Electrochemical preparation method of silicon-carbon composite and prepared silicon-carbon composite

The electrolytic parameters are adjusted under low temperature conditions through molten salt electrochemical method, and the electrolytic reaction between alkali metal chloride and graphite and silicon source is solved, and the high temperature problem in the preparation of SiC and SiC/C composites is achieved, low energy consumption and low cost The nanostructure preparation meets the application needs of SiC and SiC/C complexes.

CN118668218BActive Publication Date: 2024-11-15KUNMING UNIV OF SCI & TECH
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411147193.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-15
Estimated Expiration
2044-08-21

AI Technical Summary

Technical Problem

The prior art is difficult to controllable and directionally prepare SiC and SiC/C composites under low temperature conditions, and traditional production methods require high temperatures to lead to increased energy consumption and cost.

Method used

Using molten salt electrochemistry method, in molten salt, electrolyte parameters such as tank voltage and electrolysis time, alkali metal chloride is used as electrolyte, graphite and silicon sources are used to perform electrolysis under a protective atmosphere, and the decomposition of magnesium chloride is controlled to form magnesium oxide. Obstruct or allow the combination of silicon and carbon to achieve directional generation of SiC and SiC/C.

Benefits of technology

It realizes the preparation of SiC and SiC/C composites with high efficiency and low energy consumption under low temperature conditions. The product has nanostructure and excellent application prospects, with simple process, low cost, and controllable product morphology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118668218B_ABST
    Figure CN118668218B_ABST
Patent Text Reader

Abstract

The invention discloses an electrochemical preparation method of a silicon-carbon composite and the prepared silicon-carbon composite, and belongs to the technical field of non-ferrous metal metallurgy. The preparation method of the silicon-carbon composite is as follows: a silicon source and a carbon source are mixed and reacted to obtain an electrolytic precursor; the electrolytic precursor is pressed into a sheet and then calcined under a protective atmosphere to obtain an electrolytic cathode sheet; graphite is used as an anode, an electrolytic cathode sheet is used as a cathode, and an alkali metal chloride containing magnesium chloride is used as an electrolyte, and a carbon-silicon composite is obtained by electrolysis under a protective atmosphere; when the cell voltage is greater than the theoretical decomposition voltage of magnesium chloride, magnesium chloride decomposes to generate magnesium oxide, which hinders the combination of graphite and silicon to generate SiC / C; when the cell voltage is less than the theoretical decomposition voltage of magnesium chloride, carbon and silicon combine to generate SiC, and when the cell voltage is greater than the theoretical decomposition voltage of magnesium chloride, magnesium oxide generated by the decomposition of magnesium chloride cannot hinder the combination of graphite and silicon to generate SiC. The present invention uses an electrochemical method to directionally generate SiC and SiC / C in a molten salt.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of nonferrous metallurgy, and more specifically to an electrochemical preparation method of a silicon-carbon composite and the prepared silicon-carbon composite. Background Art

[0002] SiC and SiC / C are materials based on silicon carbide with excellent physical and chemical properties such as high temperature strength, corrosion resistance, high thermal conductivity, high oxidation resistance and high hardness. They are widely used in many fields. SiC is mainly used in: (i) Power electronics: SiC power devices have attracted widespread attention due to their high breakdown field strength and high thermal conductivity. They can be used in high temperature, high voltage, high frequency applications such as electric vehicles, solar inverters, high-speed trains, air conditioners, terahertz radio frequency and other fields; (ii) Optoelectronics: SiC has good optical and electrical properties, so it can be used to manufacture high-performance optoelectronic devices and materials, such as LEDs, lasers, detectors, etc. (iii) Nano field: Due to its hardness and chemical stability, SiC can be used to manufacture nano devices, nano catalysts and nano templates; (iv) Protection field: SiC can be used to manufacture protective materials and ceramic armor due to its high hardness, corrosion resistance and high temperature strength. SiC / C is mainly used in: (i) Aerospace: SiC / C materials can be used to manufacture aerospace devices, engine components, thermal protection materials, etc. due to their light weight, high strength, high rigidity and high temperature stability; (ii) Automotive industry: SiC / C materials can be used to manufacture automotive brake discs and clutches and other components, with high temperature stability and wear resistance. The different characteristics of the two materials need to be fully utilized, so the controllable and directional preparation of SiC and SiC / C composites has great development and application prospects.

[0003] At present, industrial SiC and SiC / C composites are mainly produced by carbon thermal reduction in coke, which inevitably requires extremely high temperatures, usually exceeding 1500 °C, resulting in increased energy consumption and related costs. Molten salt electrochemical method is a method for directly electrochemically reducing solid oxides in molten salts to obtain metals / alloys. Alkali metal chlorides are considered to be a potential molten salt. Its molten salt has significant ionic conductivity and a wide electrochemical window, while maintaining the initial structure of the raw materials at a relatively low temperature of no more than 1000 °C. Therefore, compared with other purification methods, the molten salt electrochemical method has the advantages of simple process, easy operation, low investment cost, no special requirements for raw materials, high purity of the obtained products, low impurity content, and easy control of product morphology. It has a unique charm in the preparation of metals and alloys by in-situ solid deoxidation of metal oxides.

