A method for preparing a self-oxidation layer, a laminated solar cell and a method for preparing the same
By preparing an auto-oxidation layer in a crystalline silicon/perovskite tandem solar cell, the problem of interface defects between the tin oxide buffer layer and the transparent electrode layer is solved, the photoelectric conversion efficiency and stability are improved, and higher photovoltaic power is achieved. performance and corrosion resistance.
Patent Information
- Application Number
- CN202411102858.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-08-13
AI Technical Summary
Interface defects between the tin oxide buffer layer and the transparent electrode layer in crystalline silicon/perovskite tandem solar cells lead to low photoelectric performance and poor stability, and the existing preparation methods cannot meet the usage standards.
Prepare a stable ultra-thin metal layer on the buffer layer for auto-oxidation to form an auto-oxidation layer to passivate interface defects, improve the adhesion of the transparent electrode and protect the perovskite layer from moisture erosion, using a method that combines evaporation and oxidation processes Preparation of self-oxide layer.
It improves the photoelectric conversion efficiency and stability of solar cells, enhances the adhesion of transparent electrodes, reduces non-radiative recombination losses, and enhances the hardness and corrosion resistance of chemical bonds.
Smart Images

Figure CN118647243B_ABST
Abstract
Description
Technical Field
[0001] The present invention mainly relates to the technical field of solar cells, and in particular to a method for preparing a self-oxidation layer of a perovskite cell, a stacked solar cell and a preparation method thereof. Background Art
[0002] Solar energy is a new type of clean energy that has attracted much attention, with the advantages of abundant resources and low cost. At present, photovoltaic cells are one of the most effective ways to convert solar energy into electrical energy. Perovskite has broad application prospects in the field of photovoltaic cells due to its long carrier lifetime, high carrier mobility, wide band gap, long diffusion length and low formation energy. Among them, combining perovskite cells with crystalline silicon cells to form stacked solar cells has become one of the research hotspots in the field of photovoltaic cells and has attracted much attention. The basic principle of crystalline silicon / perovskite stacked solar cells is to stack perovskite materials and crystalline silicon materials together to form a heterojunction, and to use the wide band gap, high absorption coefficient and high carrier mobility of perovskite materials and the stability and good electron transmission performance of crystalline silicon materials to improve the photoelectric conversion efficiency of solar cells. The theoretical effective photoelectric conversion efficiency is as high as more than 40%.
[0003] However, there are interface defects between the tin oxide buffer layer and the transparent electrode layer in crystalline silicon / perovskite tandem solar cells. These defects can serve as non-radiative recombination centers, resulting in a decrease in the concentration of photogenerated carriers. These defects may also become erosion centers for oxygen and water. In addition, due to the low interfacial adhesion between the transparent electrode layer and the tin oxide buffer layer, the transparent electrode layer is easily peeled off on the tin oxide buffer layer, thereby reducing the photoelectric performance and stability of the device. Therefore, improving the interface defects between the tin oxide buffer layer and the transparent electrode layer is particularly important for improving the efficiency and stability of crystalline silicon / perovskite tandem solar cells.
[0004] Regarding the problem of interface defects between the buffer layer and the transparent electrode layer, the film layers prepared by methods such as evaporation and atomic deposition will have damage to some devices and cannot meet the use standards of solar cells.
[0005] In summary, due to the defects between the buffer layer and the transparent electrode layer in the crystalline silicon / perovskite tandem solar cell, the photoelectric conversion efficiency of the solar cell is low and the stability during use is poor, which is still a problem to be solved. Summary of the invention
[0006] The present invention aims to provide a method for preparing a self-oxidation layer, a stacked solar cell and a preparation method, so as to solve the problem that when existing devices use metal oxide as a buffer layer in perovskite top cells, the interface defects between the metal oxide and the transparent electrode layer cause non-radiative recombination, resulting in a decrease in photoelectric performance and stability.
