A mixture of non-metallic powder from waste printed circuit boards and SBS-modified asphalt.

By using non-metallic powder from waste printed circuit boards and adding compatibilizers in SBS modified asphalt, the problems of waste resource utilization and asphalt pavement performance improvement were solved, achieving the effects of cost reduction and performance improvement.

CN118598581BActive Publication Date: 2026-11-17CHANGSHA UNIVERSITY OF SCIENCE AND TECHNOLOGY
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410809791.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2026-11-17
Estimated Expiration
2044-06-21

AI Technical Summary

Technical Problem

Existing technologies cannot effectively utilize the non-metallic parts of waste printed circuit boards, leading to resource waste and environmental pollution. At the same time, single SBS modified asphalt is difficult to meet the requirements of heavy traffic and multi-axle road surfaces.

Method used

By replacing part of the SBS modifier with non-metallic powder from waste printed circuit boards and improving its compatibility in SBS modified bitumen, high-performance SBS modified bitumen was prepared.

Benefits of technology

It realizes the resource utilization of waste resources, reduces production costs, and improves the high-temperature rutting resistance and low-temperature performance of asphalt pavement, meeting the needs of road engineering for environmentally friendly and low-carbon materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118598581B_ABST
    Figure CN118598581B_ABST
Patent Text Reader

Abstract

This invention discloses a SBS-modified asphalt mixture formulated with waste printed circuit board (PCB) non-metallic powder. Based on the mass of the base asphalt, the SBS modifier content is 2%–3%, the waste PCB non-metallic powder content is 20%–30%, and the compatibilizer content is 3%–5%; the compatibilizer is rubber oil. The prepared waste PCB non-metallic powder-similar SBS-modified asphalt is used to prepare AC-20 graded road asphalt mixtures, with the SBS-modified asphalt comprising 3.8%–4.6% and aggregates 95.4%–96.2% by mass. This invention partially replaces SBS with PCBN powder, reducing SBS usage and achieving resource utilization of waste materials while maintaining the comprehensive road performance of the road mixture and improving its high-temperature rutting resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a compound asphalt mixture made by combining non-metallic powder from waste printed circuit boards with SBS, belonging to the technical field of asphalt pavement materials. Background Technology

[0002] With the advancement of technology, electronic and electrical equipment has become necessities in people's lives. Due to the rapid pace of product updates, a large amount of electronic and electrical equipment is discarded every year, resulting in the generation of waste electronic and electrical equipment. Statistics show that approximately 72 million tons of electronic waste were generated globally in 2017. Printed circuit boards (PCBs) are a crucial component of electronic devices. China accounts for half of the PCB industry market share, with an exponential growth rate, requiring the processing of over 500,000 tons of waste PCBs annually. In 2022, China's total number of discarded major electrical and electronic products reached 900 million units, weighing approximately 8.44 million tons. The enormous environmental pressure and economic benefits have driven the vigorous development of waste PCB recycling technology. Exploring a green, environmentally friendly, and resource-efficient treatment method for waste PCBs is extremely important.

[0003] Printed circuit boards (PCBs) contain precious metals such as copper, nickel, gold, silver, palladium, iron, tin, and lead. One ton of waste PCBs can yield $2292.94 in recovered precious metals, with 98% of the economic value derived from gold (Waste Management, 2022, 139: 105-115). Appropriate crushing methods are used to pulverize PCBs to separate metallic and non-metallic materials, and then metals are recovered from the waste using pyrometallurgical, hydrometallurgical, or biometallurgical methods. The basic structure of a PCB is a copper-clad laminate composed of glass fiber reinforced epoxy resin and various metallic materials, including precious metals. Its composition is very complex, with 70% being non-metallic. Currently, the focus is mainly on recovering the valuable metallic components, while the non-metallic parts are not fully utilized. Most of the processed non-metallic fragments are landfilled, incinerated, or dumped in the open, posing threats to the environment and human health, and causing resource depletion.