[0004] Chinese patent CN110433836A discloses a molten salt electrochemical preparation method of a silicon carbide / carbon photocatalytic composite material, which adjusts the mass ratio of silicon and carbon elements in the raw material by adding a silicon source or pre-calcining biomass, and then presses the raw material into sheets to form electrodes, and then electrolyzes it in molten salt to obtain a silicon carbide / carbon composite material. However, the problem is that pre-calcining biomass pollutes the environment, is time-consuming and labor-intensive, and can only produce a single silicon carbide / carbon composite material, and cannot achieve controllable and directional preparation of SiC and SiC / C composites. Summary of the invention

[0005] In view of the above problems, the present invention provides an electrochemical preparation method of a silicon-carbon composite and the prepared silicon-carbon composite, which utilizes an electrochemical method to directionally generate SiC and SiC / C composites in a molten salt.

[0006] The present invention provides an electrochemical preparation method of a silicon-carbon composite, comprising the following steps:

[0007] A silicon source and a carbon source are mixed and reacted to obtain an electrolytic precursor;

[0008] The electrolytic precursor is pressed into a sheet and then calcined at 650-850° C. in a protective atmosphere to obtain an electrolytic cathode sheet;

[0009] Using graphite as anode, electrolytic cathode sheet as cathode, and alkali metal chloride containing magnesium chloride as electrolyte, electrolysis is performed under protective atmosphere to obtain carbon-silicon composite;

[0010] When the cell voltage is greater than the theoretical decomposition voltage of magnesium chloride, magnesium chloride decomposes to generate magnesium oxide in situ, which hinders the combination of graphite and silicon and generates SiC / C;

[0011] When the cell voltage is less than the theoretical decomposition voltage of magnesium chloride, carbon and silicon combine to form SiC, and when the cell voltage is greater than the theoretical decomposition voltage of magnesium chloride, magnesium oxide generated in situ by the decomposition of magnesium chloride cannot hinder the combination of graphite and silicon to form SiC.

[0012] In a preferred embodiment of the present invention, SiC / C is prepared when 2.7 V≤cell voltage≤2.8 V, the temperature is 600°C-1000°C, and the electrolysis time is 4-9 h.

[0013] In a preferred embodiment of the present invention, when 2.4 V ≤ cell voltage < 2.7 V, the temperature is 600 ℃-1000 ℃, the electrolysis time is 4-24 h, and 2.7 V ≤ cell voltage ≤ 2.8 V, the temperature is 600 ℃-1000 ℃, and the electrolysis time is greater than 9 h, the prepared silicon-carbon composite is SiC.

[0014] In a preferred embodiment of the present invention, the molar ratio of silicon to carbon in the electrolytic cathode sheet is 1:1-2.

[0015] In a preferred embodiment of the present invention, the alkali metal chloride includes molten salt A and / or molten salt B;

[0016] The amount of molten salt B added is 0.1-10% of the mass of molten salt A;

[0017] The molten salt A is a mixture of magnesium chloride, calcium chloride and calcium oxide; the molten salt B is one or more of lithium chloride, zinc chloride and potassium chloride.

[0018] In a preferred embodiment of the present invention, the silicon source is SiO, SiO2, MgSiO3 or Mg2SiO4.

[0019] In a preferred embodiment of the present invention, the carbon source is glucose, sucrose, citric acid, fructose or dopamine hydrochloride.

[0020] In a preferred embodiment of the present invention, the calcination time is 3-8 h.

[0021] In a preferred embodiment of the present invention, after the electrolysis is completed, the carbon-silicon composite is pickled with hydrochloric acid, the concentration of the hydrochloric acid is 0.1-4 wt %, and the pickling time is 0.1-12 h.

[0022] The second object of the present invention is to provide the carbon-silicon composite prepared as above, wherein the carbon-silicon composite is SiC or SiC / C.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] 1. The present invention prepares SiC or SiC / C in a directionally and controllably manner by adjusting the electrolysis parameters, that is, the cell voltage and the electrolysis time. When the voltage is higher than the theoretical decomposition voltage of magnesium chloride, magnesium chloride will decompose magnesium ions, which will then combine with oxygen ions released from the electrolytic cathode sheet to form magnesium oxide. Magnesium oxide is inert and insoluble in molten salt, which prevents the graphite migrated from the anode from combining with the silicon on the cathode to form SiC, thereby generating SiC / C; when magnesium oxide cannot prevent the combination of graphite and carbon, SiC is generated. When the cell voltage is lower than the theoretical decomposition voltage of magnesium chloride, carbon and silicon combine to form SiC, and the carbon at this time comes from the carbon in the cathode sheet itself and the graphite carbon migrated from the anode.

[0025] 2. The present invention uses silicon precursors that are abundant in source and low in price as raw materials, and has a short preparation process, low energy consumption, high efficiency, and controllable product morphology.

[0026] 3. The SiC and SiC / C composites prepared by the present invention are both nanostructured and have good application prospects. The different properties of the two materials need to be fully utilized, so the controllable and directional preparation of SiC and SiC / C composites has great development prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is the XRD pattern of SiC prepared in Example 1 of the present invention.

