Method for preparing back contact battery suitable for front large pyramid passivation and obtained battery
By adopting specific preparation methods in the back contact battery, the large pyramid suede is formed and the silicon oxide deposition conditions are optimized, the problem of poor passivation effect of the large pyramid suede on the front of the silicon wafer is solved, the current density and battery conversion efficiency are improved, and the current density and battery conversion efficiency are achieved. More uniform oxide layer coverage.
Patent Information
- Application Number
- CN202411140290.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-08-20
AI Technical Summary
The passivation effect of the large pyramid suede on the front of the silicon wafer in the existing back contact battery is poor, resulting in low current density and conversion efficiency, poor oxidation uniformity, thick spiral film layer and thin bottom film layer, covering Uneven.
The double-sided polished silicon wafer is used to form the first and second semiconductor layers, etch the openings, and the large pyramid suede is formed by velvet cleaning. The control tower bottom size is 5-8μm, the height is 0.5-1.5μm, and the silicon oxide is deposited and The alumina passivation layer uses argon-oxygen mixture and plasma-assisted oxidation technology to optimize the deposition conditions of silicon oxide and improve oxidation uniformity and density.
The passivation level of the suede of the Great Pyramid is significantly improved, the current density and battery conversion efficiency of the back contact battery are enhanced, the oxidation uniformity and film layer coverage are improved, and the overall passivation effect is improved.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of back contact batteries, and in particular relates to a method for preparing a back contact battery suitable for front large pyramid passivation and the obtained battery. Background Art
[0002] In the existing back-contact battery process, the front side of the silicon wafer is generally textured using a small pyramid process, and the size of the pyramid is generally 1-2μm; the use of small pyramid texture is to better match the existing passivation process. Only with good passivation can a higher opening voltage and current be obtained.
[0003] However, the reflectivity of the small pyramid velvet on the front of the silicon wafer is often higher than that of the large pyramid velvet, which means that the existing process of small pyramid velvet has sacrificed some short-circuit current. If a large pyramid velvet is used, the current will be further improved, and if the large pyramid velvet structure uses the previous passivation method, it is easy to cause poor oxidation uniformity, thicker film layer at the top of the pyramid, thinner film layer at the bottom of the pyramid, uneven coverage, and poor passivation effect.
[0004] It should be noted that this part of the present invention only provides background technology related to the present invention and does not necessarily constitute prior art or known technology. Summary of the invention
[0005] The purpose of the present invention is to overcome the defect of poor passivation effect of the large pyramid velvet surface on the front side of the silicon wafer in the back contact battery in the prior art, and to provide a back contact battery preparation method suitable for front large pyramid passivation and the resulting battery, which is beneficial to improving the passivation level of the large pyramid velvet surface, thereby further improving the current density of the back contact battery, and then improving the battery conversion efficiency.
[0006] In order to achieve the above-mentioned object, in a first aspect, the present invention provides a method for preparing a back contact cell suitable for front large pyramid passivation, comprising the following steps:
[0007] S1, provide double-sided polished silicon wafers;
[0008] S2, forming a first semiconductor layer and an isolation layer in sequence on the back side of the silicon wafer;
[0009] S3, etching an opening on the back surface obtained in S2 to form a second semiconductor opening region;
[0010] S4, removing the remaining isolation layer and the first semiconductor layer in the second semiconductor opening area by texturing and cleaning, and forming a large pyramid velvet surface on the front side of the silicon wafer and the second semiconductor opening area, and then selecting whether to perform a step of removing the isolation layer outside the second semiconductor opening area on the back side of the silicon wafer by cleaning according to needs; controlling the texturing and cleaning so that the base size of the pyramid in the large pyramid velvet surface is 5-8μm, and the height of the pyramid is 0.5-1.5μm;
[0011] S5, depositing a front passivation layer and an anti-reflection layer on the front side of the silicon wafer in sequence, wherein the front passivation layer comprises silicon oxide and aluminum oxide or amorphous silicon disposed on the outer surface of the silicon oxide, and the amorphous silicon is oxygen-doped or not oxygen-doped;
[0012] The silicon oxide deposition conditions include: in a tubular PECVD device, an argon-oxygen mixed gas is introduced, the flow rate of argon in the argon-oxygen mixed gas accounts for 95%-99.5%, and the flow rate of oxygen accounts for 0.5%-5%; and the flow rate of oxygen in the argon-oxygen mixed gas is controlled to increase with the extension of the deposition time t and meet the following conditions: when depositing 0-0.3t, the flow rate of oxygen accounts for 0.5%-1%, when depositing 0.4t-0.7t, the flow rate of oxygen accounts for 1.5%-3%, and when depositing 0.8tt, the flow rate of oxygen accounts for 4%-5%;
[0013] S6, depositing a second semiconductor layer on the back surface obtained in S5.
