Material for powder bed fusion techniques and use of such material in
By using thermoplastic polyamide powder with aliphatic dicarboxylic acid structural units of 16 to 22 carbon atoms, the problem of insufficient material performance and printability in powder bed fusion technology is solved, high mechanical properties and stability are achieved, and improved Smoothness and reusability of the product.
Patent Information
- Application Number
- CN202410356489.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-01
AI Technical Summary
When preparing three-dimensional parts, the existing powder bed fusion technology has deficiencies in the material's mechanical properties, printability, and smoothness, and the material's stability and reusability are poor, affecting the quality and production efficiency of the product. .
Thermoplastic polyamide powder containing aliphatic dicarboxylic acid structural units of 16 to 22 carbon atoms is used to form a fine particle state by crushing, grinding or precipitation, and is used in powder bed fusion technology, combined with electromagnetic energy focused or unfocused input to achieve selective melting and sintering.
It improves the mechanical properties, printability and smoothness of the material, ensures the stability and reusability of the product, enhances translucency and component integrity, and reduces waste material generation.
Smart Images

Figure BDA0004761517840000161 
Figure BDA0004761517840000171 
Figure BDA0004761517840000191
Abstract
Description
Technical Field
[0001] The present invention relates to powder materials for powder bed fusion (PBF) techniques such as selective laser sintering (SLS), as well as methods for making such materials, selective PBF processes such as laser sintering processes using such materials, and articles made using these materials in SLS processes. Background Art
[0002] The powder bed fusion (PBF) technique is an additive manufacturing process for producing three-dimensional structures by laser sintering starting from a powdered starting material. In this process, unconsolidated loose powder is provided in a container and the workpiece is built up continuously layer by layer by selective irradiation from above with a laser, which irradiates only the areas to be solidified and causes this solidification by melting the material. After irradiation of the layer and its liquefaction and / or solidification, a subsequent layer of powdered starting material is laid on top of it, and in a next step, the desired areas in this subsequent layer are melted and, if necessary, solidified and simultaneously fused with the molten layer below or the solidified layer.
[0003] Specifically, in order to prepare the molded part, the polymer powder is applied in a thin layer to a descendable plate of the sintering chamber, which is usually heated to a temperature slightly below the melting point of the polymer. The layer thickness is selected in such a way that a molten layer is formed during or after the subsequent laser sintering. The laser sinters the powder particles according to the specifications of the control computer. Afterwards, the plate is made to descend by the amount of the layer thickness, usually 0.05mm to 2.0mm. With the application of a new powder layer, the process is repeated. After the preselected number of cycles is completed according to the expected number of layers, a block composed of powder is formed on the outside. Inside, it contains a high viscosity melt or a substantially solidified block in the shape of the desired molded part. The non-melting area where the powder is still in solid form stabilizes the shape of the melt. Afterwards, the block composed of the powder shell and the melt is slowly cooled, and the melt solidifies when the melt is below the solidification temperature of the polymer. It is advantageous if the block is kept at the solidification temperature until the phase change is completed. This is achieved by choosing a low cooling rate within the temperature range of the phase change, so that the heat released by solidification keeps the internal molded body just at the solidification temperature until the phase change is complete. After cooling, the block is removed from the sintering chamber and the molded body is separated from the unsolidified polymer powder. The powder can be used again in the process.
[0004] Commonly used polymer powders for such processes include polyamide 11 (PA 11) or polyamide 12 (PA 12), polyamide 6 (PA 6), but also polyacetal, polypropylene (PP), polyethylene (PE) and ionomers, as described in DE 197 47 309. Polycarbonate (PC) and polystyrene (PS) have also been used.
[0005] EP-A-1 720 930 describes copolymer powders, and the use of such powders for a non-focused molding process, and molded articles made from such polymer powders. The molding process is a layer-by-layer process using powders, in which selective regions of the layers are melted by non-focused introduced electromagnetic energy. The selectivity can be achieved by masks, by applying inhibitors, absorbers, receptors. The PA 6 / 12 / 66 system works effectively and specifies MVR values in the range of 1 g / min to 12 g / min.
[0006] EP-A-2 274 363 relates to a process for lowering the crystallization temperature and melting temperature of polyamide powders resulting from the polymerization of at least one principal monomer, wherein at least one minority comonomer is selected from aminocarboxylic acids, diamine-diacid pairs, lactams and / or lactones, and wherein the at least one minor comonomer is from 0.1 to 20% by mass of the total mixture of monomers and comonomers, preferably from 0.5 to 15% by mass of the total mixture. Using PA 12 / 6 type systems, the proportion of caprolactam in said system must not exceed 20%.
[0007] WO-A-2011124278 relates to a polymer powder for a layer-by-layer process in which the regions of the individual powder layers are selectively fused by introducing electromagnetic energy. The polymer powder comprises: at least one AB-type polyamide, which is prepared by polymerization of a lactam having 10 to 12 carbon atoms in the monomer unit or polycondensation of a corresponding aminocarboxylic acid having 10 to 12 carbon atoms in the monomer unit; and at least one AABB-type polyamide, which is prepared by polycondensation of a diamine and a dicarboxylic acid each containing 10 to 14 carbon atoms in the monomer unit. The present disclosure also relates to: a method for preparing such a powder; a layer-by-layer process for producing a molded body from such a powder, in which the regions of the individual layers are selectively melted by introducing electromagnetic energy, wherein the selectivity is obtained using a mask or by applying an inhibitor, absorber or receptor or by focusing the applied energy; and a molded article produced thereby.
[0008] WO-A-2015009790 describes a component material for printing a three-dimensional component using an electrophotography-based additive manufacturing system, wherein the component material comprises a composition having a semi-crystalline thermoplastic material and a charge control agent. The component material is provided in the form of a powder having a controlled particle size and is configured for use in an electrophotography-based additive manufacturing system having a layer transfer device for printing the three-dimensional component layer by layer. Although different materials for the powder used are mentioned, a specific system is not effective.
[0009] WO-A-2020064825 relates to a sintered powder comprising a first polyamide component and a second polyamide component, wherein the melting point of the second polyamide component is higher than the melting point of the first polyamide component. The disclosure also relates to a method for preparing a molded article by sintering the sintered powder or by an FFF (fused filament fabrication) process and a molded article that can be obtained by the method. The disclosure also relates to a method for preparing a sintered powder. A mixture of aliphatic polyamide and semi-aromatic polyamide is used, and polyamide 6 and polyamide 66 are used as aliphatic polyamides in the mixture.
