A high-strength, high-life, stretch-resistant and environmentally friendly plastic packaging bag
Through the polymerization and ball milling technology of modified polyester and silica and other materials, combined with ultraviolet light irradiation, high-strength and long-life stretch-resistant packaging bags are prepared, which solves the insufficient strength and environmental protection problems of traditional packaging bags, and significantly improves the efficiency of the packaging bags. Performance and service life of packaging bags.
Patent Information
- Application Number
- CN202411117051.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-08-15
AI Technical Summary
Traditional packaging bags have low strength and cannot meet the needs of modern logistics, and most of them are disposed of in garbage after use, causing environmental problems.
Using modified polyester, modified silica, polyvinyl alcohol and other materials, high-strength, long-life stretch-resistant packaging bags are prepared through polymerization and ball milling technology, and irradiated under ultraviolet light to improve water resistance and anti-aging properties. .
It significantly improves the tensile resistance and service life of packaging bags, reduces the discard rate of packaging bags, and solves environmental problems.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of packaging bags, in particular to a high-strength, high-life, stretch-resistant and environment-friendly plastic packaging bag. Background Art
[0002] With the rapid development of logistics and e-commerce industries, packaging bags need to withstand various external pressures and tensile forces during transportation and storage. Traditional packaging bags are often weak and easily damaged, which cannot meet the needs of modern logistics.
[0003] Packaging bags refer to bags used to package various supplies, which make it convenient to transport and store goods during the production and circulation process. They are widely used in daily life and industrial production. Only 7% of packaging bags are recycled, and 80% of used packaging bags are eventually transported to landfills for treatment like general garbage, causing environmental problems.
[0004] Therefore, a packaging bag that can be used repeatedly and has a long service life is needed to solve environmental protection problems by reducing the discard rate of packaging bags. However, traditional polyol plastic packaging bags have poor water resistance and long-term contact with moisture will accelerate the aging process. Summary of the invention
[0005] The purpose of the present invention is to provide a high-strength, high-life, stretch-resistant and environmentally friendly plastic packaging bag to solve the problems existing in the prior art.
[0006] In order to solve the above technical problems, the present invention provides the following technical solutions: a high-strength, high-life, tensile-resistant and environmentally friendly plastic packaging bag, comprising the following preparation steps:
[0007] (1) Polyester, maleic anhydride, p-toluenesulfonic acid and N,N-dimethylformamide are mixed and reacted at a certain temperature for a period of time. The reaction system is precipitated in distilled water, filtered and dried at 60°C for 12 hours to obtain a filter cake. The filter cake and ethanol are mixed in a mass ratio of 1:15, stirred at 40°C and 80 rpm for 1 hour, and then 0.2 times the mass of polyester N-methyldiethanolamine is added. The stirring is continued for 10 minutes, the ethanol is removed by rotary evaporation, and the mixture is cooled to room temperature to obtain a modified polyester.
[0008] (2) Mixing silica and a vinyl coupling agent in a mass ratio of 100:8-12 in a planetary ball mill, adding ethanol until the solid content of silica is 1-25wt%, and milling under the action of zirconium balls. After the ball milling is completed, drying at 50°C and a vacuum degree of 0.1MPa to constant weight to obtain modified silica;
[0009] (3) stirring the modified silica, modified polyester, polyvinyl alcohol, camphorquinone, ethyl 4-dimethylaminobenzoate, zinc stearate, and glycerol triacetate at 100-200 rpm for 1-3 hours, and melt-extrude and granulate in a twin-screw extruder at 185-195° C. to obtain a composite masterbatch;
[0010] (4) The composite masterbatch is made into packaging film by a film blowing machine. After being irradiated under a 365nm wavelength ultraviolet lamp for 1 to 5 minutes, the packaging film is cut and bagged to obtain a high-strength, high-life, tensile-resistant and environmentally friendly plastic packaging bag.
[0011] Furthermore, the preparation method of the polyester in step (1) is as follows: 0.2-0.35 mol 2,4-dihydroxy-butyric acid, 0.1-0.15 mol N-cyclohexyl-N'-[2-hydroxy-1-(hydroxymethyl)-1-methylethyl]urea, 0.12 mol xylene and 0.001 mol p-toluenesulfonic acid are mixed, and reacted at a certain temperature under nitrogen protection until the acid value reaches 25 mg KOH·g −1 Then add 0.45~0.62mol 2,4-dihydroxy-butyric acid, 0.15~0.22mol xylene, and 0.002mol p-toluenesulfonic acid, and continue the reaction at the same temperature until the acid value reaches 25mg KOH·g −1 Then add 1.0~1.3mol 2,4-dihydroxy-butyric acid, 0.3~0.4mol xylene, and 0.004mol p-toluenesulfonic acid, and continue to react at the same temperature for 2h, then raise the temperature to 180℃ and react until the acid value reaches 20mgKOH·g −1 , remove xylene by rotary evaporation and cool to room temperature.
