A composite solvent, electrolyte and lithium metal battery based on 1,3,5,7-tetraoxocyclooctane and its derivatives
By using a composite solvent of 1,3,5,7-tetraoxocyclooctane and its derivatives and ester or ether solvents in lithium metal batteries, a stable SEI film is formed, which solves the problem of battery failure caused by the growth of lithium dendrites. Stability issues have significantly improved the cycle performance and rate performance of lithium metal batteries.
Patent Information
- Application Number
- CN202411093085.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-08-09
AI Technical Summary
Lithium metal batteries have problems with lithium dendrite growth during the cycle process, which leads to instability at the interface between the electrode and the electrolyte, destroys the solid electrolyte interface film, and affects the cycle performance and safety of the battery.
A composite solvent based on 1,3,5,7-tetraoxocyclooctane and its derivatives, supplemented by esters and/or ether solvents, is used to form a stable and tough solid electrolyte interface film (SEI film) to inhibit Dendrites form and improve the cycle performance of lithium metal batteries.
By forming an inner layer of SEI film with high toughness and high adhesion, combined with an outer SEI film rich in inorganic components, the cycle stability and rate performance of lithium metal batteries are significantly improved, and the generation of dendrites and dead lithium is prevented. Improves the overall performance of the battery.
Smart Images

Figure CN118645698B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium batteries, and in particular to a composite solvent, an electrolyte and a lithium metal battery based on 1,3,5,7-tetraoxocyclooctane and its derivatives. Background Art
[0002] Power and energy storage batteries are an important part of the energy internet and a key supporting technology for new power systems. With the increasing popularity of new energy vehicles in recent years, the demand for lithium batteries has been rising, and the requirements for the energy density, cycle performance, and fast charging performance of lithium batteries have gradually increased, while the capacity of traditional materials has reached its limit. Lithium metal batteries use metallic lithium as the negative electrode. The metallic lithium negative electrode has an ultra-high theoretical specific capacity (3860 mAh / g), an extremely low electrode potential (-3.04V compared to the standard hydrogen electrode) and a low mass, and is expected to become the mainstay of the next generation of high-energy density batteries. During the first charge and discharge process of liquid lithium-ion batteries, the electrode material and the electrolyte react at the solid-liquid interface to form a passivation layer covering the surface of the electrode material. This passivation layer is an interface layer with the characteristics of a solid electrolyte. This passivation film is called a solid electrolyte interface film (SEI film). The stability of the SEI film directly determines the performance of the battery cell.
[0003] During the cycle of lithium metal batteries, there are still problems such as lithium dendrites, which hinder their practical application. Therefore, the growth of lithium dendrites is one of the fundamental problems affecting the safety and stability of lithium-ion batteries. The growth of lithium dendrites will lead to the instability of the electrode and electrolyte interface during the cycle of lithium-ion batteries, destroying the generated solid electrolyte interface (SEI) film. During the growth process, lithium dendrites will continuously consume electrolyte and cause irreversible deposition of metallic lithium, forming dead lithium and causing low coulomb efficiency, thus affecting the cycle performance of the battery.
[0004] Lithium battery electrolyte plays the role of ion transport carrier in lithium batteries. It is one of the important components of lithium metal batteries and plays a vital role in the performance of the battery cell. For high-performance lithium metal batteries, the electrolyte not only solves the problems of electrode wetting, interface stability and interface reaction kinetics, but also plays a decisive role in the cycle performance and rate performance of the battery cell. The solvent of the electrolyte can participate in the Li + The solvation structure of the electrolyte determines the composition of the SEI film. Therefore, the type and ratio of the electrolyte solvent also play a very important role in the performance of the lithium battery.
[0005] In practice, in order to meet the demand for high-energy lithium batteries in fields such as electric vehicles and electric aircraft as soon as possible, optimizing the electrolyte formulation is considered to be one of the most promising methods for commercial application due to its simplicity and efficiency.
[0006] Based on the problems existing in the prior art, the present invention provides a new type of lithium metal battery composite solvent, which can form a stable and tough SEI film and effectively inhibit dendrite formation, which is of great significance to improving the performance of lithium metal batteries. Summary of the invention
[0007] In view of the technical problems existing in the prior art, the main purpose of the present invention is to provide a composite solvent, electrolyte and lithium metal battery based on 1,3,5,7-tetraoxocyclooctane and its derivatives. The technical solution of the present invention starts from the electrolyte design, and the tetraoxocyclooctane derivatives are used as solvents, and are supplemented with ester and / or ether solvents to form a composite solvent that can improve the cycle performance of lithium metal batteries. The composite solvent is applied to the electrolyte of lithium metal batteries to improve the stability and toughness of the SEI film, effectively inhibit the formation of dendrites, and improve the cycle performance of lithium metal batteries.
[0008] To achieve the above object, the present invention provides the following technical solution: a composite solvent based on 1,3,5,7-tetraoxocyclooctane and its derivatives, which is composed of a first organic solvent and a second organic solvent; the first organic solvent is 1,3,5,7-tetraoxocyclooctane and its derivatives; the structural formula of the first organic solvent is shown in Formula I:
[0009] Formula I;
[0010] Wherein, R1, R2, R3, and R4 are independently selected from any one or a combination of two of -H, -CF3, C1-C4 alkoxy, hydroxyl, and C1-C4 alkyl.