[0010] CN-A-107337793 introduces a copolymerized nylon powder material for selective laser sintering and a method for manufacturing the same. The method comprises the following steps: copolymerizing a short-chain nylon raw material and a long-chain nylon raw material using a copolymerization reaction principle to obtain a copolymerized nylon resin, crushing the copolymerized nylon resin at low temperature, drying and screening, and adding a flow aid and an antioxidant to obtain a copolymerized nylon powder material, and selective laser sintering is used. A system based on polyamide 1010 and polyamide 1212 and polyamide 66 or PA6 in the form of PA6 / 1010, PA66 / 1010, PA6 / 1212, PA66 / 12 is used.
[0011] CN-A-104830053 relates to the field of polymer materials and aims to solve the problem of high industrial cost of nylon 12 in the field of 3D printing. It discloses a method for preparing a caprolactam-laurolactam copolymer modified by glass fiber and its powder, wherein the relevant mechanical properties of the resulting polymer are described. The copolymer powder has good properties such as thermodynamic properties and dimensional stability, low production cost and use cost, uniform particle size, and can be used to partially replace nylon 12 to a certain extent, especially in the field of 3D printing. The specific system disclosed is only a PA 6 / 12 system, and is therefore a system based on caprolactam and laurolactam with glass fibers.
[0012] WO-A-2005082979 discloses polymer powders containing copolymers, the use of such powders in a molding method, and molded bodies produced from such polymer powders. The molding method is a method that uses powders to operate layer by layer, and during the method, the regions of each layer are fused by focusing and applying electromagnetic energy. After being cooled, the solidified molded body can be taken out from the powder bed. Compared with molded bodies produced from conventional powders, the component properties of the molded bodies produced using the powders of the invention according to the method can vary within a certain range depending on their composition. The specific systems disclosed are systems including PA6 / 12 / 612, PA 6 / 12 / 612, PA 12 / 66, PA 6 / IPDA12, and polyester systems based on terephthalic acid, wherein IPDA is isophorone diamine.
[0013] US-B-8097333 discloses pre-impregnated composite materials (prepregs) that can be cured to form composite parts with a high level of damage tolerance. The matrix resin includes a thermoplastic particle component, which is a blend of particles having a melting point above the curing temperature and particles having a melting point at or below the curing temperature. The specific system disclosed is a PA6 / 12 system, and is therefore a system based on caprolactam and laurolactam.
[0014] WO-A-2005105891 relates to a polymer powder comprising a polyamide, its use in a molding process and a molded body made from the polymer powder. The molding process comprises a layering process using a powder in which selective regions of the relevant layers are fused by introducing electromagnetic radiation. The selectivity can be achieved by masking, by applying inhibitors, absorbers or sensitizers, or by focusing the input energy. After cooling, the solidified region as a molded body can then be removed from the powder bed. Specific systems disclosed include PA12, PA1010, PA1012, PA1212, PA612, PA613.
[0015] WO-A-2016112283 also discloses powder compositions for laser sintering. Nylon copolymer compositions are described, which are said to provide enhanced performance in processing and finished products when used in 3D laser sintering processes. Specific systems disclosed include PA11, PA12, PA610 / 6T6I, PA612 / 6T6I, PA6 / 69, PA6 / 6T6I.
[0016] WO-A-2007051691 discloses a process for producing ultrafine powders based on polyamide, wherein a polyamide having a relative solution viscosity in the range of 1.5 to 2.0 is contacted with an alcoholic medium in the presence of inorganic particles at superatmospheric pressure and / or elevated temperature to produce at least a partial solution, and the polyamide is subsequently precipitated from at least a partial solution, characterized in that a suspension of inorganic particles suspended in an alcoholic medium is used. The ultrafine polyamide powder obtained has a relative viscosity at 5 m / s determined by the BET method of 0.0447 W / m. 2 / g to 100m 2 / g, a fineness d50 of less than 70 μm; a bulk density BD in the range of 250 g / L to 1000 g / L; and a particle content of inorganic particles of 0.1 wt % to 80 wt % based on the total weight of the polyamide powder. Specific systems disclosed include PA 12, PA1010, and PA1012.
[0017] EP-A-2650106 discloses polymer powders exhibiting a single melting point determined by differential scanning calorimetry, comprising polyamides of the AABB type. Specific working systems disclosed include PA1012, PA1010, PA1013, PA613, PA1212.
[0018] WO-A-2009101320 relates to PA polyamide (homopolyamide or copolyamide) powders derived at least in part from renewable materials, wherein the particles have a non-spherical shape and a median volume diameter less than or equal to 20 μm. It also relates to a method for preparing such powders. The specific working systems disclosed include PA11 and PA12.
[0019] CN-A-107337792 provides a copolymerized nylon powder material with a controllable melting point and a preparation method thereof. The method comprises the following steps: adding a first solvent, an aliphatic dibasic acid and an aliphatic diamine to a polymerization kettle, reacting to generate a copolymerized nylon salt, adding a copolymerized nylon salt solution, a molecular weight regulator, deionized water and an antioxidant to the polymerization kettle, polymerizing the added substances to obtain copolymerized nylon granules, adding the copolymerized nylon granules and a second solvent to the polymerization kettle, performing solvent pulverization to obtain copolymerized nylon powder, and post-treating the copolymerized nylon powder to obtain a copolymerized nylon powder material that can be effectively applied to a selective laser sintering process. By controlling the ratio of the two nylon salts in the copolymerized nylon, the copolymerized nylon salt is obtained from the preparation of the salt at one time, so the method has the following advantages: effectively controlling the melting point of the copolymerized nylon, omitting the separation and drying process of the salt, improving process stability, saving preparation time, saving preparation time, and improving the stability of the performance of the copolymerized nylon material.
[0020] US-A-2012041132 discloses moldings produced by a layer-by-layer process in which the individual polymer powder layers are selectively melted by introducing electromagnetic energy, wherein the process uses a powder comprising at least one homopolyamide prepared by polycondensation of diamines and dicarboxylic acids, wherein the homopolyamide has a melting enthalpy of at least 125 J / g and a recrystallization temperature of at least 148°C.
[0021] US-A-2013274435 provides a precipitation polymer powder based on AABB type polyamide, which is obtained by reprecipitating the polyamide by at least partial dissolution and then continuous cooling of the solution to below the precipitation temperature. The polyamide is prepared by polycondensation of a diamine with a dicarboxylic acid. The precipitated polyamide obtained is used for layer-by-layer forming processes, such as selective laser sintering.
[0022] WO-A-2021069851 relates to polyamide powders for a powder bonding process by sintering, which comprise at least one chain limiter.