[0004] The non-metallic materials of the processed printed circuit board contain a large amount of glass fiber and epoxy resin. These two substances are often used as modifiers for asphalt pavement to improve the pavement's performance. Meanwhile, styrene-butadiene-styrene block copolymer (SBS) is a thermoplastic elastomer. SBS-modified asphalt mixtures prepared from it have good high-temperature performance, low-temperature performance, fatigue performance, and adhesion performance, and are most widely used in high-grade pavements (Journal of Cleaner Production, 2022, 364). Nie et al. (Applied Sciences, 2023, 13(10)) recycled glass fiber from scrapped wind turbine blades and modified SBS-modified asphalt with the glass fiber. The results showed that SBS and glass fiber have good compatibility, which improves the elasticity and toughness of asphalt and provides a new green and environmentally friendly solution for the composite modification of SBS-modified asphalt. Usually, single SBS-modified asphalt is generally difficult to meet the requirements of pavement use in harsh environments such as heavy traffic, multiple axles, and high traffic volume. Therefore, SBS is often combined with other modifiers to modify the pavement performance to better meet the requirements of pavement use.

[0005] To promote the resource utilization of waste materials, meet the demand for environmentally friendly and low-carbon materials in road construction, and overcome technical challenges related to environmental protection, resource conservation, and recycling, this invention explores the use of non-metallic powder from waste printed circuit boards to replace part of the SBS modifier, achieving the same or better road performance while reducing the amount of SBS used. However, the epoxy resin in the recycled printed circuit boards has already solidified, and although it can be added to asphalt as a filler, it faces the problem of poor compatibility. Therefore, this invention improves its compatibility in SBS-modified asphalt by adding a compatibility agent. Summary of the Invention

[0006] (1) Technical issues

[0007] In order to make resource utilization of non-metallic powder from waste printed circuit boards and reduce the production cost of SBS modified asphalt, this invention uses a method of partially replacing SBS with non-metallic powder from waste printed circuit boards to prepare SBS modified asphalt, thereby reducing the amount of SBS and saving costs, while making the performance of the modified asphalt reach or exceed that of an equivalent amount of SBS modified asphalt.

[0008] (2) Technical solution

[0009] To solve the above problems, the technical solution of the present invention is as follows:

[0010] 1) Determine the compatibilizer dosage

[0011] Based on the controlled variable method, SBS modified asphalt with different amounts of waste printed circuit board (PCB) non-metallic powder was prepared. The main analytical component was a modified asphalt in which 20% of the SBS was replaced by waste PCB non-metallic powder, representing 1% SBS, within a 4% SBS modified asphalt composition. Six compatibilizer dosages were selected as research objects, representing 0%, 1%, 2%, 3%, 4%, and 5% of the base asphalt mass. To fully utilize the compatibilizer's effect, it was added simultaneously with the SBS during asphalt shearing. Asphalt segregation tests were conducted on modified asphalt samples with different compatibilizer dosages to determine the optimal compatibilizer dosage for preparing SBS modified asphalt with waste PCB non-metallic powder.

[0012] 2) Through numerous repeated experiments, a replacement solution for non-metallic powder from waste printed circuit boards was determined:

[0013] ① A 4% SBS content was selected as the control group for this experiment;

[0014] ② Use waste printed circuit board non-metallic powder to replace part of the SBS modifier. The amount of waste printed circuit board non-metallic powder in the experimental group was 10%, 20%, and 30% of the matrix asphalt mass, respectively, and each amount replaced 1% and 2% of SBS, respectively.

[0015] 3) Preparation of SBS modified bitumen mixed with non-metallic powder from waste printed circuit boards

[0016] ① Heat the base asphalt in an oven at 135℃ for 1.5 hours. Then add SBS modifier and rubber oil to the fluid base asphalt and keep the temperature at 160℃~165℃. Stir with a high-speed shear machine at a speed of 1500rad / min for 15~30 minutes. The purpose is to allow the SBS modifier to swell and develop in the base asphalt.

[0017] ② Raise the temperature to 170℃~175℃, maintain the shearing speed at 5000 rad / min, and the shearing time at 30~60 min; after shearing, pour the waste printed circuit board non-metallic powder into SBS modified asphalt, maintain the shearing speed at 5000 rad / min, and the shearing time at 30~60 min.

