A loaded low-zinc high-efficiency composite material and its preparation method and application in feed

By using loaded low-zinc high-efficiency composites in animal feed, using the combination of modified montmorillonite and modified chitosan composites, the problem of low bioavailability of zinc supplements is solved, and the low amount and high efficiency of zinc is achieved Supplementary and antibacterial effects, suitable for different pH environments.

CN118592532BActive Publication Date: 2024-11-22CHANGSHA AOXIN BIOENGINEERING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410776083.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-17
Publication Date
2024-11-22
Estimated Expiration
2044-06-17

Smart Images

  • Figure CN118592532B_ABST
    Figure CN118592532B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of composite materials, and discloses a loaded low-zinc high-efficiency composite material and its preparation method and application in feed. The preparation method includes: using montmorillonite as a microreactor, making copper particles loaded on montmorillonite, and obtaining modified montmorillonite; reacting N, N-dimethyloctadecylamine with epichlorohydrin to obtain a quaternary ammonium salt with an epoxy group, using it as a surfactant to modify the modified montmorillonite, and obtaining functionalized montmorillonite; reacting salicylaldehyde with hexyl bromide, and reacting the obtained modified salicylaldehyde with chitosan, and obtaining the modified chitosan; reacting the modified chitosan with functionalized montmorillonite, and obtaining a modified chitosan / functionalized montmorillonite composite material, and adding zinc acetate chelation to obtain a loaded low-zinc high-efficiency composite material. The loaded low-zinc high-efficiency composite material can be used in feed as a trace element supplement.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of composite materials, and in particular to a loaded low-zinc high-efficiency composite material and a preparation method thereof and application in feed. Background Art

[0002] Zinc is an essential trace element for animal bodies and is known as the "element of life". Zinc is involved in a large number of active enzymes or stabilizers of subcellular components and membrane molecular structures in organisms. It plays an important role in cell proliferation, differentiation, cell metabolic activities and gene expression, and supports the normal growth and development of organisms. Dietary intake is the most direct and effective way to supplement zinc. Zinc is widely distributed in animal feed, but animals have a low utilization rate of zinc in feed. Therefore, adding zinc supplements to feed can greatly improve the prevention rate of animal diseases and reduce mortality. Therefore, it is of great significance to supplement zinc in zinc-deficient animal individuals through effective zinc supplements.

[0003] Zinc can be added in the form of inorganic salts and organic salts. In the prior art, zinc supplements for feed often use high-zinc from inorganic sources (such as zinc oxide). However, due to its low bioavailability, it will cause environmental pollution, and excessive zinc intake by animals for a long time will lead to copper deficiency, which will have adverse effects on animals. In recent years, organic zinc has attracted widespread attention. There are a large number of literature reports that the biological efficacy of organic zinc is higher than that of inorganic zinc. Adding organic zinc to feed can reduce the zinc requirement of feed.

[0004] Prior art, such as Chinese patent application CN107549476A, discloses a highly antibacterial nano feed additive and a preparation method thereof, wherein nano copper and nano zinc oxide are prepared and physically blended to obtain a highly antibacterial nano feed additive, which has good antibacterial activity, can prevent and treat bacterial infection, enhance the body's immune function and anti-stress function, can effectively promote animal growth, improve feed utilization, and does not produce drug resistance, and is a green and safe functional feed additive. However, this additive uses zinc oxide as a zinc supplement, and zinc oxide will dissolve rapidly in gastric acid, which is not conducive to the absorption and utilization of zinc in the body, limiting the application of the additive in feed. Summary of the invention

[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a loaded low-zinc high-efficiency composite material and a preparation method thereof and an application in feed. The loaded low-zinc high-efficiency composite material has excellent antibacterial properties and controllable sustained release effects, can be controlled to release under different pH environments, has a low-amount and high-efficiency effect on organisms, and can be used in feed as a trace element supplement.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0007] A method for preparing a supported low-zinc high-efficiency composite material comprises the following steps:

[0008] Step (1), mixing montmorillonite, copper nitrate aqueous solution and water, stirring, ultrasonicating, dropping hydrazine hydrate aqueous solution, reacting, filtering after the reaction, taking the filter cake, washing and drying to obtain modified montmorillonite;

[0009] Step (2), mixing N,N-dimethyloctadecylamine, isopropanol and ethanol, adding epichlorohydrin dropwise, reacting after the addition is complete, and after the reaction is complete, removing excess epichlorohydrin, isopropanol and ethanol by rotary evaporation to obtain a crude reaction product, adding washing liquid for washing, and drying to obtain a reaction product;

[0010] The modified montmorillonite is mixed with methanol aqueous solution, stirred, the reaction product is added, ultrasonicated, filtered, the filter cake is taken, the washing liquid is added, washed three times, and dried to obtain the functionalized montmorillonite;

[0011] Step (3), mixing salicylaldehyde, hexyl bromide, anhydrous potassium carbonate and acetone, reacting, filtering after the reaction, taking the filtrate, and removing the solvent acetone by rotary evaporation to obtain a crude reaction product, and purifying to obtain modified salicylaldehyde;

[0012] Step (4), mixing chitosan, methanol and water uniformly, adding modified salicylaldehyde, reacting for the first time, filtering after the reaction, taking the filter cake, washing and extracting, and obtaining modified chitosan;

[0013] The modified chitosan and isopropanol are mixed, and functionalized montmorillonite is added to carry out a second reaction. After the reaction is completed, the filter cake is taken out by suction, washed, and extracted to obtain a modified chitosan / functionalized montmorillonite composite material;

[0014] Step (5), mixing the modified chitosan / functionalized montmorillonite composite material, zinc acetate and ethanol aqueous solution, reacting, filtering after the reaction, taking the filter cake, washing and drying, and obtaining a loaded low-zinc high-efficiency composite material.

[0015] Preferably, in the step (1), the mass ratio of montmorillonite, copper nitrate aqueous solution, water and hydrazine hydrate aqueous solution is 0.1:0.8-1:10-20:50-80, the copper nitrate aqueous solution is a 0.5wt% copper nitrate aqueous solution, and the hydrazine hydrate aqueous solution is a 0.5wt% hydrazine hydrate aqueous solution; and the reaction conditions are: reacting at room temperature for 20-30min.

[0016] Preferably, in step (2), the mass ratio of N,N-dimethyloctadecylamine, isopropanol, ethanol and epichlorohydrin is 300:45-60:30-40:105-110; the dropwise addition time of epichlorohydrin is 0.5-1h; and the reaction conditions are: reacting at a temperature of 40-50°C for 10-12h.

