A multilayer drag-reducing and ice-proof composite material and its preparation method and application

By generating a nickel-copper oxide composite porous coating and a cross-linked polymer film on a metal substrate, combined with a cross-linked flexible photothermal layer, the stability and low-temperature resistance problems of drag reduction materials in the existing technology are solved, and high performance is achieved Drag reduction effect and ice protection function.

CN118581537BActive Publication Date: 2024-10-22NINGBO INST OF MATERIALS TECH & ENG CHINESE ACAD OF SCI
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411062196.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-10-22
Estimated Expiration
2044-08-05

AI Technical Summary

Technical Problem

The existing passive bionic drag reduction technology has shortcomings in terms of stability and low temperature resistance. The rigid superhydrophobic surface is easy to wear. The flexible drag reduction technology is easy to deform under high flow fields and cannot be restored. In polar areas, it is easy to freeze and increase navigation resistance. .

Method used

The cyclic electroplating and high-temperature sintering method is used to generate a nickel-copper oxide composite porous coating on the metal substrate, and the polymer film is cross-linked on its surface and in the pores to form a rigid-flexible interlocking hybrid film layer, which is then combined with the cross-linked flexible photothermal The layers are combined to prepare a multi-layer drag reduction and anti-icing composite material.

Benefits of technology

A high-performance drag-reducing material that combines the rigidity of a superhydrophobic surface with the flexibility of dolphin skin has been realized, which can effectively reduce drag in extremely cold conditions, delay icing, accelerate de-icing, and improve navigation efficiency through non-radiative heating and thermal conductivity properties. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118581537B_ABST
    Figure CN118581537B_ABST
Patent Text Reader

Abstract

The present invention discloses a multilayer drag-reducing and anti-icing composite material and its preparation method and application. The multilayer drag-reducing and anti-icing composite material includes a nickel-copper oxide composite porous coating, a cross-linked polymer film layer and a cross-linked flexible photothermal layer stacked on a metal substrate. The preparation method includes: using cyclic electroplating and high-temperature sintering to generate a nickel-copper oxide composite porous coating on a metal substrate, and then brushing a cross-linked polymer film layer on the surface and pores of the nickel-copper oxide composite porous coating to obtain a rigid-flexible interlocking hybrid film layer; finally, a cross-linked flexible photothermal layer is generated. The multilayer drag-reducing and anti-icing composite material prepared by the present invention has both the rigidity of a super-hydrophobic surface and the flexibility of dolphin skin, as well as good non-radiative heating and thermal conductivity properties. The functional layers complement each other and are multifunctionally coupled to obtain a high-performance drag-reducing composite material, which is not only suitable for drag reduction of conventional sea vessels, but also can be used for drag reduction, energy saving and consumption reduction of vessels in extremely cold waters at the two poles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a drag reducing material, in particular to a multi-layer drag reducing and anti-icing composite material and a preparation method and application thereof, belonging to the technical field of marine drag reducing materials. Background Art

[0002] Passive bionic drag reduction technology is one of the effective means to reduce the friction resistance of navigation. It can increase the navigation speed and range of the aircraft and reduce energy consumption. Existing passive bionic drag reduction technologies include super hydrophobic drag reduction technology and flexible drag reduction technology. Super hydrophobic drag reduction technology is based on the extremely low water adhesion of rigid rough surfaces. When the fluid flows over the rigid rough super hydrophobic surface, a velocity slip phenomenon occurs in the near-wall area, thereby reducing the shear stress of the fluid, effectively increasing the thickness of the boundary layer, reducing turbulence, and achieving the purpose of reducing fluid resistance. However, the rigid rough super hydrophobic surface is easy to wear and has poor stability. Flexible drag reduction technology represented by dolphin skin is simple to construct, and its flow field restriction conditions are not as strict as super hydrophobic drag reduction technology. Flexible materials with different mechanical properties can be used to adapt to flow fields of different intensities, thereby obtaining an effective and stable drag reduction effect. However, once the external flow field is too strong, the flexible surface will be permanently deformed and cannot be restored, and the drag reduction effect will be lost. In addition, in winter or polar regions, the water temperature drops significantly, and the parts of the ship hull, propeller, etc. that are in contact with the water are prone to ice, bringing additional navigation resistance. Therefore, stable and low-temperature resistant drag-reducing materials have broader application prospects. Summary of the invention

[0003] The main purpose of the present invention is to provide a multi-layer drag-reducing and anti-icing composite material and a preparation method thereof, so as to overcome the deficiencies in the prior art.

[0004] Another object of the present invention is to provide an application of the multi-layer drag-reducing and ice-preventing composite material.

[0005] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes:

[0006] An embodiment of the present invention provides a method for preparing a multilayer drag-reducing and ice-proof composite material, which comprises:

[0007] (1) using a metal substrate as a first cathode and nickel as a first anode, making the first cathode, the first anode and a nickel salt-containing electroplating solution form a first electrochemical working system, and applying power to perform a first electrodeposition reaction to generate a nickel plating layer, thereby obtaining a metal substrate wrapped with the nickel plating layer;

[0008] The metal substrate wrapped with the nickel-plated layer is used as a second cathode and copper is used as a second anode, so that the second cathode, the second anode and a copper salt-containing electroplating solution form a second electrochemical working system, and power is supplied to perform a second electrodeposition reaction, so as to form a copper-plated layer on the nickel-plated layer, thereby obtaining a nickel-copper composite porous plating layer;

