Method for improving CO2 separation performance of mixed matrix membrane by utilizing defect type porous material

By using the etched KMnF3-EC material in the mixed matrix membrane, the problems of lack of CO2-friendly functional groups and poor interfacial compatibility in metal framework materials are solved, significantly improving the permeability and selectivity of CO2, breaking through the Robeson upper limit, Achieving more efficient CO2 separation performance.

CN118718776AInactive Publication Date: 2024-10-01DALIAN UNIV OF TECH PANJIN INST OF IND TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410917084.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing mixed-matrix membranes suffer from low permeability and insufficient selectivity in the CO2 separation process, especially the lack of CO2-philic functional groups in the metal framework materials and poor interfacial compatibility between fillers and polymers, resulting in limited separation performance.

Method used

An etching reaction is used to "punch" the KMnF3-EC metal frame material, and it is doped into the Pebax-1657 membrane matrix to form a mixed matrix membrane with a low resistance channel, taking advantage of the macroporous structure and abundant F ions of KMnF3-EC Improve membrane permeability and selectivity.

Benefits of technology

The permeability and selectivity of CO2 are significantly improved, and the CO2/N2 separation performance exceeds that of most Pebax-based mixed matrix membranes, breaking through the Robeson upper limit and achieving higher CO2 capture capacity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004935423540000141
    Figure BDA0004935423540000141
  • Figure HDA0004935423550000011
    Figure HDA0004935423550000011
  • Figure HDA0004935423550000012
    Figure HDA0004935423550000012
Patent Text Reader

Abstract

The invention discloses a method for improving CO2 separation performance of a mixed matrix membrane by using a defective porous material. The preparation method comprises the following specific steps: mixing absolute ethyl alcohol with deionized water, stirring and heating, adding modified Pebax-1657 into the mixture, and stirring to completely dissolve the modified Pebax-1657 to obtain a modified Pebax-1657 solution; adding a metal frame porous KMnF3-EC material into the prepared modified Pebax-1657 solution, and carrying out ultrasonic stirring and mixing, so as to obtain a membrane casting solution containing filler; and carrying out ultrasonic defoaming treatment on the obtained membrane casting solution, standing, then pouring the membrane casting solution onto a clean polytetrafluoroethylene flat plate, and removing the solvent in a drying oven to obtain the mixed matrix membrane. The problem that the pore diameter of a porous material is limited is solved, and high-permeability gas transmission is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of gas separation, and in particular relates to a method for improving the CO2 separation performance of a mixed matrix membrane by utilizing defective porous materials. Background Art

[0002] Over the past few decades, as the concentration of CO2 in the atmosphere continues to rise, the consequences of "global warming" and ecological destruction are threatening all living things on Earth. The greenhouse effect is mainly caused by the excessive burning of fossil energy and exhaust emissions in modern industrial society, which release a large amount of greenhouse gases into the atmosphere.

[0003] Compared with traditional CO2 separation and capture technologies such as adsorption and absorption, CO2 membrane separation technology has the advantages of small footprint, simple operation, low equipment cost, and environmental friendliness, and has received more and more attention and research. The core of CO2 membrane separation is the selection of membrane materials. With the deepening of research on membrane materials, mixed matrix membranes have unique advantages. They can combine the advantages of organic polymer membranes and inorganic membranes and make up for the shortcomings of single material membranes, becoming membrane materials with better comprehensive performance. MMMs is actually a composite membrane, which is a membrane prepared by uniformly dispersing inorganic particles in a continuous polymer matrix. In the field of gas separation membranes, mixed matrix membranes have become an alternative and more attractive method for membrane-based separation technology due to the combination of the dimensional stability and excellent separation performance of inorganic membranes and the easy preparation and low cost of polymer materials.

[0004] Generally, two types of polymers, glassy polymers and rubbery polymers, are used in the preparation of gas separation membranes. For the polymer materials in MMMs, the most important issue is to ensure the compatibility between the inorganic filler particles and the polymer. For rubbery polymers, due to their higher mobility, stronger interactions with the filler particles can be obtained, which in turn facilitates the formation of a zero-defect interface between the two components. In addition, the high fluidity of rubbery polymers gives the membranes extremely high permeability. In contrast, glassy polymers exhibit higher separation performance due to their rigid chain structure, but weaken and reduce the interaction between the filler and the polymer. Therefore, MMMs prepared using glassy polymers usually have interfacial voids, which act as transmission paths for gas molecules, thereby reducing the separation capacity of the membrane. Therefore, in this regard, a new class of polymer materials, namely block copolymers with both soft and rigid polymer segments, has been found to be applied. The classic rigid-soft structure of block copolymers is used to prepare MMMs, which can improve the interaction between the filler and the polymer and also give them better mechanical properties.

[0005] Sabetghadam et al. doped MOFs materials (NH2-MIL-53(Al), MIL-69(Al), MIL-96(Al) and ZIF-94) with different topological structures, chemical functions and pore sizes into Pebax-1657 matrix. The experiment found that the mixed matrix membrane synthesized with MIL-96(Al) as filler had the best gas separation performance, and compared with the pure Pebax membrane, the CO2 permeability and selectivity were increased by 25% and 18%, respectively.