[0017] Preferably, during the preparation of the reaction product, the washing liquid in the washing operation comprises diethyl ether.

[0018] Preferably, in step (2), the mass ratio of the modified montmorillonite to the methanol aqueous solution is 5-10:100, the methanol aqueous solution is 55 vol% methanol aqueous solution; and the mass ratio of the modified montmorillonite to the reaction product is 1:1.2.

[0019] Preferably, in the preparation process of the functionalized montmorillonite, the washing liquid in the washing operation comprises a 55 vol% methanol aqueous solution.

[0020] Preferably, in step (3), the mass ratio of salicylaldehyde, hexyl bromide, anhydrous potassium carbonate and acetone is 5-5.5:6.6-7:5.6-6:50-60; and the reaction conditions are: reflux reaction at 60-70°C for 20-24h.

[0021] Preferably, the purification operation includes: extracting the crude reaction product by mixing with ether in a mass ratio of 1:8, adding a saturated sodium carbonate aqueous solution to the extract, washing three times, separating the liquids, taking the organic layer, adding 20 wt% of anhydrous sodium sulfate by mass of the organic layer, drying for 24 hours, filtering, taking the filtrate, and rotary evaporating again at 30°C to remove the solvent, and passing through a column.

[0022] Preferably, in step (4), the mass ratio of chitosan, methanol, water and modified salicylaldehyde is 1:20-30:30-40:4-4.5, and the modified salicylaldehyde is added at 50°C; the first reaction condition is at 50-60°C for 24-28h.

[0023] Preferably, in step (4), the mass ratio of modified chitosan, isopropanol and functionalized montmorillonite is 1:55-60:8-10, and the functionalized montmorillonite is added at 70°C; the second reaction is carried out at 70-80°C for 24-26h.

[0024] Preferably, in the preparation process of the modified chitosan and the modified chitosan / functionalized montmorillonite composite material, the extraction operation comprises: washing the filter cake and then performing Soxhlet extraction with ethanol for 48 hours.

[0025] Preferably, in step (5), the mass ratio of the modified chitosan / functionalized montmorillonite composite material, zinc acetate and ethanol aqueous solution is 0.5:0.5-1:1000, and the ethanol aqueous solution is 95wt% ethanol aqueous solution; the reaction conditions are: reacting at a pH value of 6-6.5 and a temperature of 50-60°C for 8-12h.

[0026] Preferably, a supported low-zinc high-efficiency composite material is prepared by the method for preparing a supported low-zinc high-efficiency composite material as described above.

[0027] Preferably, a use of the above-mentioned supported low-zinc high-efficiency composite material in feed.

[0028] Compared with the prior art, the present invention has the following beneficial effects:

[0029] Natural inorganic porous materials have low toxicity, no irritation and good biocompatibility. Montmorillonite is a silicate mineral with a nano-layered structure. It has a large specific surface area, pore size and high surface activity. As a carrier material, it has the advantages of controllability and slow release. The present invention uses montmorillonite as a microreactor, and through the reduction of copper nitrate by a reducing agent, copper particles are grown in situ on the montmorillonite, which effectively avoids the agglomeration of copper particles and increases the stability of copper particles. The obtained modified montmorillonite has excellent antibacterial properties. At the same time, because it has a controllable slow release effect, the absorption and utilization rate of zinc is improved, thereby achieving a low-amount and high-efficiency effect.

[0030] The present invention reacts N,N-dimethyloctadecylamine with epichlorohydrin to obtain a quaternary ammonium salt with an epoxy group, and uses the quaternary ammonium salt as a surfactant to perform intercalation modification on modified montmorillonite, thereby increasing the interlayer distance of the montmorillonite, improving its dispersibility and preventing it from agglomerating, and introducing a quaternary ammonium salt with an epoxy group, which can further react with chitosan, thereby being grafted onto chitosan molecules, thereby improving the water solubility and surface activity of chitosan. The present invention reacts the hydroxyl group of salicylaldehyde with bromohexane to obtain a modified salicylaldehyde with an alkoxy group, and the modified salicylaldehyde and chitosan are grafted and composited through a Schiff base reaction of an aldehyde group and an amino group, and in the obtained modified chitosan, the oxygen atom of the alkoxy group and the nitrogen atom of the chitosan have a coordination effect on zinc ions, have high chelating activity, and can form a stable coordination complex with zinc ions.

[0031] The present invention reacts the hydroxyl group of chitosan with the epoxy group of the functionalized montmorillonite to make the chitosan intercalate between the layers of the functionalized montmorillonite, thereby obtaining a modified chitosan / functionalized montmorillonite composite material, thereby further improving the compatibility of the functionalized montmorillonite and chitosan. After the modified chitosan / functionalized montmorillonite composite material chelates zinc ions, the obtained loaded low-zinc high-efficiency composite material has a sustained release effect on both copper and zinc. At the same time, since the Schiff base bond has pH responsiveness, the release can be controlled under different pH environments, thereby improving the absorption and utilization rate of zinc, thereby achieving a low-amount and high-efficiency effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 This is a process flow chart for preparing a loaded low-zinc high-efficiency composite material in the present invention;

[0033] Figure 2 It is a bar graph of the cumulative release rate Ri of zinc ions of samples 1-7 prepared from the supported low-zinc high-efficiency composite materials prepared in Examples 1-5 and Comparative Examples 1-2 in the present invention in the comprehensive performance test. DETAILED DESCRIPTION

[0034] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0035] Example 1

[0036] This embodiment discloses a method for preparing a supported low-zinc high-efficiency composite material, comprising the following steps:

[0037] Step (1), mixing montmorillonite, 0.5 wt% copper nitrate aqueous solution and water, stirring, ultrasonicating, dropping 0.5 wt% hydrazine hydrate aqueous solution, reacting at room temperature for 20 min, filtering after the reaction, taking the filter cake, washing with water 5 times the mass of the filter cake, and drying at 40° C. for 18 h to obtain modified montmorillonite;

[0038] The mass ratio of montmorillonite, 0.5wt% copper nitrate aqueous solution, water, and 0.5wt% hydrazine hydrate aqueous solution is 0.1:0.8:10:50;

