A method for preparing a heat-insulating enamel coating resistant to gas erosion on cast iron surfaces
By using gas impact pretreatment and vacuum enameling methods, the problems of carbon reaction and insufficient adhesion of heat-insulating enamel coatings on cast iron surfaces have been solved, and the anti-peeling performance has been improved in high-temperature gas environments, making it suitable for complex structures such as diesel engine combustion chambers.
Patent Information
- Application Number
- CN202410737933.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-07
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-06-07
AI Technical Summary
Existing technologies for preparing heat-insulating enamel coatings on cast iron surfaces suffer from defects such as gas generation from the reaction of carbon with the enamel, insufficient interfacial bonding, and easy peeling of the coating under the impact of high-temperature combustion gases. They are particularly difficult to apply effectively in complex structures such as diesel engine combustion chambers.
A gas-fired impact pretreatment combined with vacuum coating method is adopted. The gas oxidizes the carbon on the surface and forms depressions. Vacuum coating slurry is then applied to eliminate pores, form a pinned and inlaid structure, improve the adhesion and prevent the coating from peeling off.
It effectively reduces porosity defects on the surface of cast iron, increases the bonding area, improves the coating's resistance to thermal shock, and ensures that the coating is not easily peeled off in a high-temperature gas environment, making it suitable for heat insulation of cast iron parts with complex structures.
Smart Images

Figure CN118704007B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of environmental barrier coating technology, specifically to a method for preparing a heat-insulating enamel coating resistant to gas erosion on cast iron surfaces. Background Technology
[0002] Vermicular graphite cast iron and alloy gray cast iron are new types of cast iron that can be used in diesel engine cylinder heads, cylinder blocks, and other fields. With the continuous improvement of internal combustion engine efficiency, the combustion chamber components have increased tolerance to combustion gas temperatures, resulting in a significant decrease in the reliability and lifespan of related cast iron parts. Improving their heat resistance has become an important issue, and heat-insulating coatings are an important means to ensure the high-temperature service capability of related components.
[0003] Currently, heat-insulating coatings are mostly prepared using methods such as thermal spraying, vapor deposition, laser cladding, and enamel firing. Diesel engine cylinder heads and exhaust manifolds have complex, small-sized, and obstructed internal structures, making thermal spraying and cladding processes impractical. Vapor deposition suffers from poor flexibility and difficulty in producing complete coatings. Enamel is a suitable heat-insulating coating for this condition. Existing technology CN92109527.9 proposes applying traditional enamel technology to the inner walls of gasoline and diesel engine cylinders to improve wear resistance.
[0004] Because cast iron has a high carbon content, the carbon reacts with the enamel during the enamel firing process, easily generating gas that is difficult to escape, leading to defects such as pinholes and bubbles at the interface. In addition, the coating is subjected to high-temperature combustion gases and high-frequency reciprocating impacts during service, and the strong thermal shock makes the coating prone to cracking and peeling. The peeling particles entering the turbocharger will cause serious damage to its blades.
[0005] The existing technology CN201480024110.X proposes a coarse glass particle toughening + fiber reinforcement enamel coating for the exhaust gas environment of internal combustion engines, but does not improve the interface between the coating and the substrate.
[0006] The prior art CN201710196863.4 proposes a method for using low-carbon castings to avoid the reaction between carbon and enamel, thereby improving the interface between the enamel coating and the substrate. This method requires controlling the carbon content in the cast iron and is not applicable to vermicular graphite cast iron and alloy gray cast iron used in diesel engine combustion chambers.