[0028] Figure 2 This is the XRD diagram of the SiC / C composite material prepared in Example 2 of the present invention.

[0029] Figure 3 These are SEM images of SiC prepared in Example 1 of the present invention, wherein Figure a is a SEM image with a scale of 10 μm, and Figure b is a SEM image with a scale of 2 μm.

[0030] Figure 4 These are SEM images of the SiC / C composite material prepared in Example 2 of the present invention, wherein Figure a is a SEM image with a scale of 20 μm, and Figure b is a SEM image with a scale of 2 μm.

[0031] Figure 5 This is a SEM image of the SiC / C composite material prepared in Example 2 of the present invention taken at another area.

[0032] Figure 6 This is a particle size distribution diagram of the SiC / C composite material prepared in Example 2 of the present invention.

[0033] Figure 7 The thermal conductivity bar graph of SiC prepared in Example 1 and SiC / C prepared in Example 2. DETAILED DESCRIPTION

[0034] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] The existing technology can only produce a single silicon carbide / carbon composite material during preparation, and cannot achieve controllable and directional preparation of SiC and SiC / C composites. Therefore, the present invention provides an electrochemical method for directional generation of SiC and SiC / C composites in molten salt to solve the above problems. The specific technical solution is as follows:

[0036] A method for electrochemically preparing a silicon-carbon composite comprises the following steps:

[0037] The silicon source and the carbon source are uniformly mixed to prepare an electrolytic precursor;

[0038] The electrolytic precursor is pressed into a sheet and then calcined at 650-850° C. in a protective atmosphere to obtain an electrolytic cathode sheet;

[0039] With graphite as anode, electrolytic cathode sheet as cathode, alkali metal chloride containing magnesium chloride as electrolyte, electrolysis is carried out under protective atmosphere to obtain carbon silicon composite.

[0040] When the cell voltage is greater than the theoretical decomposition voltage of magnesium chloride, magnesium chloride decomposes to generate magnesium oxide in situ, which hinders the combination of graphite and silicon and generates SiC / C.

[0041] When the cell voltage is less than the theoretical decomposition voltage of magnesium chloride, carbon and silicon combine to form SiC, and when the cell voltage is greater than the theoretical decomposition voltage of magnesium chloride, magnesium oxide generated in situ by the decomposition of magnesium chloride cannot hinder the combination of graphite and silicon to form SiC.

[0042] The mechanism of preparing silicon-carbon composite of the present invention is as follows:

[0043] Physical mixing mechanism: diffusion mixing.

[0044] The materials are mixed by the thermal motion between molecules, which causes the molecules to diffuse from the high concentration area to the low concentration area. During the diffusion mixing process, the molecules of the materials move randomly in space, constantly collide and exchange positions, thus gradually mixing.

[0045] During the mixing process, when the carbon source is different, the reaction mechanism is different. For example, when the carbon source is dopamine hydrochloride, the oxidative self-polymerization is coated on the surface of the silicon source.

[0046] Calcination mechanism: particle sintering.

[0047] During calcination, the bonding between particles increases, forming a larger solid structure. This is mainly achieved through atomic diffusion and surface diffusion between particles. Atomic diffusion refers to the migration of atoms within a solid, while surface diffusion refers to the migration of atoms on the surface of particles. Atomic diffusion and surface diffusion lead to close contact between particles, which promotes bonding. With increasing time and temperature, the bonding between particles becomes tighter and tighter, forming agglomerates of larger size.

[0048] Molten salt electrolysis mechanism: Using molten salt as the electrolyte, by applying a certain cell voltage, the cathode oxide is electrolytically deoxidized in a solid state to obtain the product.

[0049] In a preferred embodiment of the present invention, SiC / C is prepared when 2.7 V≤cell voltage≤2.8 V, the temperature is 600°C-1000°C, and the electrolysis time is 4-9 h.

[0050] When 2.4 V ≤ cell voltage < 2.7 V, temperature is 600 ℃-1000 ℃, electrolysis time is 4-24 h, and 2.7 V ≤ cell voltage ≤ 2.8 V, temperature is 600 ℃-1000 ℃, electrolysis time is greater than 9 h, the prepared silicon-carbon composite is SiC.

[0051] This is because 2.7 V is the theoretical decomposition voltage of magnesium chloride. When it is higher than 2.7 V, magnesium chloride will decompose, and a large number of magnesium ions will combine with oxygen ions released from the cathode to form magnesium oxide. Magnesium oxide is inert and insoluble in molten salt, which hinders the graphite migrating from the anode and combining with the silicon on the cathode to form SiC, thereby retaining the graphitized carbon at the cathode to generate SiC / C; when the time continues to extend for more than 9 h, the amount of MgO generated is not enough to hinder the driving force required to hinder the combination of silicon and carbon, so SiC is generated.