[0011] Preferably, the second organic solvent is an ester solvent and / or an ether solvent.
[0012] Preferably, the first organic solvent can be selected from any one of the following structural formulas:
[0013] Formula II Formula III Formula IV Formula V.
[0014] Preferably, the molar ratio of the first organic solvent to the second organic solvent is (0.1-1):1.
[0015] Preferably, the ester solvent includes any one or a combination of two or more of ethylene carbonate (EC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), propylene carbonate (PC), fluoroethylene carbonate (FEC), vinylene carbonate, methyl trifluoroethyl carbonate, and diethyl carbonate.
[0016] Preferably, the ether solvent includes any one of dimethyl ether (DME), diethylene glycol butyl ether (DEE), 1,3-dioxolane (DOL), tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, ethylene glycol dibutyl ether, and triethylene glycol dimethyl ether, or a combination of two or more thereof.
[0017] As another object, the present invention also provides the use of the above composite solvent as a solvent in a lithium battery electrolyte.
[0018] The lithium metal electrolyte prepared by using the composite solvent also includes lithium salt, functional additives and diluent.
[0019] Preferably, the molar ratio of the lithium salt, the composite solvent and the diluent is 1:(0.5-5):(1-8).
[0020] Preferably, the mass fraction of the functional additive in the lithium metal electrolyte is 1-10wt%.
[0021] Preferably, the lithium salt includes any one or a combination of two or more of lithium hexafluorophosphate (LiPF6), lithium bis(fluorosulfonyl)imide (LiFSI), lithium difluorooxalatoborate (LiDFOB), trifluoromethanesulfonic acid (LiCF3SO3), lithium bis(pentafluoroethylsulfonyl)imide (LiBETI), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium bis(oxalate)borate (LiBOB), and lithium bis(trifluoromethanesulfonyl)imide (LiTFSI).
[0022] Preferably, the functional additive includes any one or a combination of two or more of LiNO3, LiDFOB, 1,3-propane sultone, FEC, VC, isosorbide dinitrate, and tris(trimethylsilyl)borate.
[0023] Preferably, the diluent includes any one of BTFE (trifluoroethyl ether), 1,1,1,3,3,3-hexafluoroisopropyl methyl ether, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether, bis(2,2,2-trifluoroethyl) ether, and octafluoropentyl-1,1,2,2-tetrafluoroethyl ether, or a combination of two or more thereof.
[0024] Based on the above lithium metal electrolyte, the assembled lithium metal battery includes a positive electrode containing active materials, a negative electrode, a separator and the lithium metal electrolyte provided by the above technical solution.
[0025] Preferably, the active material contained in the positive electrode is any one of a lithiated transition metal phosphate having an olivine structure, a lithium ion embedded transition metal oxide having a layered structure, or a lithiated transition metal mixed oxide having a spinel structure.
[0026] Preferably, the negative electrode is any one of pure lithium, lithium alloy, and lithium-plated negative electrode.
[0027] Compared with the prior art, the present invention at least has the following beneficial effects:
[0028] 1) The present invention adopts tetraoxocyclooctane and its derivatives, supplemented with functional ester or ether solvents to form a composite solvent. Since the tetraoxocyclooctane derivatives have a lower LUMO energy level, they have a higher reduction potential than ester or ether solvents. During the charge and discharge process, the eight-membered ring of tetraoxocyclooctane breaks and preferentially polymerizes to obtain a polymer with high toughness and adhesion. Based on this, when the above composite solvent is used as a solvent for the electrolyte, it can participate in the Li + In the solvation structure of tetraoxocyclooctane, it is easy to form a polymer after ring opening, and participate in the formation of the SEI film. The polymer is formed in the inner layer, which improves the toughness and adhesion of the SEI film, and further ensures the stability of the SEI film during the charging and expansion process of the metal lithium negative electrode, preventing the electrolyte from continuously reacting with the metal lithium negative electrode to generate lithium dendrites and dead lithium.
[0029] 2) The composite solvent and functional additive provided by the present invention are used in combination to decompose and form an outer layer SEI rich in inorganic components, which has a high ionic conductivity and is tightly combined with the polymer of the inner layer of the SEI membrane to form a stable and high-strength SEI membrane structure, thereby ensuring the continuous stability of the battery cell and improving the cycle performance of the battery.
[0030] 3) The composite solvent provided by the technical solution of the present invention is used as the solvent of the electrolyte, and the assembled lithium metal battery shows high cycle stability; with the outer SEI film of the high ionic conductivity component, the rate performance of the battery is significantly improved; in particular, the ester electrolyte has a higher ionic conductivity, so its improvement effect is the best. DETAILED DESCRIPTION
[0031] To make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention is clearly and completely described. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the protection scope of the present invention.
[0032] The disclosures of all patent and non-patent literature cited herein are incorporated herein by reference in their entirety.