[0007] The existing technology CN202310708757.5 proposes a method to improve the adhesion of enamel coating by carbonization degreasing + shot blasting impurity removal + low temperature firing. However, the coating prepared by this method cannot meet the harsh working conditions of high frequency impact of combustion gas in diesel engine combustion chamber. Summary of the Invention
[0008] To address the shortcomings of the existing technology, the present invention aims to provide a method for preparing a gas-impact-resistant heat-insulating enamel coating on cast iron surfaces. This method utilizes a combined gas-impact pretreatment and vacuum coating control approach. The gas-impact pretreatment reduces the surface carbon content and creates depressions in the graphite phase, concentrating the heat-affected zone on the cast iron surface. The auxiliary vacuum coating treatment ensures effective slurry penetration and prevents the formation of large closed pores at the oxidized graphite phase, thereby inhibiting harmful reactions, improving adhesion, and preventing rapid peeling and failure of the coating.
[0009] To solve the above-mentioned technical problems, the present invention adopts the following technical solution:
[0010] A method for preparing a heat-insulating enamel coating resistant to gas erosion on a cast iron surface includes the following steps:
[0011] The pretreatment of cast iron surface by gas impact significantly reduces the carbon on the cast iron surface by gas oxidation, which inhibits defects such as interfacial porosity caused by subsequent reaction with glaze. At the same time, carbon oxidation roughens the surface and significantly increases the bonding area with the coating.
[0012] Preparation of enamel slurry;
[0013] The enamel slurry is coated onto the pretreated cast iron surface under vacuum conditions to obtain an enamel sample with a coating thickness of no more than 2 mm. Otherwise, it is easy to crack and fall off during subsequent drying and firing. Vacuum treatment allows the enamel slurry to be fully coated onto the surface of the cast iron substrate, effectively eliminating the closed pores between the graphite oxidation area depression and the coating. At the same time, the coating forms a nailing and inlay structure with the cast iron substrate in the graphite oxidation area depression, which greatly improves the coating's resistance to thermal shock peeling.
[0014] The enamel-coated sample was dried and fired to obtain an enamel coating.
[0015] In a preferred embodiment of the present invention, the gas used is a neutral or oxidizing gas with a gas temperature of 600–2500°C. By controlling the gas loading time per unit area and maintaining the temperature of the treated area on the material surface at 450–550°C during the impact process, the cumulative gas impact time is not greater than 10 minutes.
[0016] In a preferred embodiment of the present invention, the vacuum degree of the vacuum condition is 10. - 1 ~10 4 Pa.
[0017] In a preferred embodiment of the present invention, the prepared enamel slurry is composed of glaze, sodium silicate, potassium hydroxide, boric acid, co-solvent and deionized water. The glaze is composed of SiO2, Al2O3, B2O3, Na2O, LiO and TiO2. The particle size of the slurry is ≤10 micrometers. The co-solvent is one of anhydrous ethanol, acetone and xylene.
[0018] In a preferred embodiment of the present invention, the enamel slurry contains 5-30% SiO2, 5-30% Al2O3, 10-30% B2O3, 10-30% Na2O, 5-20% LiO, and 5-15% TiO2. Typically, the glaze accounts for 9 parts, and sodium carbonate, sodium hydroxide, boric acid, and co-solvent together account for 1 part. Deionized water is equivalent to twice the total weight mentioned above.
[0019] In a preferred embodiment of the present invention, the enamel slurry further comprises one of toughening particles, a metal powder modifier, or reinforcing fibers. The slurry matrix is a mixture composed of glaze, sodium silicate, potassium hydroxide, boric acid, and a co-solvent. When toughening particles are added, the mass fraction of the toughening particles in the slurry matrix does not exceed 20%. When a metal powder modifier is added, the mass fraction of the metal powder modifier in the slurry matrix does not exceed 30%. When reinforcing fibers are added, the mass fraction of the reinforcing fibers in the slurry matrix does not exceed 30%.
[0020] In a preferred embodiment of the present invention, the toughening particles are ZrO2 and Mo. x O y Or one of the high-entropy ceramics, wherein the metal powder modifier is one of Al, Cr, Mo, V or a high-entropy alloy, and the reinforcing fiber is one of SiC, mullite or basalt.
[0021] In a preferred embodiment of the present invention, the firing temperature is 600-900℃, the firing time is 5-30 min, the drying temperature is ≤95℃, and the drying time is 10-24 h.