[0052] When the cell voltage is less than 2.7 V, that is, lower than the theoretical decomposition voltage of magnesium chloride, the silicon and carbon in the cathode plate itself will spontaneously combine at high temperature. The Gibbs free energy of silicon-carbon combination at high temperature is negative, and the graphitized carbon migrated from the anode also combines with the silicon at the cathode plate, thereby finally generating SiC.

[0053] When preparing SiC / C, carbon exists in two forms: amorphous carbon and graphitized carbon. As the electrolysis time increases, amorphous carbon may transform into graphitized carbon. At a certain electrolysis time, carbon may exist in both forms of amorphous carbon and graphitized carbon.

[0054] When C in SiC / C is amorphous carbon, the reason for its formation is that the in-situ generated MgO isolation zone can hinder the combination of part of Si and C on the cathode, thereby retaining part of the amorphous C.

[0055] When the C in SiC / C is graphitized carbon, the formation reason is: a disproportionation reaction occurs. By converting oxygen ions into soluble CO3 in the electrolyte 2- , which is then transferred to the cathode and reduced to graphitized carbon, thereby producing a trace amount of graphite carbon at the cathode.

[0056] It should be noted that the carbon in the cathode sheet is amorphous carbon, and there is no sharp peak in the xrd. That is, even if it is SiC / C, when C is amorphous carbon, the peak is the same as that of SiC from the xrd, but the height of the peak is different. The peak height of SiC will be higher because of its high crystallinity.

[0057] The temperature during electrolysis has little effect on the directional preparation of SiC and SiC / C. The higher the temperature, the easier it is for carbon and silicon to combine.

[0058] In a preferred embodiment of the present invention, the alkali metal chloride includes molten salt A and / or molten salt B; the added amount of molten salt B is 0.1-10% of the mass of molten salt A.

[0059] Molten salt A is a mixture of magnesium chloride, calcium chloride and calcium oxide.

[0060] The molten salt B is one or more of lithium chloride, zinc chloride and potassium chloride.

[0061] Alkaline chloride has the following advantages in molten salt electrolysis:

[0062] (1) High ionic conductivity: After alkaline chloride is melted at high temperature, its ions have a high migration rate and conductivity. This makes the current conduction efficiency high during the molten salt electrolysis process, and can achieve efficient electrolysis reaction.

[0063] (2) Wide electrolysis window: Alkaline chlorides have relatively low melting points and can remain in liquid state over a relatively wide temperature range. This means that in molten salt electrolysis, an appropriate temperature range can be selected to achieve the desired reaction conditions.

[0064] (3) Stable chemical properties: Alkaline chlorides are relatively stable at high temperatures and are not easily decomposed or oxidized. This allows them to provide a stable ion source during molten salt electrolysis without causing much contamination or loss to the electrolyte.

[0065] (4) Abundant resources and low cost: Alkaline chlorides such as sodium chloride are common natural resources and are widely found in the earth's crust. They usually have relatively low costs, so using alkaline chlorides as raw materials in the molten salt electrolysis process can reduce production costs.

[0066] (5) Versatility: Alkaline chlorides can produce a variety of useful ions and chemicals in molten salt electrolysis. For example, sodium chloride can produce chlorine, hydrogen, and sodium hydroxide, which have a wide range of applications, such as the chlor-alkali industry, metal smelting, and electrochemical synthesis.

[0067] The addition of molten salt B has the following advantages:

[0068] (1) Adjusting the melting point range: By mixing molten salts of different components, the melting point range of the mixture can be adjusted to suit different operating temperatures. This is very useful for some thermal energy systems that need to operate at different temperatures.

[0069] (2) Improving thermal conductivity: Some mixed molten salts can improve thermal conductivity to a certain extent. By selecting molten salts with different compositions, the thermal conductivity of the mixture can be increased, thereby improving the efficiency of heat energy transfer.

[0070] (3) Improved stability and corrosion resistance: Some single molten salts may have corrosion problems at high temperatures. By mixing molten salts with different components, these problems can be alleviated and the stability and corrosion resistance of the molten salt can be improved.

[0071] (4) Optimization of heat storage performance: The heat storage performance of mixed molten salt can be optimized by adjusting the composition ratio. Molten salts with different compositions have different heat capacities and heat storage performances. A reasonable mixing ratio can achieve more efficient heat energy storage and release.

[0072] In a preferred embodiment of the present invention, the silicon source is SiO, SiO2, MgSiO3 or Mg2SiO4. In the preparation process, the increase of carbon source is conducive to the formation of SiC.

[0073] In a preferred embodiment of the present invention, the carbon source is glucose, sucrose, citric acid, fructose or dopamine hydrochloride.

[0074] It should be noted that the molar ratio of silicon to carbon in the electrolytic cathode sheet is 1:1-2. The molar ratio of silicon to carbon in the electrolytic cathode sheet is 1:1, the silicon source is Mg2SiO4, and the carbon source is sucrose. Assuming that the molar number of silicon is 1 mol, it can be calculated that the molar number of Mg2SiO4 is 1 mol, that is, 140.71 g is required. At this time, the molar number of carbon is 1 mol, and the molar number of sucrose required is calculated to be 0.083 mol, that is, 28.53 g is required.