[0007] The present invention prepares a stable ultra-thin metal layer as a protective layer on a buffer layer, and the metal layer is subsequently exposed to oxygen for oxidation to form a self-oxidation layer, which can passivate the interface defects between the buffer layer and the transparent electrode layer interface, reduce non-conforming losses, and improve the photoelectric conversion efficiency of the device. In addition, the self-oxidation layer has a higher strength chemical bond, so that it has higher hardness and corrosion resistance. Therefore, the self-oxidation layer can not only enhance the adhesion of the transparent electrode on the buffer layer to reduce peeling, but also protect the perovskite layer from external moisture erosion, thereby improving the stability of the device. The laminated solar cell prepared by this method has higher stability and light conversion efficiency.
[0008] To achieve the above object, the specific scheme provided by the present invention is as follows.
[0009] A method for preparing a self-oxidation layer comprises the following steps:
[0010] S1, providing a suede substrate with a buffer layer on its surface, and evaporating a self-oxidizing material on the surface of the buffer layer to form a metal film;
[0011] S2, oxidizing the metal film in air to obtain a self-oxidation layer.
[0012] Furthermore, the self-oxidizing material is at least one of metal yttrium (Yb) and metal copper (Cu).
[0013] Furthermore, the evaporation vacuum degree of the evaporation is (1-5)×10 -4 Pa, temperature is 500-800℃.
[0014] Furthermore, the evaporation rate of the evaporation is 0.05-1Å / S.
[0015] Furthermore, the thickness of the metal film is between 1-5 nm.
[0016] Furthermore, the oxidation process is to place the metal film in air for oxidation, and the oxidation time is 1-60 minutes.
[0017] Furthermore, the buffer layer is prepared from the buffer layer material by atomic accumulation deposition or evaporation.
[0018] Furthermore, the buffer layer material is zinc oxide (ZnO), tin dioxide (SnO2), titanium dioxide (TiO2), [6,6]-phenyl C 61 Methyl butyrate (PC 61 BM), carbon 60 (C 60 ), 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline (BCP).
[0019] Specifically, the velvet substrate includes a silicon substrate, and a substrate surface passivation layer, an N-type substrate doping layer, a tunneling layer, a hole transport layer, a perovskite absorption layer, a passivation layer, and an electron transport layer are sequentially arranged on the surface of the silicon substrate, and a substrate passivation layer, a P-type substrate doping layer, a first transparent electrode layer, and a first metal electrode layer are sequentially arranged on the back side of the silicon substrate, and the buffer layer is arranged on the electron transport layer.
[0020] The present invention also provides a laminated solar cell obtained by the above-mentioned self-oxidation layer preparation method, whose structure from bottom to top is a first metal electrode layer, a first transparent electrode layer, a P-type substrate doping layer, a substrate passivation layer, a silicon substrate, a substrate surface passivation layer, an N-type substrate doping layer, a tunneling layer, a hole transport layer, a perovskite absorption layer, a passivation layer, an electron transport layer, a buffer layer, a self-oxidation layer, a second transparent electrode layer, a second metal electrode layer, and an anti-reflection layer.
[0021] Furthermore, the preparation method of the stacked solar cell is: providing a silicon substrate, preparing the base passivation layer on the back side of the silicon substrate, preparing the P-type base doping layer on the surface of the base passivation layer, preparing the first transparent electrode layer on the surface of the P-type base doping layer, and preparing the first metal electrode layer on the surface of the first transparent electrode layer; and preparing the base surface passivation layer on the surface of the silicon substrate, preparing the N-type base doping layer on the surface of the base surface passivation layer, preparing the tunneling layer on the surface of the N-type base doping layer, preparing the hole transport layer on the surface of the tunneling layer, preparing the perovskite absorption layer on the surface of the hole transport layer, preparing the passivation layer on the surface of the perovskite absorption layer, preparing the electron transport layer on the surface of the passivation layer, preparing the buffer layer on the surface of the electron transport layer, preparing the self-oxidation layer on the surface of the buffer layer, preparing the second transparent electrode layer on the surface of the self-oxidation layer, preparing the second metal electrode layer on the surface of the second transparent electrode layer, and preparing an anti-reflection layer on the surface of the second metal electrode layer.