[0014] In some preferred embodiments of the present invention, the texturing liquid used for the texturing cleaning is a mixture of alkali, texturing additives and water, the mass percentage of alkali in the texturing liquid is 6%-15%, the mass percentage of the texturing additive is 0.1%-0.4%, and the mass percentage ratio of the alkali to the texturing additive is 1:(0.006-0.1).
[0015] In some preferred embodiments of the present invention, the value of the average size C of the pyramid base in μm and the value of the deposition time t of silicon oxide in seconds satisfy: t=1.2C 2 +1.5C+8.
[0016] In some preferred embodiments of the present invention, the conditions for the texturing and cleaning in S4 include: the texturing time is 10-60 minutes, and the texturing temperature is 75°C-85°C.
[0017] In some preferred embodiments of the present invention, the deposition conditions of silicon oxide in S5 further include:
[0018] The flow rate of argon gas is 8000-12000sccm, the pressure is 300-500Pa, and the power supply is 2-5kW;
[0019] and / or,
[0020] The deposition time t is 25-100s, and the deposition temperature is 350-450°C.
[0021] In some preferred embodiments of the present invention, the front passivation layer comprises silicon oxide and aluminum oxide disposed on an outer surface of the silicon oxide.
[0022] In some preferred embodiments of the present invention, the aluminum oxide in S5 is formed by an atomic layer deposition method, and the conditions of the atomic layer deposition method include: the process temperature is between 150-180°C, the reaction gases are trimethylaluminum and ozone, the flow rate of trimethylaluminum introduced in the first stage is 2000sccm-5000sccm, the reaction time is 20-40s, and then nitrogen is used to purge the chamber and pipelines; then the second stage is carried out, the flow rate of ozone introduced in the second stage is 3000sccm-6000sccm, the ozone introduction time is 15-30s, and then nitrogen is used to purge the chamber and pipelines; the first stage and the second stage are carried out in sequence as a cycle reaction, and a total of 30-80 cycle reactions are carried out.
[0023] In some preferred embodiments of the present invention, the thickness of silicon oxide in S5 is 1-2 nm, and the thickness of aluminum oxide is 3-4 nm.
[0024] In some preferred embodiments of the present invention, the anti-reflection layer is a combination of a silicon nitride layer and a silicon oxide layer, the thickness of the silicon nitride layer is 50-100 nm, and the thickness of the silicon oxide layer is 80-150 nm.
[0025] In some preferred embodiments of the present invention, the first semiconductor layer includes a first tunneling oxide layer and a first doped polysilicon layer, and the second semiconductor layer is a combination of an intrinsic amorphous silicon layer and a second doped silicon layer or a combination of a second tunneling oxide layer and a second doped polysilicon layer.
[0026] In some preferred embodiments of the present invention, the method for preparing a back contact cell suitable for front large pyramid passivation further comprises:
[0027] S7, etching an opening on a portion of the second semiconductor layer on the back side of the silicon wafer to form a first semiconductor opening region spaced apart from the second semiconductor opening region;
[0028] S8, depositing a conductive film layer on the back surface obtained in S7;
[0029] S9, etching an opening on a portion of the conductive film layer between the first semiconductor opening region and the second semiconductor opening region to form an insulating groove;
[0030] S10, forming metal electrodes on the outer surfaces of the corresponding conductive film layers in the areas where the first semiconductor opening region and the second semiconductor opening region are located.
[0031] In a second aspect, the present invention provides a back-contact battery, which is prepared by the method for preparing a back-contact battery suitable for front large pyramid passivation described in the first aspect.
[0032] Beneficial effects:
[0033] The present invention adopts the above-mentioned technical scheme, especially in the back contact battery, for the large pyramid velvet surface with specific size obtained by specific velvet cleaning, especially in the deposition of silicon oxide in the tubular PECVD equipment in the front passivation layer, argon oxygen mixed gas is introduced, and oxygen oxidation and plasma assisted oxidation, argon assisted oxygen dissociation (compared with pure oxygen and argon oxygen mixed gas, argon oxygen mixed gas has better oxygen dissociation effect under the action of plasma) are used. Under the joint action of plasma assistance and argon, oxygen is very easy to dissociate into oxygen ions, and the front side of the silicon wafer is oxidized and passivated. Silicon oxide can cover the bottom and the top of the tower more evenly, and the oxidation uniformity of the large pyramid velvet surface is improved. This passivation method is suitable for the passivation of the large pyramid velvet surface on the front side, which is beneficial to improving the passivation level of the large pyramid velvet surface, thereby further improving the current density of the back contact battery, and then improving the battery conversion efficiency.