[0012] Furthermore, the temperature is 137-145°C.
[0013] Furthermore, in step (1), the mass ratio of the polyester, maleic anhydride, p-toluenesulfonic acid and N,N-dimethylformamide is 6-8:3-4:0.05:95.
[0014] Furthermore, the temperature in step (1) is 60-80°C.
[0015] Furthermore, the reaction time of step (1) is 6 to 8 hours.
[0016] Furthermore, the conditions of the planetary ball mill in step (2) are: ball milling speed of 300-350 rpm, ball milling time of 8-12 h, and ball-to-material ratio of 3-5:1.
[0017] Furthermore, the vinyl coupling agent in step (2) includes at least one of vinyl triethoxysilane and vinyl trimethoxysilane.
[0018] Furthermore, in step (3), the mass ratio of the modified silica, modified polyester, polyvinyl alcohol, camphorquinone, ethyl 4-dimethylaminobenzoate, zinc stearate, and triacetin is 3-9:48-60:22-26:1-3:0.1-1:1-3:0.5-1.
[0019] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0020] The present invention selects N-cyclohexyl-N'-[2-hydroxy-1-(hydroxymethyl)-1-methylethyl]urea as a core monomer, and the hydroxyl groups at both ends of the urea react with the carboxyl groups of 2,4-dihydroxy-butyric acid, and the 2,4-dihydroxy-butyric acid polymerizes with its own hydroxyl groups and carboxyl groups to form branched segments, so that the generated polyester polymer has good stability and mechanical strength, and the strength and tensile strength of the prepared packaging bag are greatly improved. On this basis, the terminal hydroxyl groups of the polyester polymer react with maleic anhydride, and the maleic anhydride open-ring segments coated on the outside can fully exert the toughening effect, and improve the tensile strength of the plastic packaging bag. At the same time, the core monomer contains NH, so that it has the function of an amine antioxidant, can capture free radicals, improve the anti-aging and antioxidant performance of the packaging, and greatly increase its service life. In addition, the side chain of the core monomer contains a ring structure, which can improve the strength of the polyester, and further optimize the mechanical properties of the plastic packaging bag.
[0021] The present application adopts polyester, polyvinyl alcohol, and olefinic silica as the main raw materials for plastic packaging bags. The carboxyl group at the end of the polyester molecular chain reacts with the hydroxyl group of the polyvinyl alcohol to consume each other's carboxyl group and hydroxyl group, thereby improving the overall water resistance and weakening the accelerating effect of moisture on the oxidation process of the plastic packaging bag, thereby improving the antioxidant performance and improving the service life of the plastic packaging bag. At the same time, the cross-linking degree of the polymer molecular chain is increased, so that the mechanical properties of the plastic packaging bag are greatly improved. The olefinic silica combines with the double bonds at the end of the polyester molecular chain to increase the entanglement degree between the polymer and the silica, further improving the strength of the plastic packaging bag, thereby improving the performance and life of the packaging bag. DETAILED DESCRIPTION
[0022] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe the method in detail. The test methods of various indicators of the packaging bags prepared in the following examples are as follows:
[0024] Tensile strength: refer to GB / T1040-1992 to test the tensile strength;
[0025] Water resistance: The plastic packaging bags prepared in the examples and comparative examples were immersed in distilled water at 40° C. for 12 hours, and the water absorption was calculated.