[0022] The first transparent electrode layer is prepared by magnetron sputtering;
[0023] The first metal electrode layer is prepared by evaporation;
[0024] The tunneling layer is prepared by atomic deposition method, magnetron sputtering method or wet chemical method;
[0025] The hole transport layer is treated with an ultraviolet-ozone machine (UV-Ozone) for 0-30 minutes before preparation;
[0026] The hole transport layer is prepared by spin coating or magnetron sputtering;
[0027] The perovskite absorption layer is prepared by spin coating, flash evaporation or evaporation;
[0028] The passivation layer is prepared by evaporation, spin coating or spraying;
[0029] The electron transport layer is prepared by spin coating, inkjet or evaporation;
[0030] The buffer layer is prepared by spin coating, atomic accumulation deposition or evaporation;
[0031] The self-oxidation layer is prepared by evaporation and self-oxidation method;
[0032] The second transparent electrode layer is prepared by magnetron sputtering or evaporation;
[0033] The second metal electrode layer is prepared by evaporation;
[0034] The anti-reflection layer is prepared by magnetron sputtering or evaporation.
[0035] Furthermore, the first transparent electrode layer is prepared by a magnetron sputtering method, wherein the silicon substrate on which the P-type base doping layer, base passivation layer, base surface passivation layer and N-type base doping layer are prepared is placed in a magnetron sputtering device for preparation, and the magnetron sputtering power is 50-200W.
[0036] The first metal electrode layer is deposited by evaporation, which includes placing the prepared substrate sample on a mask plate for evaporation, and the evaporation vacuum is 5×10 -5 -2×10 -4 Pa, the evaporation temperature is 500-2000℃, and the evaporation rate is 0.1-5Å / S.
[0037] The hole transport layer is prepared by spin coating, which includes uniformly coating the hole transport layer dispersion on the surface of the tunnel layer at a spin coating speed of 1000-5000 rpm and a spin coating time of 10-100 s. After the spin coating, an annealing operation is performed at a temperature of 300-600°C and a annealing time of 10-50 min. The hole transport layer can also be prepared by magnetron sputtering, which includes placing the prepared substrate in a magnetron sputtering device and controlling the power to be 30-90 W.
[0038] The perovskite absorption layer is prepared by a spin coating method, including preparing a perovskite precursor solution, uniformly coating the perovskite precursor solution on the surface of the hole transport layer, and using an anti-solvent for dynamic spin coating. The spin coating speed is 1200-6000 rpm, the spin coating time is 20-120 s, and the anti-solvent titration time is 10-50 s after the start of the spin coating. After the spin coating is completed, an annealing operation is performed, the annealing temperature is 50-150° C., and the annealing time is 5-40 min.
[0039] Alternatively, the perovskite absorption layer may also be formed by a flash evaporation method, including preparing a perovskite precursor solution, uniformly coating the perovskite precursor solution on the surface of the hole transport layer, the spin coating speed is 1000-6000 rpm, the spin coating time is 20-120 s, after the spin coating is completed, a flash evaporation operation is performed, the flash evaporation time is 10-60 s, the flash evaporation temperature is 0-100° C., after the flash evaporation is completed, an annealing treatment is performed, the annealing temperature is 50-150° C., and the annealing time is 5-40 min;
[0040] Alternatively, the perovskite absorption layer may also be deposited by a vapor deposition method, including preparing a perovskite precursor powder, evaporating the perovskite precursor powder onto the surface of the hole transport layer, and depositing the perovskite precursor powder by a vacuum degree of 1-3×10 -4 Pa, and the evaporation temperature is 200-700℃.