[0034] In the present invention, in the deposition of silicon oxide on the front side, the argon-oxygen mixed gas with a specific oxygen ratio is controlled to be introduced, so that the oxidation rate is appropriate, and a uniform and dense silicon oxide film layer can be deposited on the large pyramid velvet surface, thereby improving the passivation effect. Under the same conditions, if the oxygen content is too high, it is easy to cause the oxidation rate to be too fast, which is easy to cause the oxide layer on the surface of the large pyramid velvet surface to have poor uniformity and reduced passivation ability; if the oxygen content is too low, the density of the formed silicon oxide film layer is poor, and the passivation performance is insufficient.
[0035] Moreover, in the front silicon oxide deposition, the present invention also controls the oxygen content in the argon-oxygen mixed gas to increase with the extension of the deposition time, which is beneficial to slowing down the oxidation rate in the initial oxidation stage, allowing oxygen ions to evenly diffuse the oxidation reaction on the surface of the velvet surface, especially the top and bottom of the large pyramid, thereby improving the oxidation uniformity; increasing the oxygen concentration with the extension of time is beneficial to improving the density of the oxidation, and improving the quality and passivation level of the overall oxide layer. DETAILED DESCRIPTION
[0036] In the present invention, unless otherwise stated, directional words such as "up, down, left, right" are generally understood in conjunction with the directions shown in actual applications.
[0037] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0038] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.
[0039] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article. Among them, the terms "optional" and "optional" all mean that they may be included or not included (or may be present or not).
[0040] In the present invention, the area close to the silicon wafer is referred to as the inside, and the area far from the silicon wafer is referred to as the outside.
[0041] In a first aspect, the present invention provides a method for preparing a back contact cell suitable for front large pyramid passivation, comprising the following steps:
[0042] S1, provide double-sided polished silicon wafers;
[0043] S2, forming a first semiconductor layer and an isolation layer in sequence on the back side of the silicon wafer;
[0044] S3, etching an opening on the back surface obtained in S2 to form a second semiconductor opening region;
[0045] S4, removing the remaining isolation layer and the first semiconductor layer in the second semiconductor opening area through texturing and cleaning, and forming a large pyramid velvet surface on the front side of the silicon wafer and the second semiconductor opening area, and then selecting whether to perform a step of removing the isolation layer outside the second semiconductor opening area on the back side of the silicon wafer through cleaning according to needs; controlling the texturing and cleaning so that the base size of the pyramid in the large pyramid velvet surface is 5-8μm (2-4 times higher than the size of the pyramid in the existing process), and the height of the pyramid is 0.5-1.5μm (1-2 times higher than the height of the pyramid in the existing process);
[0046] S5, depositing a front passivation layer and an anti-reflection layer on the front side of the silicon wafer in sequence, wherein the front passivation layer comprises silicon oxide and aluminum oxide or amorphous silicon disposed on the outer surface of the silicon oxide, and the amorphous silicon is oxygen-doped or not oxygen-doped;
[0047] S6, depositing a second semiconductor layer on the back surface obtained in S5.
[0048] The deposition conditions of silicon oxide described in S5 include: in a tubular PECVD device, an argon-oxygen mixed gas is introduced, the flow rate of argon in the argon-oxygen mixed gas accounts for 95%-99.5%, and the flow rate of oxygen accounts for 0.5%-5%; and the flow rate of oxygen in the argon-oxygen mixed gas is controlled to increase with the extension of the deposition time t and meet the following conditions: when depositing 0-0.3t, the flow rate of oxygen accounts for 0.5%-1%, preferably 0.60%-1%, when depositing 0.4t-0.7t, the flow rate of oxygen accounts for 1.5%-3%, preferably 1.9%-3%, and when depositing 0.8tt, the flow rate of oxygen accounts for 4%-5%. The use of this specific silicon oxide deposition method is conducive to improving the density and uniformity of silicon oxide on the large pyramid velvet surface, and improving the quality and passivation level of the overall silicon oxide.
[0049] In the present invention, the base size of the pyramid is 5-8μm, and the height of the pyramid is 0.5-1.5μm, which are all measured by SEM scanning electron microscope, and the sampling range is in the micron level. The corresponding base size refers to that more than 85% of the base sizes of the pyramids within the field of view of electron microscope sampling are within the range of 5-8μm. Similarly, the height of the pyramid refers to that more than 85% of the heights of the pyramids within the field of view of electron microscope sampling are within the range of 0.5-1.5μm.
[0050] The S5 front passivation layer of the present invention can be a combination of silicon oxide and aluminum oxide, or a combination of silicon oxide and oxygen-free amorphous silicon or oxygen-doped amorphous silicon. Among them, aluminum oxide or oxygen-free amorphous silicon and oxygen-doped amorphous silicon can play a field passivation role, improve the passivation effect, and at the same time play a role of high light transmittance and reduced parasitic absorption. In the preferred embodiment of the present invention, the front passivation layer is a combination of silicon oxide and aluminum oxide, and aluminum oxide is a wide bandgap material, which has a more superior transmittance performance and is more conducive to improving the battery conversion efficiency.