[0023] WO-A-2019195689 discloses an additive manufacturing composition comprising: A) 5 to 94.9 weight percent of at least one semi-crystalline copolyamide having a melting point; wherein the semi-crystalline copolyamide comprises: a-1) 5 to 40 mole percent of aromatic repeating units derived from: i) one or more aromatic dicarboxylic acids having 8 to 20 carbon atoms and aliphatic diamines having 4 to 20 carbon atoms, and a-2) 60 to 95 mole percent of aliphatic repeating units derived from: ii) an aliphatic dicarboxylic acid having 6 to 20 carbon atoms and an aliphatic diamine having 4 to 20 carbon atoms. aliphatic diamine; B) 5 to 94.9 weight percent of at least one amorphous copolyamide comprising: b-1) 60 to 90 mole percent of aromatic repeating units derived from: iii) isophthalic acid and an aliphatic diamine having 4 to 20 carbon atoms, and b-2) 10 to 40 mole percent of aromatic repeating units derived from: iv) terephthalic acid and an aliphatic diamine having 4 to 20 carbon atoms; C) 0.1 to 50 weight percent of at least one aromatic polyamide material; and D) 0 to 30 weight percent of at least one additive. These compositions provide 3D printed articles with improved physical properties. Summary of the invention
[0024] An object of the present invention is to propose a powder for a powder bed fusion method (e.g., an SLS method of the type described above). The powder bed fusion method may include the use of focused or non-focused input electromagnetic energy, thermal energy or other energy to selectively fuse, melt, sinter or solidify powder materials in an additive manufacturing process. Preferably, the powder is used to produce an article / molded article in a layer-by-layer process, in which regions of the powder layer are selectively melted using focused or non-focused input electromagnetic energy. It can be used in an SLS process, as well as in a multi jet fusion (MJF), a selective absorption fusion (SAF) or a high speed sintering (HSS) process.
[0025] A powder according to the present invention is defined as a solid substance which has been reduced (at room temperature) to a fine loose particle state, for example by crushing, grinding, breaking, settling or a combination thereof.
[0026] In particular, a powder will be provided which has at least one of the following advantageous properties:
[0027] Good or enhanced mechanical properties
[0028] Good or enhanced printability (less cracking / warping / curling and better flow)
[0029] Good or enhanced reusability for multiple print runs
[0030] Possibility to dry mix pigments in the material to print full color parts where the pigment does not bleed
[0031] Stable mechanical properties before and after conditioning (23°C, 50% humidity, 40 hours)
[0032] Possibility of subsequent coloring even after conditioning due to stable mechanical properties
[0033] Good or higher translucency
[0034] Good or better part smoothness (more complete).
[0035] According to a first aspect of the invention, it relates to the use of a powder comprising or consisting of a thermoplastic polyamide powder for producing a molding in a layered process, wherein the selective regions of the powder layer:
[0036] (1) Melting by input of electromagnetic energy (usually via a controllable laser),
[0037] (2) melting by input of thermal energy from a source other than electromagnetic energy, or
[0038] (3) Otherwise melted, fused, sintered or solidified to form a product or article.
[0039] Such a powder is characterized as claimed in claim 1. The invention relates to and claims the use of such a powder and also to such a powder having the further characteristics as detailed below.
[0040] According to the invention, the powder comprises or consists of a thermoplastic polyamide powder which comprises aliphatic dicarboxylic acid structural units having 16 to 22 carbon atoms.
[0041] This includes the case where the thermoplastic polyamide powder is a powder formed from a mixture of two or more different polyamides containing aliphatic dicarboxylic acid structural units having 16 to 22 carbon atoms.
[0042] In fact, it has been shown that the abovementioned advantages can surprisingly be achieved if the thermoplastic polyamide powder serving as the powder basis comprises these long-chain structural units.
[0043] The powder for the layer-by-layer process consists only of thermoplastic polyamide powder, or it may comprise thermoplastic polyamide powder in a mixture with a different powder material, in which the regions of the powder layer are selectively melted, sintered, fused or solidified, preferably by focused or non-focused input electromagnetic energy. The proportion of thermoplastic polyamide powder in such a mixture powder is generally at least 50% by weight relative to the total amount of powder, preferably at least 60% by weight or as further described below. Powder materials different from thermoplastic polyamide may, for example, comprise filler materials (organic or inorganic), flow aid materials, stabilizer materials (including heat stable, light stable), colorants including pigments or dyes, or powder particles of a combination thereof, or be composed of filler materials (organic or inorganic), flow aid materials, stabilizer materials (including heat stable, light stable), colorants including pigments or dyes, or powder particles of a combination thereof, or in the form of individual particles or mixture particles of such materials. Preferably, the particle size of such different powder particles is selected in the same or substantially the same range as the powder particles of the thermoplastic polyamide powder further defined below.
[0044] The thermoplastic polyamide powder in the powder itself can be composed of a single thermoplastic polyamide or a mixture of different thermoplastic polyamides, or the thermoplastic polyamide powder can be composed of particles made from a mixture of one or more thermoplastic polyamide types and other additives. Usually, relative to the total weight of 100% of the thermoplastic polyamide powder, the thermoplastic polyamide powder comprises at least 70% by weight of a thermoplastic polyamide powder comprising aliphatic dicarboxylic acid structural units with 16 to 22 carbon atoms or a mixture of different thermoplastic polyamides comprising aliphatic dicarboxylic acid structural units with 16 to 22 carbon atoms. Preferably, relative to 100% of the total thermoplastic polyamide powder, additives account for up to 20% by weight or up to 10% by weight or up to 5% by weight. According to a preferred embodiment, the thermoplastic polyamide powder is composed of only one or several thermoplastic polyamide systems comprising aliphatic dicarboxylic acid structural units with 16 to 22 carbon atoms, without any additives. The additive can be selected as described in further detail below.
[0045] According to a first preferred embodiment, the aliphatic dicarboxylic acid structural unit having 16 to 22 carbon atoms is selected from the group of linear dicarboxylic acids having a terminal carboxyl group, preferably from: hexadecanedioic acid, octadecanedioic acid, docosane-1,20-dicarboxylic acid, or mixtures thereof.
[0046] According to a particularly preferred embodiment, the aliphatic dicarboxylic acid structural unit having 16 to 22 carbon atoms is selected from only one of hexadecanedioic acid, octadecanedioic acid or docosane-1,20-dicarboxylic acid.