[0022] In a preferred embodiment of the present invention, the coating method is dip coating, spray coating or brush coating. The prepared enamel slurry is coated onto the cast iron surface prepared in S1 by dip coating under vacuum conditions, or coated by dip coating or spray coating under normal pressure conditions and then immediately vacuum treated.
[0023] In a preferred embodiment of the present invention, the cast iron includes vermicular graphite cast iron or alloy gray cast iron used for manufacturing combustion chamber components such as diesel engine cylinder heads and cylinder blocks.
[0024] In a preferred embodiment of the present invention, before or after the gas impact, grinding, polishing and purification treatment is carried out by sand-containing gas flow, water flow or polymer fluid abrasive flow, or surface smoothing and pre-stress treatment is carried out by shot peening.
[0025] In a preferred embodiment of the present invention, the interval between coating the pretreated cast iron surface with enamel paste shall not exceed 24 hours; otherwise, it shall be placed in an inert atmosphere or at 10... -1 ~10 4 Store under vacuum conditions.
[0026] Compared with the prior art, the beneficial effects of the present invention are:
[0027] 1. This invention pretreats the surface of cast iron with gas impact, and then uses vacuum coating to prepare an enamel coating. This effectively reduces defects such as porosity caused by carbon richness on the cast iron surface, increases the bonding area between the coating and the substrate, thereby improving the bonding between the coating and vermicular graphite cast iron and enhancing the coating's resistance to thermal shock. This coating can be used for heat insulation in areas such as the exhaust port of cast iron cylinder head, and has good resistance to gas impact and anti-stripping properties.
[0028] 2. After the cast iron undergoes gas impact pretreatment, the carbon on the surface of the cast iron is significantly reduced by gas oxidation, which inhibits defects such as interfacial porosity caused by subsequent reaction with the glaze. At the same time, the oxidation of carbon roughens the surface and significantly increases the bonding area with the coating. The contact time between the cast iron surface and the gas is short, and the high temperature is mainly concentrated on the material surface. The heat impact zone is concentrated. Compared with oxidation treatment in a heat treatment furnace, the heat-affected zone is small and the impact depth is shallow. The treatment process will not affect the non-coated areas.
[0029] 3. Vacuum treatment allows the enamel slurry to be fully coated on the surface of the cast iron substrate, effectively eliminating the closed pores between the graphite oxidation zone depressions and the coating. At the same time, the coating forms a pinning and inlay structure with the cast iron substrate in the graphite oxidation zone depressions, which greatly improves the coating's resistance to thermal shock peeling. Attached Figure Description
[0030] Figure 1 This is a cross-sectional scan image of the enamel-coated cast iron obtained in Example 1 of the present invention;
[0031] Figure 2 The images show a comparison of the enamel coating obtained in Example 2 of this invention and a conventional coating without secondary impact and vacuum coating after 50 thermal shock cycles of water quenching at 550°C. Detailed Implementation
[0032] The following detailed description, in conjunction with embodiments of the present invention and accompanying drawings, provides a clear and complete illustration of the technical solutions in these embodiments. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of them. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.
[0033] It should be noted that all technical terms used in this invention are for the purpose of describing specific embodiments only and are not intended to limit the scope of protection of this invention. Unless otherwise specified, all raw materials, reagents, instruments and equipment used in the following embodiments of this invention can be purchased from the market or prepared by existing methods.