[0051] More preferably, the thickness of the oxygen-free amorphous silicon and the oxygen-doped amorphous silicon is independently 2-13 nm, and the oxygen concentration of the oxygen-doped amorphous silicon is 5e17 cm -3 -9e18cm -3 .
[0052] In some preferred embodiments of the present invention, the texturing liquid used for texturing cleaning is a mixture of alkali, texturing additives and water, the mass percentage of alkali in the texturing liquid is 6%-15% (0.5-3 times higher than the existing process concentration), and the mass percentage of the texturing additive is 0.1%-0.4% (1-5 times lower than the existing process concentration).
[0053] Further preferably, the mass percentage ratio of the alkali to the texturing additive is controlled to be 1:(0.006-0.1). The above-mentioned specific texturing liquid of the present invention can be used to obtain a large pyramid velvet surface, the base size of the pyramid is 5-8μm (2-4 times higher than the size of the pyramid in the existing process), and the height of the pyramid is 0.5-1.5μm (1-2 times higher than the height of the pyramid in the existing process), which can improve the reflectivity and cooperate with a specific front silicon oxide deposition method to improve the current and battery conversion efficiency.
[0054] The alkali is potassium hydroxide or sodium hydroxide.
[0055] In some preferred embodiments of the present invention, the value of the average size C of the pyramid base in μm and the value of the deposition time t of silicon oxide in seconds satisfy: t=1.2C 2 +1.5C+8. By adopting this preferred solution, the size of the pyramid and the deposition time t of silicon oxide are controlled to meet a specific proportional relationship, which is more conducive to allowing the oxide layer to fully cover the velvet surface of the pyramid and maximize the passivation effect.
[0056] In some preferred embodiments of the present invention, the conditions for the texturing and cleaning in S4 include: the texturing time is 10-60 minutes, and the texturing temperature is 75°C-85°C.
[0057] In some preferred embodiments of the present invention, the deposition conditions of silicon oxide in S5 further include: the flow rate of argon gas is 8000-12000 sccm, and / or the flow rate of oxygen gas is 40-600 sccm.
[0058] Preferably, the deposition conditions of silicon oxide in S5 also include: a pressure of 300-500 Pa and a power supply of 2-5 kW.
[0059] In some preferred embodiments of the present invention, the deposition conditions of silicon oxide in S5 also include: a deposition time t of 25-100 s, and / or a deposition temperature of 350-450° C. Adopting a suitable deposition temperature and / or deposition time to deposit silicon oxide is more conducive to improving the passivation effect and compactness of the silicon oxide film layer, and preventing subsequent film layers from being damaged by ion bombardment.
[0060] In the present invention, the front passivation layer and the anti-reflection layer are deposited first, and then the second semiconductor layer is deposited. This is because the temperature range used for the front passivation layer and the anti-reflection layer is 350-450°C, which is a high-temperature deposition process. The high-temperature deposition of the front passivation layer and the anti-reflection layer first will not affect the passivation effect of the second semiconductor layer. In particular, when an intrinsic amorphous superimposed doped silicon layer is used as the second semiconductor layer (whose optimal deposition temperature is 150-250°C), the front high-temperature film layer is deposited first, and then the back low-temperature second semiconductor layer is deposited, which can ensure that the front and back passivation effects are both better, otherwise the passivation is likely to fail.
[0061] In some preferred embodiments of the present invention, the front passivation layer comprises silicon oxide and aluminum oxide disposed on an outer surface of the silicon oxide.
[0062] Further preferably, the aluminum oxide in S5 is formed by an atomic layer deposition method, and the conditions of the atomic layer deposition method include: a process temperature between 150-180°C.
[0063] Further preferably, the conditions of the atomic layer deposition method include: the reaction gases are trimethylaluminum and ozone, the flow rate of trimethylaluminum introduced in the first stage is 2000sccm-5000sccm, the reaction time is 20-40s, and then nitrogen is used to purge the chamber and pipelines; then the second stage is carried out, the flow rate of ozone introduced in the second stage is 3000sccm-6000sccm, the ozone introduction time is 15-30s, and then nitrogen is used to purge the chamber and pipelines; the first stage and the second stage are carried out sequentially as a cycle reaction, and a total of 30-80 cycle reactions are carried out.
[0064] The above preferred aluminum oxide deposition method is used in combination with silicon oxide to improve the field passivation effect and the open circuit voltage.
[0065] In some preferred embodiments of the present invention, the thickness of silicon oxide in S5 is 1-2 nm, and the thickness of aluminum oxide is 3-4 nm. Using silicon oxide and aluminum oxide of appropriate thickness is more conducive to avoiding parasitic absorption of the film layer and improving current density.