[0026] Example 1: (1) 0.25 mol of 2,4-dihydroxy-butyric acid, 0.1 mol of N-cyclohexyl-N'-[2-hydroxy-1-(hydroxymethyl)-1-methylethyl]urea, 0.12 mol of xylene and 0.001 mol of p-toluenesulfonic acid were mixed and reacted at 140°C under nitrogen protection until the acid value reached 25 mg KOH·g −1 Then add 0.45 mol 2,4-dihydroxy-butyric acid, 0.15 mol xylene, and 0.002 mol p-toluenesulfonic acid, and continue the reaction at the same temperature until the acid value reaches 25 mg KOH·g −1 Then, 1.0 mol 2,4-dihydroxy-butyric acid, 0.3 mol xylene, and 0.004 mol p-toluenesulfonic acid were added, and the reaction was continued at the same temperature for 2 h, and then the temperature was raised to 180°C and the reaction was continued until the acid value reached 20 mg KOH·g −1 , remove xylene by rotary evaporation, and cool to room temperature to obtain polyester;
[0027] (2) Polyester, maleic anhydride, p-toluenesulfonic acid and N,N-dimethylformamide were mixed in a mass ratio of 6:3:0.05:95, reacted at 70°C for 6 hours, the reaction system was precipitated in distilled water, filtered, and dried at 60°C for 12 hours to obtain a filter cake, the filter cake and ethanol were mixed in a mass ratio of 1:15, stirred at 40°C and 80 rpm for 1 hour, and then 0.2 times the mass of polyester N-methyldiethanolamine was added, and stirring was continued for 10 minutes. The ethanol was removed by rotary evaporation and cooled to room temperature to obtain a modified polyester;
[0028] (3) Mix silica and vinyl triethoxysilane in a mass ratio of 100:8 and place them in a planetary ball mill, add ethanol until the solid content of silica is 10wt%, and mill them under the action of zirconium balls at a ball milling speed of 350rpm, a ball milling time of 10h, a ball-to-material ratio of 4:1, and dry them at 50°C and a vacuum degree of 0.1MPa to constant weight to obtain modified silica;
[0029] (4) Modified silica, modified polyester, polyvinyl alcohol, camphorquinone, ethyl 4-dimethylaminobenzoate, zinc stearate, and glycerol triacetate were mixed in a mass ratio of 3:48:22:1:0.1:1:0.5, stirred at 200 rpm for 1 h, and melt-extruded and granulated in a twin-screw extruder at 185-195° C. to obtain a composite masterbatch;
[0030] (5) The composite masterbatch is made into packaging film by a film blowing machine. After being irradiated under a 365nm wavelength ultraviolet lamp for 1 minute, the packaging film is cut and bagged to obtain a high-strength, high-life, tensile-resistant and environmentally friendly plastic packaging bag.
[0031] Example 2: (1) 0.3 mol of 2,4-dihydroxy-butyric acid, 0.12 mol of N-cyclohexyl-N'-[2-hydroxy-1-(hydroxymethyl)-1-methylethyl]urea, 0.12 mol of xylene and 0.001 mol of p-toluenesulfonic acid were mixed and reacted at 140°C under nitrogen protection until the acid value reached 25 mg KOH·g −1 Then add 0.52 mol 2,4-dihydroxy-butyric acid, 0.19 mol xylene, and 0.002 mol p-toluenesulfonic acid, and continue the reaction at the same temperature until the acid value reaches 25 mg KOH·g −1 Then, 1.1 mol 2,4-dihydroxy-butyric acid, 0.35 mol xylene, and 0.004 mol p-toluenesulfonic acid were added, and the reaction was continued at the same temperature for 2 h. Then, the temperature was raised to 180°C and the reaction was continued until the acid value reached 20 mg KOH·g −1 , remove xylene by rotary evaporation, and cool to room temperature to obtain polyester;
[0032] (2) Polyester, maleic anhydride, p-toluenesulfonic acid, and N,N-dimethylformamide were mixed in a mass ratio of 7:3.5:0.05:95, reacted at 70°C for 7 hours, the reaction system was precipitated in distilled water, filtered, and dried at 60°C for 12 hours to obtain a filter cake, the filter cake and ethanol were mixed in a mass ratio of 1:15, stirred at 40°C and 80 rpm for 1 hour, and then 0.2 times the mass of polyester N-methyldiethanolamine was added, stirring was continued for 10 minutes, ethanol was removed by rotary evaporation, and the mixture was cooled to room temperature to obtain a modified polyester;
[0033] (3) Mix silica and vinyl triethoxysilane in a mass ratio of 100:10 and place them in a planetary ball mill, add ethanol until the solid content of silica is 18wt%, and mill them under the action of zirconium balls at a ball milling speed of 350rpm, a ball milling time of 10h, a ball-to-material ratio of 4:1, and dry them at 50°C and a vacuum degree of 0.1MPa to constant weight to obtain modified silica;
[0034] (4) Modified silica, modified polyester, polyvinyl alcohol, camphorquinone, ethyl 4-dimethylaminobenzoate, zinc stearate, and glycerol triacetate were mixed in a mass ratio of 6:54:24:2:0.6:2:0.8, stirred at 200 rpm for 2 h, and melt-extruded and granulated in a twin-screw extruder at 185-195° C. to obtain a composite masterbatch;
[0035] (5) The composite masterbatch is made into packaging film by a film blowing machine. After being irradiated under a 365nm wavelength ultraviolet lamp for 3 minutes, the packaging film is cut and bagged to obtain a high-strength, high-life, tensile-resistant and environmentally friendly plastic packaging bag.