[0018] ③ Stir at 1500 rad / min for 10~30 min to remove air bubbles generated by high-speed shearing; place the modified asphalt in an oven at 170℃~175℃ for 1 h to develop the final sample.

[0019] (3) Beneficial effects

[0020] Compared with existing SBS modified bitumen materials, the beneficial technical effects of this invention are as follows:

[0021] 1) The present invention uses non-metallic powder from waste printed circuit boards to prepare modified asphalt, which can promote the resource utilization of waste resources, meet the needs of road construction for environmentally friendly and low-carbon materials, and overcome technical problems such as environmental protection, resource conservation and recycling.

[0022] 2) The waste printed circuit board non-metallic powder in this invention contains glass fiber and cured epoxy resin. When mixed into asphalt, it can act as a filler and has a significant effect on improving the viscosity and high-temperature rutting resistance of asphalt.

[0023] 3) This invention uses non-metallic powder from waste printed circuit boards to replace part of the SBS modifier, achieving the same or better road performance while reducing the amount of SBS used, effectively reducing the cost of road construction. Attached Figure Description

[0024] Figure 1 Results of the compatibilizer dosage on the segregation of SBS modified asphalt compounded with non-metallic powder from waste printed circuit boards.

[0025] Figure 2 FTIR images of SBS-modified asphalt compounded with non-metallic powder from waste printed circuit boards Detailed Implementation

[0026] The present invention will be further described below with reference to the accompanying drawings and specific embodiments.

[0027] Example 1

[0028] The preparation method for non-metallic powder / SBS modified bitumen from waste printed circuit boards containing 1% compatibilizer mainly includes:

[0029] First, the base asphalt was heated in an oven at 135℃ for 1.5 hours. Then, 3% SBS modifier and 1% rubber oil were added to the fluid base asphalt, and the temperature was maintained at 160℃~165℃. The mixture was stirred for 15 minutes using a high-speed shear press at 1500 rad / min. The temperature was then increased to 170℃~175℃, and the shearing speed was maintained at 5000 rad / min for 30 minutes. After shearing, 20% non-metallic powder from waste printed circuit boards was added to the SBS modified asphalt, and the shearing speed was maintained at 5000 rad / min for 30 minutes. Finally, the mixture was stirred at 1500 rad / min for 10 minutes to remove air bubbles generated by the high-speed shearing. The modified asphalt was then placed in an oven at 170℃~175℃ for 1 hour to obtain the final sample. The modified asphalt sample was then subjected to an asphalt segregation test.

[0030] Example 2

[0031] The preparation method for non-metallic powder / SBS modified bitumen from waste printed circuit boards containing 2% compatibilizer mainly includes:

[0032] First, the base asphalt was heated in an oven at 135℃ for 1.5 hours. Then, 3% SBS modifier and 2% rubber oil were added to the fluid base asphalt, and the temperature was maintained at 160℃~165℃. The mixture was stirred for 15 minutes using a high-speed shear press at 1500 rad / min. The temperature was then increased to 170℃~175℃, and the shearing speed was maintained at 5000 rad / min for 30 minutes. After shearing, 20% non-metallic powder from waste printed circuit boards was added to the SBS modified asphalt, and the shearing speed was maintained at 5000 rad / min for 30 minutes. Finally, the mixture was stirred at 1500 rad / min for 10 minutes to remove air bubbles generated by the high-speed shearing. The modified asphalt was then placed in an oven at 170℃~175℃ for 1 hour to obtain the final sample. The modified asphalt sample was then subjected to an asphalt segregation test.