[0075] In a preferred embodiment of the present invention, the calcination time is 4-8 hours. As the calcination time and temperature increase, the particles are more and more tightly bound, so as to shape the pressed precursor sheet.

[0076] In a preferred embodiment of the present invention, after the electrolysis, the carbon-silicon composite is pickled with hydrochloric acid, the concentration of the hydrochloric acid is 0.1-4wt%, and the pickling time is 0.1-12 h.

[0077] The function of pickling is to wash away the molten salt and impurities remaining on the cathode sheet. It does not affect the preparation of the material. The higher the concentration of hydrochloric acid, the shorter the pickling time can be. Otherwise, the longer the pickling time can be.

[0078] In a preferred embodiment of the present invention, the protective atmosphere is one of helium, argon and nitrogen, and the gas flow rate is 50-200 mL·min -1 .

[0079] Example 1

[0080] An electrochemical method for directional generation of SiC and SiC / C composites in molten salt, the specific steps of which are as follows:

[0081] Step 1. Weigh 1 g of dopamine hydrochloride powder and dissolve it in 200 mL of Tris-HCl solution with a pH of 8.5. When the solution turns brown, add 1 g of silica powder and stir magnetically at 600 r / min for 2 h at room temperature of 25 °C, then centrifuge at 1500 r / min, and finally vacuum dry at 80 °C for 6 h to obtain SiO2@PDA electrolytic precursor.

[0082] Step 2: Press the SiO2@PDA electrolytic precursor obtained in step 1 into a sheet and place it in an argon-protected tube furnace with an argon flow rate of 50 mL min -1 The temperature was raised to 750 °C at a heating rate of 2 °C / min and calcined for 4 h to obtain the SiO2@C electrolytic cathode sheet.

[0083] Step 3: electrolysis is performed using graphite as an anode, SiO2@C electrolysis cathode sheet as a cathode, and alkali metal chloride molten salt as an electrolyte. The alkali metal chloride molten salt is MgCl2-CaCl2-CaO-LiCl2, wherein the molar ratio of MgCl2, CaCl2, and CaO is 1:1:1, and the amount of LiCl2 added is 2% of the total mass of MgCl2, CaCl2, and CaO.

[0084] The electrolysis conditions were: argon gas was introduced at a flow rate of 125 mL min -1 , applying a cell voltage of 2.3 V, the temperature was 850 ℃, and the time was 4 h.

[0085] Step 4: The electrolysis product obtained in step 3 is acid-washed with 1.5 wt% HCl for 5 h, filtered after acid washing, and dried at 85 °C for 12 h to obtain nanostructured SiC.

[0086] The SiO2@C electrolysis cathode sheet prepared in step 2 of the present invention is black and has a smooth surface. After the electrolysis in step 3, the color of the SiO2@C cathode sheet changes to gray-black and the surface is rough.

[0087] The electrolysis product obtained in step 3 is acid-washed, filtered and dried to obtain nano-scale SiC powder.

[0088] The XRD pattern of the nano-scale SiC powder prepared in this example is as follows: Figure 1 As shown, Figure 1 It can be confirmed that the present invention can indeed prepare SiC.

[0089] The SEM image of the nano-scale SiC powder prepared in this example is as follows Figure 3 As shown, from Figure 3 It can be seen from Figure a and Figure b that the prepared SiC has a nanostructure.

[0090] Example 2

[0091] An electrochemical method for directional generation of SiC and SiC / C composites in molten salt, the specific steps of which are as follows:

[0092] Step 1. Weigh 1 g of dopamine hydrochloride powder and dissolve it in 200 mL of Tris-HCl solution with a pH of 8.5. When the solution turns brown, add 1 g of silica powder and stir it magnetically at 600 r / min for 2 h at room temperature of 25 °C, then centrifuge it at 1500 r / min, and finally vacuum dry it at 80 °C for 6 h to obtain MgSiO3@PDA electrolytic precursor.

[0093] Step 2: Press the MgSiO3@PDA electrolytic precursor obtained in step 1 into a sheet and place it in an argon-protected tube furnace with an argon flow rate of 75 mL min -1 , and heated to 700 ℃ at a heating rate of 8 ℃ / min and calcined for 6 h to obtain the MgSiO3@C electrolytic cathode sheet.

[0094] Step 3: electrolysis is performed using graphite as an anode, a MgSiO3@C electrolytic cathode sheet as a cathode, and an alkali metal chloride molten salt as an electrolyte. The alkali metal chloride molten salt is MgCl2-CaCl2-CaO-KCl, wherein the molar ratio of MgCl2, CaCl2, and CaO is 1:1:1, and the amount of KCl added is 1% of the total mass of MgCl2, CaCl2, and CaO.

[0095] The electrolysis conditions were as follows: argon gas was introduced at a flow rate of 170 mL min -1 , a cell voltage of 2.7 V was applied, the temperature was 800 °C, and the time was 8 h.

[0096] Step 4: The electrolysis product obtained in step 3 was acid-washed with 3wt% HCl for 12 h, filtered after acid washing, and dried at 90°C for 12 h to obtain a nanostructured SiC / C composite material.