[0039] Step (2), N, N-dimethyloctadecylamine, isopropanol, and ethanol were mixed and stirred for 1 hour, and epichlorohydrin was added dropwise for 0.5 hour. The mass ratio of N, N-dimethyloctadecylamine, isopropanol, ethanol, and epichlorohydrin was 300:45:40:105. After the dropwise addition was completed, the reaction was carried out at 40° C. for 12 hours. After the reaction was completed, the excess epichlorohydrin, isopropanol, and ethanol were removed by rotary evaporation at a vacuum degree of 0.01 MPa and a temperature of 70° C. to obtain a crude reaction product, ether was added in an amount of 5 times the mass of the crude reaction product for washing, and the reaction product was dried at 20° C. for 12 hours to obtain a reaction product;

[0040] The modified montmorillonite was mixed with a 55 vol% methanol aqueous solution at a mass ratio of 5:100, stirred at a speed of 500 r / min for 18 h, and the reaction product was added, the mass ratio of the modified montmorillonite to the reaction product was 1:1.2, ultrasonicated for 1 h, filtered, and the filter cake was taken, and 55 vol% methanol aqueous solution with a mass of 5 times that of the filter cake was added for washing three times, and dried at a temperature of 50°C for 18 h to obtain functionalized montmorillonite;

[0041] Step (3), mixing salicylaldehyde, hexyl bromide, anhydrous potassium carbonate and acetone in a mass ratio of 5:6.6:5.6:50, and reflux reaction at 60°C for 24h. After the reaction is completed, filtering, taking the filtrate, and removing the solvent acetone by rotary evaporation at 35°C to obtain a crude reaction product, mixing the crude reaction product with ether in a mass ratio of 1:8 for extraction, adding a saturated sodium carbonate aqueous solution to the extract, washing three times, separating the liquids, taking the organic layer, adding 20wt% of the mass of the organic layer with anhydrous sodium sulfate, and drying for 24h, filtering, taking the filtrate, and again rotary evaporating at 30°C to remove the solvent, and passing through a column to obtain modified salicylaldehyde;

[0042] Chitosan, methanol and water were mixed evenly, and modified salicylaldehyde was added at 50°C, the mass ratio of chitosan, methanol, water and modified salicylaldehyde was 1:20:30:4, and the first reaction was carried out at 50°C for 28 hours. After the reaction was completed, the filter cake was taken out by suction, and ethanol with a mass of 5 times the mass of the filter cake was added for washing, and then Soxhlet extraction was performed with ethanol for 48 hours to obtain modified chitosan;

[0043] The modified chitosan was mixed with isopropanol, and functionalized montmorillonite was added at 70°C, the mass ratio of modified chitosan, isopropanol and functionalized montmorillonite was 1:60:10, and the second reaction was carried out at 70°C for 26 hours. After the reaction was completed, the filter cake was taken out by suction, and ethanol with a mass of 5 times of the filter cake was added for washing, and then Soxhlet extraction was performed with ethanol for 48 hours to obtain a modified chitosan / functionalized montmorillonite composite material;

[0044] Step (4), mixing the modified chitosan / functionalized montmorillonite composite material, zinc acetate, and 95wt% ethanol aqueous solution in a mass ratio of 0.5:0.5:1000, reacting at a pH of 6 and a temperature of 50°C for 12 hours, filtering after the reaction, taking the filter cake, adding ethanol 5 times the mass of the filter cake to wash three times, and drying at a temperature of 50°C for 24 hours to obtain a loaded low-zinc high-efficiency composite material.

[0045] Example 2

[0046] This embodiment discloses a method for preparing a supported low-zinc high-efficiency composite material, comprising the following steps:

[0047] Step (1), mixing montmorillonite, 0.5wt% copper nitrate aqueous solution and water, stirring, ultrasonicating, dropping 0.5wt% hydrazine hydrate aqueous solution, reacting at room temperature for 25 minutes, filtering after the reaction, taking the filter cake, washing with water 6 times the mass of the filter cake, and drying at 45°C for 15 hours to obtain modified montmorillonite;

[0048] The mass ratio of montmorillonite, 0.5wt% copper nitrate aqueous solution, water, and 0.5wt% hydrazine hydrate aqueous solution is 0.1:0.85:12:55;

[0049] Step (2), N, N-dimethyloctadecylamine, isopropanol, and ethanol were mixed and stirred for 1 hour, and epichlorohydrin was added dropwise for 0.6 hour. The mass ratio of N, N-dimethyloctadecylamine, isopropanol, ethanol, and epichlorohydrin was 300:50:32:106. After the dropwise addition was completed, the reaction was carried out at 45° C. for 11 hours. After the reaction was completed, the excess epichlorohydrin, isopropanol, and ethanol were removed by rotary evaporation at a vacuum degree of 0.01 MPa and a temperature of 70° C. to obtain a crude reaction product, ether was added in an amount of 6 times the mass of the crude reaction product for washing, and the reaction product was dried at 25° C. for 11 hours to obtain a reaction product;

[0050] The modified montmorillonite was mixed with a 55 vol% methanol aqueous solution at a mass ratio of 6:100, stirred at a speed of 530 r / min for 17 h, the reaction product was added, the mass ratio of the modified montmorillonite to the reaction product was 1:1.2, ultrasonicated for 1 h, filtered, the filter cake was taken, 55 vol% methanol aqueous solution with a mass of 5 times the filter cake was added, washed three times, and dried at 55 ° C for 15 h to obtain functionalized montmorillonite;

[0051] Step (3), mixing salicylaldehyde, hexyl bromide, anhydrous potassium carbonate and acetone in a mass ratio of 5.1:6.8:5.7:52, and reflux reaction at 65°C for 22h. After the reaction is completed, filtering, taking the filtrate, and removing the solvent acetone by rotary evaporation at 35°C to obtain a crude reaction product, mixing the crude reaction product with ether in a mass ratio of 1:8 for extraction, adding a saturated sodium carbonate aqueous solution to the extract, washing three times, separating the liquids, taking the organic layer, adding 20wt% of the mass of the organic layer with anhydrous sodium sulfate, and drying for 24h, filtering, taking the filtrate, and again rotary evaporating at 30°C to remove the solvent, and passing through a column to obtain modified salicylaldehyde;

[0052] Chitosan, methanol and water were mixed evenly, and modified salicylaldehyde was added at 50°C, the mass ratio of chitosan, methanol, water and modified salicylaldehyde was 1:22:33:4.2, and the first reaction was carried out at 55°C for 26 hours. After the reaction was completed, the filter cake was taken out by suction, and ethanol with a mass of 5 times the mass of the filter cake was added for washing, and then Soxhlet extraction was performed with ethanol for 48 hours to obtain modified chitosan;

[0053] The modified chitosan was mixed with isopropanol, and functionalized montmorillonite was added at 70°C, with the mass ratio of modified chitosan, isopropanol and functionalized montmorillonite being 1:59:9.5. The mixture was reacted for a second time at 75°C for 25 hours. After the reaction was completed, the filter cake was filtered and washed with ethanol 7 times the mass of the filter cake, and then extracted with ethanol Soxhlet for 48 hours to obtain a modified chitosan / functionalized montmorillonite composite material.