[0009] The first electrodeposition reaction and the second electrodeposition reaction are cyclically performed more than once, and then high-temperature sintering is performed to obtain a metal substrate wrapped with a nickel-copper oxide composite porous coating;

[0010] (2) bringing a first mixed aqueous solution comprising a charged polymer, a water-soluble polymer and a cross-linking agent into full contact with a metal substrate wrapped with the nickel-copper oxide composite porous coating prepared in step (1), thereby cross-linking on the surface and in the pores of the nickel-copper oxide composite porous coating to form a cross-linked polymer film layer, wherein the cross-linked polymer film layer and the nickel-copper oxide composite porous coating together constitute a rigid-flexible interlocking hybrid film layer;

[0011] (3) The rigid-flexible interlocking hybrid film layer prepared in step (2) is first fully contacted with a second mixed aqueous solution containing a two-dimensional sheet material, micro-nano particles, and a polymer material, and then fully contacted with an inorganic salt solution to generate a cross-linked flexible photothermal layer, thereby obtaining a multi-layer drag reduction and anti-icing composite material.

[0012] The embodiment of the present invention also provides a multi-layer drag-reducing and ice-proof composite material prepared by the aforementioned method.

[0013] In some embodiments, the multilayer drag reduction and anti-icing composite material includes a nickel-copper oxide composite porous coating, a cross-linked polymer film layer, and a cross-linked flexible photothermal layer stacked in sequence in the thickness direction of the metal substrate, wherein the nickel-copper oxide composite porous coating and the cross-linked polymer film layer together constitute a rigid-flexible interlocking hybrid film layer.

[0014] The embodiment of the present invention also provides the application of the aforementioned multi-layer drag reduction and anti-icing composite material in the field of drag reduction and protection of marine vehicles.

[0015] Compared with the prior art, the beneficial effects of the present invention include:

[0016] The multilayer drag-reducing and anti-icing composite material prepared by the present invention has both the rigidity of a super-hydrophobic surface and the flexibility of dolphin skin, as well as good non-radiative heating and thermal conductivity properties. The functional layers complement each other's advantages and are multifunctionally coupled to obtain a high-performance drag-reducing composite material, which is not only suitable for drag reduction of conventional sea vessels, but also can be used for drag reduction, energy saving and consumption reduction of vessels in extremely cold waters at the two poles. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0018] Figure 1 2 is a schematic diagram of the structure of a multilayer drag-reducing and anti-icing composite material in a typical embodiment of the present invention;

[0019] Figure 2 is a surface SEM image of the nickel-copper oxide composite porous coating prepared in Example 4 of the present invention;

[0020] Figure 3 is a surface SEM image of the cross-linked polymer film layer prepared in Example 4 of the present invention;

[0021] Figure 4 This is a surface SEM image of the cross-linked flexible photothermal layer prepared in Example 4 of the present invention.

[0022] Figure numerals: 1-metal substrate, 2-nickel-copper oxide composite porous coating, 3-cross-linked polymer film layer, 4-cross-linked flexible photothermal layer, 5-rigid-flexible interlocking hybrid film layer. DETAILED DESCRIPTION

[0023] In view of the problems existing in the above-mentioned prior art, after long-term research and a large number of experiments, the inventor of this case proposed this technical solution, which mainly adopts the cyclic electroplating and high-temperature sintering method to generate a nickel-copper oxide composite porous coating on a metal substrate, and then brushes a cross-linked polymer film on the surface and pores of the nickel-copper oxide composite porous coating to obtain a rigid-flexible interlocking hybrid film layer; finally, a cross-linked flexible photothermal layer is generated, and the advantages of multiple layers are complementary and multifunctionally coupled, and finally a composite material with high drag reduction performance is obtained. The technical solution, its implementation process and principle will be further explained as follows.

[0024] As one aspect of the technical solution of the present invention, it involves a multi-layer drag reduction and ice prevention composite material, please refer to Figure 1 As shown, it includes a nickel-copper oxide composite porous coating 2, a cross-linked polymer film layer 3 and a cross-linked flexible photothermal layer 4 which are stacked layer by layer in the thickness direction of the metal substrate 1, wherein the nickel-copper oxide composite porous coating 2 and the cross-linked polymer film layer 3 together constitute a rigid-flexible interlocking hybrid film layer 5.

[0025] Furthermore, the multilayer drag reduction and anti-icing composite material includes a first layer, i.e., a nickel-copper oxide composite porous coating 2, a second layer, i.e., a cross-linked polymer film layer 3, and a third layer, i.e., a cross-linked flexible photothermal layer 4, which are constructed layer by layer from bottom to top on a metal substrate 1, wherein the surface of the nickel-copper oxide composite porous coating 2 has a porous structure, and part of the structure in the cross-linked polymer film layer 3 infiltrates and fills into the surface and pores of the nickel-copper oxide composite porous coating 2 to generate a rigid-flexible interlocking hybrid film layer. In the present invention, the nickel-copper oxide composite porous coating can not only play the role of connecting the metal base and the cross-linked flexible photothermal layer, but also form a rigid-flexible interlocking hybrid film layer together with the cross-linked polymer film layer, thereby improving the mechanical stability of the entire composite drag reduction material and avoiding damage and failure of the composite material under high flow field velocities.

[0026] Furthermore, the cross-linked flexible photothermal layer can not only reduce resistance, but also delay icing on the surface of the composite material, accelerate deicing, and reduce the increase in external resistance caused by icing through photothermal properties and good thermal conductivity.