[0033] Example 3

[0034] The preparation method for non-metallic powder / SBS modified bitumen from waste printed circuit boards containing 3% compatibilizer mainly includes:

[0035] First, the base asphalt was heated in an oven at 135℃ for 1.5 hours. Then, 3% SBS modifier and 3% rubber oil were added to the fluid base asphalt, and the temperature was maintained at 160℃~165℃. The mixture was stirred for 15 minutes at a speed of 1500 rad / min using a high-speed shear mill. The temperature was then increased to 170℃~175℃, and the shearing speed was maintained at 5000 rad / min for 30 minutes. After shearing, 20% non-metallic powder from waste printed circuit boards was added to the SBS modified asphalt, and the shearing speed was maintained at 5000 rad / min for 30 minutes. Finally, the mixture was stirred at 1500 rad / min for 10 minutes to remove air bubbles generated by the high-speed shearing. The modified asphalt was then placed in an oven at 170℃~175℃ for 1 hour to obtain the final sample. The modified asphalt sample was then subjected to an asphalt segregation test.

[0036] Example 4

[0037] The preparation method for non-metallic powder / SBS modified bitumen from waste printed circuit boards containing 4% compatibilizer mainly includes:

[0038] First, the base asphalt was heated in an oven at 135℃ for 1.5 hours. Then, 3% SBS modifier and 4% rubber oil were added to the fluid base asphalt, and the temperature was maintained at 160℃~165℃. The mixture was stirred for 15 minutes using a high-speed shear press at 1500 rad / min. The temperature was then increased to 170℃~175℃, and the shearing speed was maintained at 5000 rad / min for 30 minutes. After shearing, 20% non-metallic powder from waste printed circuit boards was added to the SBS modified asphalt, and the shearing speed was maintained at 5000 rad / min for 30 minutes. Finally, the mixture was stirred at 1500 rad / min for 10 minutes to remove air bubbles generated by the high-speed shearing. The modified asphalt was then placed in an oven at 170℃~175℃ for 1 hour to obtain the final sample. The modified asphalt sample was then subjected to an asphalt segregation test.

[0039] Example 5

[0040] The preparation method for non-metallic powder / SBS modified bitumen from waste printed circuit boards containing 5% compatibilizer mainly includes:

[0041] First, the base asphalt was heated in an oven at 135℃ for 1.5 hours. Then, 3% SBS modifier and 4% rubber oil were added to the fluid base asphalt, and the temperature was maintained at 160℃~165℃. The mixture was stirred for 15 minutes using a high-speed shear press at 1500 rad / min. The temperature was then increased to 170℃~175℃, and the shearing speed was maintained at 5000 rad / min for 30 minutes. After shearing, 20% non-metallic powder from waste printed circuit boards was added to the SBS modified asphalt, and the shearing speed was maintained at 5000 rad / min for 30 minutes. Finally, the mixture was stirred at 1500 rad / min for 10 minutes to remove air bubbles generated by the high-speed shearing. The modified asphalt was then placed in an oven at 170℃~175℃ for 1 hour to obtain the final sample. The modified asphalt sample was then subjected to an asphalt segregation test.

[0042] Comparative Example 1

[0043] The difference from Example 1 is that no compatibilizer is added, and the dosage is 0.

[0044] First, the base asphalt was heated in an oven at 135℃ for 1.5 hours. Then, 3% SBS modifier was added to the fluid base asphalt, without adding rubber oil, and the temperature was maintained at 160℃~165℃. The mixture was stirred for 15 minutes using a high-speed shear press at 1500 rad / min. The temperature was then increased to 170℃~175℃, and the shearing speed was maintained at 5000 rad / min for 30 minutes. After shearing, 20% non-metallic powder from waste printed circuit boards was added to the SBS modified asphalt, and the shearing speed was maintained at 5000 rad / min for 30 minutes. Finally, the mixture was stirred at 1500 rad / min for 10 minutes to remove air bubbles generated by the high-speed shearing. The modified asphalt was then placed in an oven at 170℃~175℃ for 1 hour to obtain the final sample. The modified asphalt sample was then subjected to an asphalt segregation test.