[0066] The anti-reflection layer of the present invention can be a silicon nitride layer and / or a silicon oxide layer. In some preferred embodiments of the present invention, the anti-reflection layer is a combination of a silicon nitride layer and a silicon oxide layer, which is more conducive to reducing the reflection of sunlight, improving the light trapping effect, and increasing the current density.
[0067] More preferably, the thickness of the silicon nitride layer is 50-100 nm, and the thickness of the silicon oxide layer is 80-150 nm.
[0068] In some preferred embodiments of the present invention, the first semiconductor layer includes a first tunneling oxide layer and a first doped polysilicon layer, and the second semiconductor layer is a combination of an intrinsic amorphous silicon layer and a second doped silicon layer or a combination of a second tunneling oxide layer and a second doped polysilicon layer.
[0069] Further preferably, the second semiconductor layer is a combination of intrinsic amorphous silicon and a second doped silicon layer. In the two semiconductors of the present invention, the combined passivation structure is combined with the large pyramid velvet and the specific front silicon oxide deposition method, which is more conducive to ensuring the passivation effect while maximizing the utilization rate of solar light and improving the battery conversion efficiency; specifically, the specific front silicon oxide deposition method overcomes the difficulty of the large pyramid velvet being difficult to fully passivate, and ensures the passivation effect; and the passivated large pyramid velvet structure can greatly reduce the reflectivity of visible light, and the second semiconductor layer with a back amorphous structure can further reduce the parasitic absorption of the back long-wavelength light, thereby improving the overall optical utilization rate, and the second semiconductor layer with an amorphous structure has a better passivation effect than the tunneling polycrystalline second semiconductor layer, so the overall passivation and efficiency are higher.
[0070] The thickness and corresponding doping concentration of the first tunneling oxide layer, the second tunneling oxide layer or the intrinsic amorphous silicon, the first doped polysilicon layer and the second doped silicon layer, and the second doped polysilicon of the present invention can refer to the range of the prior art, and can be used in the present invention. Exemplarily, the thickness of the first tunneling oxide layer and the second tunneling oxide layer is 1-2nm, and the thickness of the intrinsic amorphous silicon is 4-8nm; the thickness of the second doped silicon layer is 6-12nm, and the thickness of the second doped polysilicon is 50-90nm. The effective doping concentrations of the second doped silicon layer and the second doped polysilicon are independently 2e18cm -3 -3e19cm -3 The thickness of the first doped polysilicon layer is 70-120nm, and the effective doping concentration is greater than 5e19cm -3 .
[0071] In S4, the step of removing the isolation layer is preferably performed. The type and thickness of the isolation layer of the present invention can refer to the prior art, for example, the isolation layer is at least one of silicon nitride, silicon oxide, silicon oxynitride or nitrogen-containing polysilicon, and the thickness of the isolation layer is 40-90nm.
[0072] Further preferably, the solution used to remove the isolation layer is HF acid solution, the mass percentage of HF in the HF acid solution is 0.5%-5%, and the mass percentage of deionized water is 95%-99.5%. The conditions for removing the isolation layer include: processing temperature of 20°C-30°C, and removal time of 60-300s.
[0073] In some preferred embodiments of the present invention, the method for preparing a back contact cell suitable for front large pyramid passivation further comprises:
[0074] S7, etching an opening on a portion of the second semiconductor layer on the back side of the silicon wafer to form a first semiconductor opening region spaced apart from the second semiconductor opening region;
[0075] S8, depositing a conductive film layer on the back surface obtained in S7;
[0076] S9, etching an opening on a portion of the conductive film layer between the first semiconductor opening region and the second semiconductor opening region to form an insulating groove;
[0077] S10, forming metal electrodes on the outer surfaces of the corresponding conductive film layers in the areas where the first semiconductor opening region and the second semiconductor opening region are located.
[0078] In a second aspect, the present invention provides a back-contact battery, which is prepared by the method for preparing a back-contact battery suitable for front large pyramid passivation described in the first aspect.
[0079] The embodiments of the present invention are described in detail below, which are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention.
[0080] Example 1
[0081] A method for preparing a back contact cell suitable for front large pyramid passivation comprises the following steps:
[0082] S1, double-sided polishing of silicon wafer;
[0083] S2. Forming a first semiconductor layer and an isolation layer on the back of the silicon wafer:
[0084] The first semiconductor layer includes a tunneling silicon oxide layer and an N-type doped polysilicon layer. The isolation layer is silicon nitride. The thickness of the tunneling silicon oxide layer is 1.5 nm, the thickness of the N-type doped polysilicon layer is 100 nm, and the effective doping concentration is 2e20 cm -3 , the thickness of the isolation layer is 70nm.