[0033] As used herein, the terms "comprises," "includes," "contains," "covers," "has," "with," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a process, method, article, or apparatus that includes a list of elements is not necessarily limited to only those elements, but may include other elements not expressly listed or inherent to the process, method, article, or apparatus. Furthermore, unless expressly specified to the contrary, "or" refers to an inclusive "or" and not an exclusive "or."
[0034] In addition, "a" or "an" is used to describe the elements and components described herein. This is done not only for convenience but also to provide a general sense of the scope of the invention. This description should be understood to include one or at least one, one or at least one, and the singular also includes the plural, unless it is obvious that it is otherwise intended.
[0035] The present invention provides a composite solvent, which is composed of a first organic solvent and a second organic solvent; the first organic solvent may be tetraoxocyclooctane and its derivatives, and its structural formula is shown in Formula I:
[0036] Formula 1;
[0037] Among them, R1, R2, R3, and R4 are independently selected from any one or a combination of two or more of -H, -CF3, C1-C4 alkoxy, hydroxyl, and C1-C4 alkyl, but are not limited thereto.
[0038] In some preferred embodiments, the structure of the first organic solvent can be selected from any one of Formula II to Formula V:
[0039] Formula II Formula III Formula IV Formula V.
[0040] Preferably, the second organic solvent includes an ester solvent and / or an ether solvent.
[0041] As a preferred embodiment, the molar ratio of the first organic solvent to the second organic solvent is (0.1-1):1.
[0042] Specifically, the ester solvent includes any one or a combination of two or more of EC, EMC, DMC, PC, FEC, vinylene carbonate, methyl trifluoroethyl carbonate, and diethyl carbonate.
[0043] Or, the ether solvent includes any one of DME, DEE, DOL, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, ethylene glycol dibutyl ether, and triethylene glycol dimethyl ether, or a combination of two or more thereof.
[0044] The present invention uses the above-mentioned composite solvent as the solvent of the lithium battery electrolyte to improve the cycle performance of the lithium battery. The specific principle includes: tetraoxocyclooctane and its derivatives can react with Li + Coordination, entering Li + In the solvation structure; in the process of forming the SEI film, the tetraoxocyclooctane ring opens to form a long-chain structure. This long-chain structure is easier to polymerize and can form the inner layer structure of the polymer SEI film. It has certain toughness and adhesion, ensuring the stability of the SEI film. During the charge and discharge process, it can effectively isolate the electrolyte from the metal lithium negative electrode and inhibit the formation of dendrites.
[0045] Furthermore, it works synergistically with functional additives containing F and N to form an SEI film rich in inorganic components, which, combined with the polymer inner layer SEI, forms a stable, high-strength SEI film, which effectively inhibits the formation of dendrites and dead lithium, and exhibits high cycle stability in battery performance.
[0046] Based on the above technical solution, another aspect of an embodiment of the present invention further provides a lithium metal electrolyte containing the aforementioned composite solvent; the composition of the lithium metal electrolyte includes the composite solvent, a lithium salt, a functional additive and a diluent.
[0047] As one of the preferred embodiments, the molar ratio of the lithium salt, the composite solvent and the diluent is in the range of 1:(0.5-5):(1-8), preferably 1:(1-2):4.
[0048] In some preferred embodiments, the lithium salt may include any one or a combination of two or more of LiPF6, LiFSI, LiDFOB, LiCF3SO3, LiBETI, LiBF4, LiClO4, LiBOB, LiTFSI, etc., but is not limited thereto.
[0049] In some preferred embodiments, the mass fraction of the functional additive is 1-10 wt %, preferably 4-6 wt %.
[0050] Specifically, the functional additive includes any one or a combination of two or more of LiNO3, LiDFOB, 1,3-propane sultone, FEC, VC, isosorbide dinitrate, and tris(trimethylsilyl)borate, but is not limited thereto.
[0051] In some preferred embodiments, the diluent includes any one or a combination of two or more of BTFE, 1,1,1,3,3,3-hexafluoroisopropyl methyl ether, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether, bis(2,2,2-trifluoroethyl) ether, and octafluoropentyl-1,1,2,2-tetrafluoroethyl ether, but is not limited thereto.
[0052] Another aspect of an embodiment of the present invention further provides a lithium metal battery comprising the aforementioned electrolyte, including a positive electrode containing active materials, a negative electrode, a separator and the aforementioned lithium metal electrolyte.
[0053] Furthermore, the active material contained in the positive electrode is any one of a lithiated transition metal phosphate having an olivine structure, a lithium ion embedded transition metal oxide having a layered structure, and a lithiated transition metal mixed oxide having a spinel structure, but is not limited thereto.
[0054] Furthermore, the negative electrode is any one of pure lithium, lithium alloy, lithium-plated negative electrode, etc., but is not limited thereto.
[0055] In summary, the electrolyte provided by the present invention uses a composite solvent containing a tetraoxocyclooctane derivative and a functional additive as an electrolyte solvent, has high cycle stability, and the lithium metal battery equipped with it shows excellent cycle performance, which weakens the electrochemical adverse reactions caused by the growth of lithium dendrites in the lithium metal battery.