[0034] This invention addresses the issue that cast iron, due to its high carbon content, is prone to gas generation during enamel firing due to the reaction between carbon and enamel, which is difficult to escape, leading to defects such as pinholes and bubbles at the interface. Furthermore, during service, the coating is subjected to high-temperature, high-frequency reciprocating impacts from combustion gases, causing strong thermal shock that easily leads to cracking and peeling. These peeling particles entering the turbocharger can severely damage its blades. Therefore, this invention provides a method for preparing a combustion gas erosion-resistant enamel coating on cast iron surfaces. This method primarily addresses the problem of rapid peeling failure of the coating in a high-frequency combustion gas impact environment caused by harmful reactions between carbon and enamel enamel on the cast iron surface, as well as insufficient adhesion. Through a combined control method of combustion gas impact pretreatment and vacuum coating, the combustion gas impact pretreatment reduces the surface carbon content and creates depressions at the surface, concentrating the heat-affected zone on the cast iron surface. The auxiliary vacuum coating treatment ensures effective slurry penetration and avoids the formation of large closed pores at the oxidized graphite phase, thereby inhibiting harmful reactions, improving adhesion, and suppressing rapid coating peeling failure.
[0035] Example 1
[0036] A method for preparing a gas-resistant erosion-resistant enamel coating on a cast iron surface includes the following steps:
[0037] (1) Remove the grease and rust from the surface of vermicular graphite cast iron by sandblasting to make the surface clean. Then, use an oxyacetylene oxidation flame to impact the clean surface with gas. Use an infrared thermometer to monitor the temperature at the center of the gas impact area in real time. When the temperature reaches 550℃, remove the gas spray gun.
[0038] (2) 90 wt% SiO2-Al2O3-B2O3-Na2O-LiO-TiO2 glaze (containing 20 wt% SiO2, 15 wt% Al2O3, 25 wt% B2O3, 20 wt% Na2O, 10 wt% LiO, and 10 wt% TiO2) with a particle size less than 10 micrometers is mixed evenly with 1.5 wt% sodium silicate, 1.3 wt% potassium hydroxide, 0.7 wt% boric acid, 6.5 wt% anhydrous ethanol as a co-solvent, and twice the weight of deionized water by ball milling for 1 hour to obtain an enamel slurry.
[0039] (3) In a vacuum glove box under 10 kPa vacuum conditions, the enamel slurry prepared in step (2) is dipped onto the surface of the vermicular graphite cast iron prepared in step (1).
[0040] (4) The coated sample prepared in step (3) is dried in an oven at 95°C for 10 hours, then fired in a heat treatment furnace at 900°C for 5 minutes, and then taken out and air-cooled to obtain the coating.
[0041] Example 2
[0042] A method for preparing a gas-resistant erosion-resistant enamel coating on a cast iron surface includes the following steps:
[0043] (1) Remove the adhering substances on the surface of alloy gray cast iron by abrasion with sand-containing water flow to make the surface clean. No drying is required. Directly use butane flame to impact the clean surface with gas. Use an infrared thermometer to monitor the temperature of the center of the gas impact area in real time. When it reaches 550℃, remove the gas spray gun.
[0044] (2) A 90wt% SiO2-Al2O3-B2O3-Na2O-LiO-TiO2 glaze with a particle size of 2000 mesh (of which 20wt% SiO2, 15wt% Al2O3, 25wt% B2O3, 20wt% Na2O, 10wt% LiO, and 10wt% TiO2) is mixed with 1.5wt% sodium silicate, 1.3wt% potassium hydroxide, 0.7wt% boric acid, 6.5wt% anhydrous ethanol as a co-solvent, 30wt% mullite short fibers, and twice the weight of deionized water. The mixture is stirred for 2 hours to obtain an enamel slurry.
[0045] (3) Spray the enamel slurry obtained in step (2) onto the surface of the alloy gray cast iron prepared in step (1), and then immediately place the coated sample in 10 - 1 Maintain vacuum for 1 hour;
[0046] (4) The coated sample prepared in step (3) is dried in an oven at 70°C for 24 hours, then fired in a heat treatment furnace at 600°C for 30 minutes, and then taken out and air-cooled to obtain the coating.
[0047] Example 3
[0048] A method for preparing a gas-resistant erosion-resistant enamel coating on a cast iron surface includes the following steps:
[0049] (1) Remove the adhering substances on the surface of alloy gray cast iron by abrasion with sand-containing water flow to make the surface clean. No drying is required. Directly use butane flame to impact the clean surface with gas. Use an infrared thermometer to monitor the temperature of the center of the gas impact area in real time. When it reaches 500℃, remove the gas spray gun.