[0097] After electrolysis in step 3 of this embodiment, the MgSiO3@C electrolysis cathode sheet is black in color and has a rough surface.

[0098] The XRD pattern of the nano-scale SiC / C powder prepared in this example is as follows: Figure 2 As shown, Figure 2 It can be confirmed that the present invention can indeed prepare SiC / C composite materials.

[0099] The SEM image of the nano-scale SiC / C powder prepared in this example is as follows Figure 4 and Figure 5 As shown, from Figure 4 Figure a and Figure b and Figure 5 It can be seen that the prepared SiC / C has a nanostructure.

[0100] The SiC / C prepared in Example 2 was analyzed for particle size. Figure 6 As shown, the particle size of SiC / C prepared in Example 2 is 127.079±15.127 nm.

[0101] Example 3

[0102] An electrochemical method for directional generation of SiC and SiC / C composites in molten salt, the specific steps of which are as follows:

[0103] Step 1. Weigh 0.8 g of Mg2SiO4 powder and add it to 100 mL of sucrose solution with a concentration of 8.16 mg / ml. At room temperature, stir it magnetically at 600 r / min for 2 h to make it completely dispersed in the sucrose solution to form a colloid. After vacuum drying at 80 °C for 6 h, the Mg2SiO4@sucrose electrolytic precursor was obtained.

[0104] Step 2: Press the Mg2SiO4@sucrose electrolytic precursor obtained in step 1 into a sheet and place it in an argon-protected tube furnace with an argon flow rate of 100 mL min -1 The temperature was raised to 800 °C at a heating rate of 4 °C / min and calcined for 3 h to obtain the Mg2SiO4@C electrolytic cathode sheet.

[0105] Step 3: Use graphite as anode, Mg2SiO4@C electrolytic cathode sheet as cathode, and alkali metal chloride molten salt as electrolyte to perform electrolysis. Wherein, alkali metal chloride molten salt is used as electrolyte to perform electrolysis. Wherein, alkali metal chloride molten salt is MgCl2-CaCl2-CaO-ZnCl2, wherein the molar ratio of MgCl2, CaCl2, and CaO is 1:1:1, and the addition amount of ZnCl2 is 0.5% of the total mass of MgCl2, CaCl2, and CaO.

[0106] The electrolysis conditions were as follows: argon gas was introduced at a flow rate of 180 mL min -1 , applying a cell voltage of 2.8 V, a temperature of 850 °C, and a time of 6 h.

[0107] Step 4: The electrolysis product obtained in step 3 was acid-washed with 2.5 wt% HCl for 9 h, filtered after acid washing, and dried at 100 °C for 12 h to obtain a nanostructured SiC / C composite material.

[0108] Example 4

[0109] An electrochemical method for directional generation of SiC and SiC / C composites in molten salt, the specific steps of which are as follows:

[0110] Step 1: Weigh 1 g of SiO powder and add it to 100 mL of sucrose solution with a concentration of 6.5 mg / ml. Then, stir it magnetically at 600 r / min for 2 h at room temperature of 25 °C to completely disperse it in the sucrose solution to form a colloid. After vacuum drying at 80 °C for 6 h, SiO@sucrose electrolytic precursor was obtained.

[0111] Step 2: Press the SiO@sucrose electrolytic precursor obtained in step 1 into a sheet and place it in an argon-protected tube furnace with an argon flow rate of 150 mL min -1 The temperature was raised to 850 ℃ at a heating rate of 4 ℃ / min and calcined for 3 h to obtain the Mg2SiO4@C electrolytic cathode sheet.

[0112] Step 3: electrolysis is performed using graphite as an anode, Mg2SiO4@C electrolytic cathode sheet as a cathode, and alkali metal chloride molten salt as an electrolyte. The alkali metal chloride molten salt is MgCl2-CaCl2-CaO-ZnCl2, wherein the molar ratio of MgCl2, CaCl2, and CaO is 1:1:1, and the amount of ZnCl2 added is 0.5% of the total mass of MgCl2, CaCl2, and CaO.

[0113] The electrolysis conditions were as follows: argon gas was introduced at a flow rate of 200 mL min -1 , a cell voltage of 2.4 V was applied, the temperature was 750 °C, and the time was 6 h.

[0114] Step 4: The electrolysis product obtained in step 3 is acid-washed with 1 wt% HCl for 10 h, filtered and dried at 60°C to obtain a nanostructured SiC composite material.

[0115] Example 5

[0116] An electrochemical method for directional generation of SiC and SiC / C composites in molten salt, the specific steps of which are as follows:

[0117] Step 1. Weigh 1 g of SiO2 powder and add it to 100 mL of glucose solution with a concentration of 5.1 mg / ml. At room temperature of 25 °C, stir it magnetically at a speed of 600 r / min for 2 h to make it completely dispersed in the glucose solution. After hydrothermal reaction at 120 °C for 6 h and vacuum drying at 80 °C for 6 h, obtain the SiO2@glucose electrolytic precursor.