[0054] Step (4), mixing the modified chitosan / functionalized montmorillonite composite material, zinc acetate, and 95wt% ethanol aqueous solution in a mass ratio of 0.5:0.7:1000, reacting at a pH of 6 and a temperature of 55°C for 10 hours, filtering after the reaction, taking the filter cake, adding ethanol 6 times the mass of the filter cake to wash three times, and drying at a temperature of 55°C for 22 hours to obtain a loaded low-zinc high-efficiency composite material.

[0055] Example 3

[0056] This embodiment discloses a method for preparing a supported low-zinc high-efficiency composite material, comprising the following steps:

[0057] Step (1), mixing montmorillonite, 0.5wt% copper nitrate aqueous solution and water, stirring, ultrasonicating, dropping 0.5wt% hydrazine hydrate aqueous solution, reacting at room temperature for 25 minutes, filtering after the reaction, taking the filter cake, washing with water 6 times the mass of the filter cake, and drying at 45°C for 15 hours to obtain modified montmorillonite;

[0058] The mass ratio of montmorillonite, 0.5wt% copper nitrate aqueous solution, water, and 0.5wt% hydrazine hydrate aqueous solution is 0.1:0.9:15:65;

[0059] Step (2), N, N-dimethyloctadecylamine, isopropanol, and ethanol were mixed and stirred for 1 hour, and epichlorohydrin was added dropwise for 0.8 hour. The mass ratio of N, N-dimethyloctadecylamine, isopropanol, ethanol, and epichlorohydrin was 300:52:35:108. After the dropwise addition was completed, the reaction was carried out at 45° C. for 11 hours. After the reaction was completed, the excess epichlorohydrin, isopropanol, and ethanol were removed by rotary evaporation at a vacuum degree of 0.01 MPa and a temperature of 75° C. to obtain a crude reaction product, ether was added in an amount of 6 times the mass of the crude reaction product for washing, and the reaction product was dried at 25° C. for 11 hours to obtain a reaction product;

[0060] The modified montmorillonite was mixed with a 55 vol% methanol aqueous solution at a mass ratio of 8:100, stirred at a speed of 550 r / min for 16 h, the reaction product was added, the mass ratio of the modified montmorillonite to the reaction product was 1:1.2, ultrasonicated for 2 h, filtered, the filter cake was taken, 6 times the mass of the filter cake was added with a 55 vol% methanol aqueous solution, washed three times, and dried at 55 ° C for 15 h to obtain functionalized montmorillonite;

[0061] Step (3), salicylaldehyde, hexyl bromide, anhydrous potassium carbonate, and acetone are mixed in a mass ratio of 5.2:6.8:5.8:55, and refluxed at 65°C for 22 hours. After the reaction is completed, filter, take the filtrate, and remove the solvent acetone by rotary evaporation at 38°C to obtain a crude reaction product, mix the crude reaction product with ether in a mass ratio of 1:8 for extraction, add a saturated sodium carbonate aqueous solution to the extract, wash three times, separate the liquids, take the organic layer, add 20wt% of the mass of the organic layer, anhydrous sodium sulfate, dry for 24 hours, filter, take the filtrate, and again rotary evaporate at 30°C to remove the solvent, and pass through a column to obtain modified salicylaldehyde;

[0062] Chitosan, methanol and water were mixed evenly, and modified salicylaldehyde was added at 50°C, the mass ratio of chitosan, methanol, water and modified salicylaldehyde was 1:25:35:4.3, and the first reaction was carried out at 55°C for 26 hours. After the reaction was completed, the filter cake was taken out by suction, and ethanol 6 times the mass of the filter cake was added for washing, and then Soxhlet extraction was performed with ethanol for 48 hours to obtain modified chitosan;

[0063] The modified chitosan was mixed with isopropanol, and functionalized montmorillonite was added at 70°C, the mass ratio of modified chitosan, isopropanol and functionalized montmorillonite was 1:58:9, and the second reaction was carried out at 75°C for 25h. After the reaction was completed, the filter cake was taken out by suction, and 7 times the mass of ethanol was added to wash the filter cake, and then Soxhlet extraction was performed with ethanol for 48h to obtain a modified chitosan / functionalized montmorillonite composite material;

[0064] Step (4), mixing the modified chitosan / functionalized montmorillonite composite material, zinc acetate, and 95wt% ethanol aqueous solution in a mass ratio of 0.5:0.8:1000, reacting at a pH of 6.2 and a temperature of 55°C for 10 hours, filtering after the reaction, taking the filter cake, adding ethanol 6 times the mass of the filter cake to wash three times, and drying at a temperature of 55°C for 22 hours to obtain a loaded low-zinc high-efficiency composite material.

[0065] Example 4

[0066] This embodiment discloses a method for preparing a supported low-zinc high-efficiency composite material, comprising the following steps:

[0067] Step (1), mixing montmorillonite, 0.5wt% copper nitrate aqueous solution and water, stirring, ultrasonicating, dropping 0.5wt% hydrazine hydrate aqueous solution, reacting at room temperature for 25min, filtering after the reaction, taking the filter cake, washing with water 8 times the mass of the filter cake, and drying at 45°C for 15h to obtain modified montmorillonite;

[0068] The mass ratio of montmorillonite, 0.5wt% copper nitrate aqueous solution, water, and 0.5wt% hydrazine hydrate aqueous solution is 0.1:0.95:18:75;

[0069] Step (2), N, N-dimethyloctadecylamine, isopropanol and ethanol are mixed and stirred for 1 hour, epichlorohydrin is added dropwise, the dropping time is 1 hour, the mass ratio of N, N-dimethyloctadecylamine, isopropanol, ethanol and epichlorohydrin is 300:55:38:110, after the dropwise addition is completed, the reaction is carried out at a temperature of 45°C for 11 hours, after the reaction is completed, the excess epichlorohydrin, isopropanol and ethanol are removed by rotary evaporation at a vacuum degree of 0.01 MPa and a temperature of 75°C to obtain a crude reaction product, ether of 6 times the mass of the crude reaction product is added for washing, and the reaction product is dried at a temperature of 25°C for 11 hours to obtain a reaction product;