[0050] (2) A 90wt% SiO2-Al2O3-B2O3-Na2O-LiO-TiO2 glaze with a particle size of 2000 mesh (of which 20wt% SiO2, 15wt% Al2O3, 25wt% B2O3, 20wt% Na2O, 10wt% LiO, and 10wt% TiO2) is mixed with 1.5wt% sodium silicate, 1.3wt% potassium hydroxide, 0.7wt% boric acid, 6.5wt% anhydrous ethanol as a co-solvent, 30wt% mullite short fibers, and twice the weight of deionized water. The mixture is stirred for 2 hours to obtain an enamel slurry.
[0051] (3) Spray the enamel slurry obtained in step (2) onto the surface of the alloy gray cast iron prepared in step (1), and then immediately place the coated sample in 10 - 1 Maintain vacuum for 1 hour;
[0052] (4) The coated sample prepared in step (3) is dried in an oven at 70°C for 24 hours, then fired in a heat treatment furnace at 700°C for 25 minutes, and then taken out and air-cooled to obtain the coating.
[0053] Example 4
[0054] A method for preparing a gas-resistant erosion-resistant enamel coating on a cast iron surface includes the following steps:
[0055] (1) Remove the adhering substances on the surface of alloy gray cast iron by abrasion with sand-containing water flow to make the surface clean. No drying is required. Directly use butane flame to impact the clean surface with gas. Use an infrared thermometer to monitor the temperature of the center of the gas impact area in real time. When it reaches 450℃, remove the gas spray gun.
[0056] (2) A 90wt% SiO2-Al2O3-B2O3-Na2O-LiO-TiO2 glaze with a particle size of 2000 mesh (of which 5wt% SiO2, 30wt% Al2O3, 10wt% B2O3, 30wt% Na2O, 20wt% LiO, and 5wt% TiO2) is mixed with 1.5wt% sodium silicate, 1.3wt% potassium hydroxide, 0.7wt% boric acid, 6.5wt% acetone co-solvent, 30wt% mullite short fibers, and twice the weight of deionized water by stirring for 2 hours to obtain an enamel slurry.
[0057] (3) Spray the enamel slurry obtained in step (2) onto the surface of the alloy gray cast iron prepared in step (1), and then immediately place the coated sample in 10 4 Maintain vacuum for 1 hour;
[0058] (4) The coated sample prepared in step (3) is dried in an oven at 70°C for 24 hours, then fired in a heat treatment furnace at 800°C for 10 minutes, and then taken out and air-cooled to obtain the coating.
[0059] Example 5
[0060] A method for preparing a gas-resistant erosion-resistant enamel coating on a cast iron surface includes the following steps:
[0061] (1) Remove the grease and rust from the surface of vermicular graphite cast iron by sandblasting to make the surface clean. Then, use an oxyacetylene oxidation flame to impact the clean surface with gas. Use an infrared thermometer to monitor the temperature at the center of the gas impact area in real time. When the temperature reaches 550℃, remove the gas spray gun.
[0062] (2) A 90wt% SiO2-Al2O3-B2O3-Na2O-LiO-TiO2 glaze with a particle size of 2000 mesh (of which 30wt% SiO2, 5wt% Al2O3, 30wt% B2O3, 10wt% Na2O, 10wt% LiO, and 15wt% TiO2) is mixed with 1.5wt% sodium silicate, 1.3wt% potassium hydroxide, 0.7wt% boric acid, 6.5wt% xylene co-solvent, 20wt% ZrO2, and twice the weight of deionized water by stirring for 2 hours to obtain an enamel slurry.
[0063] (3) Spray the enamel slurry obtained in step (2) onto the surface of the alloy gray cast iron prepared in step (1), and then immediately place the coated sample in 10 - 1 Maintain vacuum for 1 hour;
[0064] (4) The coated sample prepared in step (3) is dried in an oven at 70°C for 24 hours, then fired in a heat treatment furnace at 600°C for 30 minutes, and then taken out and air-cooled to obtain the coating.