[0085] S3, etching an opening on the back side of the silicon wafer for the first time to form a second semiconductor opening region;
[0086] S4, texturing and cleaning the opening areas on the front and back sides of the silicon wafer;
[0087] The opening areas on the front and back of the silicon wafer are cleaned by texturing, and the texturing liquid is a mixture of sodium hydroxide, a texturing additive and water, wherein the mass percentage of sodium hydroxide is 10%, and the mass percentage of the texturing additive is 0.2%. The texturing time is 30 minutes, and the texturing temperature is 80°C. It is calculated that the mass percentage ratio of the sodium hydroxide to the texturing additive is 1:0.02. Controlling the ratio of the two is beneficial to controlling the size of the large pyramid velvet surface: measured by SEM scanning electron microscopy, the bottom size of the pyramid is 5-8μm, the height of the pyramid is 0.5-1.5μm, and the average size C of the bottom of the pyramid is 6.5μm, and the average height of the pyramid is 1μm.
[0088] During the texturing cleaning process, the silicon nitride isolation layer on the back of the silicon wafer is also removed by the final cleaning solution. The solution used to remove the mask layer is HF acid solution, with a HF mass percentage of 0.5% and a deionized water mass percentage as the remainder. The processing temperature is 25°C and the removal time is 100s.
[0089] S5, forming a front passivation layer and an anti-reflection layer on the front side of the silicon wafer;
[0090] The front passivation layer is a combination of silicon oxide and aluminum oxide, with a thickness of 1nm for silicon oxide and 3nm for aluminum oxide.
[0091] During the silicon oxide deposition, in the tubular PECVD equipment, the gas introduced is an argon-oxygen mixture, the flow rate of the introduced argon is 9000sccm; the pressure is 400Pa, the power is 3kW, the deposition time t is 68.5s, and the deposition temperature is 430°C. During the deposition process, the flow rate ratio of oxygen in the argon-oxygen mixture increases with the extension of the deposition time t, and satisfies: when depositing 0-0.3t, the flow rate ratio of oxygen is 0.85%; when depositing 0.4t-0.7t, the flow rate ratio of oxygen is 2%; when depositing 0.8tt, the flow rate ratio of oxygen is 4%.
[0092] The aluminum oxide is formed by an atomic layer deposition method, and the conditions of the atomic layer deposition method include: the process temperature is 150° C., the reaction gases are trimethylaluminum and ozone, the flow rate of trimethylaluminum introduced in the first stage is 3000sccm, the reaction time is 30s, and then the chamber and pipeline are purged with nitrogen; then the second stage is carried out, the flow rate of ozone introduced in the second stage is 5000sccm, the ozone introduction time is 20s, and then the chamber and pipeline are purged with nitrogen; the first stage and the second stage are carried out in sequence as a cycle reaction, and a total of 40 cycle reactions are carried out.
[0093] The anti-reflection layer is a combination of a silicon nitride layer and a silicon oxide layer deposited in sequence, the thickness of the silicon nitride layer is 80 nm, and the thickness of the silicon oxide layer is 100 nm;
[0094] S6, forming a second semiconductor layer on the back side of the silicon wafer;
[0095] The second semiconductor layer is an intrinsic hydrogenated amorphous silicon layer (5 nm thick) and a P-type doped amorphous silicon layer (10 nm thick, with an effective doping concentration of 2e19 cm -3 ) combination.
[0096] S7, etching an opening on the back side of the silicon wafer for the second time to form a first semiconductor opening region;
[0097] S8, depositing a transparent conductive film layer on the back side of the silicon wafer;
[0098] S9, etching an opening on the back side of the silicon wafer for the third time to form an insulating groove;
[0099] S10, forming metal electrodes on the outer surfaces of the corresponding areas of the first semiconductor opening region and the second semiconductor opening region on the back side of the silicon wafer.
[0100] Example 2
[0101] The method of Example 1 is referred to, except that the mass percentage of the texturing additive in the texturing solution used in the texturing cleaning is 0.4%, the alkali content remains unchanged, the average size C of the pyramid bottom is 5.4 μm, and the average height of the pyramid is 0.64 μm. The mass percentage ratio of the alkali to the texturing additive is calculated to be 1:0.04.
[0102] Example 3
[0103] The method of Example 1 is referred to, except that the deposition time t of silicon oxide is 35s, and the following conditions are satisfied: when depositing 0-0.3t, the flow rate of oxygen accounts for 0.85%; when depositing 0.4t-0.7t, the flow rate of oxygen accounts for 2%; when depositing 0.8tt, the flow rate of oxygen accounts for 4%.
