High-stability super-capacitor carbon material prepared from water extraction and alcohol precipitation waste and preparation method of high-stability super-capacitor carbon material
Patent Information
- Application Number
- CN202410707601.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-03
- Publication Date
- 2024-10-01
AI Technical Summary
Existing technology is difficult to effectively treat water extraction and alcohol precipitation waste, resulting in environmental pollution and resource waste. Different types of waste require different treatment methods, which increases the difficulty of treatment and may produce new pollutants.
By mixing water extraction and alcohol precipitation waste with chloride, and performing heat treatment to form a supercapacitor carbon material with a multi-level pore structure, non-corrosive sodium chloride is used as a pore template to regulate the pore shape and size of the carbon material to form a highly stable Carbon materials for supercapacitors.
It realizes the resource utilization of waste, reduces environmental pressure, and improves economic benefits. The supercapacitor carbon material formed has excellent electrochemical performance and cycle stability.
Smart Images

Figure CN118723968A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of waste recycling, and particularly relates to a high-stability supercapacitor carbon material prepared by water-extraction and alcohol-precipitation of waste and a preparation method thereof. Background Art
[0002] Water extraction and alcohol precipitation is a common method for obtaining active ingredients from traditional Chinese medicines. It is widely used due to its low cost, easy operation, high solvent safety, and strong impurity removal capabilities. The water extract of water extraction and alcohol precipitation is used for medicinal substances, while the precipitate becomes waste. With the continuous development of traditional Chinese medicine production, the discharge of alcohol precipitation waste has gradually increased.
[0003] In order to solve this problem, many researchers have begun to explore ways to recycle alcohol precipitation waste. One common method is to biodegrade the waste, decomposing the organic matter in the waste into simpler compounds through the action of microorganisms, thereby reducing the impact on the environment. Another method is to recycle the useful components in the waste, such as preparing new drugs or functional compounds by extracting secondary metabolites from the waste.
[0004] In addition to biodegradation and resource utilization, some researchers have also tried to incinerate or pyrolyze alcohol precipitation waste to burn organic matter into carbon dioxide and water vapor, thereby reducing the volume of waste and the emission of organic matter. In addition, there are studies that show that waste can be treated physically and chemically, such as oxidizing and decomposing organic matter through high-temperature pyrolysis or chemical oxidation to reduce its impact on the environment.
[0005] Although there are many ways to treat alcohol precipitation waste, there are still some challenges. First, the composition of waste is complex and diverse, and different types of waste may require different treatment methods, which increases the difficulty of treatment. Second, some treatment methods may produce new pollutants or by-products, causing new negative impacts on the environment. Therefore, further research and improvement of waste treatment technology is needed to achieve resource utilization of waste and reduce the impact on the environment.
[0006] In general, the treatment of alcohol precipitation waste is a complex and challenging issue, and efforts are needed to find more environmentally friendly and sustainable treatment methods.
[0007] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention and should not be regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art. Summary of the invention
[0008] The purpose of the present invention is to provide a method for preparing a high-stability supercapacitor carbon material by water extraction and alcohol precipitation of waste, so as to generate new commercial value for waste recycling and overcome the defects in the above-mentioned prior art.
[0009] To achieve the above object, the present invention provides a method for preparing a high-stability supercapacitor carbon material from water-extraction and alcohol-precipitation waste, comprising a carbonized product formed by mixing chloride with water-extraction and alcohol-precipitation waste of Chinese medicinal materials, wherein the chloride is removed by washing with water. The main components of the water-extraction and alcohol-precipitation waste are starch, pectin, protein, polysaccharide and other water-soluble macromolecular residues.
[0010] We found that the carbon material with a multi-level pore structure and supercapacitor performance formed by mixing water-extraction and alcohol-precipitation waste with chloride and then heat-treating it has higher economic value and can achieve the recycling of resources.
[0011] Preferably, in the above technical solution, the supercapacitor carbon material formed by the carbonized product of the waste of water extraction and alcohol precipitation of traditional Chinese medicine has a multi-level pore structure.
[0012] Preferably, in the above technical solution, the chloride has a melting point of 700°C-850°C, is stable in nature, will not be reduced or oxidized by the waste of water extraction and alcohol precipitation of traditional Chinese medicine, and can be removed by soaking in water or washing at a later stage. Because the oxygen-containing groups in some sugars in the waste are reducing, it needs to be carefully selected.