[0006] Zheng et al. developed a three-dimensional hollow CoNi-LDH nanocage by in-situ etching of the ZIF-67 template, and constructed a low-resistance and CO2-philic transport channel in MMMs. The resulting material exhibits a hollow structure with a cavity size of about 500nm, and the LDH stacking and ZIF-67 template form a mesoporous and microporous structure. The outer layer of layered CoNi-LDH nanosheets can attract more CO2 molecules through their abundant hydroxyl groups, thereby improving the dissolution selectivity of CO2 to N2. At the same time, the tortuous gas diffusion path formed by the stacking of two-dimensional nanosheets further improves the selectivity of CO2 to N2. In addition, the hollow nanocage provides a fast transport path for CO2 molecules, thereby improving the permeability of CO2. The results show that compared with pure Pebax membrane and 2D LDH / Pebax MMM, 3D hollow CoNi-LDH-2h / Pebax MMM has the highest CO2 permeability, reaching 135.49 Barrer, which is 141.95% and 71.50% higher than the first two membranes, respectively. The present membranes have a good CO2 capture capacity compared to most reported Pebax-based MMMs and exceed the Robeson upper limit.

[0007] As one of the main greenhouse gases, large amounts of CO2 emissions will have a significant impact on global climate change. In view of the above situation, active measures need to be taken to reduce greenhouse gas emissions. Researchers have proposed the concept of CO2 capture, utilization and storage (CCS). Carbon capture and storage technology includes capturing, purifying, compressing, transporting and storing CO2, and is considered to be a feasible strategy to reduce CO2 emissions from various sources. Therefore, the development of efficient CO2 capture technology has become one of the key issues at present.

[0008] This patent selects Pebax-1657 as the membrane matrix. Pebax-1657 is copolymerized by 40wt% PA and 60wt% PE. This model is selected because the membrane needs to have a certain mechanical strength and good adsorption performance for CO2. Compared with other models, the mechanical strength and adsorption performance are more balanced. If a model with a higher PE content is selected, the membrane surface will be very prone to agglomeration. If a model with a higher PA content is selected, the membrane will have weaker adsorption performance for CO2. At the same time, if some metal organic skeletons with special carbon dioxide adsorption functions are introduced into polyether block amides to prepare mixed matrix membranes, the separation performance of the membrane material can be further improved, thereby solving the problem of low permeability of organic polymer gas separation membranes. Summary of the invention

[0009] In view of the contents described in the above background technology, the present invention proposes a method for improving the performance of mixed matrix membrane for separating CO2 by using defective porous materials. The KMnF3-EC metal frame material is "punched" by etching reaction, and finally it is doped into Pebax to prepare a mixed matrix membrane with low resistance channels. Its macroporous structure and the Lewis acid-base reaction of the rich F ions with CO2 improve the permeability of the prepared membrane while ensuring its selectivity.

[0010] The technical solution of the present invention:

[0011] A method for improving the performance of mixed matrix membrane for separating CO2 by using defective porous materials, characterized in that it comprises the following steps:

[0012] (1) After mixing anhydrous ethanol and deionized water, heat them to 80-90° C. in an oil bath under stirring conditions, and then add modified Pebax-1657 thereto, keep stirring at 80-90° C. for 4-6 hours to completely dissolve them, thereby obtaining a modified Pebax-1657 solution;

[0013] (2) adding the metal frame porous KMnF3-EC material to 15 to 20 parts of the modified Pebax-1657 solution prepared in step (1), stirring and mixing by ultrasonic stirring, to obtain a casting solution containing fillers;

[0014] (3) The casting solution obtained in step (2) is subjected to ultrasonic degassing for 10 to 30 minutes and allowed to stand for 4 to 10 minutes. The solution is then poured onto a clean polytetrafluoroethylene plate and placed in a constant temperature oven at 50 to 70° C. for 10 to 15 hours. The solution is then placed in a vacuum oven and dried under vacuum for 18 to 24 hours to obtain a mixed matrix membrane.

[0015] Based on the above technical solution, preferably, the preparation method of the KMnF3-EC material is:

[0016] Weigh 0.3-0.6 parts of MnCl2·4H2O, 2-6 parts of hexadecyltrimethylammonium bromide, 2-6 parts of 1-butanol, 12-18 parts of octane and 0.5-2.5 parts of deionized water by mass and add them into a reaction beaker, then stir under strong magnetic stirring at room temperature for 30-60 minutes to form a MnCl2·4H2O aqueous solution microemulsion;

[0017] At the same time, 0.3-0.6 parts of KF·2H2O, 2-6 parts of hexadecyltrimethylammonium bromide, 2-6 parts of 1-butanol, 12-18 parts of octane and 0.5-2.5 parts of deionized water were weighed and added into a reaction beaker, and then stirred with a strong magnetic stirrer at room temperature for 30-60 minutes to prepare a potassium fluoride aqueous solution microemulsion;

[0018] The KF·2H2O micellar solution was slowly added dropwise to the MnCl2·4H2O solution, and the solution was reacted for 5-10 minutes, and then an excess of CHCl3 / CH3OH was added, and the mixed solution destroyed the synthesis reaction and terminated the reaction;

[0019] The precipitate is collected by centrifugation and washed with methanol and deionized water for 3-6 times. Finally, the precipitate is dried in a drying oven at 60-80°C for 12-24 hours to obtain the required KMnF3 nanoparticles. 10-30 parts of KMnF3 nanoparticles are weighed and dissolved in 5-15 parts of methanol solution. At the same time, 2.5-7.5 parts of ammonia solution are measured and added to 10-30 parts of anhydrous ethanol solution. Then, the prepared ammonia solution is slowly added to the methanol solution containing KMnF3, stirred at room temperature for 1-3 hours, washed with ethanol for 3-6 times at the end of the reaction, and the obtained black precipitate is placed in a 60-80°C oven and dried for 12-24 hours to obtain porous KMnF3-EC nanoparticles.