[0070] The modified montmorillonite was mixed with a 55 vol% methanol aqueous solution at a mass ratio of 9:100, stirred at a speed of 580 r / min for 15 h, the reaction product was added, the mass ratio of the modified montmorillonite to the reaction product was 1:1.2, ultrasonicated for 2 h, filtered, the filter cake was taken, 6 times the mass of the filter cake was added with a 55 vol% methanol aqueous solution, washed three times, and dried at 55 ° C for 15 h to obtain functionalized montmorillonite;

[0071] Step (3), salicylaldehyde, hexyl bromide, anhydrous potassium carbonate, and acetone are mixed in a mass ratio of 5.4:6.9:5.9:58, and refluxed at 70°C for 20 hours. After the reaction is completed, filter, take the filtrate, and remove the solvent acetone by rotary evaporation at 40°C to obtain a crude reaction product, mix the crude reaction product with ether in a mass ratio of 1:8 for extraction, add a saturated sodium carbonate aqueous solution to the extract, wash three times, separate the liquids, take the organic layer, add 20wt% of the mass of the organic layer, anhydrous sodium sulfate, dry for 24 hours, filter, take the filtrate, and again rotary evaporate at 30°C to remove the solvent, and pass through a column to obtain modified salicylaldehyde;

[0072] Chitosan, methanol and water were mixed evenly, and modified salicylaldehyde was added at 50°C, the mass ratio of chitosan, methanol, water and modified salicylaldehyde was 1:28:38:4.4, and the first reaction was carried out at 60°C for 24 hours. After the reaction was completed, the filter cake was taken out by suction, and ethanol of 8 times the mass of the filter cake was added for washing, and then Soxhlet extraction was performed with ethanol for 48 hours to obtain modified chitosan;

[0073] The modified chitosan was mixed with isopropanol, and functionalized montmorillonite was added at 70°C, with the mass ratio of modified chitosan, isopropanol and functionalized montmorillonite being 1:56:8.5. The modified chitosan / functionalized montmorillonite composite material was obtained by filtering the mixture at 78°C for 25 hours, and then washing the mixture with ethanol 8 times the mass of the filter cake, and then extracting the mixture with ethanol Soxhlet for 48 hours to obtain the modified chitosan / functionalized montmorillonite composite material.

[0074] Step (4), mixing the modified chitosan / functionalized montmorillonite composite material, zinc acetate, and 95wt% ethanol aqueous solution in a mass ratio of 0.5:0.9:1000, reacting at a pH of 6.5 and a temperature of 55°C for 10 hours, filtering after the reaction, taking the filter cake, adding ethanol 8 times the mass of the filter cake to wash three times, and drying at a temperature of 60°C for 20 hours to obtain a loaded low-zinc high-efficiency composite material.

[0075] Example 5

[0076] This embodiment discloses a method for preparing a supported low-zinc high-efficiency composite material, comprising the following steps:

[0077] Step (1), mixing montmorillonite, 0.5wt% copper nitrate aqueous solution and water, stirring, ultrasonicating, dropping 0.5wt% hydrazine hydrate aqueous solution, reacting at room temperature for 30min, filtering after the reaction, taking the filter cake, washing with water 8 times the mass of the filter cake, and drying at 50°C for 12h to obtain modified montmorillonite;

[0078] The mass ratio of montmorillonite, 0.5wt% copper nitrate aqueous solution, water, and 0.5wt% hydrazine hydrate aqueous solution is 0.1:1:20:80;

[0079] Step (2), N, N-dimethyloctadecylamine, isopropanol and ethanol are mixed and stirred for 1 hour, epichlorohydrin is added dropwise, the dropping time is 1 hour, the mass ratio of N, N-dimethyloctadecylamine, isopropanol, ethanol and epichlorohydrin is 300:60:30:110, after the dropwise addition is completed, the reaction is carried out at a temperature of 50°C for 10 hours, after the reaction is completed, the excess epichlorohydrin, isopropanol and ethanol are removed by rotary evaporation at a vacuum degree of 0.01 MPa and a temperature of 75°C to obtain a crude reaction product, ether of 8 times the mass of the crude reaction product is added for washing, and the reaction product is dried at a temperature of 30°C for 10 hours to obtain a reaction product;

[0080] The modified montmorillonite was mixed with a 55 vol% methanol aqueous solution at a mass ratio of 10:100, stirred at 600 r / min for 15 h, the reaction product was added, the mass ratio of the modified montmorillonite to the reaction product was 1:1.2, ultrasonicated for 3 h, filtered, the filter cake was taken, 8 times the mass of the filter cake was added with a 55 vol% methanol aqueous solution, washed three times, and dried at 60 ° C for 12 h to obtain functionalized montmorillonite;

[0081] Step (3), salicylaldehyde, hexyl bromide, anhydrous potassium carbonate, and acetone are mixed in a mass ratio of 5.5:7:6:60, and refluxed at 70°C for 20 hours. After the reaction is completed, filter, take the filtrate, and remove the solvent acetone by rotary evaporation at 40°C to obtain a crude reaction product, mix the crude reaction product with ether in a mass ratio of 1:8 for extraction, add a saturated sodium carbonate aqueous solution to the extract, wash three times, separate the liquids, take the organic layer, add 20wt% of the mass of the organic layer, anhydrous sodium sulfate, dry for 24 hours, filter, take the filtrate, and again rotary evaporate at 30°C to remove the solvent, and pass through a column to obtain modified salicylaldehyde;

[0082] Chitosan, methanol and water were mixed evenly, and modified salicylaldehyde was added at 50°C, the mass ratio of chitosan, methanol, water and modified salicylaldehyde was 1:30:40:4.5, and the first reaction was carried out at 60°C for 24 hours. After the reaction was completed, the filter cake was taken out by suction, and ethanol of 8 times the mass of the filter cake was added for washing, and then Soxhlet extraction was performed with ethanol for 48 hours to obtain modified chitosan;

[0083] The modified chitosan was mixed with isopropanol, and functionalized montmorillonite was added at 70°C, with the mass ratio of modified chitosan, isopropanol and functionalized montmorillonite being 1:55:8. The modified chitosan, isopropanol and functionalized montmorillonite were reacted for a second time at 80°C for 24 hours. After the reaction was completed, the filter cake was filtered and washed with ethanol 8 times the mass of the filter cake, and then extracted with ethanol Soxhlet for 48 hours to obtain a modified chitosan / functionalized montmorillonite composite material.