[0118] Step 2: Press the SiO2@glucose electrolytic precursor obtained in step 1 into a sheet and place it in an argon-protected tube furnace for calcination to obtain a SiO2@C electrolytic cathode sheet. The argon flow rate is 150 mL min -1 The calcination temperature was 700 °C, the time was 4 h, and the heating rate was 5 °C / min.

[0119] Step 3: electrolysis is performed with graphite as anode, Mg2SiO4@C electrolytic cathode sheet as cathode, and alkali metal chloride molten salt as electrolyte. The alkali metal chloride molten salt is MgCl2-CaCl2-CaO-ZnCl2-LiCl2, wherein the molar ratio of MgCl2, CaCl2, and CaO is 1:1:1, and the total addition amount of ZnCl2 and LiCl2 is 5% of the total mass of MgCl2, CaCl2, and CaO; the molar ratio of ZnCl2 and LiCl2 is 1:1.

[0120] The electrolysis conditions were as follows: argon gas was introduced at a flow rate of 150 mL min -1 , applying a cell voltage of 2.7 V, a temperature of 850 °C, and a time of 9 h.

[0121] Step 4: The electrolysis product obtained in step 3 is pickled with 3.5 wt% HCl for 7 h, filtered, and dried at 95° C. for 12 h to obtain a nanostructured SiC / C composite material.

[0122] Example 6

[0123] An electrochemical method for directional generation of SiC and SiC / C composites in molten salt, the specific steps of which are as follows:

[0124] Step 1: Weigh 1 g of SiO2 powder and mix it with 0.82 g of citric acid, and ball mill it at 400 rpm for 2 minutes to obtain a SiO2@citric acid electrolytic precursor.

[0125] Step 2: Press the SiO2@citric acid electrolytic precursor obtained in step 1 into sheets and place them in a tubular furnace protected by helium for calcination to obtain SiO2@C electrolytic cathode sheets. The flow rate of helium is 50 mL min -1 The calcination temperature is 650 ℃, the time is 8 h, and the heating rate is 5 ℃ / min.

[0126] Step 3: electrolysis is performed using graphite as an anode, a Mg2SiO4@C electrolytic cathode sheet as a cathode, and an alkali metal chloride molten salt as an electrolyte. The alkali metal chloride molten salt is MgCl2-CaCl2-CaO-KCl, wherein the molar ratio of MgCl2, CaCl2, and CaO is 1:1:1, and the amount of KCl added is 0.1% of the total mass of MgCl2, CaCl2, and CaO.

[0127] The electrolysis conditions are as follows: helium gas is introduced at a flow rate of 50 mL min -1 , a cell voltage of 2.75 V was applied, the temperature was 1000 °C, and the time was 4 h.

[0128] Step 4: The electrolysis product obtained in step 3 was acid-washed with 0.1 wt% HCl for 12 h, filtered and dried at 95 °C for 12 h to obtain a nanostructured SiC / C composite material.

[0129] Example 7

[0130] An electrochemical method for directional generation of SiC and SiC / C composites in molten salt, the specific steps of which are as follows:

[0131] Step 1: Weigh 1 g of SiO2 powder and add it to 100 mL of fructose solution with a concentration of 10.21 mg / ml. Evaporate the solvent in a tube furnace at a constant argon flow rate at 200 °C to obtain a SiO2@fructose electrolytic precursor.

[0132] Step 2: Press the SiO2@fructose electrolytic precursor obtained in step 1 into a sheet and place it in a nitrogen-protected tubular furnace for calcination to obtain a SiO2@C electrolytic cathode sheet. The nitrogen flow rate is 200 mL min -1 The calcination temperature is 850 ℃, the time is 4 h, and the heating rate is 5 ℃ / min.

[0133] Step 3: Electrolysis is performed using graphite as the anode, Mg2SiO4@C electrolytic cathode sheet as the cathode, and alkali metal chloride molten salt as the electrolyte. The alkali metal chloride molten salt is MgCl2-CaCl2-CaO-KCl-LiCl2, wherein the molar ratio of MgCl2, CaCl2, and CaO is 1:1:1, and the total addition amount of KCl and LiCl2 is 10% of the total mass of MgCl2, CaCl2, and CaO; the molar ratio of KCl and LiCl2 is 1:1.

[0134] The electrolysis conditions were as follows: nitrogen was introduced at a flow rate of 200 mL min -1 , a cell voltage of 2.6 V was applied, the temperature was 600 °C, and the time was 24 h.

[0135] Step 4: The electrolysis product obtained in step 3 was acid-washed with 4 wt% HCl for 0.1 h, filtered after acid washing, and dried at 95° C. for 12 h to obtain a nanostructured SiC composite material.

[0136] Example 8

[0137] An electrochemical method for directional generation of SiC and SiC / C composites in molten salt, the specific steps of which are as follows:

[0138] Step 1. Weigh 1 g of SiO2 powder and add it to 100 mL of glucose solution with a concentration of 5.1 mg / ml. At room temperature of 25 °C, stir it magnetically at a speed of 600 r / min for 2 h to make it completely dispersed in the glucose solution. After hydrothermal reaction at 120 °C for 6 h and vacuum drying at 80 °C for 6 h, obtain the SiO2@glucose electrolytic precursor.