[0056] Unless otherwise defined, the meaning of all technical and scientific terms used herein is the same as that generally understood by those of ordinary skill in the art to which the present disclosure belongs. Although methods and materials similar or equivalent to those described herein can be used in the practice or testing of the disclosed composition embodiments, suitable methods and materials are described below. Unless citing a specific paragraph, all publications, patent applications, patents and other references mentioned herein are incorporated herein by reference in their entirety. If a conflict occurs, this specification and the definitions included therein shall prevail. In addition, materials, methods and examples are illustrative only, and not restrictive.
[0057] It should be particularly noted that, throughout the present invention, tetraoxocyclooctane or 1,3,5,7-tetraoxocyclooctane derivatives are the same as 1,3,5,7-tetraoxocyclooctane derivatives.
[0058] The technical scheme of the present invention, its implementation process and principle, etc. will be further explained through specific embodiments as follows. It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. The described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present invention. Unless otherwise specified, the reagents and raw materials used in the following examples are commercially available, and the test methods for which specific conditions are not specified are usually carried out under conventional conditions or according to the conditions recommended by the manufacturers. In addition, unless otherwise specified, the experimental methods, detection methods, and preparation methods disclosed in the present invention all adopt conventional techniques in the art. These technologies have been fully described in the existing literature.
[0059] Example 1
[0060] This embodiment provides a tetraoxocyclooctane derivative, the structural formula of which is as follows:
[0061] .
[0062] This embodiment provides a method for preparing compound 1, comprising the following steps:
[0063] The synthesis steps of tetraoxocyclooctane derivatives are as follows:
[0064] Cool 125 mL of acetaldehyde to 0 °C, then add 28 mL of ether, stir continuously, control the reaction temperature to -15 °C, and slowly add 5 mL of pyridine. Add 2.6 mL of thionyl chloride to the reaction solution, which is used as a catalyst. Control the rate of catalyst addition (5 min / mL) to ensure that the temperature of the reaction mixture remains at -5 °C. After the catalyst is added, stir vigorously at -15 °C for 2 h. The mixture is extracted with ether, then dried with anhydrous magnesium sulfate, and finally collected by vacuum distillation at 40 °C to obtain a solvent (referred to as "Solvent 1").
[0065] Its infrared spectrum data are as follows: IR (KBr, cm -1 ): 1875, 1716, 1239, 1100, 938, 633. The infrared spectrum was analyzed at a wavelength of 1875 cm -1 and 1716 cm -1 The peak at wavelength 938 is the stretching vibration peak of methyl CH, and the peak at wavelength 938 is the stretching vibration peak of polyoxymethylene CO, confirming that the prepared substance is a tetraoxocyclooctane derivative of the above structure.
[0066] Prepare the electrolyte sample. The specific steps are as follows:
[0067] In an argon glove box with moisture ≤10 ppm, lithium bis(fluorosulfonyl)imide (LiFSI) was slowly added to dimethyl ether (DME). After LiFSI was completely dissolved, solvent 1 was added, stirred evenly, and then BTFE was added. The electrolyte was stirred for 4 h to obtain an electrolyte (referred to as "electrolyte 1"), wherein LiFSI:DME:solvent 1:BTFE=1:1:0.5:4.
[0068] To prepare a lithium metal battery, the specific steps are as follows:
[0069] The positive electrode active material (NMC811), the conductive agent (acetylene black), and the binder (polytetrafluoroethylene) were mixed in a mass ratio of NMC811: acetylene black: polytetrafluoroethylene = 95:3:2. After the mixing was completed, N-methylpyrrolidone (NMP) was added and stirred to obtain a positive electrode slurry. The positive electrode slurry was evenly coated on an aluminum foil with a thickness of 15 μm, and the positive electrode sheet was obtained after drying. The negative electrode material was a pure lithium sheet with a thickness of 100 μm. The soft-pack laminated battery was made in a dry environment with a dew point temperature below -40 ℃. The positive electrode sheet, the separator and the negative electrode sheet were stacked in order to ensure that the separator completely separated the positive and negative electrode sheets, and the aluminum-plastic film was used to seal and weld the pole ears to form a battery to be injected. Before the injection, the battery moisture content was baked to below 300 ppm, and the electrolyte 1 was injected. After sealing, formation and volume separation, the experimental battery (referred to as "battery 1") was obtained.
[0070] Example 2
[0071] The solvent 1 provided in this example is the same as that in Example 1.
[0072] Preparation of electrolyte: In an argon glove box with a water content of ≤10 ppm, lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) was slowly added to DME. After LiTFSI was completely dissolved, solvent 1 was added, and BTFE was added after stirring evenly. Then, additives LiDFOB and VC were added, and the electrolyte (referred to as "electrolyte 2") was obtained after stirring for 4 h, wherein LiTFSI:DME:solvent 1:BTFE=1:1:0.5:4. The mass fraction of additives was 3wt%LiDFOB and 2wt%VC.
[0073] A lithium metal battery (referred to as "battery 2") was prepared according to the method of Example 1, with the only difference being that the electrolyte therein was electrolyte 2 prepared in this example.
[0074] Example 3
[0075] The solvent 1 provided in this example is the same as that in Example 1.