[0013] Preferably, in the above technical solution, the chloride is sodium chloride or potassium chloride.
[0014] Preferably, in the above technical scheme, the waste of water extraction and alcohol precipitation of Chinese medicinal materials is water extraction and alcohol precipitation of wild chrysanthemum, honeysuckle, heather leaf, mulberry leaf, salvia miltiorrhiza, sophora flavescens, forsythia suspensa, gardenia or other Chinese medicinal materials; the main components of the water extraction and alcohol precipitation are starch, pectin, protein, polysaccharides and other water-soluble macromolecular residues.
[0015] A method for preparing a high-stability supercapacitor carbon material by water extraction and alcohol precipitation of waste, comprising the following steps: S1 dissolves a certain amount of chloride in water to obtain a first solution; S2 The waste of Chinese medicinal materials water extraction and alcohol precipitation is dissolved in the first solution to form a second solution; S3 drying the second solution to obtain a dried first mixture; S4 carbonizes the first mixture at high temperature under the protection of an inert gas to obtain a mixture of supercapacitor carbon and sodium chloride; S5 soaks the mixture obtained in S4 with water, washes, and dries to obtain supercapacitor carbon material; the chloride has a melting point of 700°C-850°C, is stable in nature, will not be reduced or oxidized by the waste of water extraction and alcohol precipitation of traditional Chinese medicine, and can be removed by soaking in water or washing in the later stage.
[0016] Preferred chlorides are sodium chloride and potassium chloride.
[0017] Preferably, in the above technical scheme, the waste of water extraction and alcohol precipitation of Chinese medicinal materials is water extraction and alcohol precipitation of wild chrysanthemum, honeysuckle, heather leaf, mulberry leaf, salvia miltiorrhiza, sophora flavescens, forsythia suspensa, gardenia or other Chinese medicinal materials; the main components of the water extraction and alcohol precipitation are starch, pectin, protein, polysaccharides and other water-soluble macromolecular residues.
[0018] Preferably, in the above technical solution, in step S1, the mass ratio of sodium chloride to water is between 1:56 and 1:3.
[0019] Preferably, in the above technical solution, in step S2, the waste of water extraction and alcohol precipitation of Chinese medicinal materials is slowly added to the first solution under stirring until the second solution is a paste-like and uniformly mixed paste, wherein the mass ratio of chloride to the waste of water extraction and alcohol precipitation is between 1:20 and 1:5.
[0020] Preferably, in the above technical solution, the drying in step S3 is heating drying or freeze drying, the heating drying temperature is 60°C to 80°C, and the freeze drying temperature is -20°C to -80°C.
[0021] Preferably, in the above technical solution, the inert gas used in step S4 is argon.
[0022] Preferably, in the above technical solution, the carbonization process includes two steps: pre-carbonization and carbonization. The pre-carbonization temperature is 200°C, the heating rate is 2°C / min, and the pre-carbonization time is 1.5 h; the carbonization temperature is 800-850°C, the heating rate is 10°C / min, and the carbonization time is 1.5-2 h.
[0023] Compared with the prior art, the present invention has the following beneficial effects: Compared with the traditional disposal method of water extraction and alcohol precipitation waste, the present invention has the following significant advantages: the waste is disposed of as a resource, which reduces environmental pressure and improves economic benefits; compared with the existing biomass preparation of carbon materials, the advantages of the present invention are: (1) the use of non-corrosive sodium chloride as a pore template is more economical and more environmentally friendly; (2) the main component of the water extraction and alcohol precipitation waste is water-soluble macromolecules, and the shape and size of the pores formed after carbonization can be regulated by the template agent. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 is a flow chart of the preparation method of the present invention; Figure 2 This is the SEM image of supercapacitor carbon; Figure 3 is the electrochemical performance diagram of the supercapacitor; Figure 4(a) Carbon materials prepared from water-extracted and alcohol-precipitated wild chrysanthemum, honeysuckle, heather leaf, mulberry leaf, salvia miltiorrhiza, sophora flavescens, forsythia suspensa, and gardenia jasmine at 0.5 A g -1 The specific capacitance at the current density, Figure 4 (b) Activated carbon prepared from water-extracted ethanol precipitations of Gardenia jasminoides and Forsythia suspensa under different annealing conditions at 5 A g -1 Cyclic performance test under current density. DETAILED DESCRIPTION
[0025] The specific embodiments of the present invention are described in detail below, but it should be understood that the protection scope of the present invention is not limited by the specific embodiments.