[0139] Step 2: Press the SiO2@glucose electrolytic precursor obtained in step 1 into a sheet and place it in an argon-protected tube furnace for calcination to obtain a SiO2@C electrolytic cathode sheet. The argon flow rate is 150 mL min -1 The calcination temperature is 750 ℃, the time is 4 h, and the heating rate is 5 ℃ / min.

[0140] Step 3: electrolysis is performed using graphite as an anode, a Mg2SiO4@C electrolytic cathode sheet as a cathode, and an alkali metal chloride molten salt as an electrolyte. The alkali metal chloride molten salt is MgCl2-CaCl2-CaO-KCl, wherein the molar ratio of MgCl2, CaCl2, and CaO is 1:1:1, and the amount of KCl added is 8% of the total mass of MgCl2, CaCl2, and CaO.

[0141] The electrolysis conditions were as follows: argon gas was introduced at a flow rate of 150 mL min -1 , a cell voltage of 2.8 V was applied, the temperature was 800 °C, and the time was 10 h.

[0142] Step 4: The electrolysis product obtained in step 3 is acid-washed with 2 wt% HCl for 10 h, filtered after acid washing, and dried at 95°C for 12 h to obtain a nanostructured SiC composite material.

[0143] The present invention tests the thermal conductivity of SiC prepared in Example 1 and SiC / C prepared in Example 2 at room temperature of 25°C. The results are as follows: Figure 7 As shown, the thermal conductivity of SiC prepared in Example 1 is 101.27 W·m -1 ·k -1 The thermal conductivity of SiC / C prepared in Example 2 is 126.58 W·m-1 ·k -1 , indicating that both SiC and SiC / C prepared in the present invention have excellent thermal conductivity.

[0144] Although the preferred embodiments of the present invention have been described, those skilled in the art may make other changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.

[0145] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. An electrochemical preparation method of a silicon-carbon composite, characterized in that: The following steps are involved: A silicon source and a carbon source are mixed and reacted to obtain an electrolytic precursor; The electrolytic precursor is pressed into a sheet and then calcined at 650-850° C. in a protective atmosphere to obtain an electrolytic cathode sheet; the molar ratio of silicon to carbon in the electrolytic cathode sheet is 1:1-2; Using graphite as anode, electrolytic cathode sheet as cathode, and alkali metal chloride containing magnesium chloride as electrolyte, electrolysis is performed under protective atmosphere to obtain carbon-silicon composite; When the cell voltage is greater than the theoretical decomposition voltage of magnesium chloride, magnesium chloride decomposes to generate magnesium oxide in situ, which hinders the combination of graphite and silicon and generates SiC / C. When 2.7 V≤cell voltage≤2.8 V, the temperature is 600℃-1000℃, and the electrolysis time is 4-9 h, SiC / C is prepared. When the cell voltage is less than the theoretical decomposition voltage of magnesium chloride, carbon and silicon combine to form SiC, and when the cell voltage is greater than the theoretical decomposition voltage of magnesium chloride, magnesium oxide generated in situ by the decomposition of magnesium chloride cannot hinder the combination of graphite and silicon to form SiC; when 2.4 V≤cell voltage<2.7 V, the temperature is 600 ℃-1000 ℃, the electrolysis time is 4-24 h, and 2.7 V≤cell voltage≤2.8 V, the temperature is 600 ℃-1000 ℃, and the electrolysis time is greater than 9 h, the prepared silicon-carbon composite is SiC.

2. The electrochemical preparation method of a silicon-carbon composite according to claim 1, characterized in that: The alkali metal chloride includes molten salt A and / or molten salt B; The amount of molten salt B added is 0.1-10% of the mass of molten salt A; The molten salt A is a mixture of magnesium chloride, calcium chloride and calcium oxide; the molten salt B is one or more of lithium chloride, zinc chloride and potassium chloride.

3. The electrochemical preparation method of a silicon-carbon composite according to claim 1, characterized in that: The silicon source is SiO, SiO2, MgSiO3 or Mg2SiO4.

4. The electrochemical preparation method of a silicon-carbon composite according to claim 1, characterized in that: The carbon source is glucose, sucrose, citric acid, fructose or dopamine hydrochloride.

5. The electrochemical preparation method of a silicon-carbon composite according to claim 1, characterized in that: The calcination time is 3-8 h.

6. The electrochemical preparation method of a silicon-carbon composite according to claim 1, characterized in that: After the electrolysis, the carbon-silicon composite is pickled with hydrochloric acid, the concentration of the hydrochloric acid is 0.1-4 wt%, and the pickling time is 0.1-12 h.

Citation Information

Patent Citations

  • Molten salt electrochemical preparation method for silicon carbide / carbon photocatalytic composite material

    CN110433836A

  • Preparation method of nano silicon carbide

    CN103232038A

  • Method for preparing carbide derived carbon by fused salt electrolysis method

    CN103436904A

  • Electrochemical preparation method for silicon / carbon composite material by using molten salt

    CN108011084A

  • Method for preparing silicon-carbon composite negative electrode material by fused salt electrolysis method

    CN116445938A