[0076] Preparation of electrolyte: In an argon glove box with a water content of ≤10 ppm, slowly add LiTFSI to triethylene glycol dimethyl ether. After LiTFSI is completely dissolved, add solvent 1, stir evenly, then add D2 (bis(2,2,2-trifluoroethyl) ether), then add additives LiDFOB and isosorbide nitrate, stir for 4 h to obtain an electrolyte (referred to as "electrolyte 3"), wherein LiTFSI: triethylene glycol dimethyl ether: solvent 1: D2 = 1:1:0.5:4. The mass fraction of the additives is 3 wt% LiDFOB and 1 wt% isosorbide nitrate.
[0077] A lithium metal battery (referred to as "battery 3") was prepared according to the method of Example 1, with the only difference being that the electrolyte therein was electrolyte 3 prepared in this example.
[0078] Example 4 This example provides a tetraoxocyclooctane derivative, the structure of which is as follows:
[0079] .
[0080] The synthesis steps of the tetraoxocyclooctane derivative are as follows:
[0081] Cool 125 mL of acetaldehyde to 0 °C, then add 32 mL of ether, stir continuously, control the reaction temperature to -15 °C, slowly add 5 mL of pyridine, stir continuously, and after the temperature stabilizes, slowly add 14 mL of 96% sulfuric acid, stirring continuously. Add 3.8 mL of thionyl chloride to the reaction solution, thionyl chloride is used as a catalyst, and the rate of catalyst addition is controlled (0.5 min / mL) to ensure that the temperature of the reaction mixture remains at -5 °C. After the catalyst is added, stir vigorously at -15 °C for 2 h to obtain a mixture. The above mixture is extracted with ether, then dried with anhydrous magnesium sulfate, and finally collected by vacuum distillation at 40 °C to obtain a solvent (referred to as "Solvent 2").
[0082] Its infrared spectrum data are as follows: IR (KBr, cm -1 ): 2853, 1875, 1716, 1239, 1100, 938, 633. The infrared spectrum is analyzed at a wavelength of 2853 cm -1 、1875 cm -1 and 1716 cm -1 The peak at wavelength 938 is the stretching vibration peak of methyl CH, and the peak at wavelength 938 is the stretching vibration peak of polyoxymethylene CO, confirming that the prepared substance is a tetraoxocyclooctane derivative of the above structure.
[0083] Preparation of electrolyte: In an argon glove box with moisture ≤10 ppm, LiTFSI was slowly added to diethylene glycol butyl ether (DEE). After LiTFSI was completely dissolved, solvent 2 was added, and BTFE was added after stirring. Then, additives lithium difluorooxalatoborate (LiDFOB) and vinylene carbonate (VC) were added, and stirred for 4 h to obtain an electrolyte (referred to as "electrolyte 4"), wherein LiTFSI:DEE: solvent 2:BTFE=1:1:0.5:4; the mass fractions of the additives were 3 wt% LiDFOB and 2 wt% VC.
[0084] A lithium metal battery (referred to as "battery 4") was prepared according to the method of Example 1, with the only difference being that the electrolyte therein was electrolyte 4 prepared in this example.
[0085] Example 5
[0086] The solvent 2 provided in this embodiment is the same as that in embodiment 4.
[0087] Preparation of electrolyte: In an argon glove box with moisture ≤10 ppm, LiTFSI was slowly added to 1,3-dioxolane (DOL). After LiTFSI was completely dissolved, solvent 2 was added, and BTFE was added after stirring. Then, additives LiDFOB and VC were added, and stirred for 4 h to obtain an electrolyte (referred to as "electrolyte 5"), wherein LiTFSI:DOL:solvent 2:BTFE=1:1:0.5:4; the mass fractions of the additives were 3 wt% LiDFOB and 2 wt% VC.
[0088] A lithium metal battery (referred to as "battery 5") was prepared according to the method of Example 1, with the only difference being that the electrolyte therein was electrolyte 5 prepared in this example.
[0089] Example 6
[0090] This embodiment provides a tetraoxocyclooctane derivative whose structure is as follows:
[0091] .
[0092] The synthesis steps of the tetraoxocyclooctane derivative of the above structural formula are as follows:
[0093] Cool 55 mL of acetaldehyde to 0 °C, then add 78 mL of ether, stir continuously, control the reaction temperature to -15 °C, then add 32 mL of diethylene glycol, and continue stirring for 30 min. Slowly add 5 mL of pyridine and continue stirring for 2 h. Add 5.6 mL of thionyl chloride to the reaction solution, thionyl chloride is used as a catalyst, and the catalyst addition rate is controlled (0.5 min / mL) to ensure that the temperature of the reaction mixture remains below -5 °C. After the catalyst is added, vigorously stir at -15 °C for 2 h to obtain a mixture; extract the above mixture with ether, then dry it with anhydrous magnesium sulfate, and finally collect it by vacuum distillation at 40 °C to obtain a solvent (recorded as "Solvent 3").
[0094] Its infrared spectrum data are as follows: IR (KBr, cm -1 ): 1875, 1716, 1465, 1239, 1100, 938, 633. The infrared spectrum was analyzed at a wavelength of 1875 cm -1 and 1716 cm -1 The peak at wavelength 938 is the stretching vibration peak of methyl CH, the peak at wavelength 1465 is the stretching vibration peak of polyoxymethylene CO, and the peak at wavelength 1465 is the bending vibration peak of polyoxymethylene CH, confirming that the prepared substance is a tetraoxocyclooctane derivative of the above structure.