[0026] Unless explicitly stated otherwise, throughout the specification and claims, the term “comprise” or variations such as “include” or “comprising”, etc., will be understood to include the stated elements or components but not to exclude other elements or components.
[0027] Combination Figure 1 The method for preparing supercapacitor carbon materials by converting water-extracted and alcohol-precipitated waste into supercapacitor carbon materials adopted by the present invention comprises the following steps: S1. Prepare sodium chloride solution, the mass ratio of sodium chloride to water is between 1:56-1:3; S2. The water-extracted alcohol-precipitated waste was added to the sodium chloride solution obtained in S1 and stirred to obtain a paste mixture of water-extracted alcohol-precipitated waste and sodium chloride; S3 S3 obtained high concentration uniform mixed solution was dried, the drying method is oven drying, the temperature is 60 ℃, or freeze drying, to obtain a dry mixture of water-extracted alcohol-precipitated waste and sodium chloride; S4. The mixture obtained in S3 was pre-carbonized in an inert atmosphere at a heating rate of 2°C / min, a temperature of 200°C, and a time of 1.5 h; S5. The product obtained in S4 is further carbonized in an inert gas at a heating rate of 10°C / min, a carbonization temperature of 800-850°C, a carbonization time of 1.5-2 h, and naturally cooled to room temperature to obtain a mixture of supercapacitor carbon and sodium chloride; S6. Wash the mixture obtained in S5 with water, and freeze-dry the obtained solid product to obtain supercapacitor carbon.
[0028] The present invention is further described in detail below in conjunction with embodiments and drawings: Example
[0029] S1. Weigh 0.3 g of sodium chloride and dissolve it in 5.6 g of water to obtain a sodium chloride aqueous solution; S2. Weigh 2.0 g of wild chrysanthemum water-extracted alcohol-precipitated waste, disperse it in the sodium chloride aqueous solution obtained in S1, and stir to obtain a paste mixture; S3. The paste mixture obtained in S2 was frozen and dried in a freeze dryer to obtain a dry mixture of wild chrysanthemum water-extracted alcohol-precipitated waste and sodium chloride; S4. The dried mixture obtained in S3 was heated from room temperature to 200°C at a heating rate of 2°C / min under argon protection and maintained for 1.5 h; S5. The temperature of S4 was raised to 850°C at 10°C / min and maintained for 1.5 h. After the program was completed, it was naturally cooled to room temperature to obtain a mixture of supercapacitor carbon and sodium chloride; S6. The mixture obtained in S5 is washed with water for 6 times to remove sodium chloride to obtain supercapacitor carbon.
[0030] from Figure 2 It can be seen from the SEM image that the obtained supercapacitor carbon has a rich pore structure.
[0031] from Figure 3 It can be seen from the CV graph of a that the obtained supercapacitor carbon has pseudocapacitive characteristics. Figure 3 From the EIS diagram of b, it can be seen that the obtained capacitor carbon has a smaller intrinsic resistance and diffusion resistance. Figure 3 c It can be seen that the obtained supercapacitor carbon has good charge and discharge performance. Example
[0032] S1. Weigh 0.1 g of sodium chloride and dissolve it in 5.6 g of water to obtain a sodium chloride aqueous solution; S2. Weigh 2.0 g of wild chrysanthemum water-extracted alcohol-precipitated waste, disperse it in the sodium chloride aqueous solution obtained in S1, and stir to obtain a paste mixture; S3. The paste mixture obtained in S2 was frozen and dried in a freeze dryer to obtain a dry mixture of wild chrysanthemum water-extracted alcohol-precipitated waste and sodium chloride; S4. The dried mixture obtained in S3 was heated from room temperature to 200°C at a heating rate of 2°C / min under argon protection and maintained for 1.5 h; S5. The temperature of S4 was raised to 850°C at 10°C / min and maintained for 1.5 h. After the program was completed, it was naturally cooled to room temperature to obtain a mixture of supercapacitor carbon and sodium chloride; S6. The mixture obtained in S5 is washed with water for 6 times to remove sodium chloride to obtain supercapacitor carbon. Example