[0084] Step (4), mixing the modified chitosan / functionalized montmorillonite composite material, zinc acetate, and 95wt% ethanol aqueous solution in a mass ratio of 0.5:1:1000, reacting at a pH of 6.5 and a temperature of 60°C for 8 hours, filtering after the reaction, taking the filter cake, adding ethanol 8 times the mass of the filter cake to wash three times, and drying at a temperature of 60°C for 20 hours to obtain a loaded low-zinc high-efficiency composite material.

[0085] Comparative Example 1

[0086] This comparative example discloses a method for preparing a supported low-zinc high-efficiency composite material, comprising the following steps:

[0087] Step (1), mixing montmorillonite, 0.5 wt% copper nitrate aqueous solution and water, stirring, ultrasonicating, dropping 0.5 wt% hydrazine hydrate aqueous solution, reacting at room temperature for 20 min, filtering after the reaction, taking the filter cake, washing with water 5 times the mass of the filter cake, and drying at 40° C. for 18 h to obtain modified montmorillonite;

[0088] The mass ratio of montmorillonite, 0.5wt% copper nitrate aqueous solution, water, and 0.5wt% hydrazine hydrate aqueous solution is 0.1:0.8:10:50;

[0089] Step (2), salicylaldehyde, hexyl bromide, anhydrous potassium carbonate, and acetone are mixed in a mass ratio of 5:6.6:5.6:50, and refluxed at 60°C for 24 hours. After the reaction is completed, filter, take the filtrate, and remove the solvent acetone by rotary evaporation at 35°C to obtain a crude reaction product, mix the crude reaction product with ether in a mass ratio of 1:8 for extraction, add a saturated sodium carbonate aqueous solution to the extract, wash three times, separate the liquids, take the organic layer, add 20wt% of the mass of the organic layer, anhydrous sodium sulfate, dry for 24 hours, filter, take the filtrate, and again rotary evaporate at 30°C to remove the solvent, and pass through a column to obtain modified salicylaldehyde;

[0090] Chitosan, methanol and water were mixed evenly, and modified salicylaldehyde was added at 50°C, the mass ratio of chitosan, methanol, water and modified salicylaldehyde was 1:20:30:4, and the first reaction was carried out at 50°C for 28 hours. After the reaction was completed, the filter cake was taken out by suction, and ethanol with a mass of 5 times the mass of the filter cake was added for washing, and then Soxhlet extraction was performed with ethanol for 48 hours to obtain modified chitosan;

[0091] The modified chitosan and isopropanol were mixed, and the modified montmorillonite was added at a temperature of 70°C, the mass ratio of the modified chitosan, isopropanol and the modified montmorillonite was 1:60:10, and the second reaction was carried out at a temperature of 70°C for 26 hours. After the reaction was completed, the filter cake was taken out by suction filtration, and ethanol with a mass of 5 times of the filter cake was added for washing, and then Soxhlet extraction with ethanol was performed for 48 hours to obtain a modified chitosan / modified montmorillonite composite material;

[0092] Step (3), mixing the modified chitosan / modified montmorillonite composite material, zinc acetate, and 95wt% ethanol aqueous solution in a mass ratio of 0.5:0.5:1000, reacting at a pH of 6 and a temperature of 50°C for 12 hours, filtering after the reaction, taking the filter cake, adding ethanol 5 times the mass of the filter cake to wash three times, and drying at a temperature of 50°C for 24 hours to obtain a loaded low-zinc high-efficiency composite material.

[0093] Comparative Example 2

[0094] This comparative example discloses a method for preparing a supported low-zinc high-efficiency composite material, comprising the following steps:

[0095] Step (1), mixing montmorillonite, 0.5 wt% copper nitrate aqueous solution and water, stirring, ultrasonicating, dropping 0.5 wt% hydrazine hydrate aqueous solution, reacting at room temperature for 20 min, filtering after the reaction, taking the filter cake, washing with water 5 times the mass of the filter cake, and drying at 40° C. for 18 h to obtain modified montmorillonite;

[0096] The mass ratio of montmorillonite, 0.5wt% copper nitrate aqueous solution, water, and 0.5wt% hydrazine hydrate aqueous solution is 0.1:0.8:10:50;

[0097] Step (2), N, N-dimethyloctadecylamine, isopropanol, and ethanol were mixed and stirred for 1 hour, and epichlorohydrin was added dropwise for 0.5 hour. The mass ratio of N, N-dimethyloctadecylamine, isopropanol, ethanol, and epichlorohydrin was 300:45:40:105. After the dropwise addition was completed, the reaction was carried out at 40° C. for 12 hours. After the reaction was completed, the excess epichlorohydrin, isopropanol, and ethanol were removed by rotary evaporation at a vacuum degree of 0.01 MPa and a temperature of 70° C. to obtain a crude reaction product, ether was added in an amount of 5 times the mass of the crude reaction product for washing, and the reaction product was dried at 20° C. for 12 hours to obtain a reaction product;

[0098] The modified montmorillonite was mixed with a 55 vol% methanol aqueous solution at a mass ratio of 5:100, stirred at a speed of 500 r / min for 18 h, and the reaction product was added, the mass ratio of the modified montmorillonite to the reaction product was 1:1.2, ultrasonicated for 1 h, filtered, and the filter cake was taken, and 55 vol% methanol aqueous solution with a mass of 5 times that of the filter cake was added for washing three times, and dried at a temperature of 50°C for 18 h to obtain functionalized montmorillonite;

[0099] Step (3), mixing chitosan with isopropanol, adding functionalized montmorillonite at a temperature of 70° C., wherein the mass ratio of chitosan, isopropanol, and functionalized montmorillonite is 1:60:10, and reacting for a second time at a temperature of 70° C. for 26 hours. After the reaction is completed, filtering with suction, taking the filter cake, adding ethanol 5 times the mass of the filter cake for washing, and then extracting with ethanol Soxhlet for 48 hours to obtain a chitosan / functionalized montmorillonite composite material;

[0100] Step (4), mixing chitosan / functionalized montmorillonite composite material, zinc acetate, and 95wt% ethanol aqueous solution in a mass ratio of 0.5:0.5:1000, reacting at a pH of 6 and a temperature of 50°C for 12 hours, filtering after the reaction, taking the filter cake, adding ethanol 5 times the mass of the filter cake to wash three times, and drying at a temperature of 50°C for 24 hours to obtain a loaded low-zinc high-efficiency composite material.