[0027] Furthermore, the rigid-flexible interlocking hybrid film layer and the cross-linked flexible photothermal layer synergistically form a composite material with high drag reduction performance and stable structure. The composite material has both the rigidity of a superhydrophobic surface and the flexibility of dolphin skin, and can convert liquid-solid contact into liquid-liquid contact, and reduce the deformation of the flexible coating in the downstream direction, thereby improving the drag reduction rate; the deformation of the flexible coating can absorb the fluid energy in the direction perpendicular to the wall, effectively reducing the intensity and complexity of the flow field, delaying the transition of the coating flow to turbulence, increasing the thickness of the boundary coating, and further reducing the resistance.

[0028] As another aspect of the technical solution of the present invention, it also relates to a method for preparing a multilayer drag-reducing and anti-icing composite material, which mainly comprises firstly using a cyclic electroplating and high-temperature sintering method to generate a nickel-copper oxide composite porous coating on a metal substrate, and then applying a cross-linked polymer film on the surface and pores of the nickel-copper oxide composite porous coating to obtain a rigid-flexible interlocking hybrid film layer; finally, a cross-linked flexible photothermal layer is generated.

[0029] In some embodiments, the method for preparing the multilayer drag reduction and ice prevention composite material comprises the following steps:

[0030] (1) using a metal substrate as a first cathode and nickel as a first anode, making the first cathode, the first anode and a nickel salt-containing electroplating solution form a first electrochemical working system, and applying power to perform a first electrodeposition reaction to generate a nickel plating layer, thereby obtaining a metal substrate wrapped with the nickel plating layer;

[0031] The metal substrate wrapped with the nickel-plated layer is used as a second cathode and copper is used as a second anode, so that the second cathode, the second anode and a copper salt-containing electroplating solution form a second electrochemical working system, and power is supplied to perform a second electrodeposition reaction, so as to form a copper-plated layer on the nickel-plated layer, thereby obtaining a nickel-copper composite porous plating layer;

[0032] The first electrodeposition reaction and the second electrodeposition reaction are cyclically performed more than once, and then high-temperature sintering is performed to obtain a metal substrate wrapped with a nickel-copper oxide composite porous coating;

[0033] (2) bringing a first mixed aqueous solution comprising a charged polymer, a water-soluble polymer and a cross-linking agent into full contact with a metal substrate wrapped with the nickel-copper oxide composite porous coating prepared in step (1), thereby cross-linking on the surface and in the pores of the nickel-copper oxide composite porous coating to form a cross-linked polymer film layer, wherein the cross-linked polymer film layer and the nickel-copper oxide composite porous coating together constitute a rigid-flexible interlocking hybrid film layer;

[0034] (3) The rigid-flexible interlocking hybrid film layer prepared in step (2) is first fully contacted with a second mixed aqueous solution containing a two-dimensional sheet material, micro-nano particles, and a polymer material, and then fully contacted with an inorganic salt solution to generate a cross-linked flexible photothermal layer, thereby obtaining a multi-layer drag reduction and anti-icing composite material.

[0035] In some embodiments, in step (1), the nickel salt electroplating solution includes 0.5-10wt% nickel sulfate, 0.2-15wt% nickel chloride, 0.01-4wt% boric acid, 0.02-8wt% citric acid, 0.1-2wt% sodium dodecyl sulfate, 0.5-5wt% polyoxyethylene alkylphenol ether sodium sulfate, and the balance water. Polyoxyethylene alkylphenol ether sodium sulfate, as a surfactant, forms a composite surfactant together with sodium dodecyl sulfate to reduce the interfacial tension between the electrode / solution, so that the nickel plating layer is easy to spread on the electrode surface and thus form a uniform electroplated nickel layer.

[0036] In some embodiments, in step (1), the copper salt-containing electroplating solution includes 1-20 wt% copper sulfate, 0.1-20 wt% copper chloride, 0.2-7 wt% sulfuric acid, 0.3-6 wt% hydrochloric acid, 0.2-8 wt% sodium chloride and 0.1-7 wt% sodium sulfate.

[0037] In some embodiments, in step (1), the process conditions of the first electrodeposition reaction include: a current density of 0.1 to 20 A / dm 2 , the electrodeposition temperature is 15~70℃, and the electrodeposition time is 1~60 minutes.

[0038] Further, the first anode may include a nickel plate, but is not limited thereto.

[0039] In some embodiments, in step (1), the process conditions of the second electrodeposition reaction include: a current density of 0.1 to 20 A / dm 2 , the electrodeposition temperature is 15~70℃, and the electrodeposition time is 1~60 minutes.

[0040] Further, the second anode may include a copper sheet, but is not limited thereto.

[0041] In some embodiments, in step (1), the preparation method comprises: cyclically performing the first electrodeposition reaction and the second electrodeposition reaction 1 to 20 times.

[0042] In some embodiments, in step (1), the high temperature sintering temperature is 400-900° C., and the time is 0.1-24 h.

[0043] In some embodiments, in step (2), the first mixed aqueous solution comprises 0.1-20 g / L of a charged polymer, 0.1-20 g / L of a water-soluble polymer, and 0.01-5 g / L of a cross-linking agent.

[0044] In some more preferred embodiments, step (2) comprises: coating the first mixed aqueous solution on the metal substrate coated with the nickel-copper oxide composite porous coating prepared in step (1).

[0045] In some embodiments, in step (2), the charged polymer may include at least any one of polyacrylic acid, polyethyleneimine, polyacrylamide, etc., but is not limited thereto.

[0046] In some embodiments, in step (2), the water-soluble polymer may include at least any one of polyvinyl alcohol, chitosan and cellulose, but is not limited thereto.