[0034] S1. Weigh 0.2 g of sodium chloride and dissolve it in 5.6 g of water to obtain a sodium chloride aqueous solution; S2. Weigh 2.0 g of wild chrysanthemum water-extracted alcohol-precipitated waste, disperse it in the sodium chloride aqueous solution obtained in S1, and stir to obtain a paste mixture; S3. The paste mixture obtained in S2 was frozen and dried in a freeze dryer to obtain a dry mixture of wild chrysanthemum water-extracted alcohol-precipitated waste and sodium chloride; S4. The dried mixture obtained in S3 was heated from room temperature to 200°C at a heating rate of 2°C / min under argon protection and maintained for 1.5 h; S5. The temperature of S4 was raised to 850°C at 10°C / min and maintained for 1.5 h. After the program was completed, it was naturally cooled to room temperature to obtain a mixture of supercapacitor carbon and sodium chloride; S6. The mixture obtained in S5 is washed with water for 6 times to remove sodium chloride to obtain supercapacitor carbon. Example
[0035] S1. Weigh 0.4 g of sodium chloride and dissolve it in 5.6 g of water to obtain a sodium chloride aqueous solution; S2. Weigh 2.0 g of wild chrysanthemum water-extracted alcohol-precipitated waste, disperse it in the sodium chloride aqueous solution obtained in S1, and stir to obtain a paste mixture; S3. The paste mixture obtained in S2 was frozen and dried in a freeze dryer to obtain a dry mixture of wild chrysanthemum water-extracted alcohol-precipitated waste and sodium chloride; S4. The dried mixture obtained in S3 was heated from room temperature to 200°C at a heating rate of 2°C / min under argon protection and maintained for 1.5 h; S5. The temperature of S4 was raised to 850°C at 10°C / min and maintained for 1.5 h. After the program was completed, it was naturally cooled to room temperature to obtain a mixture of supercapacitor carbon and sodium chloride; S6. The mixture obtained in S5 is washed with water for 6 times to remove sodium chloride to obtain supercapacitor carbon. Example
[0036] S1. Weigh 0.4 g of sodium chloride and dissolve it in 1.2 g of water to obtain a sodium chloride aqueous solution; S2. Weigh 2.0 g of wild chrysanthemum water-extracted alcohol-precipitated waste, disperse it in the sodium chloride aqueous solution obtained in S1, and stir to obtain a paste mixture; S3. The paste mixture obtained in S2 was frozen and dried in a freeze dryer to obtain a dry mixture of wild chrysanthemum water-extracted alcohol-precipitated waste and sodium chloride; S4. The dried mixture obtained in S3 was heated from room temperature to 200°C at a heating rate of 2°C / min under argon protection and maintained for 1.5 h; S5. The temperature of S4 was raised to 850°C at 10°C / min and maintained for 1.5 h. After the program was completed, it was naturally cooled to room temperature to obtain a mixture of supercapacitor carbon and sodium chloride; S6. The mixture obtained in S5 is washed with water for 6 times to remove sodium chloride to obtain supercapacitor carbon. Example
[0037] S1. Weigh 0.4 g of sodium chloride and dissolve it in 1.2 g of water to obtain a sodium chloride aqueous solution; S2. Weigh 2.0 g of the waste of honeysuckle water extraction and alcohol precipitation, disperse it in the sodium chloride aqueous solution obtained in S1, and stir to obtain a paste mixture; S3. The paste mixture obtained in S2 was frozen and dried in a freeze dryer to obtain a dry mixture of wild chrysanthemum water-extracted alcohol-precipitated waste and sodium chloride; S4. The dried mixture obtained in S3 was heated from room temperature to 200°C at a heating rate of 2°C / min under argon protection and maintained for 1.5 h; S5. The temperature of S4 was raised to 850°C at 10°C / min and maintained for 1.5 h. After the program was completed, it was naturally cooled to room temperature to obtain a mixture of supercapacitor carbon and sodium chloride; S6. The mixture obtained in S5 is washed with water for 6 times to remove sodium chloride to obtain supercapacitor carbon. Example
[0038] S1. Weigh 0.4 g of sodium chloride and dissolve it in 1.2 g of water to obtain a sodium chloride aqueous solution; S2. Weigh 2.0 g of the waste of Gardenia water extraction and alcohol precipitation, disperse it in the sodium chloride aqueous solution obtained in S1, and stir to obtain a paste mixture; S3. The paste mixture obtained in S2 was frozen and dried in a freeze dryer to obtain a dry mixture of wild chrysanthemum water-extracted alcohol-precipitated waste and sodium chloride; S4. The dried mixture obtained in S3 was heated from room temperature to 200°C at a heating rate of 2°C / min under argon protection and maintained for 1.5 h; S5. The temperature of S4 was raised to 850°C at 10°C / min and maintained for 1.5 h. After the program was completed, it was naturally cooled to room temperature to obtain a mixture of supercapacitor carbon and sodium chloride; S6. The mixture obtained in S5 is washed with water for 6 times to remove sodium chloride to obtain supercapacitor carbon. Example