[0101] In the above embodiments and comparative examples: montmorillonite is from Shanghai Aladdin Biochemical Technology Co., Ltd., model K-10, item number M109698, CAS number: 1318-93-0; copper nitrate is from Jinan Yuyi Chemical Co., Ltd., CAS number: 3251-23-8; hydrazine hydrate is from Anhui Jinyueguan New Material Technology Co., Ltd., CAS number: 10217-52-4; N,N-dimethyloctadecylamine is from Shandong Guohua Chemical Co., Ltd., CAS number: 124-28-7; isopropanol is from Shanghai Hongzhuang Chemical Technology Co., Ltd., CAS number: 67-63-0; ethanol is from Guangdong Lin's Chemical Reagent Co., Ltd., CAS number: 64-17-5; epichlorohydrin is from, CAS number: 106-89-8; ether is from AlfaAesar, item number ALFAC12399, CAS number: 60-29-7 ; Methanol was from Shaanxi Yangyuanshen Biotechnology Co., Ltd., analytical grade, CAS number: 67-56-1; salicylaldehyde was from Shandong Shouhua Chemical Co., Ltd., CAS number: 90-02-8; bromohexane was from Hubei Xinghengye Technology Co., Ltd., CAS number: 111-25-1; anhydrous potassium carbonate was from Hubei Xinghengye Technology Co., Ltd., CAS number: 584-08-7; acetone was from Shandong Wenshao Chemical Co., Ltd., CAS number: 67-64-1; sodium carbonate was from Shandong Haihua New Materials Co., Ltd., CAS number: 497-19-8; anhydrous sodium sulfate was from Shandong Weilun Chemical Co., Ltd., CAS number: 7757-82-6; chitosan was from Shanghai McLean Biochemical Technology Co., Ltd., Mw=50000, item number C850347; zinc acetate was from Shaanxi Rankang Biotechnology Co., Ltd., CAS number: 557-34-6.

[0102] Test example

[0103] (1) Comprehensive performance test

[0104] The comprehensive performance of the supported low-zinc high-efficiency composite materials prepared in Examples 1-5 and Comparative Examples 1-2 was tested, and the specific test results are shown in Table 1:

[0105] Table 1

[0106]

[0107] The detection of each index in Table 1 is based on the following standards: the antibacterial rate is determined by referring to GB / T21510-2008 "Nano-inorganic material antibacterial performance detection method", and the bacterial species are Escherichia coli and Staphylococcus aureus; the sustained-release performance is represented by the cumulative release rate Ri of zinc ions, and the test method is as follows: 50 mg of the loaded low-zinc high-efficiency composite materials prepared in Examples 1-5 and Comparative Examples 1-2 are sampled respectively, and recorded as samples 1-7 respectively, and samples 1-7 are placed in dialysis bags respectively, and the dialysis bags containing the samples are placed in a conical flask containing 75 mL of simulated gastric juice, wherein the simulated gastric juice is a hydrochloric acid aqueous solution with a pH of 1.5-2.0, at a temperature of 37°C. The sustained-release performance was determined in a water bath shaker. 1 mL of simulated gastric fluid was extracted with a pipette every 20 minutes to determine the concentration of zinc ions, and 1 mL of simulated gastric fluid was added to a conical flask for 2 hours. After the test, the simulated gastric fluid was adjusted to simulated intestinal fluid by adding 0.23 mol / L sodium bicarbonate aqueous solution and 1 mol / L sodium hydroxide aqueous solution, wherein the pH of the simulated intestinal fluid was 7.1-7.5, and then cysteine ​​of the same mass as the sample was added. The sustained-release performance was determined in a water bath shaker at 37°C. 1 mL of simulated intestinal fluid was extracted with a pipette every 1 hour to determine the concentration of zinc ions, and 1 mL of deionized water was added to a conical flask for 2 hours. The cumulative release of zinc ions was calculated as the cumulative release rate Ri, and the calculation formula was Ri = (Ci·V) / (m·CC)×100%, where i = 1, 2, 3, …, m is the sample mass (mg), CC is the zinc content in the sample (mg / g), Ci is the measured zinc ion concentration (mg / L), V is the simulated fluid volume (mL), simulated gastric fluid is recorded as 75 mL, and simulated intestinal fluid is recorded as 100 mL.

[0108] According to the test results in Table 1, it can be seen that the loaded low-zinc high-efficiency composite material prepared by the present invention has excellent antibacterial properties and controllable sustained release effects, can be controlled to release under different pH environments, and has a low-amount and high-efficiency effect on organisms.

[0109] The present invention uses montmorillonite as a microreactor, and grows the copper particles in situ on the montmorillonite through the reducing effect of a reducing agent on the copper particles, thereby effectively avoiding the agglomeration of the copper particles and increasing the stability of the copper particles. The obtained modified montmorillonite has excellent antibacterial properties, and at the same time, because it has a controllable slow-release effect, it improves the absorption and utilization rate of zinc, thereby achieving a low-amount and high-efficiency effect.

[0110] The present invention reacts N,N-dimethyloctadecylamine with epichlorohydrin to obtain a quaternary ammonium salt with an epoxy group, and uses the quaternary ammonium salt as a surfactant to perform intercalation modification on modified montmorillonite, thereby increasing the interlayer distance of the montmorillonite, improving its dispersibility and preventing it from agglomerating, and introducing a quaternary ammonium salt with an epoxy group, which can further react with chitosan, thereby being grafted onto chitosan molecules, thereby improving the water solubility and surface activity of chitosan. The hydroxyl group of salicylaldehyde is reacted with hexyl bromide to obtain a modified salicylaldehyde with an alkoxy group, and the modified salicylaldehyde is grafted and composited with chitosan through a Schiff base reaction of an aldehyde group and an amino group, and in the obtained modified chitosan, the oxygen atom of the alkoxy group and the nitrogen atom of the chitosan have a coordination effect on zinc ions, have high chelating activity, and can form a stable coordination complex with zinc ions.

[0111] The present invention reacts the hydroxyl group of chitosan with the epoxy group of the functionalized montmorillonite to make the chitosan intercalate between the layers of the functionalized montmorillonite, thereby obtaining a modified chitosan / functionalized montmorillonite composite material, wherein the copper particles in the functionalized montmorillonite and the unreacted amino groups in the modified chitosan have a chelating effect, thereby further improving the compatibility of the functionalized montmorillonite and the chitosan. After the modified chitosan / functionalized montmorillonite composite material chelates zinc ions, the obtained loaded low-zinc high-efficiency composite material has a sustained release effect on both copper and zinc, and at the same time, because the Schiff base bond has pH responsiveness, the release can be controlled under different pH environments, thereby improving the absorption and utilization rate of zinc, thereby achieving a low-amount and high-efficiency effect.