[0020] Based on the above technical solution, preferably, the solvent is 1-2 of methanol, deionized water, ethanol, N,N-dimethylformamide, and N,N-diethylformamide.

[0021] Based on the above technical solution, preferably, the volume ratio of CHCl3 / CH3OH is 1:1-3.

[0022] Based on the above technical solution, preferably, the rotation speed of the centrifuge is 7000-10000, and the centrifugation time is 5-10 min.

[0023] Based on the above technical solution, preferably, the mass ratio of ethanol to water is 6-9:1-4.

[0024] Based on the above technical solution, preferably, the solid content of the modified Pebax-1657 solution is 1-5%, and the method for modifying Pebax-1657 is:

[0025] Pebax-1657: 100-120 parts, placed in plasma equipment;

[0026] Plasma gas: ammonia: hexafluorobutyl acrylate vapor: 2-mercaptothiazoline vapor, volume ratio = 1-1.2: 0.05-0.1: 0.05-0.08; mixed gas flow rate = 10-20 ml / min, temperature: 80-90°C;

[0027] Plasma treatment time: 10-20 minutes, take out and dry at 80-100℃ for 20-30 hours;

[0028] Plasma equipment parameters:

[0029] Frequency: 13.56MHz,

[0030] Power: 200 -300W.

[0031] Based on the above technical solution, preferably, the mass fraction of pure porous KMnF3-EC nanoparticles in the casting solution is 0.5-2wt%.

[0032] Based on the above technical solution, preferably, the ultrasonic stirring mixing method is: ultrasonic dispersion for 15 to 45 minutes, followed by stirring at a speed of 500 to 1000 rpm for 30 to 60 minutes at room temperature.

[0033] Based on the above technical solution, the mixed matrix membrane prepared by the present invention is used for CO2 / N2 gas separation.

[0034] Basic principles of the present invention:

[0035] The present invention improves the existing mixed matrix membrane based on the properties of carbon dioxide. The polyether copolyamide (Pebax-1657) is composed of polyethylene oxide (PEO) and polyamide (PA) in a mass ratio of 40 / 60. The presence of PEO in the polymer ensures a high affinity for CO2 relative to non-polar gases (such as CH4 and N2), providing good CO2 gas permeability. Glassy PA has good mechanical strength. Therefore, Pebax-1657 is an ideal polymer for separating CO2 and has good application prospects. KMnF3 nanoparticles have a hollow nanocube skeleton with a nanoshell, with high capacity and high specific surface area. The three-dimensional-metal framework KMnF3 material is "punched" by etching reaction to successfully synthesize a "large-aperture" three-dimensional-metal framework KMnF3-EC and prepare a mixed matrix membrane, thereby improving the CO2 separation performance of Pebax. The etching reaction enriches KMnF3-EC with a large number of hydroxyls, which, combined with the rich F ions contained in itself, improves the CO2 / N2 selectivity. The "macroporous structure" of KMnF3-EC provides a path for rapid gas transmission, thereby improving gas permeability. The present invention solves the problem that the pore size of porous materials is limited, it is difficult to achieve high permeability transmission of gas, resulting in relatively poor permeability, and the lack of CO2-philic functional groups in metal frame materials, the interface compatibility between fillers and polymers is relatively poor, and selective screening cannot be guaranteed.

[0036] The beneficial effects achieved by the present invention using the above technical solution are as follows:

[0037] Under plasma conditions, ammonia, hexafluorobutyl acrylate vapor and 2-mercaptothiazoline vapor are excited by high energy states to generate free radicals. These free radicals attack the surface of Pebax-1657, capture hydrogen atoms to form new polymer free radicals. The free radicals on Pebax-1657 react with the surrounding unsaturated hexafluorobutyl acrylate and 2-mercaptothiazoline to form a graft copolymer. When the free radicals on the two polymer chains meet, they can terminate the reaction by combining with each other to form a stable graft copolymer.

[0038] After the membrane surface is modified, the polarity of the material increases due to the introduction of thiazoline rings and fluorine atoms, which makes CO2 (a quadrupole molecule) more easily dissolved in the membrane, thereby improving the permeability of CO2. The introduction of fluorine atoms may increase the free volume between polymer chains, providing more space for CO2 molecules to diffuse, thereby increasing the permeation rate. Due to its higher affinity for CO2, the solubility and diffusion rate of CO2 are greatly improved compared to other gases such as N2 or CH4, thereby improving the separation selectivity of CO2 from other gases.