[0104] Example 4
[0105] The method of Example 1 is referred to, except that the argon flow rate remains unchanged, and the oxygen flow rate changes to meet the following requirements: when depositing 0-0.3t, the oxygen flow rate accounts for 0.55%, when depositing 0.4t-0.7t, the oxygen flow rate accounts for 1.5%, and when depositing 0.8tt, the oxygen flow rate accounts for 4%.
[0106] Example 5
[0107] The method of Example 1 is followed, except that the second semiconductor layer is a tunneling oxide layer (1 nm thick) and a P-type doped polysilicon layer (80 nm thick, with an effective doping concentration of 2e19 cm -3 ) combination.
[0108] Example 6
[0109] The method of Example 1 is referred to, except that in the front passivation layer, oxygen-free amorphous silicon is used instead of aluminum oxide, and the thickness of the oxygen-free amorphous silicon is 3.5 nm.
[0110] Example 7
[0111] The method of Example 1 is followed, except that in the front passivation layer, oxygen-doped amorphous silicon is used instead of aluminum oxide, the thickness of the oxygen-doped amorphous silicon is 6nm, and the oxygen concentration is 3e18cm -3 .
[0112] Comparative Example 1
[0113] The method of Example 1 is referred to, except that pure oxygen is introduced instead of argon-oxygen mixed gas, argon is not introduced, and the oxygen flow rate is the same as that of Example 1.
[0114] Comparative Example 2
[0115] The method of Example 1 is referred to, except that the argon gas flow rate remains unchanged, and the flow rate of oxygen in the argon-oxygen mixture accounts for 9.5% when depositing 0.8tt.
[0116] Comparative Example 3
[0117] The method of Example 1 is referred to, except that the argon flow rate remains unchanged, the oxygen content in the argon-oxygen mixture does not change with the extension of the deposition time t, but remains unchanged, and the oxygen flow rate accounts for 5%.
[0118] Comparative Example 4
[0119] The method of Example 1 is referred to, except that the mass percentage of the texturing additive in the texturing solution used in the texturing cleaning is 0.8%, the alkali content remains unchanged, the average size of the base of the obtained pyramid is 3.9 μm, and the average height of the pyramid is 0.48 μm. The mass percentage ratio of the alkali to the texturing additive is calculated to be 1:0.08.
[0120] Test Case
[0121] The back contact cells obtained in the above embodiments and comparative examples were subjected to performance tests, and the results are shown in Table 1. Among them, the performance indicators of each embodiment and comparative example were converted using embodiment 1 as a reference benchmark, the data of embodiment 1 was normalized benchmark 1, and other examples were converted based on embodiment 1, such as the battery conversion efficiency of comparative example 1 / battery conversion efficiency of embodiment 1 was 0.957. In the normalization process, the unit of open circuit voltage is V, the unit of current density is mA / cm², and the unit of battery conversion efficiency is %.
[0122] Table 1
[0123] Performance Indicators Current density Open circuit voltage Battery conversion efficiency Example 1 1 1 1 Example 2 0.998 0.999 0.996 Example 3 0.996 0.995 0.988 Example 4 0.995 0.994 0.984 Example 5 0.993 0.986 0.980 Example 6 0.990 0.991 0.980 Example 7 0.992 0.993 0.983 Comparative Example 1 0.988 0.978 0.957 Comparative Example 2 0.991 0.984 0.972 Comparative Example 3 0.990 0.980 0.965 Comparative Example 4 0.983 0.983 0.962
[0124] It can be seen from the above results that, compared with the comparative example, the embodiment of the present invention can improve the passivation level of the large pyramid velvet surface, thereby further improving the current density of the back contact battery and further improving the battery conversion efficiency.
[0125] Furthermore, according to Example 1 and Examples 2-7, it can be seen that the preferred back-contact battery preparation method of the present invention is more conducive to improving the current density of the back-contact battery, thereby improving the battery conversion efficiency.
