C for 90min;
[0044] A3: 0.08 g of 4-allyl-2,6-di-tert-butylphenol, 2.1 g of (ferrocenyl) hexanethiol, and 3 g of triethylamine were added, the reaction temperature was 65° C., the reaction time was 60 min, and DMF was removed by distillation to obtain an antioxidant polyurethane prepolymer.
[0045] The stirring speed is 250r / min.
[0046] The reaction temperature of S1 is 55°C.
[0047] The curing agent is tripropylamine.
[0048] The molecular weight of the polyoxypropylene ether glycol is 600.
[0049] The reaction temperature of S2 is 80°C and the reaction time is 100 min.
[0050] Example 3: A method for preparing a polyurethane-epoxy resin composite adhesive, the operating steps of which are as follows:
[0051] S1: Weigh 95g of epoxy resin E44 and 38g of antioxidant polyurethane prepolymer into a reaction kettle, stir under nitrogen protection, and degas under vacuum for 110min;
[0052] S2: Add 4 g of curing agent and stir evenly to obtain a polyurethane-epoxy resin composite adhesive;
[0053] The preparation method of the antioxidant polyurethane prepolymer is:
[0054] A1: Add 28g toluene diisocyanate, 5g ethyl isocyanate acrylate and 280g DMF into a reaction kettle and stir evenly under nitrogen protection;
[0055] A2: Add 15g of trans-3-hydroxypropylene pinacol borate, 16g of polyoxypropylene ether glycol, and 4g of stannous octoate, and react at 65°C for 130min;
[0056] A3: 0.13 g of 4-allyl-2,6-di-tert-butylphenol, 3.2 g of (ferrocenyl) hexanethiol, and 4 g of triethylamine were added, the reaction temperature was 65° C., the reaction time was 80 min, and DMF was removed by distillation to obtain an antioxidant polyurethane prepolymer.
[0057] The stirring speed is 250r / min.
[0058] The reaction temperature of S1 is 55°C.
[0059] The curing agent is tributylamine.
[0060] The molecular weight of the polyoxypropylene ether glycol is 800.
[0061] The reaction temperature of S2 is 85°C and the reaction time is 120 minutes.
[0062] Example 4: A method for preparing a polyurethane-epoxy resin composite adhesive, the operating steps of which are as follows:
[0063] S1: Weigh 100g of epoxy resin E44 and 40g of antioxidant polyurethane prepolymer into a reaction kettle, stir under nitrogen protection, and keep warm and vacuum degas for 120min;
[0064] S2: Add 5 g of curing agent and stir evenly to obtain a polyurethane-epoxy resin composite adhesive;
[0065] The preparation method of the antioxidant polyurethane prepolymer is:
[0066] A1: Add 34g toluene diisocyanate, 6g ethyl isocyanate acrylate and 300g DMF into a reaction kettle and stir evenly under nitrogen protection;
[0067] A2: Add 16g of trans-3-hydroxypropylene pinacol borate, 18g of polyoxypropylene ether glycol, and 5g of stannous octoate, and react at 70°C for 150min;
[0068] A3: 0.15 g of 4-allyl-2,6-di-tert-butylphenol, 3.5 g of (ferrocenyl) hexanethiol, and 5 g of triethylamine were added, the reaction temperature was 70° C., the time was 100 min, DMF was removed by distillation, and an antioxidant polyurethane prepolymer was obtained.
[0069] The stirring speed is 300r / min.
[0070] The reaction temperature of S1 is 60°C.
[0071] The curing agent is maleic anhydride.
[0072] The molecular weight of the polyoxypropylene ether glycol is 1000.
[0073] The reaction temperature of S2 is 90°C and the reaction time is 130 minutes.
[0074] Comparative Example 1: DW3432 polyurethane prepolymer was used instead of the antioxidant polyurethane prepolymer, and the rest was the same as Example 1.
[0075] Comparative Example 2: 4-allyl-2,6-di-tert-butylphenol was not added, and the other steps were the same as in Example 1.
[0076] Comparative Example 3: Trans-3-hydroxypropylene boric acid pinacol ester was not added, and the other conditions were the same as those in Example 1.
[0077] Table 1: Test results of various embodiments and comparative examples
[0078]
[0079] Through the data analysis of the above embodiments and comparative examples, the polyurethane prepolymer obtained by the present invention through polyurethane modified epoxy resin contains key groups such as ferrocene, borate and tert-butylphenol; the combined effect of these groups makes the polyurethane-epoxy resin composite adhesive not only have good mechanical properties, but also improve the heat resistance, which can effectively improve the mechanical properties and heat resistance of the material.
[0080] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. A method for preparing a polyurethane-epoxy resin composite adhesive, characterized in that: The operation steps are: S1: Weigh 80-100 parts of epoxy resin E44 and 30-40 parts of antioxidant polyurethane prepolymer in a reaction kettle by weight, stir, keep warm and degas in vacuum for 90-120 minutes under nitrogen protection; S2: adding 1-5 parts of curing agent and stirring evenly to obtain a polyurethane-epoxy resin composite adhesive; The preparation method of the antioxidant polyurethane prepolymer is: A1: Add 17-34 parts of toluene diisocyanate, 2.5-6 parts of ethyl isocyanate acrylate and 200-300 parts of DMF to a reactor by mass, and stir evenly under nitrogen protection; A2: Add 10-16 parts of trans-3-hydroxypropylene boric acid pinacol ester, 10-18 parts of polyoxypropylene ether glycol, and 2-5 parts of stannous octoate, and react at 60-70°C for 50-150 minutes; A3: Add 0.04-0.15 parts of 4-allyl-2,6-di-tert-butylphenol, 1.4-3.5 parts of (ferrocenyl) hexanethiol, and 2-5 parts of triethylamine, the reaction temperature is 60-70°C, the time is 40-100 minutes, and DMF is removed by distillation to obtain an antioxidant polyurethane prepolymer.
2. The method for preparing a polyurethane-epoxy resin composite adhesive according to claim 1, characterized in that: The stirring speed is 200-300r / min.
3. The method for preparing a polyurethane-epoxy resin composite adhesive according to claim 1, characterized in that: The reaction temperature of S1 is 50-60°C.
4. The method for preparing a polyurethane-epoxy resin composite adhesive according to claim 1, characterized in that: The curing agent is one of triethylamine, tripropylamine, tributylamine, maleic anhydride and N-benzyldimethylamine.
5. The method for preparing a polyurethane-epoxy resin composite adhesive according to claim 1, characterized in that: The molecular weight of the polyoxypropylene ether glycol is 400, 600, 800 or 1000.
6. The method for preparing a polyurethane-epoxy resin composite adhesive according to claim 1, characterized in that: The reaction temperature of S2 is 75-90°C and the reaction time is 85-130min.
Citation Information
Patent Citations
A preparation method of a polyurethane / epoxy resin composite material
CN103524703B
Preparation method of single-component adhesive capable of resisting high and low temperatures
CN114214019A
Preparation method of polyurethane toughened epoxy resin
CN114773610A
Thermoplastic polyurethane material and preparation method thereof
CN117659390A
Epoxy resin batch for composite material pultrusion and preparation method therefor
WO2023221619A1