[0047] According to yet another preferred embodiment, the thermoplastic polyamide powder comprises or consists of structural units built up from diamines and dicarboxylic acids, and the molar ratio of aliphatic dicarboxylic acid structural units having 16 to 22 carbon atoms relative to all dicarboxylic acids of the polyamide is at least 20%, or at least 40%, or at least 50%, preferably at least 60%, or in the range of 65 to 100%, or in the range of 85 to 100%.
[0048] The diamine is preferably selected from linear or branched aliphatic, cycloaliphatic or aromatic diamines having 4 to 20 carbon atoms.
[0049] The linear aliphatic diamine is preferably selected from linear aliphatic diamines having 6 to 12 carbon atoms, preferably from the group of tetramethylenediamine, hexamethylenediamine, octanediamine, nonanediamine, decanediamine, or mixtures thereof.
[0050] The alicyclic diamine is preferably selected from bis(4-amino-3-methylcyclohexyl)methane (MACM, CAS No. 6864-37-5), bis(4-aminocyclohexyl)methane (PACM, CAS No. 1761-71-3), or a mixture thereof.
[0051] The aromatic diamine is preferably selected from xylylenediamine, in particular p-xylylenediamine, m-xylylenediamine, or a mixture thereof.
[0052] Structural units based on diamines and dicarboxylic acids which are not based on the abovementioned aliphatic dicarboxylic acid structural units having 16 to 22 carbon atoms may also be present, however, as indicated above, preferably in a lower proportion than structural units based on aliphatic dicarboxylic acid structural units having 16 to 22 carbon atoms.
[0053] For these different structural units, the dicarboxylic acid different from the aliphatic dicarboxylic acid structural unit having 16 to 22 carbon atoms is preferably selected from the group of linear or branched aliphatic, alicyclic or aromatic dicarboxylic acids having 4 to 20 carbon atoms, wherein preferably the linear aliphatic dicarboxylic acid is selected from succinic acid, adipic acid, suberic acid, sebacic acid, dodecanoic acid, or a mixture thereof, and wherein the aromatic dicarboxylic acid is selected from terephthalic acid, isophthalic acid, or a mixture thereof.
[0054] The thermoplastic polyamide powder preferably comprises or consists of structural units constructed from diamines and aliphatic dicarboxylic acid structural units having 16 to 22 carbon atoms, and is selected from PA 616, PA 618, PA 620, PA1016, PA1018, PA 1020, PA1216, PA 1218, PA 1220, or a mixture thereof. According to a particularly preferred embodiment, the thermoplastic polyamide powder does not contain lactam structural units.
[0055] According to another preferred embodiment, the thermoplastic polyamide powder is based on a polyamide further comprising lactam structural units, wherein the lactam structural units have 4 to 20 carbon atoms, preferably 6 to 12 carbon atoms. In this case, preferably, the molar ratio of lactam structural units relative to the structural units built up from diamines and dicarboxylic acids is at most 50%, or at most 40%, or at most 30%.
[0056] According to another preferred embodiment, the thermoplastic polyamide powder is selected from PA 616, PA 1016, PA 1016 / 101, PA 6 / 66 / 610 / 616, PA 620, PA 1020, or mixtures thereof. In each of these cases in which not only structural units based on aliphatic dicarboxylic acid structural units having 16 to 22 carbon atoms are present, the proportion of aliphatic dicarboxylic acid structural units having 16 to 22 carbon atoms is preferably at least as defined above.
[0057] According to a particularly preferred embodiment, the powder consists of a thermoplastic polyamide powder or comprises only a single thermoplastic polyamide component, wherein the thermoplastic polyamide powder or the thermoplastic polyamide component comprises at least one aliphatic dicarboxylic acid structural unit having 16 carbon atoms, which is preferably selected as hexadecanedioic acid.
[0058] Preferably, the thermoplastic polyamide powder or thermoplastic polyamide component is constructed from diamine and dicarboxylic acid structural units and lactam, wherein the molar ratio of lactam is less than 40 mol%, preferably less than 30 mol%, wherein the molar percentage is relative to the total molar amount of lactam and half of the total molar amount of diamine and dicarboxylic acid. By way of example, the system can be provided by 27 mol% caprolactam and 73 mol% hexadecanedioic acid and 73 mol% hexamethylenediamine.
[0059] According to a preferred embodiment, the thermoplastic polyamide powder or thermoplastic polyamide component does not contain any lactam structural units and contains only one aliphatic diamine structural unit and hexadecanedioic acid as dicarboxylic acid structural unit. In this case, preferably the diamine structural unit has 6 or 10 carbon atoms.
[0060] According to another preferred embodiment, the thermoplastic polyamide powder or thermoplastic polyamide component does not contain any lactam structural units and contains only one aliphatic diamine structural unit, preferably 1,6-hexamethylenediamine, and contains at least 90 mol % of hexadecanedioic acid as dicarboxylic acid structural unit, the remaining dicarboxylic acid is preferably selected from aromatic dicarboxylic acid systems, preferably isophthalic acid and / or terephthalic acid.
[0061] According to a further preferred embodiment, the thermoplastic polyamide powder or thermoplastic polyamide component is built up from at least 50 mol % of hexadecanedioic acid and the remaining dicarboxylic acids (aliphatic dicarboxylic acids, preferably adipic acid and / or sebacic acid) and aliphatic diamines (preferably only hexamethylenediamine) and lactams (preferably caprolactam), wherein the proportion of lactam is less than 40 mol %, wherein the molar percentages are in each case relative to the total amount of lactam and half of the molar sum of diamines and dicarboxylic acids.
[0062] Preferably, the thermoplastic polyamide powder has
[0063] a melting point measured according to ISO 11357-3 greater than 160°C, preferably in the range of 165°C to 210°C,
[0064] and / or having a glass transition temperature of at least 25°C, preferably measured by dynamic mechanical analysis according to ISO 6721-2:2008.
[0065] According to a further preferred embodiment, the powder used does not contain any amorphous polyamide fraction.Thus, preferably, the powder used comprises or even consists of only semi-crystalline polyamide, which preferably has a melting point as defined above.
[0066] According to yet another preferred embodiment, the powder used does not contain any aromatic polyamide materials, wherein aromatic polyamide materials are understood to be those made from polyamides in which at least 85% of the amide (-CONH) bonds are directly attached to two aromatic rings, including aromatic polyamides such as poly(p-phenylene terephthalamide) known as PPD-T.
[0067] Preferably, the thermoplastic polyamide powder is a ground or milled polyamide powder, and wherein preferably in the case of a ground powder it is produced by a cryogenic grinding process.
[0068] Preferably, the thermoplastic polyamide powder has a relative viscosity in the range of 1.5 to 2.1, preferably in the range of 1.6 to 2.0, preferably measured according to ISO 307 in m-cresol at a temperature of 20° C. and a concentration of 0.5% by weight.