[0041] The passivation layer is deposited by evaporation, which includes evaporating propylene diamine iodide onto the surface of the perovskite absorption layer, and the evaporation vacuum is 1-5×10 -4 Pa, the evaporation temperature is 50-400℃, the evaporation rate is 0.05-1Å / S, and after the evaporation, annealing operation is performed, the annealing temperature is 0-150℃, and the annealing time is 0-30min;
[0042] Alternatively, the passivation layer may also be coated by a spin coating method, including preparing a passivation layer dispersion and uniformly coating it on the surface of the perovskite absorption layer, wherein the passivation layer dispersion is prepared by dissolving propylenediamine iodine in an organic solvent including but not limited to methanol, ethanol or isopropanol, ultrasonically dissolving and spin coating, wherein the concentration of propylenediamine iodine is 0.1-6 mg / mL, the ultrasonic time is 0-30 min, the spin coating speed is 1000-7000 rpm, the spin coating time is 20-120 s, and after the spin coating is completed, an annealing operation is performed, the annealing temperature is 40-160° C., and the annealing time is 5-40 min;
[0043] Alternatively, the passivation layer may also be sprayed, including spraying the passivation layer dispersion on the perovskite absorption layer at a spraying rate of 0-100 cm / s. After spraying, annealing is performed at a temperature of 20-170° C. for a time of 0-30 min.
[0044] The electron transport layer is formed by a spin coating method, which includes uniformly coating the electron transport layer dispersion on the surface of the passivation layer, with a spin coating speed of 500-4000 rpm and a spin coating time of 10-80 s;
[0045] The electron transport layer can also be deposited by evaporating the electron transport layer material onto the surface of the passivation layer. The evaporation vacuum is 5×10 -5 -5×10 -4 Pa, the evaporation temperature is 100-400℃, and the evaporation rate is 0.05-1Å / S.
[0046] The buffer layer adopts the atomic accumulation deposition method, which includes depositing the buffer layer material onto the surface of the electron transport layer using an atomic accumulation deposition device, and the deposition vacuum is 0-1×10 4 Pa, the deposition pipeline temperature is between 50-150°C, and the deposition chamber temperature is 40-150°C;
[0047] The buffer layer can also be deposited by evaporating the buffer layer material onto the surface of the electron transport layer. The evaporation vacuum is 6×10 -5 -4×10 -4 Pa, the evaporation temperature is 100-500℃, and the evaporation rate is 0.05-1Å / S.
[0048] The self-oxidation layer is prepared by evaporation and self-oxidation method, including evaporating the self-oxidation material onto the surface of the buffer layer, and the evaporation vacuum degree is 1-5×10 -4 Pa, the evaporation temperature is 500-800℃, the evaporation rate is 0.05-1Å / S, the thickness is controlled at 0-5nm, and after the evaporation is completed, the sample is placed in the air and oxidized for 0-60min.
[0049] The second transparent electrode layer is formed by a magnetron sputtering method, which includes sputtering the transparent electrode material onto the surface of the self-oxidation layer, with a control power of 30-200W;
[0050] Alternatively, the second transparent electrode layer may also be formed by evaporation of the transparent electrode material onto the surface of the self-oxidation layer, with the evaporation vacuum being 1×10 -5 -5×10 -4 Pa, the evaporation temperature is 1000-2000℃, and the evaporation rate is 0.05-3Å / S.
[0051] Furthermore, the hole transport layer is poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine] (PTAA), poly-3-hexylthiophene (P3HT), nickel oxide (NiO x ), molybdenum trioxide (MoO3), cuprous iodide (CuI), and cuprous thiocyanate (CuSCN).
[0052] The passivation layer is propylenediamine iodide, including but not limited to at least one of propylenediamine bromide (PDADBr), butylammonium chloride (BACl), butylammonium bromide (BABr), butylammonium iodide (BAI), N,N-dimethyl-1,3-propylenediamine hydrochloride (DMePDADCl), and dodecanediaminium bromide (DDDADBr); it can also be at least one of magnesium fluoride (MgF), lithium fluoride (LiF), and sodium fluoride (NaF).
[0053] The dissolving solvent of the perovskite precursor solution includes at least one of dimethylformamide (DMF), G-butyrolactone (GBL), dimethyl sulfoxide (DMSO) and N,N-dimethylacetamide (DMA), and the solvent ratio is between 0-3:10-7.
[0054] The anti-solvent includes at least one of toluene (Tol), chlorobenzene (CB), and ethyl acetate (EA).
[0055] The electron transport layer is zinc oxide (ZnO), tin dioxide (SnO2), titanium dioxide (TiO2), [6,6]-phenyl C 61 Methyl butyrate (PC 61 BM), carbon 60 (C 60 ), 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline (BCP).