[0039] The present invention improves the existing mixed matrix membrane based on the properties of carbon dioxide. The polyether block amide (Pebax) is copolymerized by a rigid segment polyamide (PA) providing mechanical strength and a flexible segment polyether (PE) providing free volume. The flexible segment PE has extremely excellent preferential adsorption for polar gas CO2, so Pebax has extremely excellent performance in separating polar and non-polar mixed gases. KMnF3 nanoparticles have a hollow nanocube skeleton with a nanoshell, and have high capacity and high specific surface area. The three-dimensional metal framework KMnF3 material is "punched" by etching reaction to successfully synthesize a "large-aperture" three-dimensional metal framework KMnF3-EC and prepare a mixed matrix membrane, thereby improving the CO2 separation performance of Pebax. The etching reaction enriches KMnF3-EC with a large number of hydroxyls, and combined with the rich F ions contained in itself, improves the CO2 / N2 selectivity. The "macroporous structure" of KMnF3-EC provides a path for rapid gas transmission, thereby improving the permeability of the gas. The present invention solves the problem that the porous material has limited pore size, it is difficult to achieve high permeability transmission of gas, resulting in relatively poor permeability, and the lack of CO2-philic functional groups in the metal frame material, the relatively poor interface compatibility between the filler and the polymer, and the inability to ensure selective screening. The use of deionized water as a solvent in the method for preparing the filler is in line with the current concept of environmental protection development. The entire preparation is mild and simple, and the cost is relatively low, providing method support for large-scale separation of CO2 by mixed matrix membranes in future green development.

[0040] As the feed pressure increases, the permeability and selectivity of CO2 gas are on an upward trend. CO2 itself is a condensable gas, which can be adsorbed more in the Pebax matrix as the pressure increases. At the same time, the Pebax-1657 polymer with polar PEO segments has a higher affinity for CO2 with permanent quadrupole moment. N2 is a non-condensable gas, which is basically unaffected by the feed pressure. Therefore, the permeability and selectivity are increased.

[0041] The mixed matrix membrane has a CO2 permeability of 70.33 to 153.69 Barrer, and a CO2 / N2 selectivity of 49.77 to 77.14. Under the same conditions, Pebax / KMnF3-EC MMM-1.5wt.% exhibits the best CO2 / N2 separation performance, with a CO2 permeability of 153.69 Barrer and a selectivity of 77.14, which exceeds most Pebax-based mixed matrix membranes and breaks through the Robeson upper limit in 2008. Compared with pure Pebax-1657 membrane, both CO2 permeability coefficient and CO2 / N2 selectivity are improved, indicating that designing "macroporous defective" materials rich in CO2 gas-philic groups as fillers for MMMs has great research significance in improving CO2 gas separation. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 This is the X-ray diffraction pattern of the synthesized material.

[0043] Figure 2 The Fourier transform infrared spectra of the mixed matrix membranes obtained in Examples 1 to 4 are shown in Figure 1. From top to bottom, they correspond to the mixed matrix membranes of Example 4, Example 3, Example 2, and Example 1, respectively.

[0044] Figure 3 Graph showing the gas separation performance of the mixed matrix membrane obtained in Examples 1-4. DETAILED DESCRIPTION

[0045] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme of the present invention will be clearly and completely described below in conjunction with the embodiments. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially.

[0046] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0047] Example 1

[0048] A method for improving the performance of mixed matrix membrane for separating CO2 by using defective porous materials, characterized in that it comprises the following steps:

[0049] (1) After mixing anhydrous ethanol and deionized water, heat them to 80° C. in an oil bath under stirring conditions, and then add modified Pebax-1657 thereto and keep stirring at 80° C. for 4 hours to completely dissolve them, thereby obtaining a modified Pebax-1657 solution;

[0050] (2) adding the metal frame porous KMnF3-EC material to 15 g of the modified Pebax-1657 solution prepared in step (1), and mixing by ultrasonic stirring to obtain a casting solution containing fillers;

[0051] (3) The casting solution obtained in step (2) was subjected to ultrasonic degassing for 10 minutes and allowed to stand for 4 minutes. It was then poured onto a clean polytetrafluoroethylene plate and placed in a 55° C. constant temperature oven for 10 hours. It was then placed in a vacuum oven and dried under vacuum for 18 hours to obtain a mixed matrix membrane.

[0052] Preparation method of the KMnF3-EC material:

[0053] 0.3 g MnCl2·4H2O, 2 g hexadecyltrimethylammonium bromide, 2 g 1-butanol, 12 g octane and 0.5 g deionized water were weighed and added into a reaction beaker, and then stirred under strong magnetic stirring at room temperature for 30 min to form a MnCl2·4H2O aqueous solution microemulsion;

[0054] At the same time, 0.3 g KF·2H2O, 2 g hexadecyltrimethylammonium bromide, 2 g 1-butanol, 12 g octane and 0.5 g deionized water were weighed and added into the reaction beaker, and then stirred under strong magnetic stirring at room temperature for 30 min to prepare a potassium fluoride aqueous solution microemulsion;

[0055] The KF·2H2O micellar solution was slowly added dropwise to the MnCl2·4H2O solution, and the solution was reacted for 5 min. Then, an excess of CHCl3 / CH3OH was added, and the mixed solution destroyed the synthesis reaction and terminated the reaction.