[0039] S1. Weigh 0.4 g of sodium chloride and dissolve it in 1.2 g of water to obtain a sodium chloride aqueous solution; S2. Weigh 2.0 g of the waste of water extraction and alcohol precipitation of Forsythia suspensa, disperse it in the sodium chloride aqueous solution obtained in S1, and stir to obtain a paste mixture; S3. The paste mixture obtained in S2 was frozen and dried in a freeze dryer to obtain a dry mixture of wild chrysanthemum water-extracted alcohol-precipitated waste and sodium chloride; S4. The dried mixture obtained in S3 was heated from room temperature to 200°C at a heating rate of 2°C / min under argon protection and maintained for 1.5 h; S5. The temperature of S4 was raised to 850°C at 10°C / min and maintained for 1.5 h. After the program was completed, it was naturally cooled to room temperature to obtain a mixture of supercapacitor carbon and sodium chloride; S6. The mixture obtained in S5 is washed with water for 6 times to remove sodium chloride to obtain supercapacitor carbon.
[0040] Figure 3 The "salt melting annealing" in a is the specific capacitance of the carbon material prepared by water extraction and alcohol precipitation of wild chrysanthemum, honeysuckle, heather leaf, mulberry leaf, salvia miltiorrhiza, sophora flavescens, forsythia suspensa, and gardenia under the conditions of Example 8, and the "direct annealing" is the carbon material prepared by the same method as Example 8 but excluding the step of adding sodium chloride. It can be seen that the carbon material prepared by the salt melting method with the addition of sodium chloride has a higher specific capacitance.
[0041] Figure 3 b is a cyclic stability test of carbon materials prepared from wastes of water extraction and alcohol precipitation of Forsythia suspensa and Gardenia jasminoides. In the figure, Forsythia suspensa N and Gardenia jasminoides N are carbon materials obtained by the method of Example 8. Forsythia suspensa and Gardenia jasminoides are carbon materials prepared by the same method as Example 8, but without the step of adding sodium chloride. It can be seen from the figure that the cyclic stability of the carbon materials obtained by the method of Example 8 is significantly improved. Example
[0042] S1. Weigh 0.4 g of sodium chloride and dissolve it in 1.2 g of water to obtain a sodium chloride aqueous solution; S2. Weigh 2.0 g of the waste of water extraction and alcohol precipitation of Salvia miltiorrhiza, disperse it in the sodium chloride aqueous solution obtained in S1, and stir to obtain a paste mixture; S3. The paste mixture obtained in S2 was frozen and dried in a freeze dryer to obtain a dry mixture of wild chrysanthemum water-extracted alcohol-precipitated waste and sodium chloride; S4. The dried mixture obtained in S3 was heated from room temperature to 200°C at a heating rate of 2°C / min under argon protection and maintained for 1.5 h; S5. The temperature of S4 was raised to 850°C at 10°C / min and maintained for 1.5 h. After the program was completed, it was naturally cooled to room temperature to obtain a mixture of supercapacitor carbon and sodium chloride; S6. The mixture obtained in S5 is washed with water for 6 times to remove sodium chloride to obtain supercapacitor carbon.
[0043] S1. Weigh 0.4 g of sodium chloride and dissolve it in 1.2 g of water to obtain a sodium chloride aqueous solution; S2. Weigh 2.0 g of the waste of Sophora flavescens water extraction and alcohol precipitation, disperse it in the sodium chloride aqueous solution obtained in S1, and stir to obtain a paste mixture; S3. The paste mixture obtained in S2 was frozen and dried in a freeze dryer to obtain a dry mixture of wild chrysanthemum water-extracted alcohol-precipitated waste and sodium chloride; S4. The dried mixture obtained in S3 was heated from room temperature to 200°C at a heating rate of 2°C / min under argon protection and maintained for 1.5 h; S5. The temperature of S4 was raised to 850°C at 10°C / min and maintained for 1.5 h. After the program was completed, it was naturally cooled to room temperature to obtain a mixture of supercapacitor carbon and sodium chloride; S6. The mixture obtained in S5 is washed with water for 6 times to remove sodium chloride to obtain supercapacitor carbon.