[0036] Example 3: (1) 0.35 mol of 2,4-dihydroxy-butyric acid, 0.15 mol of N-cyclohexyl-N'-[2-hydroxy-1-(hydroxymethyl)-1-methylethyl]urea, 0.12 mol of xylene and 0.001 mol of p-toluenesulfonic acid were mixed and reacted at 140°C under nitrogen protection until the acid value reached 25 mg KOH·g −1 Then add 0.62 mol 2,4-dihydroxy-butyric acid, 0.22 mol xylene, and 0.002 mol p-toluenesulfonic acid, and continue the reaction at the same temperature until the acid value reaches 25 mg KOH·g −1 Then, 1.3 mol 2,4-dihydroxy-butyric acid, 0.4 mol xylene, and 0.004 mol p-toluenesulfonic acid were added, and the reaction was continued at the same temperature for 2 h. The temperature was then raised to 180 °C and the reaction was continued until the acid value reached 20 mg KOH·g −1 , remove xylene by rotary evaporation, and cool to room temperature to obtain polyester;
[0037] (2) Polyester, maleic anhydride, p-toluenesulfonic acid, and N,N-dimethylformamide were mixed in a mass ratio of 8:4:0.05:95, reacted at 70°C for 8 hours, the reaction system was precipitated in distilled water, filtered, and dried at 60°C for 12 hours to obtain a filter cake, the filter cake and ethanol were mixed in a mass ratio of 1:15, stirred at 40°C and 80 rpm for 1 hour, and then 0.2 times the mass of polyester N-methyldiethanolamine was added, stirring was continued for 10 minutes, ethanol was removed by rotary evaporation, and the mixture was cooled to room temperature to obtain a modified polyester;
[0038] (3) Mix silica and vinyl triethoxysilane in a mass ratio of 100:12 and place them in a planetary ball mill, add ethanol until the solid content of silica is 25wt%, and ball mill under the action of zirconium balls at a ball milling speed of 350rpm, a ball milling time of 10h, a ball-to-material ratio of 4:1, and dry at 50°C and a vacuum degree of 0.1MPa to constant weight to obtain modified silica;
[0039] (4) Modified silica, modified polyester, polyvinyl alcohol, camphorquinone, ethyl 4-dimethylaminobenzoate, zinc stearate, and glycerol triacetate were mixed in a mass ratio of 9:60:26:3:1:3:1, stirred at 200 rpm for 3 h, and melt-extruded and granulated in a twin-screw extruder at 185-195° C. to obtain a composite masterbatch;
[0040] (5) The composite masterbatch is made into packaging film by a film blowing machine. After being irradiated under a 365nm wavelength ultraviolet lamp for 5 minutes, the packaging film is cut and bagged to obtain a high-strength, high-life, tensile-resistant and environmentally friendly plastic packaging bag.
[0041] Comparative Example 1: The only difference between Comparative Example 1 and Example 2 is that polybutylene terephthalate PBT 1100 is used instead of polyester, and the remaining steps are the same as Example 2.
[0042] Comparative Example 2; The only difference between Comparative Example 2 and Implementation 2 is that PBS resin is used instead of polyester, the PBS resin melt index is 5.0g / 10min, the melt index test conditions are 190°C, 2.16Kg, the melting point is 108°C, and the remaining steps are the same as in Example 2.
[0043] Comparative Example 3: The only difference between Comparative Example 3 and Example 2 is that maleic anhydride is not added, and the remaining steps are the same as Example 2.
[0044] Comparative Example 4: The difference between Comparative Example 4 and Example 2 is that the white carbon black is not modified, and the remaining steps are the same as Example 2.
[0045] Comparative Example 5: The difference between Comparative Example 5 and Example 2 is that modified white carbon black is not added, and the remaining steps are the same as Example 2.
[0046] Comparative Example 6: The difference between Comparative Example 6 and Example 2 is that polyvinyl alcohol is not added, and the remaining steps are the same as Example 2.
[0047] Comparative Example 7: The difference between Comparative Example 7 and Example 2 is that no ultraviolet irradiation is performed, and the remaining steps are the same as Example 2.
[0048] Effect example
[0049] Table 1 below shows the performance analysis results of the plastic packaging bags using Examples 1 to 3 of the present invention and Comparative Examples 1 to 7.