[0045] according to Figure 1 It can be seen that, compared with Comparative Example 1, when there is no compatibilizer in the modified asphalt, the segregation of the waste printed circuit board non-metallic powder / SBS modified asphalt is more obvious. The difference in softening points between the upper and lower parts of the modified asphalt is 4.1℃, indicating that without compatibilizer, the compatibility between the components in the modified asphalt is poor, and the segregation phenomenon is very serious. As the amount of compatibilizer increases, the difference in softening points between the upper and lower parts of the modified asphalt decreases significantly. The difference in softening points is smallest when the amount of compatibilizer is 2%~3%, indicating that the compatibilizer has a significant effect on improving the compatibility of the modified asphalt. However, as the amount of compatibilizer continues to increase, the difference in softening points between the upper and lower parts of the modified asphalt increases. Therefore, the recommended amount of compatibilizer is 2%~3%.

[0046] Example 6

[0047] The preparation method involves replacing 1% SBS modifier in 4% modified asphalt with 10% non-metallic powder from waste printed circuit boards. The main components include:

[0048] First, the base asphalt was heated in an oven at 135℃ for 1.5 hours. Then, 3% SBS modifier and 2% rubber oil were added to the fluid base asphalt, and the temperature was maintained at 160℃~165℃. The mixture was stirred for 15 minutes using a high-speed shearing machine at a speed of 1500 rad / min. The temperature was then increased to 170℃~175℃, and the shearing speed was maintained at 5000 rad / min for 30 minutes. After shearing, 10% non-metallic powder from waste printed circuit boards was added to the SBS modified asphalt, and the shearing speed was maintained at 5000 rad / min for 30 minutes. Finally, the mixture was stirred at 1500 rad / min for 10 minutes to remove air bubbles generated by the high-speed shearing. The modified asphalt was then placed in an oven at 170℃~175℃ for 1 hour to obtain the final sample.

[0049] Example 7

[0050] The preparation method involves replacing 1% SBS modifier in 4% modified asphalt with 20% waste printed circuit board non-metallic powder. The main components include:

[0051] First, the base asphalt was heated in an oven at 135℃ for 1.5 hours. Then, 3% SBS modifier and 2% rubber oil were added to the fluid base asphalt, and the temperature was maintained at 160℃~165℃. The mixture was stirred for 15 minutes using a high-speed shearing machine at a speed of 1500 rad / min. The temperature was then increased to 170℃~175℃, and the shearing speed was maintained at 5000 rad / min for 30 minutes. After shearing, 20% non-metallic powder from waste printed circuit boards was added to the SBS modified asphalt, and the shearing speed was maintained at 5000 rad / min for 30 minutes. Finally, the mixture was stirred at 1500 rad / min for 10 minutes to remove air bubbles generated by the high-speed shearing. The modified asphalt was then placed in an oven at 170℃~175℃ for 1 hour to obtain the final sample.

[0052] Example 8

[0053] The preparation method involves replacing 1% SBS modifier in 4% modified asphalt with 30% non-metallic powder from waste printed circuit boards. The main components include:

[0054] First, the base asphalt was heated in an oven at 135℃ for 1.5 hours. Then, 3% SBS modifier and 2% rubber oil were added to the fluid base asphalt, and the temperature was maintained at 160℃~165℃. The mixture was stirred for 15 minutes using a high-speed shearing machine at a speed of 1500 rad / min. The temperature was then increased to 170℃~175℃, and the shearing speed was maintained at 5000 rad / min for 30 minutes. After shearing, 30% of waste printed circuit board non-metallic powder was added to the SBS modified asphalt, and the shearing speed was maintained at 5000 rad / min for 30 minutes. Finally, the mixture was stirred at 1500 rad / min for 10 minutes to remove air bubbles generated by the high-speed shearing. The modified asphalt was then placed in an oven at 170℃~175℃ for 1 hour to obtain the final sample.