[0044] S1. Weigh 0.4 g of sodium chloride and dissolve it in 1.2 g of water to obtain a sodium chloride aqueous solution; S2. Weigh 2.0 g of mulberry leaf water-extracted alcohol-precipitated waste, disperse it in the sodium chloride aqueous solution obtained in S1, and stir to obtain a paste mixture; S3. The paste mixture obtained in S2 was frozen and dried in a freeze dryer to obtain a dry mixture of wild chrysanthemum water-extracted alcohol-precipitated waste and sodium chloride; S4. The dried mixture obtained in S3 was heated from room temperature to 200°C at a heating rate of 2°C / min under argon protection and maintained for 1.5 h; S5. The temperature of S4 was raised to 850°C at 10°C / min and maintained for 1.5 h. After the program was completed, it was naturally cooled to room temperature to obtain a mixture of supercapacitor carbon and sodium chloride; S6. The mixture obtained in S5 is washed with water for 6 times to remove sodium chloride to obtain supercapacitor carbon.
[0045] S1. Weigh 0.4 g of sodium chloride and dissolve it in 1.2 g of water to obtain a sodium chloride aqueous solution; S2. Weigh 2.0 g of the waste of water-extracted alcohol precipitation of Photinia fraseri, disperse it in the aqueous sodium chloride solution obtained in S1, and stir to obtain a paste mixture; S3. The paste mixture obtained in S2 was frozen and dried in a freeze dryer to obtain a dry mixture of wild chrysanthemum water-extracted alcohol-precipitated waste and sodium chloride; S4. The dried mixture obtained in S3 was heated from room temperature to 200°C at a heating rate of 2°C / min under argon protection and maintained for 1.5 h; S5. The temperature of S4 was raised to 850°C at 10°C / min and maintained for 1.5 h. After the program was completed, it was naturally cooled to room temperature to obtain a mixture of supercapacitor carbon and sodium chloride; S6. The mixture obtained in S5 is washed with water for 6 times to remove sodium chloride to obtain supercapacitor carbon.
[0046] S1. Weigh 2 g of sodium chloride and dissolve it in 5 g of water to obtain a sodium chloride aqueous solution; S2. Weigh 20 g of the waste of water extraction and alcohol precipitation of Forsythia suspensa, disperse it in the sodium chloride aqueous solution obtained in S1, and stir to obtain a paste mixture; S3. The paste mixture obtained in S2 was frozen and dried in a freeze dryer to obtain a dry mixture of wild chrysanthemum water-extracted alcohol-precipitated waste and sodium chloride; S4. The dried mixture obtained in S3 was heated from room temperature to 200°C at a heating rate of 2°C / min under argon protection and maintained for 1.5 h; S5. The temperature of S4 was raised to 850°C at a rate of 10°C / min and maintained for 2 h. After the program was completed, it was naturally cooled to room temperature to obtain a mixture of supercapacitor carbon and sodium chloride; S6. The mixture obtained in S5 is washed with water for 6 times to remove sodium chloride to obtain supercapacitor carbon.
[0047] The foregoing description of specific exemplary embodiments of the present invention is for the purpose of illustration and demonstration. These descriptions are not intended to limit the present invention to the precise form disclosed, and it is clear that many changes and variations can be made based on the above teachings. The purpose of selecting and describing the exemplary embodiments is to explain the specific principles of the present invention and its practical application, so that those skilled in the art can realize and utilize various different exemplary embodiments of the present invention and various different selections and changes. The scope of the present invention is intended to be limited by the claims and their equivalents.
Claims
1. A method for preparing high-stability supercapacitor carbon materials by water extraction and alcohol precipitation of waste. It is characterized in that It includes carbonized products formed by mixing chloride with wastes from water extraction and alcohol precipitation of traditional Chinese medicine, wherein the chloride is removed by water washing.
2. The method for preparing high-stability supercapacitor carbon material from water-extraction and alcohol-precipitation waste according to claim 1, Features: The carbonized product of the waste from water extraction and alcohol precipitation of Chinese medicinal materials has a multi-level pore structure.