[0056] The precipitate was collected by centrifugation and washed three times with methanol and deionized water. Finally, the precipitate was dried in a drying oven at 60°C for 12 h to obtain the required KMnF3 nanoparticles. 10 g of KMnF3 nanoparticles were weighed and dissolved in 5 g of methanol solution. At the same time, 2.5 g of ammonia solution was measured and added to 10 g of anhydrous ethanol solution. Then, the prepared ammonia solution was slowly added to the methanol solution containing KMnF3 and stirred at room temperature for 1 h. At the end of the reaction, it was washed three times with ethanol and the obtained black precipitate was placed in a 60°C oven and dried for 12 h to obtain porous KMnF3-EC nanoparticles.

[0057] The solvent is one or two of methanol, deionized water, ethanol, N,N-dimethylformamide and N,N-diethylformamide.

[0058] The volume ratio of CHCl3 / CH3OH is 1:1.

[0059] The rotation speed of the centrifuge is 7000, and the centrifugation time is 5 minutes.

[0060] The mass ratio of the ethanol to water is 6:1.

[0061] The modified Pebax-1657 solution has a solid content of 1%. The method for modifying Pebax-1657 is as follows:

[0062] Pebax-1657: 100 g, placed in plasma equipment;

[0063] Plasma gas: ammonia: hexafluorobutyl acrylate vapor: 2-mercaptothiazoline vapor, volume ratio = 1:0.05:0.05; mixed gas flow rate = 10ml / min, temperature: 80°C;

[0064] Plasma treatment time: 10 minutes, take out, and dry at 80°C for 20 hours;

[0065] Plasma equipment parameters:

[0066] Frequency: 13.56MHz,

[0067] Power: 200W.

[0068] The mass fraction of pure porous KMnF3-EC nanoparticles in the casting solution is 0.5wt%.

[0069] The ultrasonic stirring and mixing method includes: ultrasonic dispersion for 15 minutes, and then stirring at 500 rpm for 30 minutes at room temperature.

[0070] Example 2

[0071] A method for improving the performance of mixed matrix membrane for separating CO2 by using defective porous materials, characterized in that it comprises the following steps:

[0072] (1) After mixing anhydrous ethanol and deionized water, heat them to 85° C. in an oil bath under stirring conditions, and then add modified Pebax-1657 thereto and keep stirring at 85° C. for 5 hours to completely dissolve them, thereby obtaining a modified Pebax-1657 solution;

[0073] (2) adding the metal frame porous KMnF3-EC material to 16 g of the Pebax-1657 solution prepared in step (1), and mixing by ultrasonic stirring to obtain a casting solution containing fillers;

[0074] (3) The casting solution obtained in step (2) was subjected to ultrasonic degassing for 15 minutes and allowed to stand for 6 minutes. It was then poured onto a clean polytetrafluoroethylene plate and placed in a 55° C. constant temperature oven for 12 hours. It was then placed in a vacuum oven and evacuated for 20 hours to obtain a mixed matrix membrane.

[0075] Preparation method of the KMnF3-EC material:

[0076] 0.5 g MnCl2·4H2O, 3 g hexadecyltrimethylammonium bromide, 3 g 1-butanol, 14 g octane and 1 g deionized water were weighed and added into a reaction beaker, and then stirred under strong magnetic stirring at room temperature for 40 min to form a MnCl2·4H2O aqueous solution microemulsion;

[0077] At the same time, 0.4 g KF·2H2O, 3 g hexadecyltrimethylammonium bromide, 3 g 1-butanol, 14 g octane and 1 g deionized water were weighed and added into the reaction beaker, and then stirred under strong magnetic stirring at room temperature for 40 min to prepare a potassium fluoride aqueous solution microemulsion;

[0078] The KF·2H2O micellar solution was slowly added dropwise to the MnCl2·4H2O solution, and the solution was reacted for 6.5 min. Then, an excess of CHCl3 / CH3OH was added, and the mixed solution destroyed the synthesis reaction and terminated the reaction.

[0079] The precipitate was collected by centrifugation and washed four times with methanol and deionized water. Finally, the precipitate was dried in a drying oven at 70°C for 16 hours to obtain the required KMnF3 nanoparticles. 20g of KMnF3 nanoparticles were weighed and dissolved in 10g of methanol solution. At the same time, 5g of ammonia solution was measured and added to 20g of anhydrous ethanol solution. Then, the prepared ammonia solution was slowly added to the methanol solution containing KMnF3 and stirred at room temperature for 2h. At the end of the reaction, it was washed four times with ethanol and the obtained black precipitate was dried in a 70°C oven for 16h to obtain porous KMnF3-EC nanoparticles.

[0080] The solvent is one or two of methanol, deionized water, ethanol, N,N-dimethylformamide and N,N-diethylformamide.

[0081] The volume ratio of CHCl3 / CH3OH is 1:2.

[0082] The rotation speed of the centrifuge is 8000 and the centrifugation time is 6 minutes.

[0083] The mass ratio of the ethanol to water is 7:2.