[0050] Table 1
[0051]
[0052] From the comparison of the experimental data of the embodiment and the comparative example, it can be found that the present invention uses N-cyclohexyl-N'-[2-hydroxy-1-(hydroxymethyl)-1-methylethyl] urea and 2,4-dihydroxy-butyric acid to form a branched polyester, and uses maleic anhydride open-ring chain segments to coat the outside, so as to give full play to the toughening effect and improve the tensile strength of the plastic packaging bag. Then, modified polyester, polyvinyl alcohol and modified white carbon black are used as the main raw materials of the plastic packaging bag, and the materials are polymerized with each other to improve the overall water resistance and the service life of the plastic packaging bag. At the same time, the cross-linking degree of the polymer molecular chain is increased, so that the mechanical properties of the plastic packaging bag are greatly improved.
[0053] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A high-strength, high-life, tensile-resistant and environmentally friendly plastic packaging bag, characterized in that: The method comprises the following preparation steps: (1) A polyester, maleic anhydride, p-toluenesulfonic acid and N,N-dimethylformamide are mixed and reacted at 60-80°C for 6-8h. The reaction system is precipitated in distilled water, filtered and dried at 60°C for 12h to obtain a filter cake. The filter cake and ethanol are mixed at a mass ratio of 1:15, stirred at 40°C and 80rpm for 1h, and then 0.2 times the mass of the polyester is added with N-methyldiethanolamine. The stirring is continued for 10min, and the ethanol is removed by rotary evaporation. The polyester is cooled to room temperature to obtain a modified polyester. The preparation method of the polyester is as follows: 0.2-0.35mol 2,4-dihydroxy-butyric acid, 0.1-0.15mol N-cyclohexyl-N'-[2-hydroxy-1-(hydroxymethyl)-1-methylethyl]urea, 0.12mol xylene and 0.001mol p-toluenesulfonic acid are mixed, and reacted at 137-145°C under nitrogen protection until the acid value is 25mg KOH·g −1 Then add 0.45~0.62mol 2,4-dihydroxy-butyric acid, 0.15~0.22mol xylene, and 0.002mol p-toluenesulfonic acid, and continue the reaction at the same temperature until the acid value reaches 25mg KOH·g −1 Then add 1.0-1.3 mol 2,4-dihydroxy-butyric acid, 0.3-0.4 mol xylene, and 0.004 mol p-toluenesulfonic acid, and continue to react at the same temperature for 2 h, then raise the temperature to 180 °C and react until the acid value reaches 20 mg KOH·g −1 , remove xylene by rotary evaporation, and cool to room temperature; (2) Mixing silica and a vinyl coupling agent in a mass ratio of 100:8-12 in a planetary ball mill, adding ethanol until the solid content of silica is 1-25wt%, and milling under the action of zirconium balls. After the ball milling is completed, drying at 50°C and a vacuum degree of 0.1MPa to constant weight to obtain modified silica; (3) stirring the modified silica, modified polyester, polyvinyl alcohol, camphorquinone, ethyl 4-dimethylaminobenzoate, zinc stearate, and glycerol triacetate at 100-200 rpm for 1-3 hours, and melt-extrude and granulate in a twin-screw extruder at 185-195° C. to obtain a composite masterbatch; (4) The composite masterbatch is made into packaging film by a film blowing machine. After being irradiated under a 365nm wavelength ultraviolet lamp for 1 to 5 minutes, the packaging film is cut and bagged to obtain a high-strength, high-life, tensile-resistant and environmentally friendly plastic packaging bag.
2. The high-strength, high-life, tensile-resistant and environmentally friendly plastic packaging bag according to claim 1, characterized in that: The mass ratio of the polyester, maleic anhydride, p-toluenesulfonic acid and N,N-dimethylformamide in step (1) is 6-8:3-4:0.05:
95.
3. The high-strength, high-life, tensile-resistant and environmentally friendly plastic packaging bag according to claim 1, characterized in that: The conditions of the planetary ball mill in step (2) are: ball milling speed of 300-350 rpm, ball milling time of 8-12 h, and ball-to-material ratio of 3-5:
1.
4. The high-strength, high-life, tensile-resistant and environmentally friendly plastic packaging bag according to claim 1, characterized in that: The vinyl coupling agent in step (2) includes at least one of vinyl triethoxysilane and vinyl trimethoxysilane.
5. The high-strength, high-life, tensile-resistant and environmentally friendly plastic packaging bag according to claim 1, characterized in that: In step (3), the mass ratio of the modified silica, modified polyester, polyvinyl alcohol, camphorquinone, ethyl 4-dimethylaminobenzoate, zinc stearate and glycerol triacetate is 3-9:48-60:22-26:1-3:0.1-1:1-3:0.5-1.