[0047] In some embodiments, in step (2), the cross-linking agent may include at least any one of glutaraldehyde, glycerol, malic acid, etc., but is not limited thereto.

[0048] In some embodiments, in step (2), the cross-linking temperature is 10-80° C., and the cross-linking time is 30 s-60 min.

[0049] In some embodiments, in step (3), the second mixed aqueous solution comprises 0.01-15 g / L of two-dimensional sheet material, 0.01-15 g / L of micro-nano particles, and 0.1-20 g / L of polymer material.

[0050] In some embodiments, in step (3), the concentration of the inorganic salt in the inorganic salt solution is 1-100 g / L.

[0051] In some more preferred embodiments, step (3) includes: first brushing the second mixed aqueous solution on the surface of the rigid-flexible interlocking hybrid film layer prepared in step (2), and then brushing the inorganic salt solution, reacting at 10 ~ 80 ° C for 10s ~ 60min, to generate a cross-linked flexible photothermal layer. The reaction mechanism of this step is as follows: the two-dimensional sheet material and the micro-nano particles are composited to form a multi-scale composite material, which increases the absorption-reflection-reabsorption of sunlight in the photothermal layer, improves the solar light absorption rate, and reduces the radiation loss of sunlight, and finally increases the net photothermal power of the photothermal layer and enhances the photothermal effect. The cations in the inorganic salt undergo a chemical cross-linking reaction with the polymer material, and together with the two-dimensional sheet material and the micro-nano particles, form a cross-linked flexible photothermal layer, which can improve the stability of the two-dimensional sheet material and the micro-nano particles in the cross-linked flexible photothermal layer.

[0052] In some embodiments, in step (3), the two-dimensional sheet material may include at least any one of reduced graphene oxide, boron carbide, and C3N4, but is not limited thereto.

[0053] In some embodiments, in step (3), the micro-nanoparticles may include at least any one of carbon black particles and polypyrrole particles, but are not limited thereto.

[0054] Furthermore, the particle size of the micro-nano particles is 5nm~500µm.

[0055] In some embodiments, in step (3), the polymer material may include at least any one of sodium alginate, gelatin, and agar, but is not limited thereto.

[0056] In some embodiments, in step (3), the inorganic salt may include at least any one of calcium chloride, magnesium chloride, and calcium carbonate, but is not limited thereto.

[0057] As one of the more specific embodiments, the method for preparing the multilayer drag-reducing and ice-proof composite material may include the following steps:

[0058] (1) A first electrochemical working system is composed of a metal substrate as a first cathode, a nickel plate as a first anode, and a nickel salt electroplating solution, and a first electrodeposition reaction is performed by applying power to generate a nickel coating; a second electrochemical working system is composed of a metal substrate wrapped with the nickel coating as a second cathode, a copper sheet as a second anode, and a copper salt electroplating solution, and a second electrodeposition reaction is performed by applying power to generate a copper coating on the nickel coating, that is, a nickel-copper composite porous coating is obtained, and one assembly is completed; the first electrodeposition reaction and the second electrodeposition reaction are cycled for several times to achieve multiple assemblies; and then high-temperature sintering is performed to obtain a metal substrate wrapped with a nickel-copper oxide composite porous coating;

[0059] (2) coating a first mixed aqueous solution consisting of 0.1-20 g / L of a charged polymer, 0.1-20 g / L of a water-soluble polymer and 0.01-5 g / L of a cross-linking agent on the metal substrate coated with the nickel-copper oxide composite porous coating prepared in step (1), cross-linking the surface of the nickel-copper oxide composite porous coating and the pores thereof into a polymer film, thereby generating a rigid-flexible interlocking hybrid film layer;

[0060] (3) The surface of the rigid-flexible interlocking hybrid film layer prepared in step (2) is coated with a second mixed aqueous solution consisting of 0.01-15 g / L of two-dimensional sheet material, 0.01-15 g / L of micro-nano particles, and 0.1-20 g / L of polymer material, and then coated with 1-100 g / L of inorganic salt solution to obtain a cross-linked flexible photothermal layer, that is, to obtain the multilayer drag reduction and anti-icing composite material.

[0061] Furthermore, in step (1), the number of cycles of nickel-copper assembly is 1 to 20 times.

[0062] In summary, the present invention firstly adopts a cyclic electroplating and high-temperature sintering method to generate a nickel-copper oxide composite porous coating on a metal substrate, and then applies a cross-linked polymer film on the surface and pores of the nickel-copper oxide composite porous coating to obtain a rigid-flexible interlocking hybrid film layer; finally, a cross-linked flexible photothermal layer is generated, and the advantages of multiple layers are complementary and multifunctionally coupled, ultimately obtaining a composite material with high drag reduction performance.

[0063] As another aspect of the technical solution of the present invention, it also relates to a multilayer drag-reducing and anti-icing composite material prepared by the aforementioned method.

[0064] In some embodiments, the multilayer drag reduction and anti-icing composite material includes a nickel-copper oxide composite porous coating, a cross-linked polymer film layer, and a cross-linked flexible photothermal layer stacked in sequence in the thickness direction of the metal substrate, wherein the nickel-copper oxide composite porous coating and the cross-linked polymer film layer together constitute a rigid-flexible interlocking hybrid film layer.

[0065] Furthermore, the thickness of the nickel-copper oxide composite porous coating is 50nm~1000µmµm.

[0066] Furthermore, the pores contained in the nickel-copper oxide composite porous coating have a pore size of 2nm~50µm and a porosity of 30%~90%.