[0056] The buffer layer is at least one of zinc oxide (ZnO), tin dioxide (SnO2), and titanium dioxide (TiO2).
[0057] The self-oxidizing material is at least one of metal yttrium (Yb) and metal copper (Cu).
[0058] The first transparent electrode layer and the second transparent electrode layer are at least one of indium tin oxide (ITO), indium zinc oxide (IZO), and aluminum zinc oxide (AZO).
[0059] The second metal electrode layer is at least one of silver (Ag), gold (Au), copper (Cu), aluminum (Al), and carbon (C).
[0060] The anti-reflection layer is at least one of magnesium fluoride, lithium fluoride (LiF), sodium fluoride (NaF), and silicon oxide (SiO2).
[0061] The present invention has obvious advantages over the prior art. Specifically, it can be seen from the above technical scheme that it mainly provides a method for preparing a self-oxidation layer. The method combines evaporation and oxidation processes. Compared with traditional direct evaporation, atomic deposition and other methods, this step can ensure that no damage is caused to the device. A layer of highly stable metal oxide film material is added between the buffer layer and the transparent electrode layer, which can effectively enhance the adhesion of the transparent electrode on the buffer layer to reduce peeling, protect the perovskite layer from external moisture erosion, and thereby improve the stability of the device. BRIEF DESCRIPTION OF THE DRAWINGS
[0062] Figure 1 A schematic diagram of the structure of a stacked solar cell in an embodiment of the present invention;
[0063] Figure 2 is a flow chart for preparing the self-oxidation layer described in an embodiment of the present invention;
[0064] The numbers in the figure are: 1, anti-reflection layer; 2, second metal electrode layer; 3, second transparent electrode layer; 4, self-oxidation layer; 5, buffer layer; 6, electron transport layer; 7, passivation layer; 8, perovskite absorption layer; 9, hole transport layer; 10, tunneling layer; 11, N-type substrate doping layer; 12, substrate surface passivation layer; 13, silicon substrate; 14, substrate passivation layer; 15, P-type substrate doping layer; 16, first transparent electrode layer; 17, first metal electrode layer. DETAILED DESCRIPTION
[0065] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0066] In the description of the present invention, unless otherwise specified, "multiple" means two or more; the terms "center", "longitudinal", "lateral", "up", "down", "left", "right", "inside", "outside", "front end", "rear end", "head", "tail", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate the orientation or position relationship based on the orientation or position relationship shown in the drawings, which is only for the convenience of describing the present invention and simplifying the description, and does not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operate in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", "third" and the like are used for descriptive purposes only and cannot be understood as indicating or implying relative importance.
[0067] Example 1
[0068] See also Figure 1~2 The present embodiment provides a stacked solar cell, whose structure from bottom to top is a first metal electrode layer 17, a first transparent electrode layer 16, a P-type base doping layer 15, a base passivation layer 14, a silicon substrate 13, a base surface passivation layer 12, an N-type base doping layer 11, a tunneling layer 10, a hole transport layer 9, a perovskite absorption layer 8, a passivation layer 7, an electron transport layer 6, a buffer layer 5, a self-oxidation layer 4, a second transparent electrode layer 3, a second metal electrode layer 2, and an anti-reflection layer 1, and is prepared by the following method, including the steps of:
[0069] Step 1: providing a silicon substrate 13, sequentially preparing a base passivation layer 14 and a P-type base doping layer 15 on the back side of the silicon substrate 13, and sequentially preparing a base surface passivation layer 12 and an N-type base doping layer 11 on the surface;
[0070] Step 2: preparing a first transparent electrode layer 16;
[0071] By using magnetron sputtering method, the sample is placed in a magnetron sputtering device, an ITO target is set, the power is controlled to 60W, the operation time is 1.5h, and a first transparent electrode layer 16 is formed on the P-type base doping layer, and the film thickness is 100nm;
[0072] Step 3: preparing a first metal electrode layer 17;
[0073] Using the evaporation method, the substrate sample is placed on the mask and placed in the evaporation chamber. The vacuum degree of evaporation is 2×10 - 4 Pa, the evaporation voltage is adjusted to the evaporation temperature, the evaporation rate is controlled at 2.5Å / S, and silver is evaporated onto the first transparent electrode layer 16 to a thickness of 200nm;
[0074] Step 4: preparing a tunneling layer 10 on the surface of the N-type base doping layer 11;