[0069] Preferably, the recrystallization temperature (T rc ) is in the range of 70°C to 180°C, preferably in the range of 80°C to 170°C, or in the range of 80°C to 160°C, or in the range of 80°C to 150°C. More preferably, the recrystallization temperature (T rc ) is less than 148°C or less than 145°C, or in the range of 70°C to 147°C, preferably in the range of 80°C to 145°C, or in the range of 80°C to 145°C, or in the range of 80°C to 145°C.
[0070] According to the invention, the powder used does not contain chain limiters as additives independent of the polyamide powder. This means that the thermoplastic polyamide does not contain any free chain limiters in the vicinity of the actual polyamide polymer. If a chain limiter is used, it is added to the polyamide monomer starting material during the manufacturing process, as well as at the beginning and before starting the polymerization process. Therefore, any such chain limiter will react with the actual polyamide polymer and become part of the actual polyamide polymer and will not be present as a further additive in the vicinity of the polyamide polymer. In particular, chain limiters of the monoacid, dicarboxylic acid, monoamine, diamine type as additives are not present in the powder.
[0071] According to another preferred embodiment, no chain limiters are used during the manufacturing process either, and thus the polyamide polymer of the powder also does not contain chain limiters as part of the polymer chain.
[0072] Preferably, the sintering window of the thermoplastic polyamide powder is in the range of 5° C. to 90° C., preferably in the range of 6° C. to 80° C. The sintering window is defined as the melting temperature T m and recrystallization temperature T rc The window between m -T rc ).
[0073] The thermoplastic polyamide powder and / or the powder as a whole preferably has an average particle size D50 in the range of 50 to 80 μm, preferably in the range of 50 to 65 μm, more preferably in the range of 50 to 60 μm, preferably measured according to ISO 13322-2.
[0074] Preferably, the particle size distribution is such that 80%, preferably 90%, of the particles are located in the size range of 20 μm to 100 μm, preferably in the range of 40 μm to 90 μm.
[0075] Preferably, the D10 value measured according to ISO 13322-2 is in the range of 15 to 45 μm, preferably in the range of 20 to 30 μm, and / or the D95 value measured according to ISO 13322-2 is in the range of 80 to 150 μm, preferably in the range of 85 to 98 μm.
[0076] Typically, the powder and / or the thermoplastic polyamide powder has a diameter D50 measured according to ISO 13322-2 of 50 to 80 μm, preferably 50 to 65 μm, more preferably 50 to 60 μm.
[0077] The powder particles preferably have substantially a slightly jagged or irregular shape (eg, sphericity much less than 1), a spherical shape, or a potato shape.
[0078] The thermoplastic ground polyamide powder also preferably has an MFR value, preferably measured according to ISO 1133, in the range of 6 to 17 g / 10 min.
[0079] Typically, thermoplastic polyamide powders contain no fillers.
[0080] Alternatively or additionally, the thermoplastic polyamide powder contains no flame retardant additives.
[0081] Alternatively or additionally, the thermoplastic polyamide powder contains no aromatic structural units.
[0082] According to a further preferred embodiment, the thermoplastic polyamide powder consists of polyamide and further additives, the amount of the further additives being not more than 20 wt.-% or 15 wt.-%, preferably in the range of 1 wt.-% to 12 wt.-% or 5 wt.-% to 10 wt.-%, relative to the total weight of the powder.
[0083] Preferably, the additive is one or a combination of the following: a filler, preferably selected from the group of talc, alumina-based fillers, glass fillers, metal carbonates (including calcium carbonate); a flow aid, preferably selected from the group of fumed or precipitated silica, metal salts of long-chain fatty acids (including metal stearates), titanium dioxide, Group 1 salts, fumed alumina; a flame retardant, preferably selected from the group of organic or inorganic monophosphinates / salts or diphosphinates / salts, preferably metal alkylphosphinates / salts, in particular aluminum diethylphosphinate, alone or in combination with a synergist compound, preferably containing nitrogen and / or phosphorus, including melem, melam, melon or other melamines or derivatives thereof.
[0084] According to another aspect of the invention, it relates to a method for producing a thermoplastic polyamide powder for use in a process as described above. In one example, the method is characterized in particular in that a particle size distribution suitable for the printing process is achieved by a suitable screening technique (drum-type air-jet screen, ultrasonic drum or air classifier). In other examples, the method may not use screening techniques.
[0085] More generally, the present invention also relates to a process for preparing a thermoplastic polyamide powder as defined above, wherein the thermoplastic polyamide is subjected to a cryogenic grinding process or a precipitation process and preferably subsequently to a particle size screening (sieving) process, preferably for producing a particle size distribution such that the average particle size D50 is in the range of 50 μm to 80 μm, preferably in the range of 50 μm to 65 μm, more preferably in the range of 50 μm to 60 μm, the average particle size D50 being preferably measured according to ISO 13322-2.
[0086] If necessary to prepare a final powder, the thermoplastic polyamide powder can be mixed with different powder particles, as described in further detail below. The above-mentioned particle size screening can be performed before or after mixing with different powder particles, or both.
[0087] In addition, in some examples, if desired, after mixing with additives, the method includes forming the thermoplastic polyamide powder using solvent precipitation, solvent pulverization, melt emulsification, melt pulverization or another micronization technique. In addition, in some embodiments, the composition for additive manufacturing can be prepared by blending the polyamide powder with one or more additional components or additives (e.g., additives or fillers). In some examples, such a composition can be prepared by dry blending or wet blending.
[0088] According to another aspect, the present invention describes (sinterable) powders for additive manufacturing, such as SLS or other additive manufacturing methods, in which granular or particulate materials are melted, fused, sintered or otherwise solidified in a selective manner. According to the present invention, such powders include thermoplastic polyamide powders as described herein as components. Thermoplastic polyamide powders can form all or part of sinterable powders. In some cases, thermoplastic polyamide powders are the main or most components of sinterable powder compositions. For example, in some embodiments, based on the gross weight of powder, the powders for additive manufacturing described herein include up to 100% by weight, up to 99% by weight, up to 95% by weight, or up to 90% by weight of thermoplastic (co) polyamide powders. In some cases, the powder comprises 50 wt % to 100 wt %, 50 wt % to 99 wt %, 50 wt % to 90 wt %, 50 wt % to 80 wt %, 50 wt % to 70 wt %, 60 wt % to 100 wt %, 60 wt % to 99 wt %, 60 wt % to 90 wt %, 70 wt % to 100 wt %, 70 wt % to 99 wt %, 70 wt % to 90 wt %, 80 wt % to 100 wt %, 80 wt % to 99 wt %, 80 wt % to 95 wt %, 85 wt % to 100 wt %, 85 wt % to 99 wt %, 85 wt % to 95 wt %, 90 wt % to 100 wt %, or 90 wt % to 99 wt % of the thermoplastic (co)polyamide powder, based on the total weight of the powder. In some cases, the powder comprises, in addition to the thermoplastic (co)polyamide powder component, further granular, granular or powdered components.