[0067] Furthermore, the thickness of the cross-linked polymer film layer is 100nm~1000µm.

[0068] Furthermore, the thickness of the cross-linked flexible photothermal layer is 10~2000µm.

[0069] Furthermore, the surface roughness of the multilayer drag reduction and ice prevention composite material is 0.5-2 µm, the drag reduction rate is 9.7-27.2%, and the net light-to-heat conversion power is 812-923 W m -2 .

[0070] In summary, the rigid-flexible interlocking hybrid film layer and the cross-linked flexible photothermal layer in the multilayer drag-reducing and anti-icing composite material prepared by the present invention cooperate to form a composite material with high drag-reducing performance and stable structure, which has both the rigidity of the superhydrophobic surface and the flexibility of the dolphin skin, and can transform the liquid-solid contact into liquid-liquid contact, and reduce the deformation of the flexible coating in the downstream direction, thereby improving the drag reduction rate; the deformation of the flexible coating can absorb the fluid energy in the direction perpendicular to the wall, effectively reduce the intensity and complexity of the flow field, delay the transition of the coating flow to turbulence, increase the thickness of the boundary coating, and further reduce the resistance. In addition, the good non-radiative heating and thermal conductivity characteristics can delay ice coating, accelerate deicing, and reduce the external resistance caused by ice.

[0071] Another aspect of an embodiment of the present invention further provides an application of the aforementioned multi-layer drag-reducing and anti-icing composite material. Specifically, the composite material is not only suitable for drag reduction of conventional sea vessels, but can also be used for drag reduction, energy saving and consumption reduction of vessels in extremely cold waters at the polar regions.

[0072] Furthermore, the multi-layer drag-reducing and anti-icing composite material has both the rigidity of a super-hydrophobic surface and the flexibility of dolphin skin, as well as good non-radiative heating and thermal conductivity properties. The functional layers complement each other and are multifunctionally coupled, ultimately resulting in a composite material with high drag-reducing performance and excellent stability, which can be used to achieve drag reduction, anti-fouling and energy saving for water vessels, underwater ships, etc.

[0073] The present invention will be described in more detail below in conjunction with the embodiments and drawings, but the embodiments do not limit the present invention. All variations associated with or derived from the contents disclosed in the present invention are considered to be within the protection scope of the present invention.

[0074] Example 1

[0075] The first electrochemical working system is composed of a metal plate as a first cathode, a nickel plate as a first anode, and a nickel salt plating solution (including 0.5wt% nickel sulfate, 0.2wt% nickel chloride, 0.01wt% boric acid, 0.02wt% citric acid, 0.1wt% sodium dodecyl sulfate, 0.5wt% polyoxyethylene alkylphenol ether sodium sulfate and the balance of water). The first electrodeposition reaction is carried out by powering on (current density is 20A / dm 2, the electrodeposition temperature is 70°C, and the electrodeposition time is 60 minutes), to generate a nickel coating; a second electrochemical working system is composed of a metal plate wrapped with the nickel coating as a second cathode, a copper sheet as a second anode, and a copper salt electroplating solution (including 1wt% copper sulfate, 0.1wt% copper chloride, 0.2wt% sulfuric acid, 0.3wt% hydrochloric acid, 0.2wt% sodium chloride, and 0.1wt% sodium sulfate), and a second electrodeposition reaction is carried out by powering on (the current density is 20A / dm 2 , the electrodeposition temperature is 70°C, the electrodeposition time is 60 minutes), a copper coating is generated on the nickel coating, that is, a nickel-copper composite porous coating is obtained, and one assembly is completed; the first electrodeposition reaction and the second electrodeposition reaction are cycled 20 times to achieve 20 assemblies; and then high-temperature sintering (temperature is 900°C, time is 0.1h) is performed to obtain a metal plate wrapped with a nickel-copper oxide composite porous coating;

[0076] A mixed aqueous solution consisting of 0.1 g / L polyacrylic acid, 0.1 g / L polyvinyl alcohol and 0.01 g / L glutaraldehyde was coated on a metal substrate wrapped with a nickel-copper oxide composite porous coating, and a polymer film was cross-linked on the surface and in the pores of the nickel-copper oxide composite porous coating. The cross-linking temperature was 40 °C and the cross-linking time was 20 min to generate a rigid-flexible interlocking hybrid film layer.

[0077] A mixed aqueous solution consisting of 0.01 g / L reduced graphene oxide, 15 g / L carbon black particles and polypyrrole particles, 0.1 g / L sodium alginate, gelatin and agar was applied on the surface of the rigid-flexible interlocking hybrid film layer, and then 100 g / L calcium chloride, magnesium chloride and calcium carbonate solution was applied. The reaction was carried out at 50 ℃ for 30 min to obtain a cross-linked flexible photothermal layer, thus obtaining a multi-layer drag reduction and anti-icing composite material.

[0078] After testing (ship speed 12m / s, water flow speed 2m / s, ambient temperature -18℃), the drag reduction rate of the multilayer drag reduction and anti-icing composite material obtained in this embodiment is 9.7%, the surface roughness is 0.5µm, and the net light-heat conversion power is 812W m -2 .