[0075] Using magnetron sputtering, the sample was placed on a mask and then placed in a magnetron sputtering device, the control power was 60W, the operation time was 1h, and a silicon dioxide layer was formed on the surface of the N-type base doping layer 11, and the film thickness was 40nm;
[0076] Step 5: preparing a hole transport layer 9;
[0077] The sample was treated with UV-Ozone for 15 minutes, and a hole transport layer dispersion was prepared by spin coating. 0.05 mol NiOx powder was weighed and dissolved in 1 mL ultrapure water. Ultrasonic vibration was performed for 20 minutes, and the hole transport layer dispersion was evenly coated on the surface of the sample. The spin coating speed was set to 2000 rpm, the spin coating time was 40 seconds, and the solution volume was 100 uL. After the spin coating, annealing was performed at 450°C and 30 minutes. A hole transport layer 9 was formed on the surface of the tunneling layer 10 with a thickness of about 20 nm.
[0078] Step 6: preparing a perovskite absorption layer 8;
[0079] Using the flash evaporation method, prepare the perovskite precursor solution, weigh an appropriate amount of perovskite powder and dissolve it in 1mL DMF and DMSO solvents, the solvent ratio is 8:2, and magnetic stirring is performed for 30 minutes. Then the sample is placed on the base of the spin coater, the spin coating speed is set to 3500rpm, the spin coating time is 30s, and the perovskite precursor solution volume is 120uL to coat the surface of the sample. After the spin coating is completed, the sample is placed on the flash evaporation table, the flash evaporation time is set to 30s, and the flash evaporation temperature is set to 30℃. After the flash evaporation is completed, annealing is performed, the annealing temperature is set to 100℃, and the annealing time is 15min to form a perovskite absorption layer 8 with a thickness of 500nm;
[0080] Step 7: preparing a passivation layer 7;
[0081] Using the evaporation method, 3 mg of propylene diamine iodide was weighed and placed in a crucible. The substrate sample was placed on the mask and placed in the evaporation chamber. The vacuum degree of evaporation was 2×10 -4 Pa, the evaporation voltage was adjusted to the evaporation temperature, the evaporation rate was controlled at 0.1Å / S, propylenediamine iodide was evaporated onto the perovskite absorption layer 8, the thickness was 4nm, and after the annealing table temperature was set to 100℃, and the annealing operation was performed for 8min;
[0082] Step 8: preparing the electron transport layer 6;
[0083] Using the evaporation method, place the sample on the mask and put it into the evaporation chamber until the evaporation vacuum degree is 1×10 -4 Pa, adjust the evaporation voltage to the evaporation temperature, control the evaporation rate at 0.1-0.15Å / S, and 60 Evaporation onto the passivation layer 7 with a thickness of 20 nm;
[0084] Step nine: preparing a buffer layer 5;
[0085] Using atomic accumulation deposition, the vacuum degree of the atomic accumulation deposition equipment was set to 0.5×10 4 Pa, the deposition pipeline temperature is between 60°C, the deposition chamber temperature is 70°C, and SnO2 is evaporated onto the electron transport layer 6 with a thickness of 15 nm;
[0086] Step 10: preparing a self-oxidation layer 4;
[0087] Using the evaporation method, place the substrate sample on the mask and put it into the evaporation chamber until the evaporation vacuum degree is 1×10 -4 Pa, the evaporation voltage was adjusted to an evaporation temperature of 800 degrees, the evaporation rate was controlled at 0.1Å / S, and metal yttrium was evaporated onto the buffer layer 5 with a thickness of 1nm; then the sample was placed in the air for self-oxidation for 5 minutes to form a 1nm yttrium oxide (YbOx) film;
[0088] Step 11: preparing a second transparent electrode layer 3;
[0089] By using magnetron sputtering method, an IZO target is set, the power is controlled to be 50W, the operation time is 1h, and a second transparent electrode layer 3 is formed on the surface of the self-oxidation layer 4, and the film thickness is 100nm;
[0090] Step 12: preparing a second metal electrode layer 2;
[0091] Using the evaporation method, the substrate sample prepared in the previous step was placed in the chamber of the evaporation machine and the evaporation vacuum was 2×10-4 Pa, adjusting the evaporation voltage to the evaporation temperature, controlling the evaporation rate at 2.5Å / S, and evaporating silver onto the second transparent electrode layer to obtain a second metal electrode layer with a thickness of 100nm;
[0092] Step 13: preparing an anti-reflection layer 1;
[0093] Magnesium fluoride is evaporated on the second metal electrode layer by an evaporation method, the evaporation rate is controlled at 2Å / S, and the thickness is 100nm, and finally a stacked solar cell is obtained.