[0065] Comparative Example 1
[0066] A method for preparing an enamel coating includes the following steps:
[0067] (1) Remove grease and rust from the surface of vermicular graphite cast iron by sandblasting to make the surface clean;
[0068] (2) 90wt% of SiO2-Al2O3-B2O3-Na2O-LiO-TiO2 glaze (containing 20wt% SiO2, 15wt% Al2O3, 25wt% B2O3, 20wt% Na2O, 10wt% LiO, and 10wt% TiO2) with a particle size less than 10 micrometers is mixed evenly with 1.5wt% sodium silicate, 1.3wt% potassium hydroxide, 0.7wt% boric acid, 6.5wt% anhydrous ethanol as a co-solvent, and twice the weight of deionized water by ball milling for 1 hour to obtain an enamel slurry.
[0069] (3) Apply the enamel slurry prepared in step (2) to the surface of the vermicular graphite cast iron prepared in step (1);
[0070] (4) The enamel-coated sample prepared in step (3) is dried in an oven at 95°C for 10 hours, then fired in a heat treatment furnace at 900°C for 5 minutes, and then taken out and air-cooled to obtain an enamel coating.
[0071] The preparation methods of Examples 3-5 of this invention are the same as those of Examples 1 and 2. The only difference is that the pretreatment method of cast iron, the composition of enamel slurry, and the firing temperature and time of the enamel-coated sample are changed without affecting the experimental results. This does not affect the performance of the enamel coating. Therefore, the enamel coatings obtained in Examples 3-5 have similar performance to those obtained in Examples 1 and 2, and all have good adhesion to the cast iron substrate and resistance to thermal shock peeling.
[0072] Results Analysis
[0073] Figure 1 The cross-sectional morphology of the enamel coating obtained in Example 1 of the present invention shows that the coating and the cast iron substrate are well bonded, and the two form an embedded pinned structure. This is mainly because the carbon on the cast iron surface is greatly reduced by the oxidation of the carbon by the gas impact during the pretreatment of the cast iron surface, which suppresses defects such as interfacial porosity caused by subsequent reaction with the enamel. At the same time, the oxidation of carbon roughens the surface and significantly increases the bonding area with the coating, thereby increasing the bonding performance between the coating and the cast iron substrate.
[0074] Figure 2 The images show a comparison of the enamel coating obtained in Example 2 of this invention and the conventional coating obtained in Comparative Example 1 without gas impact + vacuum coating after 50 thermal shock cycles of water quenching at 550°C. Compared with the conventional coating without gas impact + vacuum coating, the thermal shock resistance to peeling is significantly improved. This is mainly because the vacuum treatment allows the enamel slurry to be fully coated on the surface of the cast iron substrate, effectively eliminating the closed pores between the graphite oxidation depressions and the coating. At the same time, the coating forms a pinning and inlay structure with the cast iron substrate in the graphite oxidation depressions, which greatly improves the thermal shock resistance to peeling.
[0075] In summary, this invention pretreats the cast iron surface with combustion gas impact, followed by vacuum coating to prepare an enamel coating. This effectively reduces defects such as porosity caused by carbon richness on the cast iron surface, increases the bonding area between the coating and the substrate, thereby improving the bonding between the coating and vermicular graphite cast iron and enhancing the coating's resistance to thermal shock. This coating can be used for heat insulation in areas such as the exhaust port of cast iron cylinder heads, and has good resistance to combustion gas impact and anti-stripping properties.
[0076] It should be noted that when numerical ranges are involved in this invention, it should be understood that both endpoints of each numerical range and any value between the two endpoints can be selected. Since the steps and methods used are the same as in the embodiments, preferred embodiments are described here to avoid redundancy. Although preferred embodiments of the invention have been described, those skilled in the art, once they understand the basic inventive concept, can make other changes and modifications to these embodiments. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments as well as all changes and modifications falling within the scope of this invention.