[0079] Example 2

[0080] The first electrochemical working system is composed of a metal plate as a first cathode, a nickel plate as a first anode, and a nickel salt plating solution (including 10wt% nickel sulfate, 15wt% nickel chloride, 4wt% boric acid, 8wt% citric acid, 2wt% sodium dodecyl sulfate, 5wt% polyoxyethylene alkylphenol ether sodium sulfate and the balance of water). The first electrodeposition reaction is carried out by powering on (current density is 0.1A / dm 2, the electrodeposition temperature is 15°C, and the electrodeposition time is 1 minute), to generate a nickel coating; a second electrochemical working system is composed of a metal plate wrapped with the nickel coating as a second cathode, a copper sheet as a second anode, and a copper salt electroplating solution (including 20wt% copper sulfate, 20wt% copper chloride, 7wt% sulfuric acid, 6wt% hydrochloric acid, 8wt% sodium chloride, and 7wt% sodium sulfate), and a second electrodeposition reaction is carried out by powering on (the current density is 0.1A / dm 2 , the electrodeposition temperature is 15°C, the electrodeposition time is 1 minute), a copper coating is generated on the nickel coating, that is, a nickel-copper composite porous coating is obtained, and one assembly is completed; the first electrodeposition reaction and the second electrodeposition reaction are cycled 20 times to achieve 20 assemblies; and then high-temperature sintering (temperature is 400°C, time is 24h) is performed to obtain a metal substrate wrapped with a nickel-copper oxide composite porous coating;

[0081] A mixed aqueous solution consisting of 20 g / L polyethyleneimine, 20 g / L chitosan and 5 g / L glycerol was coated on a metal substrate wrapped with a nickel-copper oxide composite porous coating, and a polymer film was cross-linked on the surface and in the pores of the nickel-copper oxide composite porous coating. The cross-linking temperature was 60 °C and the cross-linking time was 10 min to generate a rigid-flexible interlocking hybrid film layer.

[0082] A mixed aqueous solution consisting of 15 g / L boron carbide, 0.01 g / L polypyrrole particles, and 20 g / L gelatin was applied on the surface of the rigid-flexible interlocking hybrid film layer, and then a 1 g / L magnesium chloride solution was applied. The mixture was reacted at 30°C for 40 min to obtain a cross-linked flexible photothermal layer, thereby obtaining a multi-layer drag reduction and anti-icing composite material.

[0083] After testing (ship speed 12m / s, water flow velocity 2m / s, ambient temperature -18℃), the drag reduction rate of the multilayer drag reduction and anti-icing composite material obtained in this embodiment is 14.7%, the surface roughness is 2µm, and the net light-heat conversion power is 901 W m -2 .

[0084] Example 3

[0085] The first electrochemical working system is composed of a metal plate as a first cathode, a nickel plate as a first anode, and a nickel salt plating solution (including 4wt% nickel sulfate, 6wt% nickel chloride, 2wt% boric acid, 3wt% citric acid, 1wt% sodium dodecyl sulfate, 2wt% polyoxyethylene alkylphenol ether sodium sulfate and the remainder of water). The first electrodeposition reaction is carried out by powering on (current density is 10A / dm 2, the electrodeposition temperature is 60°C, the electrodeposition time is 10 minutes), a nickel coating is generated; a second electrochemical working system is composed of a metal plate wrapped with the nickel coating as a second cathode, a copper sheet as a second anode, and a copper salt electroplating solution (including 6wt% copper sulfate, 7wt% copper chloride, 3wt% sulfuric acid, 4wt% hydrochloric acid, 5wt% sodium chloride, and 4wt% sodium sulfate), and a second electrodeposition reaction is carried out by powering on (the current density is 13A / dm 2 , the electrodeposition temperature is 55°C, the electrodeposition time is 5 minutes), a copper coating is generated on the nickel coating, that is, a nickel-copper composite porous coating is obtained, and one assembly is completed; the first electrodeposition reaction and the second electrodeposition reaction are cycled once to achieve one assembly; and then high-temperature sintering (temperature is 800°C, time is 2h) is performed to obtain a metal substrate wrapped with a nickel-copper oxide composite porous coating;

[0086] A mixed aqueous solution consisting of 8 g / L polyacrylamide, 5 g / L cellulose and 4 g / L malic acid was coated on a metal substrate wrapped with a nickel-copper oxide composite porous coating, and a polymer film was cross-linked on the surface and in the pores of the nickel-copper oxide composite porous coating. The cross-linking temperature was 10°C and the cross-linking time was 60 min to generate a rigid-flexible interlocking hybrid film layer.

[0087] A mixed aqueous solution consisting of 3g / L C3N4, 6g / L carbon black particles, and 8g / L agar was applied on the surface of the rigid-flexible interlocking hybrid membrane layer, and then a 25g / L calcium carbonate solution was applied. The mixture was reacted at 10°C for 60min to obtain a cross-linked flexible photothermal layer, thereby obtaining a multi-layer drag reduction and anti-icing composite material.

[0088] After testing (ship speed 12m / s, water flow velocity 2m / s, ambient temperature -18°C), the drag reduction rate of the multilayer drag reduction and anti-icing composite material obtained in this embodiment is 18.9%, the surface roughness is 1.5µm, and the net light-to-heat conversion power is 867 W m -2 .