[0095] Preparation of electrolyte: In an argon glove box with water content ≤10 ppm, slowly add LiPF6 to DMC, wait until LiPF6 is completely dissolved, add solvent 3, stir evenly, then add TTE, then add additives LiDFOB and VC, stir for 4 h to obtain electrolyte (referred to as "electrolyte 6"), where LiPF6:DMC:solvent 3:TTE=1:1:0.5:4. The mass fraction of additives is 3wt%LiDFOB and 2wt%VC.
[0096] A lithium metal battery (referred to as "battery 6") was prepared according to the method of Example 1, with the only difference being that the electrolyte therein was electrolyte 6 prepared in this example.
[0097] Example 7
[0098] This embodiment provides a tetraoxocyclooctane derivative whose structure is as follows:
[0099] .
[0100] The synthesis steps of the tetraoxocyclooctane derivatives of the above structure are as follows:
[0101] Acetaldehyde (125 mL) was cooled to 0 °C, and then 28 mL of ether was added, stirring continuously, the reaction temperature was controlled at -15 °C, and 5 mL of pyridine was slowly added, stirring continuously for 2 h. Then 12 mL of 96% sulfuric acid was slowly added, the temperature was maintained at -5 °C, and 32 g of 1,1,1-trifluoro-2,3-propanediol was quickly added while stirring to obtain a reaction solution.
[0102] 4.3 mL of thionyl chloride was added to the reaction solution, and thionyl chloride was used as a catalyst. The rate of catalyst addition was controlled (5 min / mL) to ensure that the temperature of the reaction solution was maintained at -5 °C. After the catalyst was added, it was vigorously stirred at -15 °C for 2 h. The mixture was extracted with ether, then dried with anhydrous magnesium sulfate, and finally collected by vacuum distillation at 40 °C to obtain a solvent (referred to as "Solvent 4").
[0103] Its infrared spectrum data are as follows: IR (KBr, cm -1 ): 1875, 1716, 1239, 1100, 938, 730, 633. The infrared spectrum was analyzed at a wavelength of 1875 cm -1 and 1716 cm -1 The peak at wavelength 938 is the stretching vibration peak of methyl CH, the peak at wavelength 938 is the stretching vibration peak of polyoxymethylene CO, and the peak at wavelength 730 is the stretching vibration peak of polyoxymethylene CF, confirming that the prepared substance is a tetraoxocyclooctane derivative of the above structure.
[0104] Preparation of electrolyte: In an argon glove box with water content ≤10 ppm, slowly add LiTFSI to DEE, wait until LiTFSI is completely dissolved, add solvent 4, stir evenly, then add BTFE, then add additives LiDFOB and VC, stir for 4 h to obtain electrolyte (referred to as "electrolyte 7"), where LiTFSI:DEE: solvent 4:BTFE = 1:1:0.5:4. The mass fraction of additives is 3wt% LiDFOB and 2wt% VC.
[0105] A lithium metal battery (referred to as "battery 7") was prepared according to the method of Example 1, with the only difference being that the electrolyte therein was electrolyte 7 prepared in this example.
[0106] Example 8
[0107] A lithium metal battery (referred to as "battery 8") was prepared according to the method of Example 1, with the only difference being that the electrolyte was electrolyte 7 prepared in Example 7, and lithium iron phosphate (LFP) was used as the positive electrode material.
[0108] Example 9
[0109] A lithium metal battery (referred to as "battery 9") was prepared according to the method of Example 1, with the only difference being that the electrolyte therein was electrolyte 7 prepared in Example 7, and a lithium-plated copper current collector was used for the negative electrode.
[0110] Comparative Example 1
[0111] Preparation of electrolyte: In an argon glove box with water content ≤10 ppm, slowly add LiFSI to DEE, and after LiFSI is completely dissolved, stir evenly and then add BTFE, then add additives LiDFOB and VC, and stir for 4 h to obtain an electrolyte (referred to as "electrolyte 8"), where LiFSI:DEE: BTFE=1:1:4. The mass fraction of the additives is 3wt%LiDFOB and 2wt%VC.
[0112] A lithium metal battery (referred to as "battery 10") was prepared according to the method of Example 1, with the only difference being that the electrolyte therein was electrolyte 8 prepared in this comparative example.
[0113] Comparative Example 2
[0114] Preparation of electrolyte: In an argon glove box with a water content of ≤10 ppm, slowly add LiTFSI to dimethyl ether (DME), and after LiTFSI is completely dissolved, stir evenly before adding BTFE, and then add additives LiDFOB and VC, and stir for 4 hours to obtain an electrolyte (referred to as "electrolyte 9"), wherein LiTFSI:DME:BTFE=1:1:4. The mass fraction of the additives is 3wt%LiDFOB and 2wt%VC.
[0115] A lithium metal battery (referred to as "battery 11") was prepared according to the method of Example 1, with the only difference being that the electrolyte therein was electrolyte 9 prepared in this comparative example.