[0084] The modified Pebax-1657 solution has a solid content of 2.5%. The method for modifying Pebax-1657 is as follows:

[0085] Pebax-1657: 110 g, placed in plasma equipment;

[0086] Plasma gas: ammonia: hexafluorobutyl acrylate vapor: 2-mercaptothiazoline vapor, volume ratio = 1.1:0.06:0.06; mixed gas flow rate = 15 ml / min, temperature: 85°C;

[0087] Plasma treatment time: 15 minutes, take out, and dry at 90°C for 25 hours;

[0088] Plasma equipment parameters:

[0089] Frequency: 13.56MHz,

[0090] Power: 250W.

[0091] The mass fraction of pure porous KMnF3-EC nanoparticles in the casting solution is 1 wt%.

[0092] The ultrasonic stirring and mixing method includes: ultrasonic dispersion for 25 minutes, and then stirring at 650 rpm for 40 minutes at room temperature.

[0093] Example 3

[0094] A method for improving the performance of mixed matrix membrane for separating CO2 by using defective porous materials, characterized in that it comprises the following steps:

[0095] (1) After mixing anhydrous ethanol and deionized water, heat them to 85° C. in an oil bath under stirring conditions, and then add modified Pebax-1657 thereto and keep stirring at 85° C. for 5 hours to completely dissolve them, thereby obtaining a modified Pebax-1657 solution;

[0096] (2) adding the metal frame porous KMnF3-EC material to 18 g of the Pebax-1657 solution prepared in step (1), and mixing by ultrasonic stirring to obtain a casting solution containing fillers;

[0097] (3) The casting solution obtained in step (2) was subjected to ultrasonic degassing for 20 minutes and allowed to stand for 8 minutes. It was then poured onto a clean polytetrafluoroethylene plate and placed in a 60° C. constant temperature oven for 13.5 hours. It was then placed in a vacuum oven and dried under vacuum for 20 hours to obtain a mixed matrix membrane.

[0098] Preparation method of the KMnF3-EC material:

[0099] 0.5 g MnCl2·4H2O, 5 g hexadecyltrimethylammonium bromide, 4 g 1-butanol, 16 g octane and 2 g deionized water were weighed and added into a reaction beaker, and then stirred under strong magnetic stirring at room temperature for 50 min to form a MnCl2·4H2O aqueous solution microemulsion;

[0100] At the same time, 0.5 g KF·2H2O, 5 g hexadecyltrimethylammonium bromide, 5 g 1-butanol, 16 g octane and 2 g deionized water were weighed and added into the reaction beaker, and then stirred under strong magnetic stirring at room temperature for 50 min to prepare a potassium fluoride aqueous solution microemulsion;

[0101] The KF·2H2O micellar solution was slowly added dropwise to the MnCl2·4H2O solution, and the solution was reacted for 8.5 min. Then, an excess of CHCl3 / CH3OH was added, and the mixed solution destroyed the synthesis reaction and terminated the reaction.

[0102] The precipitate was collected by centrifugation and washed with methanol and deionized water for 5 times. Finally, the precipitate was dried in a drying oven at 70°C for 20 hours to obtain the required KMnF3 nanoparticles. 20g of KMnF3 nanoparticles were weighed and dissolved in 10g of methanol solution. At the same time, 5g of ammonia solution was measured and added to 20g of anhydrous ethanol solution. Then, the prepared ammonia solution was slowly added to the methanol solution containing KMnF3 and stirred at room temperature for 2h. At the end of the reaction, it was washed with ethanol 5 times and the obtained black precipitate was placed in a 70°C oven and dried for 20h to obtain porous KMnF3-EC nanoparticles.

[0103] The solvent is one or two of methanol, deionized water, ethanol, N,N-dimethylformamide and N,N-diethylformamide.

[0104] The volume ratio of CHCl3 / CH3OH is 1:2.

[0105] The rotation speed of the centrifuge is 9000 and the centrifugation time is 8.5 min.

[0106] The mass ratio of the ethanol to water is 8:3.

[0107] The modified Pebax-1657 solution has a solid content of 4%. The method for modifying Pebax-1657 is as follows:

[0108] Pebax-1657: 110 g, placed in plasma equipment;

[0109] Plasma gas: ammonia: hexafluorobutyl acrylate vapor: 2-mercaptothiazoline vapor, volume ratio = 1.2:0.08:0.07; mixed gas flow rate = 15 ml / min, temperature: 85°C;

[0110] Plasma treatment time: 15 minutes, take out, and dry at 90°C for 25 hours;

[0111] Plasma equipment parameters:

[0112] Frequency: 13.56MHz,

[0113] Power: 250W.

[0114] The mass fraction of pure porous KMnF3-EC nanoparticles in the casting solution is 1.5 wt%.

[0115] The ultrasonic stirring and mixing method includes: ultrasonic dispersion for 35 minutes, and then stirring at 800 rpm for 50 minutes at room temperature.