[0089] Example 4

[0090] The first electrochemical working system is composed of a metal plate as the first cathode, a nickel plate as the first anode, and a nickel salt plating solution (including 3wt% nickel sulfate, 7wt% nickel chloride, 3wt% boric acid, 3wt% citric acid, 1wt% sodium dodecyl sulfate, 2wt% polyoxyethylene alkylphenol ether sodium sulfate and the remainder of water). The first electrodeposition reaction is carried out by powering on (current density is 15A / dm 2, the electrodeposition temperature is 60° C., and the electrodeposition time is 7 minutes), to generate a nickel coating; a second electrochemical working system is composed of a metal plate wrapped with the nickel coating as a second cathode, a copper sheet as a second anode, and a copper salt electroplating solution (including 6wt% copper sulfate, 7wt% copper chloride, 3wt% sulfuric acid, 4wt% hydrochloric acid, 5wt% sodium chloride, and 4wt% sodium sulfate), and a second electrodeposition reaction is carried out by powering on (the current density is 13A / dm 2 , the electrodeposition temperature is 65°C, the electrodeposition time is 5 minutes), a copper coating is generated on the nickel coating, that is, a nickel-copper composite porous coating is obtained, and one assembly is completed; the first electrodeposition reaction and the second electrodeposition reaction are cycled 15 times to achieve 15 assemblies; and then after high-temperature sintering (temperature is 700°C, time is 5h), a metal plate wrapped with a nickel-copper oxide composite porous coating is obtained, wherein the surface morphology of the nickel-copper oxide composite porous coating is as shown Figure 2 As shown;

[0091] A mixed aqueous solution of 5 g / L polyacrylic acid, 15 g / L polyvinyl alcohol and 5 g / L glutaraldehyde was coated on a metal plate wrapped with a nickel-copper oxide composite porous coating, and a polymer film was cross-linked on the surface and in the pores of the nickel-copper oxide composite porous coating. The cross-linking temperature was 80 ° C and the cross-linking time was 30 s to generate a rigid-flexible interlocking hybrid film layer. Its surface morphology is as follows Figure 3 As shown;

[0092] A mixed aqueous solution consisting of 4 g / L reduced graphene oxide, 5 g / L carbon black particles, and 6 g / L sodium alginate was applied on the surface of the rigid-flexible interlocking hybrid film layer, and then 20 g / L calcium chloride solution was applied, and the reaction was carried out at 80 ° C for 10 seconds to obtain a cross-linked flexible photothermal layer, whose surface morphology is as follows: Figure 4 As shown, a multi-layer drag reduction and anti-icing composite material is finally prepared.

[0093] After testing (ship speed 12m / s, water flow speed 2m / s, ambient temperature -18°C), the drag reduction rate of the multilayer drag reduction and anti-icing composite material obtained in this embodiment is 27.2%, the surface roughness is 1µm, and the net light-to-heat conversion power is 923 W m -2 .

[0094] Comparative Example 1

[0095] This control example is basically the same as Example 4, except that the metal plate wrapped with the nickel-copper oxide composite porous coating is not constructed. After testing (ship speed 12m / s, water flow velocity 2m / s, ambient temperature -18°C), the drag reduction rate of the composite material obtained in this control example is 0%. This is because without the nickel-copper oxide composite porous coating, the cross-linked polymer film layer and the cross-linked flexible photothermal layer cannot be constructed on the metal substrate.

[0096] Comparative Example 2

[0097] This control example is basically the same as Example 4, except that no cross-linking polymer film is constructed on the surface and in the pores of the nickel-copper oxide composite porous coating, that is, a rigid-flexible interlocking hybrid film layer cannot be generated. After testing (ship speed 12m / s, water flow velocity 2m / s, ambient temperature -18℃), the drag reduction rate of the composite material obtained in this control example is -15.7%, the surface roughness is 6.9µm, and the net light-to-heat conversion power is 813 W m -2 This is because at a speed of 12 m / s, the hard and brittle nickel-copper oxide composite porous coating is destroyed, and the remaining particulate matter increases the surface resistance.

[0098] Comparative Example 3

[0099] This control example is basically the same as Example 4, except that no cross-linked flexible photothermal layer is constructed. After testing (ship speed 12m / s, water flow velocity 2m / s, ambient temperature -18°C), the drag reduction rate of the composite material obtained in this control example is -5.2%, and the surface roughness of the composite material is 15µm. Under the irradiation of the sun, the cross-linked flexible photothermal layer can heat up quickly, causing the temperature of the thin liquid layer on the surface of the composite material to increase, the water viscosity to decrease, and the resistance to decrease. When there is no cross-linked flexible photothermal layer, the surface of the composite material freezes, resulting in increased resistance.

[0100] In addition, the inventors of this case also conducted experiments with other raw materials and conditions listed in this specification with reference to the methods of Examples 1 to 4, and also produced high-performance multi-layer drag-reducing and anti-icing composite materials.

[0101] It should be understood that the above are only specific application examples of the present invention and do not constitute any limitation on the protection scope of the present invention. Any technical solution formed by equivalent transformation or equivalent replacement falls within the protection scope of the present invention.