[0112] In Comparative Example 1, the montmorillonite was not modified by intercalation of quaternary ammonium salt with epoxy group, and the compatibility of montmorillonite with chitosan was reduced, thereby reducing the influence of the sustained release effect of montmorillonite on the composite material. Therefore, the cumulative release rate of zinc ions of sample 6 prepared by Comparative Example 1 in simulated gastric fluid and simulated intestinal fluid was improved.

[0113] In Comparative Example 2, no modified salicylaldehyde is added, so it cannot form a Schiff base bond with chitosan. Since the Schiff base bond has the characteristic of acidic pH responsive breaking, the structure of the composite material will disintegrate in simulated gastric fluid, thereby causing more zinc elements to be separated from the composite material in the form of zinc acetate. The synergistic effect of the Schiff base bond and the coordination bond causes more zinc ions to be released, so the pH responsiveness of Comparative Example 2 is reduced, and the cumulative release rate of zinc ions in simulated gastric fluid and simulated intestinal fluid of Sample 7 prepared by Comparative Example 2 is reduced. At the same time, since Comparative Example 2 does not add modified salicylaldehyde with an alkoxy group, the chelation amount of zinc ions by the composite material is reduced, so the antibacterial rate of Comparative Example 2 is lower than that of the embodiment.

[0114] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a supported low-zinc high-efficiency composite material, characterized in that: The following steps are involved: Step (1), mixing montmorillonite, copper nitrate aqueous solution and water, stirring, ultrasonicating, dropping hydrazine hydrate aqueous solution, reacting, filtering after the reaction, taking the filter cake, washing and drying to obtain modified montmorillonite; The reaction conditions are: react at room temperature for 20-30 minutes; Step (2), N, N-dimethyloctadecylamine, isopropanol and ethanol are mixed and stirred, epichlorohydrin is added dropwise, and after the addition is complete, the mixture is reacted. After the reaction is complete, excess epichlorohydrin, isopropanol and ethanol are removed by rotary evaporation to obtain a crude reaction product, which is washed with washing liquid and dried to obtain a reaction product; The reaction conditions are: reacting at 40-50°C for 10-12h; The modified montmorillonite is mixed with methanol aqueous solution, stirred, the reaction product is added, ultrasonicated, filtered, the filter cake is taken, the washing liquid is added, washed three times, and dried to obtain the functionalized montmorillonite; Step (3), mixing chitosan, methanol and water evenly, adding modified salicylaldehyde, reacting for the first time, filtering after the reaction, taking the filter cake, washing and extracting, and obtaining modified chitosan; The first reaction conditions are: the first reaction is carried out at a temperature of 50-60°C for 24-28 hours; The modified salicylaldehyde is prepared by the following steps: Salicylaldehyde, hexyl bromide, anhydrous potassium carbonate and acetone are mixed and reacted. After the reaction is completed, the mixture is filtered and the filtrate is taken. The solvent acetone is removed by rotary evaporation to obtain a crude reaction product, which is purified to obtain modified salicylaldehyde. The mass ratio of salicylaldehyde, hexyl bromide, anhydrous potassium carbonate and acetone is 5-5.5:6.6-7:5.6-6:50-60. The reaction conditions are: reflux reaction at 60-70°C for 20-24h. The modified chitosan and isopropanol are mixed, and functionalized montmorillonite is added to carry out a second reaction. After the reaction is completed, the filter cake is taken out by suction, washed, and extracted to obtain a modified chitosan / functionalized montmorillonite composite material; The second reaction conditions are as follows: the second reaction is carried out at 70-80°C for 24-26h; Step (4), mixing the modified chitosan / functionalized montmorillonite composite material, zinc acetate, and ethanol aqueous solution, reacting, filtering after the reaction, taking the filter cake, washing, and drying to obtain a loaded low-zinc high-efficiency composite material; The reaction conditions are as follows: the reaction is carried out at a pH value of 6-6.5 and a temperature of 50-60° C. for 8-12 hours.

2. The method for preparing a supported low-zinc high-efficiency composite material according to claim 1, characterized in that: In the step (1), the mass ratio of montmorillonite, copper nitrate aqueous solution, water and hydrazine hydrate aqueous solution is 0.1:0.8-1:10-20:50-80, the copper nitrate aqueous solution is a 0.5wt% copper nitrate aqueous solution, and the hydrazine hydrate aqueous solution is a 0.5wt% hydrazine hydrate aqueous solution.

3. The method for preparing a supported low-zinc high-efficiency composite material according to claim 1, characterized in that: In the step (2), the mass ratio of N,N-dimethyloctadecylamine, isopropanol, ethanol and epichlorohydrin is 300:45-60:30-40:105-110; and the dripping time of epichlorohydrin is 0.5-1h.

4. The method for preparing a supported low-zinc high-efficiency composite material according to claim 1, characterized in that: In the step (2), the mass ratio of the modified montmorillonite to the methanol aqueous solution is 5-10:100, the methanol aqueous solution is 55 vol% methanol aqueous solution; the mass ratio of the modified montmorillonite to the reaction product is 1:1.

2.

5. The method for preparing a supported low-zinc high-efficiency composite material according to claim 1, characterized in that: In the step (3), the mass ratio of chitosan, methanol, water and modified salicylaldehyde is 1:20-30:30-40:4-4.5, and the modified salicylaldehyde is added at a temperature of 50°C.

6. The method for preparing a supported low-zinc high-efficiency composite material according to claim 1, characterized in that: In the step (3), the mass ratio of modified chitosan, isopropanol and functionalized montmorillonite is 1:55-60:8-10, and the functionalized montmorillonite is added at a temperature of 70°C.

7. The method for preparing a supported low-zinc high-efficiency composite material according to claim 1, characterized in that: In the step (4), the mass ratio of the modified chitosan / functionalized montmorillonite composite material, zinc acetate and ethanol aqueous solution is 0.5:0.5-1:1000, and the ethanol aqueous solution is 95wt% ethanol aqueous solution.

8. A supported low-zinc high-efficiency composite material prepared by the method for preparing a supported low-zinc high-efficiency composite material according to any one of claims 1 to 7.

9. Use of the supported low-zinc and high-efficiency composite material as claimed in claim 8 in feed.