[0089] For example, in some embodiments, the powders for additive manufacturing described herein include a flow aid component. Therefore, in order to achieve enhanced fluidity of the powder during layer fusion, a small amount of flow aid or a combination of flow aids can be used. Such flow aids are, for example, talc, aluminum hydroxide or other Al-based flow aids, glass fillers, CaCO3 (or other metal carbonates), Aerosil (pyrogenic or precipitated silica), Sipernat variants, magnesium stearate (or other stearates), TiO2 (or other metal oxides), Group 1 salts, and metal-based long-chain fatty acids.
[0090] It is also possible to have a coating on the thermoplastic polyamide powder particles, which coating has corresponding additives which support the additive manufacturing process.
[0091] Furthermore, the present invention relates to a method for printing a three-dimensional article, comprising:
[0092] providing a powder as detailed above; and selectively curing layers of the powder to form an article, preferably using focused or unfocused input electromagnetic energy.Preferably the composition is provided in a layer-by-layer process.
[0093] More generally, the present invention also relates to a method for printing a three-dimensional article, comprising the steps of:
[0094] providing a powder consisting of or comprising a thermoplastic polyamide powder as detailed above; and
[0095] selectively solidifying layers of powder to form an article, preferably using focused or non-focused input electromagnetic energy, wherein preferably the composition is provided in a layer-by-layer process,
[0096] Preferably, the powder has a particle size D50 measured according to ISO 13322-2 of 50 to 80 μm, preferably 50 to 65 μm, more preferably 50 to 60 μm.
[0097] Furthermore, the present invention relates to a molded body produced using the method as described above, or a molded body produced or formed from the powder as described above.
[0098] Further embodiments of the invention are claimed in the dependent claims. DETAILED DESCRIPTION
[0099] Preferred embodiments of the invention are described below based on embodiments which serve only as illustrations and which should not be interpreted restrictively. According to the invention, condensation reactions as well as grinding methods and uses are described.
[0100] Step A1 - Copolyamide, general procedure for polymer production, PA 616, E1:
[0101] Hexadecanedioic acid (28.46 kg, 100 mol%), hexane-1,6-diamine (11.58 kg, 100 mol%, added as a 60% water mixture) were transferred to an autoclave together with water (3 kg), where the mixture was stirred at 160 to 200° C. for 140 minutes. The mixture was then heated to 290° C. and 20 bar and stirred at 290° C. for 5 hours at a constant pressure of 20 bar. After 2.5 hours, the polymer was cooled to 270° C. and the pressure was reduced to 0.3 bar. The temperature was then reduced to 260° C.
[0102] The polycondensate was then pelletized and dried according to standard procedures.
[0103] Analysis: Melting point: 190.0°C, Recrystallization temperature: 165°C, Relative viscosity (0.5% in m-cresol): 1.90 to 2.00.
[0104] Step A2 uses a copolyamide based on an aromatic component, such as E3:
[0105] In a synthesis procedure similar to A.2, only 95 mol% of hexadecanedioic acid is used, and the remaining 5 mol% is replaced by an aromatic-based dicarboxylic acid (e.g. IPS or TPS). The diamine ratio remains unchanged, and the production procedure is the same as above. The polycondensate is then granulated and dried by standard procedures.
[0106] Analysis: Melting point: 174° C., Recrystallization temperature: 136° C. Relative viscosity (0.5% in m-cresol): 1.62 to 1.66.
[0107] Step A3 – Copolyamide, general procedure for the production of lactam-containing polymers, PA6 / 66 / 610 / 616, such as E4 and E5:
[0108] Hexadecanedioic acid (43.53 kg, 51 mol%), adipic acid (3.05 kg, 7 mol%), sebacic acid (9.04 kg, 15 mol%), hexane-1,6-diamine (60% in water, 42.13 kg, 73 mol%) and caprolactam (9.11 kg, 27 mol%) were transferred to an autoclave together with water (3 kg), where the mixture was stirred at 160 to 200° C. for 140 minutes. The mixture was then heated to 290° C. and 20 bar and stirred at 290° C. for 5 hours at a constant pressure of 20 bar. After 2.5 hours, the polymer was cooled to 270° C. and the pressure was reduced to 0.3 bar. The temperature was subsequently reduced to 260° C.
[0109] The polycondensate was then pelletized and dried according to standard procedures.
[0110] Analysis: Melting point: 173.2° C., Recrystallization temperature: 115.7° C. Relative viscosity (0.5% in m-cresol): 1.70 to 1.72.
[0111] Step A4 uses docosane-1,20-dicarboxylic acid to form a copolyamide:
[0112] Docosane-1,20-dicarboxylic acid (100 mol%) and a diamine (100 mol% of hexane-1,6-diamine or decane-1,10-diamine) were combined and heated to 260° C. in an inert atmosphere. After 6 hours, the material was cooled, leaving clear white solids PA620 and PA1020, respectively.
[0113] The polycondensate was then pelletized and dried according to standard procedures.
[0114] analyze:
[0115] PA620: Melting point: 188.9°C, recrystallization temperature: 139.4°C.
[0116] PA1020: Melting point: 169.3°C, recrystallization temperature: 108.7°C.
[0117] Step B1 - Powder produced by grinding:
[0118] The granules obtained from step A were ground into the original ground material at -50°C using a Hosokawa 160C pin mill with addition of liquid nitrogen in reverse operation.
[0119] Subsequently, the raw ground material was separated into a particle size distribution of about 40 μm to 90 μm by ultrasonic sieving using a sieving fabric of corresponding mesh size.
[0120] Analysis: Measured particle size distribution (μm): D10: 30.9, D50: 56.0, D95: 85.7, determined on a Camsizer XT according to ISO 13322-2.
[0121] Step B2 - Powder produced by precipitation:
[0122] In a sealed container, the granules obtained from step A were dissolved in ethanol / butanone (250:1) at an elevated temperature of 130° C. to 150° C. with continuous stirring. After the granules were completely dissolved, the temperature of the mixture was slowly reduced along with the stirring speed to reach 100° C. to 120° C. After this slow cooling process, filtration and vacuum drying were then performed to obtain white fine granules.