3. The method for preparing high-stability supercapacitor carbon material from water-extraction and alcohol-precipitation waste according to claim 1, Features: Chloride has a melting point of 700°C-850°C, is stable in nature, will not be reduced or oxidized by waste products from water extraction and alcohol precipitation of Chinese medicinal materials, and can be removed by soaking in water or washing in the later stage.
4. The method for preparing high-stability supercapacitor carbon material from waste water extraction and alcohol precipitation according to claim 1 or 3, Features: The chloride is sodium chloride or potassium chloride.
5. The method for preparing high-stability supercapacitor carbon material from water-extraction and alcohol-precipitation waste according to claim 1, Features: The Chinese medicinal material water extraction and alcohol precipitation waste is water extraction and alcohol precipitation of wild chrysanthemum, honeysuckle, heather leaf, mulberry leaf, salvia miltiorrhiza, sophora flavescens, forsythia suspensa, gardenia or other Chinese medicinal materials; the main components of the water extraction and alcohol precipitation are starch, pectin, protein, polysaccharide and other water-soluble macromolecular residues.
6. A method for preparing supercapacitor carbon materials by water extraction and alcohol precipitation of waste, It is characterized in that The following steps are involved: S1, dissolving a certain amount of chloride in water to obtain a first solution; S2, dissolving the waste of Chinese medicinal materials water extraction and alcohol precipitation into the first solution to form a second solution; S3, drying the second solution to obtain a dried first mixture; S4, carbonizing the first mixture at high temperature under the protection of an inert gas to obtain a mixture of supercapacitor carbon and sodium chloride; S5, soaking the mixture obtained in S4 in water, washing, and drying to obtain supercapacitor carbon material; the chloride has a melting point of 700°C-850°C, is stable in nature, will not be reduced or oxidized by the waste of water extraction and alcohol precipitation of traditional Chinese medicine, and can be removed by soaking in water or washing in the later stage.
7. The method for preparing supercapacitor carbon material by water extraction and alcohol precipitation of waste according to claim 6, It is characterized in that Chlorides are sodium chloride and potassium chloride.
8. The method for preparing supercapacitor carbon material by water extraction and alcohol precipitation of waste according to claim 6, It is characterized in that The waste products of water extraction and alcohol precipitation of Chinese medicinal materials are water extraction and alcohol precipitation of wild chrysanthemum, honeysuckle, heather leaf, mulberry leaf, salvia miltiorrhiza, sophora flavescens, forsythia suspensa, gardenia or other Chinese medicinal materials; the main components of the water extraction and alcohol precipitation are starch, pectin, protein, polysaccharide and other water-soluble macromolecular residues.
9. The method for preparing supercapacitor carbon material from water extraction and alcohol precipitation waste according to claim 6, It is characterized in that In step S1, the mass ratio of sodium chloride to water is between 1:56 and 1:
3.
10. The method for preparing supercapacitor carbon material by water extraction and alcohol precipitation of waste according to claim 6, It is characterized in that In step S2, the waste of water extraction and alcohol precipitation of Chinese medicinal materials is slowly added to the first solution under stirring until the second solution is a paste-like and uniformly mixed paste, wherein the mass ratio of chloride to the waste of water extraction and alcohol precipitation is between 1:20 and 1:
5.
11. The method for preparing supercapacitor carbon material by water extraction and alcohol precipitation of waste according to claim 6, It is characterized in that In step S3, the drying is heating drying or freeze drying, the heating drying temperature is 60°C to 80°C, and the freeze drying temperature is -20°C to -80°C.
12. The method for preparing supercapacitor carbon material from wastes extracted with water and precipitated with alcohol according to claim 6, It is characterized in that In step S4, the inert gas used is argon.
13. The method for preparing supercapacitor carbon material by water extraction and alcohol precipitation of waste according to claim 6, It is characterized in that The carbonization process includes two steps: pre-carbonization and carbonization. The pre-carbonization temperature is 200°C, the heating rate is 2°C / min, and the pre-carbonization time is 1.5 h; the carbonization temperature is 800-850°C, the heating rate is 10°C / min, and the carbonization time is 1.5-2 h.
Citation Information
Patent Citations
Carbon quantum point as well as preparation method, membrane material with quantum point and preparation method and application thereof
CN109913211A
Preparation method and application of high-rate-performance bamboo-based hard carbon negative electrode material
CN117623277A