[0116] Example 4

[0117] A method for improving the performance of mixed matrix membrane for separating CO2 by using defective porous materials, characterized in that it comprises the following steps:

[0118] (1) After mixing anhydrous ethanol and deionized water, heat them to 90° C. in an oil bath under stirring conditions, and then add modified Pebax-1657 thereto and keep stirring at 90° C. for 6 hours to completely dissolve them, thereby obtaining a modified Pebax-1657 solution;

[0119] (2) adding the metal frame porous KMnF3-EC material to 20 g of the Pebax-1657 solution prepared in step (1), and mixing by ultrasonic stirring to obtain a casting solution containing fillers;

[0120] (3) The casting solution obtained in step (2) was subjected to ultrasonic degassing for 30 minutes and allowed to stand for 10 minutes. It was then poured onto a clean polytetrafluoroethylene plate and placed in a 70° C. constant temperature oven for 15 hours. It was then placed in a vacuum oven and dried under vacuum for 24 hours to obtain a mixed matrix membrane.

[0121] Preparation method of the KMnF3-EC material:

[0122] 0.6 g MnCl2·4H2O, 6 g hexadecyltrimethylammonium bromide, 6 g 1-butanol, 18 g octane and 2.5 g deionized water were weighed and added into a reaction beaker, and then stirred under strong magnetic stirring at room temperature for 60 min to form a MnCl2·4H2O aqueous solution microemulsion;

[0123] At the same time, 0.6 g KF·2H2O, 6 g hexadecyltrimethylammonium bromide, 6 g 1-butanol, 18 g octane and 2.5 g deionized water were weighed and added into the reaction beaker, and then stirred under strong magnetic stirring at room temperature for 60 min to prepare a potassium fluoride aqueous solution microemulsion;

[0124] The KF·2H2O micellar solution was slowly added dropwise to the MnCl2·4H2O solution, and the solution was reacted for 10 min. Then, an excess of CHCl3 / CH3OH was added, and the mixed solution destroyed the synthesis reaction and terminated the reaction.

[0125] The precipitate was collected by centrifugation and washed with methanol and deionized water for 6 times. Finally, the precipitate was dried in a drying oven at 70°C for 24 hours to obtain the required KMnF3 nanoparticles. 30g of KMnF3 nanoparticles were weighed and dissolved in 15g of methanol solution. At the same time, 7.5g of ammonia solution was measured and added to 30g of anhydrous ethanol solution. Then, the prepared ammonia solution was slowly added to the methanol solution containing KMnF3 and stirred at room temperature for 3h. At the end of the reaction, it was washed with ethanol 6 times and the obtained black precipitate was placed in an oven at 80°C and dried for 24h to obtain porous KMnF3-EC nanoparticles.

[0126] The solvent is one or two of methanol, deionized water, ethanol, N,N-dimethylformamide and N,N-diethylformamide.

[0127] The volume ratio of CHCl3 / CH3OH is 1:3.

[0128] The rotation speed of the centrifuge is 10000, and the centrifugation time is 10 min.

[0129] The mass ratio of the ethanol to water is 9:4.

[0130] The modified Pebax-1657 solution has a solid content of 5%. The method for modifying Pebax-1657 is as follows:

[0131] Pebax-1657: 120 g, placed in plasma equipment;

[0132] Plasma gas: ammonia: hexafluorobutyl acrylate vapor: 2-mercaptothiazoline vapor, volume ratio = 1-1.2:0.1:0.08; mixed gas flow rate = 20 ml / min, temperature: 90°C;

[0133] Plasma treatment time: 20 minutes, take out, and dry at 100°C for 30 hours;

[0134] Plasma equipment parameters:

[0135] Frequency: 13.56MHz,

[0136] Power: 300W.

[0137] The mass fraction of pure porous KMnF3-EC nanoparticles in the casting solution is 2 wt%.

[0138] The ultrasonic stirring and mixing method includes: ultrasonic dispersion for 45 minutes, and then stirring at a speed of 1000 rpm for 60 minutes at room temperature.

[0139] Comparative Example 1

[0140] This example is a comparative example of Example 1, except that the content of KMnF3-EC is 0 wt%.

[0141] Comparative Example 2

[0142] This example is a comparative example of Example 1, except that Pebax-1657 is not modified.

[0143] Table 1 shows the composition ratios of the Pebax / KMnF3-EC mixed matrix membranes prepared in Examples 1 to 4 and Comparative Examples 1 to 2 and the related performance test results.

[0144]

[0145] The Pebax / KMnF3-EC mixed matrix membrane prepared by the present invention has a CO2 permeability of 70.33-153.69 Barrer and a CO2 / N2 selectivity of 49.77-77.14. Under the same conditions, 1.5wt.% MMMs exhibited the best CO2 permeability coefficient and CO2 / N2 selectivity, with a CO2 permeability coefficient of 153.69 Barrer and a CO2 / N2 selectivity of 77.14.

[0146] The present invention has been described above through specific implementation methods and examples, but these descriptions are only illustrative and should not be understood as limiting the scope of protection of the present invention. Without departing from the spirit and scope of protection of the present invention, those skilled in the art may make various improvements, modifications or equivalent substitutions to the technical solutions and implementation methods of the present invention, all of which should fall within the scope of protection of the present invention.