[0126] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for preparing a back contact cell suitable for front large pyramid passivation, characterized in that: The steps include: S1, provide double-sided polished silicon wafers; S2, forming a first semiconductor layer and an isolation layer in sequence on the back side of the silicon wafer; S3, etching an opening on the back surface obtained in S2 to form a second semiconductor opening region; S4, removing the isolation layer and the first semiconductor layer remaining in the second semiconductor opening area through texturing cleaning, and forming a large pyramid velvet surface on the front side of the silicon wafer and the second semiconductor opening area at the same time, and then selecting whether to perform a step of removing the isolation layer outside the second semiconductor opening area on the back side of the silicon wafer through cleaning according to needs; controlling the texturing cleaning so that the base size of the pyramid in the large pyramid velvet surface is 5-8μm, and the height of the pyramid is 0.5-1.5μm; the texturing cleaning adopts a texturing liquid which is a mixture of alkali, texturing additives and water, the mass percentage of alkali in the texturing liquid is 6%-15%, the mass percentage of the texturing additive is 0.1%-0.4%, and the mass percentage ratio of the alkali to the texturing additive is 1:(0.006-0.1); S5, depositing a front passivation layer and an anti-reflection layer on the front side of the silicon wafer in sequence, wherein the front passivation layer comprises silicon oxide and aluminum oxide or amorphous silicon disposed on the outer surface of the silicon oxide, and the amorphous silicon is oxygen-doped or not oxygen-doped; The silicon oxide deposition conditions include: in a tubular PECVD device, an argon-oxygen mixed gas is introduced, the flow rate of argon in the argon-oxygen mixed gas accounts for 95%-99.5%, and the flow rate of oxygen accounts for 0.5%-5%; and the flow rate of oxygen in the argon-oxygen mixed gas is controlled to increase with the extension of the deposition time t and meet the following conditions: when depositing 0-0.3t, the flow rate of oxygen accounts for 0.5%-1%, when depositing 0.4t-0.7t, the flow rate of oxygen accounts for 1.5%-3%, and when depositing 0.8tt, the flow rate of oxygen accounts for 4%-5%; S6, depositing a second semiconductor layer on the back surface obtained in S5.
2. The method for preparing a back contact cell suitable for front large pyramid passivation according to claim 1, characterized in that: The value of the average size C of the pyramid base in μm and the value of the deposition time t of silicon oxide in seconds satisfy: t=1.2C 2 +1.5C+8.
3. The method for preparing a back contact cell suitable for front large pyramid passivation according to claim 1, characterized in that: The conditions for the texturing and cleaning described in S4 include: the texturing time is 10-60 minutes, and the texturing temperature is 75°C-85°C.
4. The method for preparing a back contact cell suitable for front large pyramid passivation according to claim 1, characterized in that: The deposition conditions of silicon oxide in S5 also include: the flow rate of argon gas is 8000-12000sccm, the flow rate of oxygen gas is 40-600sccm, the pressure is 300-500Pa, and the power supply power is 2-5kW.
5. The method for preparing a back contact cell suitable for front large pyramid passivation according to claim 1, characterized in that: The deposition conditions of silicon oxide in S5 also include: deposition time t is 25-100s, and deposition temperature is 350-450°C.
6. The method for preparing a back contact cell suitable for front large pyramid passivation according to claim 1, characterized in that: The front passivation layer includes silicon oxide and aluminum oxide disposed on an outer surface of the silicon oxide.
7. The method for preparing a back contact cell suitable for front large pyramid passivation according to claim 6, characterized in that: Aluminum oxide is formed by an atomic layer deposition method, and the conditions of the atomic layer deposition method include: the process temperature is between 150-180° C., the reaction gases are trimethylaluminum and ozone, the flow rate of trimethylaluminum introduced in the first stage is 2000sccm-5000sccm, the reaction time is 20-40s, and then the chamber and pipeline are purged with nitrogen; then the second stage is carried out, the flow rate of ozone introduced in the second stage is 3000sccm-6000sccm, the ozone introduction time is 15-30s, and then the chamber and pipeline are purged with nitrogen; the first stage and the second stage are sequentially carried out as a cycle reaction, and a total of 30-80 cycle reactions are carried out; and / or, The thickness of silicon oxide in S5 is 1-2 nm, and the thickness of aluminum oxide is 3-4 nm.
8. The method for preparing a back contact cell suitable for front large pyramid passivation according to claim 1, characterized in that: The first semiconductor layer includes a first tunneling oxide layer and a first doped polysilicon layer, and the second semiconductor layer includes a combination of an intrinsic amorphous silicon layer and a second doped silicon layer or includes a combination of a second tunneling oxide layer and a second doped polysilicon layer; and / or, The anti-reflection layer is a combination of a silicon nitride layer and a silicon oxide layer. The thickness of the silicon nitride layer is 50-100 nm, and the thickness of the silicon oxide layer is 80-150 nm.
9. The method for preparing a back contact cell suitable for front large pyramid passivation according to claim 1, characterized in that: The method for preparing a back contact cell suitable for front large pyramid passivation also includes: S7, etching an opening on a portion of the second semiconductor layer on the back side of the silicon wafer to form a first semiconductor opening region spaced apart from the second semiconductor opening region; S8, depositing a conductive film layer on the back surface obtained in S7; S9, etching an opening on a portion of the conductive film layer between the first semiconductor opening region and the second semiconductor opening region to form an insulating groove; S10, forming metal electrodes on the outer surfaces of the corresponding conductive film layers in the areas where the first semiconductor opening region and the second semiconductor opening region are located.
10. A back contact battery, characterized in that: The battery is prepared by the method for preparing a back contact battery suitable for front large pyramid passivation as described in any one of claims 1 to 9.