[0055] Example 9

[0056] The preparation method involves replacing 2% SBS modifier in 4% modified asphalt with 10% waste printed circuit board non-metallic powder. The main components include:

[0057] First, the base asphalt was heated in an oven at 135℃ for 1.5 hours. Then, 2% SBS modifier and 2% rubber oil were added to the fluid base asphalt, and the temperature was maintained at 160℃~165℃. The mixture was stirred for 15 minutes using a high-speed shearing machine at a speed of 1500 rad / min. The temperature was then increased to 170℃~175℃, and the shearing speed was maintained at 5000 rad / min for 30 minutes. After shearing, 10% non-metallic powder from waste printed circuit boards was added to the SBS modified asphalt, and the shearing speed was maintained at 5000 rad / min for 30 minutes. Finally, the mixture was stirred at 1500 rad / min for 10 minutes to remove air bubbles generated by the high-speed shearing. The modified asphalt was then placed in an oven at 170℃~175℃ for 1 hour to obtain the final sample.

[0058] Example 10

[0059] The preparation method involves replacing 2% SBS modifier in 4% modified asphalt with 20% non-metallic powder from waste printed circuit boards. The main components include:

[0060] First, the base asphalt was heated in an oven at 135℃ for 1.5 hours. Then, 2% SBS modifier and 2% rubber oil were added to the fluid base asphalt, and the temperature was maintained at 160℃~165℃. The mixture was stirred for 15 minutes using a high-speed shearing machine at a speed of 1500 rad / min. The temperature was then increased to 170℃~175℃, and the shearing speed was maintained at 5000 rad / min for 30 minutes. After shearing, 20% non-metallic powder from waste printed circuit boards was added to the SBS modified asphalt, and the shearing speed was maintained at 5000 rad / min for 30 minutes. Finally, the mixture was stirred at 1500 rad / min for 10 minutes to remove air bubbles generated by the high-speed shearing. The modified asphalt was then placed in an oven at 170℃~175℃ for 1 hour to obtain the final sample.

[0061] Example 11

[0062] The preparation method involves replacing 2% SBS modifier in 4% modified asphalt with 30% non-metallic powder from waste printed circuit boards. The main components include:

[0063] First, the base asphalt was heated in an oven at 135℃ for 1.5 hours. Then, 2% SBS modifier and 2% rubber oil were added to the fluid base asphalt, and the temperature was maintained at 160℃~165℃. The mixture was stirred for 15 minutes using a high-speed shearing machine at a speed of 1500 rad / min. The temperature was then increased to 170℃~175℃, and the shearing speed was maintained at 5000 rad / min for 30 minutes. After shearing, 30% of waste printed circuit board non-metallic powder was added to the SBS modified asphalt, and the shearing speed was maintained at 5000 rad / min for 30 minutes. Finally, the mixture was stirred at 1500 rad / min for 10 minutes to remove air bubbles generated by the high-speed shearing. The modified asphalt was then placed in an oven at 170℃~175℃ for 1 hour to obtain the final sample.

[0064] Comparative Example 2

[0065] The control group consisted of 4% SBS modified asphalt, prepared using the following methods:

[0066] First, the base asphalt was heated in an oven at 135℃ for 1.5 hours. Then, SBS modifier was added to the flowing base asphalt, and the temperature was maintained at 160℃~165℃. The mixture was stirred for 15 minutes at a speed of 1500 rad / min using a high-speed shear press. The temperature was then increased to 170℃~175℃, and the shearing speed was maintained at 5000 rad / min for 60 minutes. Finally, the mixture was stirred at a speed of 1500 rad / min for 10 minutes to remove air bubbles generated by the high-speed shearing. The modified asphalt was then placed in an oven at 170℃~175℃ for 1 hour to develop and obtain the final sample.

[0067] Table 1. Test results of various properties of modified asphalt with different admixtures

[0068]