[0123] Analysis: Measured particle size distribution (μm): D10: 40.0, D50: 76.9, D95: 149.8, determined on a Camsizer XT according to ISO 13322-2.
[0124] For the powder from step B2: melting point: 174.8°C, recrystallization temperature: 135.6°C
[0125] Step C: SLS molding:
[0126] The powder obtained from step B was printed using an SLS printer SPro60 from 3D Systems (equipped with a CO2 laser) to produce a test body (ISO 527).
[0127] For Examples E1 to E7 according to the invention and Comparative Examples CE1 to CE3, the printer was set up with the parameters given in Table 1 below. Table 2 summarizes the mechanical properties.
[0128] Table 1: Thermal properties of monomer base, powders and SLS parameters of printed samples
[0129]
[0130] *: ground; **: precipitated; ***: filling laser power (W), contour laser power (W), microtome filling scan spacing (mm); ': single scan; ": double scan; nd: not determined. All materials were measured after conditioning at 23 °C, 50% humidity for 40 hours. If not otherwise stated, powders are ground powders.
[0131] Table 2: Mechanical properties of monomer-based, printed examples
[0132]
[0133] *: ground; **: precipitated; nd: not determined. All materials were measured after conditioning at 23°C, 50% humidity for 40 hours. If not otherwise stated, powders are ground powders.
[0134] method:
[0135] The flowability is assessed visually by the filling degree of the parts after recoating: excellent: completely filled, good: some parts have slight defects. The flowability means that a defect-free powder bed is created by the insertion of the next powder layer, so that for example the powder does not clump.
[0136] The relative viscosity of the residual powder was measured in accordance with ISO 307 in m-cresol at a temperature of 20° C. and a concentration of 0.5% by weight.
[0137] The tensile modulus is measured according to ISO 527 at a temperature of 23° C. using an ISO tensile bar (standard: ISO / CD 3167, type A1, 170 mm×20 mm / 10 mm×4 mm) at a pulling speed of 1 mm / min.
[0138] Tensile strength and elongation at break were measured according to ISO 527 at a temperature of 23° C. using an ISO tensile bar (standard: ISO / CD 3167, type A1, 170 mm×20 mm / 10 mm×4 mm) at a tensile speed of 5 mm / min.
[0139] Charpy impact strength was measured according to ISO 179 / *eA at 23° C. on ISO test bars (according to standard: ISO / CD 3167, type B1, 80 mm×10 mm×4 mm).
[0140] Surface quality as well as cracks, warping, curling and part color are visually assessed. Cracking is a crack created in the powder bed that interferes with the powder layering process, which may result in the area below being laser processed several times. Such a situation may only result in cracks in the finished component in the best case, but more likely, the cracks may ruin the entire printing process through oversintering, agglomeration formation or demolding due to scratching effects. Curling refers to deformation of the edges of the component (usually around the edges) during laser processing, for example. Warping, on the other hand, refers to deformation over the entire component, which usually occurs when the laser bed cools down, i.e. only after the laser is applied.
[0141] The total light transmittance was measured and evaluated according to ISO 13468-2:2021 from 380 nm to 780 nm through a film with a layer thickness of 1.0 mm.
[0142] Glass transition temperature (T g )、Melting point (T m ), recrystallization temperature (T rc ): ISO standards 11357-1, 11357-2, 11357-3 (2013); powdered material; Differential scanning calorimetry (DSC) was performed using a DSC 2920 instrument from TA Instruments at a heating rate of 10 K / min and a cooling rate of 5 K / min. Thermograms were analyzed using the Universal Analysis 2000 program from TA Instruments.
[0143] For the purpose of determining the glass transition temperature, the samples were quenched in dry ice after the first heating run. The glass transition temperature (T g The midpoint of the glass transition range (which is reported as the glass transition temperature (T g ))Determined by the "half-height" method.
[0144] For the recrystallization temperature (T rc ), record the value recorded during the cooling phase of the first heating cycle.
[0145] Recycle:
[0146] Polymer B3 was printed again with the recycled powder (remaining part of the bed powder), the parts were split, half was sent for analysis after conditioning and the other half was dyed with a Dyemansion DM60 machine. The results are summarized in Table 3.
[0147] Table 3:
[0148]
[0149] Results and Discussion:
[0150] As can be seen from the evidence in the table, the new powder allows the production of parts with significantly higher translucency than materials according to the prior art. In addition, excellent mechanical properties can be obtained. At the same time, better or at least equivalent flow properties, printing properties (cracking / warping / curling) can be obtained. In addition, the remaining powder from the bath can be used for further processes, so there is less waste material than with materials of the prior art, in which case usually the remaining powder in the bath must be discarded after use.
[0151] Furthermore, it should be noted that the mechanical values refer to conditioned (40 hours, 50% humidity at 23°C) parts that retain good mechanical properties. Possible coloring of the parts with Dyemansion DM60 has a similar effect as the conditioning. In this Dyemansion DM60 process, the parts are colored in a bath at 115°C under pressure for 2.5 hours. The advantage of the printed parts is the increased transmittance, which also allows for better coloring. The trials with Dyemansion DM60 showed that the powder can be recycled, but also showed that the coloring process has no effect on the mechanical properties.
Claims
1. Use of the powder in a layer-by-layer process in which regions of the powder layer are selectively melted, sintered, fused or solidified, preferably by focused or unfocused input electromagnetic energy, The powder comprises or consists of a thermoplastic polyamide powder which comprises aliphatic dicarboxylic acid structural units having 16 to 22 carbon atoms.
2. The use according to claim 1, wherein the aliphatic dicarboxylic acid structural unit having 16 to 22 carbon atoms is selected from the group of linear dicarboxylic acids having a terminal carboxyl group, preferably selected from: hexadecanedioic acid, octadecanedioic acid, docosane-1,20-dicarboxylic acid, or a mixture thereof, wherein preferably the aliphatic dicarboxylic acid structural unit having 16 to 22 carbon atoms is selected from only one of hexadecanedioic acid, octadecanedioic acid or docosane-1,20-dicarboxylic acid.
3. The use according to any one of the preceding claims, wherein the thermoplastic polyamide powder comprises or consists of structural units built up from diamines and dicarboxylic acids, and wherein the molar proportion of the aliphatic dicarboxylic acid structural units having 16 to 22 carbon atoms relative to the total dicarboxylic acids of the polyamide is at least 20%, or at least 40%, or at least 50%, preferably at least 60%, or in the range of 65 to 100%, or in the range of 85 to 100%.