Claims

1. A method for preparing a multilayer drag-reducing and ice-proof composite material, characterized in that: include: (1) using a metal substrate as a first cathode and nickel as a first anode, making the first cathode, the first anode and a nickel salt-containing electroplating solution form a first electrochemical working system, and applying power to perform a first electrodeposition reaction to form a nickel plating layer on the metal substrate, thereby obtaining a metal substrate wrapped with the nickel plating layer; The metal substrate wrapped with the nickel-plated layer is used as a second cathode and copper is used as a second anode, so that the second cathode, the second anode and a copper salt-containing electroplating solution form a second electrochemical working system, and power is supplied to perform a second electrodeposition reaction, so as to form a copper-plated layer on the nickel-plated layer, thereby obtaining a nickel-copper composite porous plating layer; The first electrodeposition reaction and the second electrodeposition reaction are cyclically performed more than once, and then high-temperature sintering is performed to obtain a metal substrate wrapped with a nickel-copper oxide composite porous coating; (2) bringing a first mixed aqueous solution comprising a charged polymer, a water-soluble polymer and a cross-linking agent into full contact with a metal substrate wrapped with the nickel-copper oxide composite porous coating prepared in step (1), thereby cross-linking on the surface and in the pores of the nickel-copper oxide composite porous coating to form a cross-linked polymer film layer, wherein the cross-linked polymer film layer and the nickel-copper oxide composite porous coating together constitute a rigid-flexible interlocking hybrid film layer, wherein the first mixed aqueous solution comprises 0.1-20 g / L of a charged polymer, 0.1-20 g / L of a water-soluble polymer and 0.01-5 g / L of a cross-linking agent, wherein the charged polymer is selected from at least any one of polyacrylic acid, polyethyleneimine and polyacrylamide, the water-soluble polymer is selected from at least any one of polyvinyl alcohol, chitosan and cellulose, and the cross-linking agent is selected from at least any one of glutaraldehyde, glycerol and malic acid; (3) The rigid-flexible interlocking hybrid film layer prepared in step (2) is first fully contacted with a second mixed aqueous solution comprising a two-dimensional sheet material, micro-nano particles, and a polymer material, and then fully contacted with an inorganic salt solution to generate a cross-linked flexible photothermal layer, thereby obtaining a multi-layer drag reduction and anti-icing composite material, wherein the second mixed aqueous solution comprises 0.01-15 g / L of a two-dimensional sheet material, 0.01-15 g / L of micro-nano particles, and 0.1-20 g / L of a polymer material, wherein the concentration of the inorganic salt in the inorganic salt solution is 1-100 g / L, the two-dimensional sheet material is selected from at least one of reduced graphene oxide, boron carbide, and C3N4, the micro-nano particles are selected from at least one of carbon black particles and polypyrrole particles, the polymer material is selected from at least one of sodium alginate, gelatin, and agar, and the inorganic salt is selected from at least one of calcium chloride, magnesium chloride, and calcium carbonate.

2. The preparation method according to claim 1, characterized in that: In step (1), the nickel salt electroplating solution comprises 0.5-10wt% nickel sulfate, 0.2-15wt% nickel chloride, 0.01-4wt% boric acid, 0.02-8wt% citric acid, 0.1-2wt% sodium dodecyl sulfate, 0.5-5wt% polyoxyethylene alkylphenol ether sodium sulfate and the balance water; And / or, the copper salt-containing electroplating solution includes 1-20wt% copper sulfate, 0.1-20wt% copper chloride, 0.2-7wt% sulfuric acid, 0.3-6wt% hydrochloric acid, 0.2-8wt% sodium chloride and 0.1-7wt% sodium sulfate.

3. The preparation method according to claim 1, characterized in that: In step (1), the current density of the first electrodeposition reaction or the second electrodeposition reaction is 0.1-20 A / dm 2 , the electrodeposition temperature is 15~70℃, and the electrodeposition time is 1~60 minutes; And / or, the preparation method comprises: cyclically performing the first electrodeposition reaction and the second electrodeposition reaction 1 to 20 times; and / or, the first anode comprises a nickel plate; and / or, the second anode comprises a copper sheet; And / or, the high temperature sintering temperature is 400-900° C., and the time is 0.1-24 h.

4. The preparation method according to claim 1, characterized in that: Step (2) comprises: coating the first mixed aqueous solution on the metal substrate coated with the nickel-copper oxide composite porous coating prepared in step (1).

5. The preparation method according to claim 1, characterized in that: The cross-linking temperature is 10-80°C, and the cross-linking time is 30s-60min.

6. The preparation method according to claim 1, characterized in that Step (3) comprises: firstly applying the second mixed aqueous solution on the surface of the rigid-flexible interlocking hybrid film layer prepared in step (2), and then applying the inorganic salt solution, reacting at 10 to 80° C. for 10 seconds to 60 minutes to generate a cross-linked flexible photothermal layer.

7. The preparation method according to claim 6, characterized in that: The particle size of the micro-nano particles is 5nm~500μm.

8. The multilayer drag-reducing and ice-proof composite material prepared by the preparation method according to any one of claims 1 to 7, characterized in that: The multilayer drag-reducing and anti-icing composite material includes a nickel-copper oxide composite porous coating, a cross-linked polymer film layer and a cross-linked flexible photothermal layer which are sequentially stacked in the thickness direction of a metal substrate, wherein the nickel-copper oxide composite porous coating and the cross-linked polymer film layer together constitute a rigid-flexible interlocking hybrid film layer.

9. The multilayer drag-reducing and ice-proof composite material according to claim 8, characterized in that: The thickness of the nickel-copper oxide composite porous coating is 50nm~1000µmµm; and / or, the pore size of the holes contained in the nickel-copper oxide composite porous coating is 2nm~50µm, and the porosity is 30%~90%; and / or, the thickness of the cross-linked polymer film layer is 100nm~1000µm; and / or, the thickness of the cross-linked flexible photothermal layer is 10~2000µm; And / or, the surface roughness of the multilayer drag reduction and anti-icing composite material is 0.5-2 µm, the drag reduction rate is 9.7-27.2%, and the net light-to-heat conversion power is 812-923 W m -2 .

10. Application of the multi-layer drag-reducing and anti-icing composite material according to claim 8 in the field of drag reduction and protection of marine vehicles.

Citation Information

Cited By

  • Ice-resistant and snow-inhibiting composite material suitable for cold regions as well as preparation method and application of ice-resistant and snow-inhibiting composite material

    CN122168047A