[0069] The performance of SBS modified asphalt was comprehensively evaluated using multiple indicators, including Brinell viscosity, rutting factor, PG classification, and traffic grade, as shown in Table 1. Compared to 4% SBS modified asphalt, replacing 2% SBS with waste printed circuit board non-metallic powder resulted in a certain degree of decline in all indicators of the SBS modified asphalt, and the overall performance of the SBS modified asphalt could not be guaranteed. Therefore, this substitution scheme is not recommended. When replacing 1% SBS with waste printed circuit board non-metallic powder, the high-temperature performance of the SBS modified asphalt improved with the increase of the waste printed circuit board non-metallic powder content. Furthermore, when the content of waste printed circuit board non-metallic powder exceeded 20%, the high-temperature performance of the SBS modified asphalt with waste printed circuit board non-metallic powder was better than that of 4% SBS modified asphalt, while the low-temperature performance decreased from PG-28 to PG-22. Comprehensive analysis shows that, compared with 4% SBS modified bitumen, modified bitumen with more than 20% waste printed circuit board non-metallic powder replacing 1% SBS has significantly improved performance and can be applied in areas with high temperatures throughout the year and high requirements for high-temperature performance. Figure 2 The Fourier transform infrared (FTIR) test results of the modified asphalt show that no new functional groups were generated after the non-metallic powder of waste printed circuit boards was added to the SBS modified asphalt. This indicates that the non-metallic powder of waste printed circuit boards undergoes a chemical reaction in the SBS modified asphalt, that is, the addition of the non-metallic powder of waste printed circuit boards to the SBS modified asphalt is a physical mixing process.

[0070] Example 12

[0071] In this embodiment, the SBS-modified asphalt AC-20 mixture containing waste printed circuit board non-metallic powder is prepared by adding waste printed circuit board non-metallic powder and SBS-modified asphalt to aggregates. The AC-20 asphalt mixture is prepared by replacing 1% of the SBS modifier with waste printed circuit board non-metallic powder. The mass of the SBS modifier is 3% of the asphalt mass, and the mass of the waste printed circuit board non-metallic powder is 15% of the asphalt mass. The asphalt-aggregate ratio of the asphalt mixture is 4.0%~4.8%.

[0072] The asphalt mixture adopts AC-20 gradation, with limestone as the aggregate material and granulated steel slag powder as the mineral powder material. The overall gradation range of the aggregate is as follows:

[0073] Table 2 Gradation Design Results

[0074]

[0075] Example 13

[0076] In this embodiment, the SBS-modified asphalt AC-20 mixture containing waste printed circuit board non-metallic powder is prepared by adding waste printed circuit board non-metallic powder and SBS-modified asphalt to aggregates. The AC-20 asphalt mixture is prepared by replacing 1% of the SBS modifier with waste printed circuit board non-metallic powder. The mass of the SBS modifier is 3% of the asphalt mass, and the mass of the waste printed circuit board non-metallic powder is 20% of the asphalt mass. The asphalt-aggregate ratio of the asphalt mixture is 4.0%~4.8%.

[0077] Example 14

[0078] In this embodiment, the SBS-modified asphalt AC-20 mixture containing waste printed circuit board non-metallic powder is prepared by adding waste printed circuit board non-metallic powder and SBS-modified asphalt to aggregates. The AC-20 asphalt mixture is prepared by replacing 1% of the SBS modifier with waste printed circuit board non-metallic powder. The mass of the SBS modifier is 3% of the asphalt mass, and the mass of the waste printed circuit board non-metallic powder is 25% of the asphalt mass. The asphalt-aggregate ratio of the asphalt mixture is 4.0%~4.8%.

[0079] Comparative Example 3

[0080] In this embodiment, the SBS-modified asphalt AC-20 mixture containing waste printed circuit board non-metallic powder is prepared by adding waste printed circuit board non-metallic powder and SBS-modified asphalt to aggregates. The AC-20 asphalt mixture is prepared by replacing 1% of the SBS modifier with waste printed circuit board non-metallic powder. The mass of the SBS modifier is 4% of the asphalt mass, and no waste printed circuit board non-metallic powder is added. The asphalt-aggregate ratio of the asphalt mixture is 4.0%~4.8%.