[0116] Comparative Example 3
[0117] In an argon glove box with a water content of ≤10 ppm, LiPF6 was slowly added to dimethyl carbonate (DMC). After LiPF6 was completely dissolved, 1,2,2-trifluoro-1,1,2-trichloroethane (TTE) was added after stirring evenly. Then, additives LiDFOB and VC were added and stirred for 4 h to obtain an electrolyte (referred to as "electrolyte 10"), in which LiPF6:DMC:TTE=1:1:4. The mass fraction of the additives was 3wt%LiDFOB and 2wt%VC.
[0118] A lithium metal battery (referred to as "battery 12") was prepared according to the method of Example 1, with the only difference being that the electrolyte therein was the electrolyte 10 prepared in this comparative example.
[0119] The electrolyte compositions and contents of Examples 1-9 and Comparative Examples 1-3 are shown in Table 1.
[0120] Table 1 Electrolyte compositions of Examples 1-9 and Comparative Examples 1-3
[0121]
[0122] Furthermore, the present invention tests the battery performance of the lithium metal batteries assembled in the above-mentioned embodiments and comparative examples, and the results are as follows:
[0123] (1) Cycle performance and rate performance test of lithium metal batteries
[0124] Cycle performance test: The lithium metal batteries of Examples 1-9 and Comparative Examples 1-3 after capacity division were placed in a 25°C room temperature working room and connected to a charge and discharge tester, first charged to 4.3 V with a constant current and constant voltage of 1 C, and the cut-off current was set to 0.01 C; after standing for 10 min, they were discharged to 3.0 V with a constant current of 1 C, and the cycle charge and discharge test was performed in this way, and the discharge capacity of each time was recorded, and the cell capacity retention rate of the 100th week, 200th week and 300th week was calculated respectively, wherein the cycle capacity retention rate of the lithium metal cell in the Nth week (%) = discharge capacity in the Nth week / discharge capacity in the first week * 100%, and the comparative data of the test results are shown in Table 2.
[0125] Rate performance test: The lithium metal batteries of Examples 1-9 and Comparative Examples 1-3 after capacity division were placed in a 25°C room temperature workroom and connected to a charge and discharge tester. First, they were charged to 4.3 V at 0.5 C constant current and constant voltage, and the cut-off current was set to 0.01 C. After standing for 10 min, they were discharged to 3.0 V at 0.5 C constant current, and cycled 5 times, recording the discharge capacity each time. Then, the charge and discharge cycles were performed at 1 C, 2 C, 3 C, 4 C, 5 C and 1 C currents, and the cycles were repeated 5 times at each current density, and the discharge capacities were recorded respectively. Among them, the capacity retention rate of the lithium metal battery in the Nth week cycle (%) = the discharge capacity in the Nth week / the discharge capacity in the first week*100%, and the comparative data of the test results are shown in Table 2.
[0126] Table 2 Battery performance test results obtained in various embodiments and comparative examples
[0127]
[0128] According to the test results in Table 2, we can see that:
[0129] 1. It can be seen from the cycle data of Examples 1-2 and Comparative Examples 1-3 that the addition of tetraoxocyclooctane derivatives enables the electrolyte to form a stable SEI film, effectively improving the cycle performance of the lithium metal battery; and the additives are combined to form an SEI film rich in inorganic components. The overall SEI film has high strength, inhibits the formation of dendrites, and can greatly improve the cycle stability.
[0130] 2. It can be seen from the cycle data of Examples 1-9 and Comparative Examples 1-3 that the tetraoxocyclooctane derivatives prepared by the examples are universal in different electrolyte systems, and can synergize with functional solvents and other additives of the electrolyte. The tetraoxocyclooctane derivatives are preferentially polymerized to form an inner layer structure of the SEI film with high toughness and adhesion, and then combined with the outer layer SEI film rich in inorganic components, which can effectively resist the volume change of the metal lithium negative electrode during the charge and discharge process, effectively isolate the metal lithium negative electrode from the electrolyte, prevent continuous reaction, cause electrolyte loss and the formation of lithium dendrites, and show higher cycle stability in battery performance.
[0131] 3. From the comparison of the performance test results of Example 6 and Example 7, it can be seen that when -CF3 exists in the tetraoxocyclooctane derivative, -CF3 is prevented from opening the ring to form a polymer due to the steric hindrance, and a high-strength SEI film cannot be formed, resulting in a decrease in the cycle performance.
[0132] 4. From the data of the rate performance test results of Examples 1-9 and Comparative Examples 1-3, it can be seen that in the examples, due to the presence of tetraoxocyclooctane derivatives, a stable SEI film can be formed, and with the functional additives, an outer SEI film containing high ionic conductivity components is formed, and its rate performance is significantly improved. However, at a high rate of 5C, the ionic conductivity of the electrolyte itself is required to be high, so different electrolyte systems show different improvement effects, and ester electrolytes have higher ionic conductivity, so their improvement effect is the best.
[0133] In summary, the present invention synthesizes a tetraoxocyclooctane derivative solvent and combines it with relevant functional solvents to form a high-performance composite solvent, thereby forming a polymer inner layer SEI with high toughness, and combines it with functional additives to form an outer layer SEI rich in inorganic components, thereby comprehensively forming a stable and high-strength SEI, which exhibits excellent cycle performance in battery performance.