[0094] Example 2
[0095] This embodiment provides a stacked solar cell having the same device structure as that of the embodiment 1, but differs from the embodiment 1 in that the thickness of the self-oxidation layer 4 is 2 nm.
[0096] Example 3
[0097] This embodiment provides a stacked solar cell having the same device structure as that of the embodiment 1, but differs from the embodiment 1 in that the thickness of the self-oxidation layer 4 is 3 nm.
[0098] Comparative Example 1
[0099] This comparative example provides a stacked solar cell, which is different from Example 1 in that the preparation process of the self-oxidation layer in step 10 is omitted.
[0100] Comparative Example 2
[0101] This comparative example provides a stacked solar cell, which is different from Example 2 in that the evaporation voltage is adjusted to an evaporation temperature of 3000 degrees in step 10. Specifically, the substrate sample is placed on a mask plate and placed in a chamber of an evaporation machine by an evaporation method. The vacuum degree of the evaporation is 1×10 -4 Pa, the evaporation voltage was adjusted to an evaporation temperature of 3000 degrees, the evaporation rate was controlled at 0.1Å / S, and the yttrium oxide material was evaporated onto the film with a thickness of 2nm.
[0102] A solar simulator was used to calibrate the intensity of a standard sun and to measure the intensity of a standard sun with an area of 1.0 cm. 2 The devices obtained in the above embodiments and comparative examples were subjected to long-term IV tests, with the starting voltage set to 1.95V, the cut-off voltage set to 0V, the range set to 100mA, and the results retained two decimal places. The test results are shown in the following table;
[0103] Devices Open circuit voltage (V) Photoelectric conversion efficiency (%) Decay rate / stability (% / year) Example 1 1.92 29.88 0.6 Example 2 1.93 30.62 0.5 Example 3 1.91 29.68 0.8 Comparative Example 1 1.88 28.21 8.2 Comparative Example 2 0.62 0.18 /
[0104] From the test data obtained from the experiment, it can be known that the stacked solar cells described in Examples 1-3 use tin dioxide as a buffer layer, and an additional self-oxidation layer is added. The self-oxidation layer can effectively eliminate the interface defects between the buffer layer and the transparent electrode layer, reduce non-radiative recombination, and thus improve the photoelectric conversion efficiency of the device. Compared with the device structure without a self-oxidation layer in Example 1 of Example 1, the photoelectric performance of the device is worse, and the photoelectric conversion efficiency is reduced from 29.68-30.62% to 28.21%, and the attenuation rate is significantly increased. Compared with Examples 1-3, Comparative Example 2 also prepared a self-oxidation layer. The difference is that the evaporation temperature in Comparative Example 2 is an ultra-high temperature evaporation of 3000°C. Too high a temperature will cause impossible damage to the device, causing the device to not work, thereby reducing the open circuit voltage and photoelectric conversion efficiency.
[0105] The above embodiments are only preferred implementation modes of the present invention. It should be pointed out that for ordinary technicians in this technical field, various changes, modifications, substitutions and deformations can be made to these embodiments without departing from the principles of the present invention. These technical solutions that are equivalent to the claims of the present invention all fall within the protection scope of the present invention, and the protection scope of the present invention is limited by the attached claims and their equivalents.