4. The method according to claim 3, wherein the diamine is selected from linear or branched aliphatic, cycloaliphatic or aromatic diamines having 4 to 20 carbon atoms, preferably linear aliphatic diamines having 6 to 12 carbon atoms, and wherein the linear aliphatic diamine is preferably selected from the group of tetramethylenediamine, hexamethylenediamine, octanediamine, nonanediamine, decanediamine, or mixtures thereof, and / or wherein the cycloaliphatic diamine is preferably selected from MACM, PACM, or mixtures thereof, and / or wherein the aromatic diamine is preferably selected from p-xylylenediamine, m-xylylenediamine, or mixtures thereof.
5. The method according to claim 3 , wherein the dicarboxylic acid different from the aliphatic dicarboxylic acid structural unit having 16 to 22 carbon atoms is selected from the group of linear or branched aliphatic, alicyclic or aromatic dicarboxylic acids having 4 to 20 carbon atoms, wherein preferably the linear aliphatic dicarboxylic acid is selected from succinic acid, adipic acid, suberic acid, sebacic acid, dodecanoic acid, or mixtures thereof, and wherein the aromatic dicarboxylic acid is selected from terephthalic acid, isophthalic acid, or mixtures thereof.
6. The use according to any one of the preceding claims, wherein the thermoplastic polyamide powder comprises or consists of structural units built up from a diamine and the aliphatic dicarboxylic acid structural units having 16 to 22 carbon atoms, the thermoplastic polyamide powder being selected from PA616, PA618, PA620, PA1016, PA1018, PA1020, PA1216, PA1218, PA1220, or a mixture thereof.
7. The method according to claim 1, wherein the thermoplastic polyamide powder does not contain lactam structural units. or wherein the thermoplastic polyamide powder further comprises a lactam structural unit, wherein the lactam structural unit has 4 to 20 carbon atoms, preferably 6 to 12 carbon atoms, Or wherein the thermoplastic polyamide powder further comprises lactam structural units, and wherein the molar ratio of the lactam structural units relative to the structural units constructed from diamines and dicarboxylic acids is at most 50%, or at most 40%, or at most 30%, or at most 20%.
8. Use according to any one of the preceding claims, wherein the thermoplastic polyamide powder is selected from PA616, PA1016, PA1016 / 101, PA6 / 66 / 610 / 616, PA620, PA1020, or mixtures thereof.
9. The use according to any one of the preceding claims, wherein the thermoplastic polyamide powder having a melting point measured according to ISO 11357 greater than 160°C, preferably in the range of 165°C to 210°C, and / or having a glass transition temperature of at least 25° C., the glass transition temperature preferably being measured by dynamic mechanical analysis according to ISO 6721-2:2008, and / or is a ground or precipitated polyamide powder, and wherein preferably in the case of a ground powder, the thermoplastic polyamide powder is produced by a cryogenic grinding process, and / or having a relative viscosity in the range of 1.5 to 2.1, preferably in the range of 1.6 to 2.0, preferably measured in m-cresol according to ISO 307 at a temperature of 20° C. and a concentration of 0.5% by weight, and / or having a recrystallization temperature (Tc) in the range of 70°C to 180°C, preferably in the range of 80°C to 170°C, or in the range of 80°C to 160°C, or in the range of 80°C to 150°C, or below 148°C, or below 145°C. rc ), and / or having a sintering window in the range of 5°C to 90°C, preferably in the range of 6°C to 80°C.
10. The use according to any one of the preceding claims, wherein the powder and / or the thermoplastic polyamide powder has an average particle size D50 in the range of 50 to 80 μm, preferably in the range of 50 to 65 μm, more preferably in the range of 50 to 60 μm, the average particle size D50 being preferably measured according to ISO 13322-2, And / or wherein the thermoplastic ground polyamide powder has an MFR value in the range of 6 to 17 g / 10 min, said MFR value being preferably measured according to ISO 1133.
11. The method according to claim 1, wherein the thermoplastic polyamide powder contains no fillers and / or no flame retardant additives and / or no aromatic structural units, or wherein the thermoplastic polyamide powder consists of the polyamide and further additives, the amount of the further additives being not more than 20% by weight or 15% by weight, preferably in the range of 1% to 12% by weight or 5% to 10% by weight, relative to the total weight of the powder, and wherein preferably the additive is one or a combination of: a filler, preferably selected from the group of talc, a filler based on alumina, a glass filler, a metal carbonate, the metal carbonate including calcium carbonate; a flow aid, preferably selected from the group of fumed or precipitated silica, metal salts of long-chain fatty acids, titanium dioxide, salts of Group 1, fumed alumina, the metal salts of long-chain fatty acids including metal stearates; a flame retardant, preferably selected from the group of organic or inorganic monophosphinates / salts or diphosphinates / salts, preferably metal alkylphosphinates / salts, in particular aluminium diethylphosphinate, alone or in combination with a synergist compound, preferably containing nitrogen and / or phosphorus, including melem, melam, melonamine or other melamines or derivatives thereof.
12. A method for preparing a thermoplastic polyamide powder for use according to any of the preceding claims, wherein the thermoplastic polyamide is subjected to a cryogenic grinding process or a precipitation process and subsequently to a particle size screening process, preferably for producing a particle size distribution such that the average particle size D50 is in the range of 50 μm to 80 μm, preferably in the range of 50 μm to 65 μm, more preferably in the range of 50 μm to 60 μm, the average particle size D50 preferably being measured according to ISO 13322-2.
13. A method for printing a three-dimensional product, comprising the following steps: Providing a powder for use as claimed in any one of claims 1 to 11; and selectively solidifying layers of said powder to form said article, preferably using focused or unfocused input electromagnetic energy, wherein preferably said powder is provided in a layer-by-layer process, Preferably, the powder has a particle size D50 measured according to ISO 13322-2 of 50 μm to 80 μm, preferably 50 μm to 65 μm, more preferably 50 μm to 60 μm.
14. An article prepared using the method defined in claim 13.
15. A powder for producing a moulding in a layer-by-layer process in which regions of the powder layers are selectively melted, sintered, fused or solidified, preferably by focused or unfocused input electromagnetic energy, wherein the powder comprises or consists of a thermoplastic polyamide powder comprising aliphatic dicarboxylic acid structural units having 16 to 22 carbon atoms, wherein preferably the powder and / or the thermoplastic polyamide powder has a particle size D50 measured according to ISO 13322-2 of 50 to 80 μm, preferably 50 to 65 μm, more preferably 50 to 60 μm.