[0077] Obviously, those skilled in the art can make various modifications and variations to this invention without departing from its spirit and scope. Therefore, if these modifications and variations fall within the scope of the claims of this invention and their equivalents, this invention also intends to include these modifications and variations.
Claims
1. A method for preparing a heat-insulating enamel coating resistant to gas erosion on a cast iron surface, characterized in that, Includes the following steps: Pretreatment of cast iron surface with gas impact reduces the carbon content of cast iron surface; Prepare enamel slurry; The enamel slurry is coated onto the pretreated cast iron surface under vacuum conditions to obtain an enamel-coated sample. Vacuum treatment eliminates the closed pores between the graphite oxidation depressions and the coating, while the coating forms a pinning and inlay structure with the cast iron substrate in the graphite oxidation depressions. Finally, the enamel-coated sample is dried and fired to obtain an enamel coating. The gas used is neutral or oxidizing gas, the gas temperature is 600~2500℃, the surface temperature of the gas impact zone is 450~550℃, and the impact time is ≤10 min. The firing temperature is 600~900℃, the firing time is 5~30 min, the drying temperature is ≤95℃, and the drying time is 10~24h; The cast iron is vermicular graphite cast iron or alloy gray cast iron.
2. The method for preparing a heat-insulating enamel coating resistant to gas erosion on cast iron surface according to claim 1, characterized in that, The vacuum level of the vacuum condition is 10. -1 ~ 10 4 Pa.
3. The method for preparing a heat-insulating enamel coating resistant to gas erosion on cast iron surface according to claim 1, characterized in that, The coating thickness of the enamel slurry is no more than 2 mm.
4. The method for preparing a heat-insulating enamel coating resistant to gas erosion on cast iron surface according to claim 1, characterized in that, The coating method is dip coating, spray coating, or brush coating.
5. The method for preparing a heat-insulating enamel coating resistant to gas erosion on cast iron surface according to claim 1, characterized in that, The prepared enamel slurry is composed of glaze, sodium silicate, potassium hydroxide, boric acid, flux, and water. The glaze is composed of SiO2, Al2O3, B2O3, Na2O, LiO, and TiO2. The flux is one of anhydrous ethanol, acetone, and xylene. The mass ratio of the glaze to sodium silicate, potassium hydroxide, boric acid, and flux is 9:
1. In the glaze, the mass fractions of SiO2, Al2O3, B2O3, Na2O, LiO, and TiO2 are 5-30%, 5-30%, 10-30%, 10-30%, 5-20%, and 5-15%.
6. The method for preparing a heat-insulating enamel coating resistant to gas erosion on cast iron surface according to claim 5, characterized in that, The enamel slurry also contains one of toughening particles, metal powder modifier, or reinforcing fibers. The slurry matrix is a mixture of glaze, sodium silicate, potassium hydroxide, boric acid, and co-solvent. When toughening particles are added, the mass fraction of toughening particles in the slurry matrix does not exceed 20%. When metal powder modifier is added, the mass fraction of metal powder modifier in the slurry matrix does not exceed 30%. When reinforcing fibers are added, the mass fraction of reinforcing fibers in the slurry matrix does not exceed 30%.
7. The method for preparing a heat-insulating enamel coating resistant to gas erosion on cast iron surface according to claim 6, characterized in that, The toughening particles are ZrO2 and Mo. x O y The metal powder modifier is one of Al, Cr, Mo, V or a high-entropy alloy, and the reinforcing fiber is one of SiC, mullite or basalt.
Citation Information
Patent Citations
Cast iron enamel and preparation method thereof
CN107059007A
Wear-proof technique for gasoline or diesel engine
CN1083191A
Enamel base glaze material of cast iron enamel pot and preparation method of low-temperature enamel
CN116730616A
Method for preparing enamel coating
CN101973707A
Enamel powder, metal component having a surface portion provided with an enamel coating and method for producing such a metal component