Claims
1. A method for preparing a self-oxidation layer, characterized in that: The self-oxidation layer is applied to the perovskite top cell, comprising the following steps: S1, providing a suede substrate with a buffer layer on its surface, and evaporating a self-oxidizing material on the surface of the buffer layer to form a metal film; S2, oxidizing the metal film in air to obtain a self-oxidation layer; S3, preparing a transparent electrode layer on the self-oxidation layer.
2. The method for preparing a self-oxidation layer according to claim 1, characterized in that: The self-oxidizing material is at least one of metal yttrium (Yb) and metal copper (Cu).
3. The method for preparing a self-oxidation layer according to claim 2, characterized in that: The evaporation vacuum of the evaporation is 1×10 -4 -5×10 -4 Pa, temperature is 500-800℃.
4. The method for preparing a self-oxidation layer according to claim 1, characterized in that: The evaporation rate of the evaporation is 0.05-1Å / S.
5. The method for preparing a self-oxidation layer according to claim 1, characterized in that: The thickness of the metal film is between 1-5 nm.
6. The method for preparing a self-oxidation layer according to claim 1, characterized in that: The oxidation process is to place the metal film in air for oxidation, and the oxidation time is 1-60 minutes.
7. The method for preparing a self-oxidation layer according to claim 1, characterized in that: The buffer layer is prepared from the buffer layer material by using an atomic accumulation method or an evaporation method.
8. The method for preparing a self-oxidation layer according to claim 7, characterized in that: The buffer layer material is zinc oxide (ZnO), tin dioxide (SnO2), titanium dioxide (TiO2), [6,6]-phenyl C 61 Methyl butyrate (PC 61 BM), carbon 60 (C 60 ), 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline (BCP).
9. A stacked solar cell, characterized in that: The stacked solar cell structure comprises, from bottom to top, a first metal electrode layer, a first transparent electrode layer, a P-type substrate doping layer, a substrate passivation layer, a silicon substrate, a substrate surface passivation layer, an N-type substrate doping layer, a tunneling layer, a hole transport layer, a perovskite absorption layer, a passivation layer, an electron transport layer, a buffer layer, a self-oxidation layer, a second transparent electrode layer, a second metal electrode layer, and an anti-reflection layer, wherein the self-oxidation layer is obtained by the self-oxidation layer preparation method according to any one of claims 1 to 8.
10. A method for preparing a laminated solar cell according to claim 9, characterized in that: Includes steps: Providing a silicon substrate, preparing the base passivation layer on the back side of the silicon substrate, preparing the P-type base doping layer on the surface of the base passivation layer, preparing the first transparent electrode layer on the surface of the P-type base doping layer, and preparing the first metal electrode layer on the surface of the first transparent electrode layer; And preparing the substrate surface passivation layer on the surface of the silicon substrate, preparing an N-type substrate doping layer on the surface of the substrate surface passivation layer, preparing the tunneling layer on the surface of the N-type substrate doping layer, preparing the hole transport layer on the surface of the tunneling layer, preparing the perovskite absorption layer on the surface of the hole transport layer, preparing the passivation layer on the surface of the perovskite absorption layer, preparing the electron transport layer on the surface of the passivation layer, preparing the buffer layer on the surface of the electron transport layer, preparing the self-oxidation layer on the surface of the buffer layer, preparing the second transparent electrode layer on the surface of the self-oxidation layer, preparing the second metal electrode layer on the surface of the second transparent electrode layer, and preparing an anti-reflection layer on the surface of the second metal electrode layer.
Citation Information
Patent Citations
Preparation method of polycrystalline silicon thin film based on metal inducement
CN103199151A
RGO / m-TiO2-based inorganic cesium-lead-bromine perovskite solar cell and preparation method thereof
CN117119810A
Tinned copper conductor for high-voltage cable in new energy vehicle
CN217822130U
Efficient and stable perovskite solar cells with all solution processed metal oxide transporting layers