Claims

1. A method for improving the performance of mixed matrix membrane for separating CO2 by using defective porous materials, characterized in that: The following steps are involved: (1) After mixing anhydrous ethanol and deionized water, heat them to 80-90° C. in an oil bath under stirring conditions, then add modified Pebax-1657 thereto and keep stirring at 80-90° C. for 4-6 hours to completely dissolve them, thereby obtaining a modified Pebax-1657 solution; (2) adding the metal frame porous KMnF3-EC material to 15 to 20 parts of the modified Pebax-1657 solution prepared in step (1), stirring and mixing by ultrasonic stirring, to obtain a casting solution containing fillers; (3) The casting solution obtained in step (2) is subjected to ultrasonic degassing for 10 to 30 minutes and allowed to stand for 4 to 10 minutes. The solution is then poured onto a clean polytetrafluoroethylene plate and placed in a constant temperature oven at 50 to 70° C. for 10 to 15 hours. The mixture is then placed in a vacuum oven and dried under vacuum for 18 to 24 hours to obtain a mixed matrix membrane.

2. A method for improving the performance of mixed matrix membrane for separating CO2 by using defective porous materials according to claim 1, characterized in that: Preparation method of the KMnF3-EC material: Weigh 0.3-0.6 parts of MnCl2·4H2O, 2-6 parts of hexadecyltrimethylammonium bromide, 2-6 parts of 1-butanol, 12-18 parts of octane and 0.5-2.5 parts of deionized water by mass and add them into a reaction beaker, then stir under strong magnetic stirring at room temperature for 30-60 minutes to form a MnCl2·4H2O aqueous solution microemulsion; At the same time, 0.3-0.6 parts of KF·2H2O, 2-6 parts of hexadecyltrimethylammonium bromide, 2-6 parts of 1-butanol, 12-18 parts of octane and 0.5-2.5 parts of deionized water were weighed and added into a reaction beaker, and then stirred with a strong magnetic stirrer at room temperature for 30-60 minutes to prepare a potassium fluoride aqueous solution microemulsion; The KF·2H2O micellar solution was slowly added dropwise to the MnCl2·4H2O solution, and the solution was reacted for 5-10 minutes, and then an excess of CHCl3 / CH3OH was added, and the mixed solution destroyed the synthesis reaction and terminated the reaction; The precipitate is collected by centrifugation and washed with methanol and deionized water for 3-6 times. Finally, the precipitate is dried in a drying oven at 60-80°C for 12-24 hours to obtain the required KMnF3 nanoparticles. 10-30 parts of KMnF3 nanoparticles are weighed and dissolved in 5-15 parts of methanol solution. At the same time, 2.5-7.5 parts of ammonia solution are measured and added to 10-30 parts of anhydrous ethanol solution. Then, the prepared ammonia solution is slowly added to the methanol solution containing KMnF3, stirred at room temperature for 1-3 hours, washed with ethanol for 3-6 times at the end of the reaction, and the obtained black precipitate is placed in a 60-80°C oven and dried for 12-24 hours to obtain porous KMnF3-EC nanoparticles.

3. A method for improving the performance of mixed matrix membrane for separating CO2 by using defective porous materials according to claim 2, characterized in that: The solvent is one or two of methanol, deionized water, ethanol, N,N-dimethylformamide and N,N-diethylformamide.

4. The method of claim 2 for improving the performance of mixed matrix membrane for separating CO2 by using defective porous materials, characterized in that: The volume ratio of CHCl3 / CH3OH is 1:1-3.

5. The method of improving the CO2 separation performance of mixed matrix membrane using defective porous materials according to claim 2, characterized in that: The rotation speed of the centrifuge is 7000-10000, and the centrifugation time is 5-10 minutes.

6. The method of claim 1 for improving the performance of mixed matrix membrane for separating CO2 by using defective porous materials, characterized in that: The mass ratio of the ethanol to water is 6-9:1-4.

7. The method of claim 1 for improving the performance of mixed matrix membrane for separating CO2 by using defective porous materials, characterized in that: The modified Pebax-1657 solution has a solid content of 1-5%. The method for modifying Pebax-1657 is as follows: Pebax-1657: 100-120 parts, placed in plasma equipment; Plasma gas: ammonia: hexafluorobutyl acrylate vapor: 2-mercaptothiazoline vapor, volume ratio = 1-1.2: 0.05-0.1: 0.05-0.08; mixed gas flow rate = 10-20 ml / min, temperature: 80-90°C; Plasma treatment time: 10-20 minutes, take out and dry at 80-100℃ for 20-30 hours; Plasma equipment parameters: Frequency: 13.56MHz, Power: 200-300W.

8. The method of claim 1 for improving the performance of mixed matrix membrane for separating CO2 by using defective porous materials, characterized in that: The mass fraction of pure porous KMnF3-EC nanoparticles in the casting solution is 0.5-2wt%.

9. The method of claim 1 for improving the performance of mixed matrix membrane for separating CO2 by using defective porous materials, characterized in that: The ultrasonic stirring and mixing method comprises: ultrasonic dispersion for 15 to 45 minutes, and then stirring at a speed of 500 to 1000 rpm for 30 to 60 minutes at room temperature.

10. A method for improving the performance of mixed matrix membrane for separating CO2 by using defective porous materials according to claims 1-9, characterized in that: The mixed matrix membrane prepared by the invention is used for CO2 / N2 gas separation.

Citation Information

Patent Citations

  • Method for preparing hollow KMnF3 nano square granules

    CN107487787A

  • Separation of alcohol vapor from the mixture of alcohol vapor and nitrogen with mixed matrix membranes

    WO2022046013A1