[0134] The various aspects, embodiments, features and examples of the present invention should be considered to be illustrative in all aspects and are not intended to limit the present invention. Other embodiments, modifications and uses will be apparent to those skilled in the art without departing from the spirit and scope of the claimed invention.
[0135] The use of headings and sections in this disclosure is not meant to limit the disclosure; each section may apply to any aspect, embodiment, or feature of the disclosure. Throughout this disclosure, where a composition is described as having, comprising, or including particular components, or where a process is described as having, comprising, or including particular process steps, it is contemplated that the compositions taught by the present disclosure also consist essentially of or consist of the recited components, and that the processes taught by the present disclosure also consist essentially of or consist of the recited process steps.
[0136] Unless specifically stated otherwise, use of the terms "include," "includes," "including," "have," "has," or "having" should generally be construed as open ended and non-limiting.
[0137] It should be understood that the order of the various steps or the order in which a particular action is performed is not very important, as long as the teachings of the present invention remain operable. In addition, two or more steps or actions may be performed simultaneously.
[0138] Although the present invention has been described with reference to illustrative embodiments, it will be appreciated by those skilled in the art that various other changes, omissions and / or additions may be made and that elements of the described embodiments may be substituted with substantial equivalents without departing from the spirit and scope of the present invention. In addition, many modifications may be made to adapt particular circumstances or materials to the teachings of the present invention without departing from the scope of the present invention. Furthermore, unless specifically stated, any use of the terms first, second, etc. does not indicate any order or importance, but rather the terms first, second, etc. are used to distinguish one element from another.
Claims
1. A composite solvent based on 1,3,5,7-tetraoxocyclooctane and its derivatives, characterized in that: It is composed of a first organic solvent and a second organic solvent; the first organic solvent is 1,3,5,7-tetraoxocyclooctane and its derivatives; The structural formula of the first organic solvent is shown in Formula I: Formula I; Wherein, R1, R2, R3, and R4 are independently selected from any one or a combination of two of -H, -CF3, C1-C4 alkoxy, hydroxyl, and C1-C4 alkyl; The second organic solvent is an ester solvent and / or an ether solvent.
2. The composite solvent according to claim 1, characterized in that The structural formula of the first organic solvent is shown in any one of Formula II to Formula V: Formula II Formula III Formula IV Formula V.
3. The composite solvent according to claim 1 or 2, characterized in that The molar ratio of the first organic solvent to the second organic solvent is (0.1-1):
1.
4. The composite solvent according to claim 1 or 2, characterized in that The ester solvent includes any one of ethylene carbonate, ethyl methyl carbonate, dimethyl carbonate, propylene carbonate, fluoroethylene carbonate, vinylene carbonate, methyl trifluoroethyl carbonate, and diethyl carbonate, or a combination of two or more thereof.
5. The composite solvent according to claim 1 or 2, characterized in that: The ether solvent includes any one of dimethyl ether, diethylene glycol butyl ether, 1,3-dioxolane, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, ethylene glycol dibutyl ether, and triethylene glycol dimethyl ether, or a combination of two or more thereof.
6. Use of the composite solvent according to any one of claims 1 to 5 as a solvent in a lithium battery electrolyte.
7. A lithium metal electrolyte, characterized in that include: A lithium salt, a functional additive, a diluent and a composite solvent as claimed in any one of claims 1 to 5.
8. The lithium metal electrolyte according to claim 7, characterized in that: The molar ratio of the lithium salt, the composite solvent and the diluent is 1:(0.5-5):(1-8); The mass fraction of the functional additive in the lithium metal electrolyte is 1-10wt%; The lithium salt includes any one or a combination of two or more of lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, lithium difluorooxalatoborate, trifluoromethanesulfonic acid, lithium bis(pentafluoroethylsulfonyl)imide, lithium tetrafluoroborate, lithium perchlorate, lithium bis(oxalate)borate, and lithium bis(trifluoromethanesulfonyl)imide; The functional additives include any one or a combination of two or more of LiNO3, LiDFOB, 1,3-propane sultone, FEC, VC, isosorbide dinitrate, and tris(trimethylsilyl) borate; The diluent includes any one of trifluoroethyl ether, 1,1,1,3,3,3-hexafluoroisopropyl methyl ether, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether, bis(2,2,2-trifluoroethyl) ether, and octafluoropentyl-1,1,2,2-tetrafluoroethyl ether, or a combination of two or more thereof.
9. A lithium metal battery comprising a positive electrode containing active materials, a negative electrode, a separator and the lithium metal electrolyte as claimed in claim 7 or 8.
10. The lithium metal battery according to claim 9, characterized in that: The active material contained in the positive electrode is any one of a lithiated transition metal phosphate with an olivine structure, a lithium ion embedded transition metal oxide with a layered structure, and a lithiated transition metal mixed oxide with a spinel structure; the negative electrode is any one of pure lithium, a lithium alloy, and a lithium-plated negative electrode.
Citation Information
Patent Citations
Electrolyte and lithium ion battery
CN108598461A
Gellable system for lithium-air battery, and preparation method and application thereof
CN108963389A