[0081] Table 3. Road Performance Tests of Asphalt Mixtures

[0082]

[0083] Table 3 shows that when 25% of waste printed circuit board (PCB) non-metallic powder is added to 3% SBS modified asphalt, the dynamic stability of the mixture is 5553 cycles / mm, which is about 8.8% higher than that of the 4% SBS modified asphalt mixture. This indicates that replacing 1% SBS with 25% waste PCB non-metallic powder significantly improves the high-temperature rutting resistance of the SBS modified asphalt mixture. The addition of waste PCB non-metallic powder affects the low-temperature performance of the SBS modified asphalt mixture. When 20% and 25% of waste PCB non-metallic powder are used to replace 1% SBS, respectively, the maximum flexural tensile strain of the 3% SBS modified asphalt mixture is reduced by 11.4% and 13% compared to the 4% SBS modified asphalt mixture. The incorporation of non-metallic powder from waste printed circuit boards can improve the high-temperature water damage resistance of SBS modified asphalt mixtures. When 25% of waste printed circuit board non-metallic powder is used to replace 1% of SBS, the high-temperature water damage resistance of SBS modified asphalt mixtures can be improved.

[0084] The above description is merely a preferred embodiment of the present invention, and the scope of protection of the present invention is not limited to the above embodiments. For those skilled in the art, any improvements and modifications obtained without departing from the technical concept of the present invention should also be considered within the scope of protection of the present invention.

Claims

1. A kind of SBS modified asphalt mixture with waste and old printed circuit board non-metal powder, which is composed of the following components: By mass percentage, the non-metallic powder from waste printed circuit boards is compounded with SBS modified asphalt at 3.8%~4.6%, and the aggregate at 95.4%~96.2%. The asphalt mixture adopts AC-20 gradation. The waste printed circuit board non-metallic powder is compounded with SBS modified asphalt, wherein, based on the mass of the base asphalt, the SBS modifier content is 3%, the waste printed circuit board non-metallic powder content is 20%~30%, and the compatibilizer content is 2%~3%; the compatibilizer is rubber oil; after the waste printed circuit board non-metallic powder swells in the base asphalt with SBS modifier and rubber oil and is subjected to high-speed shearing to form SBS modified asphalt, it is added to the SBS modified asphalt for further high-speed shearing, followed by low-speed stirring, degassing, and development to obtain the waste printed circuit board non-metallic powder compounded with SBS modified asphalt.

2. The non-metallic powder of waste printed circuit board and compound SBS modified asphalt mixture according to claim 1, characterized in that, The non-metallic powder from the waste printed circuit boards is mainly composed of 33%~35% bisphenol A type epoxy resin, 47%~48% glass fiber, 12%~14% brominated epoxy resin, and 4%~5% aluminum hydroxide.

3. The waste printed circuit board non-metallic powder compounded with SBS modified asphalt mixture as described in claim 1 or 2, characterized in that, Based on the quality of the base asphalt, the amount of non-metallic powder added to the waste printed circuit board is 25%.

4. The preparation process of the waste printed circuit board non-metallic powder compounded with SBS modified asphalt mixture as described in any one of claims 1 to 3, characterized in that, Includes the following steps: ① Heat the base asphalt in an oven at 135℃ for 1.5 hours. Then add SBS modifier and rubber oil to the fluid base asphalt and keep the temperature at 160℃~165℃. Stir at 1500rpm for 15~30 minutes using a high-speed shear machine to allow the SBS modifier to swell and develop in the base asphalt. ② Raise the temperature to 170℃~175℃, maintain the shearing speed at 5000rpm, and shear for 30~60min to form SBS modified asphalt; then add the non-metallic powder of waste printed circuit boards to the SBS modified asphalt, maintain the shearing speed at 5000rpm, and continue high-speed shearing for 30~60min. ③ Stir at 1500 rpm for 10-30 minutes to remove air bubbles generated by high-speed shearing; place the modified asphalt in an oven at 170℃-175℃ for 1 hour to obtain SBS modified asphalt compounded with non-metallic powder from waste printed circuit boards. ④ Add the waste printed circuit board non-metallic powder compounded with SBS modified asphalt and the mineral aggregate according to the AC-20 gradation into the mixing pot and stir to prepare the waste printed circuit board non-metallic powder compounded with SBS modified asphalt mixture.

Citation Information

Patent Citations

  • PCB (Printed Circuit Board) modified asphalt sizing material and preparation method thereof