Photosensitive prepolymer, photosensitive resin composition and application thereof

By designing polymer polyols, alicyclic diisocyanates, chain extenders and photosensitive prepolymers containing hydroxyl acrylates, the problem of difficulty in balancing the aesthetics and mechanical properties of orthodontic materials is solved, achieving shape memory function and safety. The improvement of environmental protection increases the correction power and user comfort.

CN118725249APending Publication Date: 2024-10-01AIDITE (QINHUANGDAO) TECH CO LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202410920044.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

It is difficult to balance the aesthetics and mechanical properties of existing orthodontic materials, and the shape memory materials are not degradable, safe and environmentally friendly, resulting in insufficient correction power and limited application.

Method used

The photosensitive prepolymer is designed using raw materials such as polymer polyol, alicyclic diisocyanate, chain extender and hydroxyl-containing acrylate, and is compounded with each other to form a photosensitive resin composition with thermally induced shape memory characteristics, which is suitable for 3D printing technology. Provide excellent mechanical properties and safety and environmental protection.

Benefits of technology

It has improved the shape memory function, safety and environmental protection and mechanical properties of orthodontic products, increased the correction force, is suitable for 3D printing materials, and provides excellent correction effects and user comfort.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_10
    Figure SMS_10
  • Figure SMS_11
    Figure SMS_11
  • Figure SMS_12
    Figure SMS_12
Patent Text Reader

Abstract

The invention provides a photosensitive prepolymer, a photosensitive resin composition and application thereof. The photosensitive prepolymer is prepared from the following raw materials: a combination of polymer polyol, alicyclic diisocyanate, a chain extender and hydroxyl-containing acrylate, the chain extender comprises dihydric alcohol containing an aliphatic heterocyclic structure. Through the design and mutual compounding of the preparation raw materials, the photosensitive prepolymer has the characteristic of thermally induced shape memory, is biodegradable, safe and environment-friendly, has proper viscosity, can be used for preparing a photosensitive resin composition suitable for 3D printing, obtains a safe and degradable 3D printing material with a shape memory function, can be used as an oral support, and can be used for preparing the 3D printing material. The material has excellent mechanical properties, can increase the correction force, can change and recover the shape under the temperature change, provides an excellent correction effect, and improves the comfort level of a user. The photosensitive prepolymer and the photosensitive resin composition can provide various customized dental products, and have wide application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of polymer materials, specifically to the technical field of 3D printing materials and oral materials, and in particular relates to a photosensitive prepolymer, a photosensitive resin composition and applications thereof. Background Art

[0002] With the continuous improvement of living standards, people are paying more and more attention to orthodontics. The most widely used orthodontic treatment method is bracket fixation, which is to fix brackets on teeth and use the elasticity of orthodontic wires and rubber bands to move teeth so that the teeth are gradually aligned; commonly used fixing devices are usually made of metal and are easy to be noticed.

[0003] In order to solve the problem that metal brackets are easily noticed during treatment, the transparent correction method was developed. That is, taking advantage of the fact that teeth move when stressed, the manufactured transparent dental correction devices are fitted to the teeth, so that the teeth are stressed and gradually change to the desired neat state. This type of correction frame is mainly made of plastic, does not contain metal, and is almost transparent in color. It is not easy to attract attention from the outside, which is very useful for the daily social life of orthodontic patients. At the same time, this type of device is thin and comfortable to wear. Patients can put on and take off the transparent orthodontic device as needed. For example, they can be temporarily removed from the mouth when eating or brushing their teeth, which significantly reduces discomfort in daily life. Transparent orthodontic devices provide great convenience for many people who want to receive orthodontic treatment, and have been one of the hot topics in the field of oral medicine in recent years.

[0004] In order to manufacture the above-mentioned transparent orthodontic device, it is necessary to scan the patient's teeth, program to simulate tooth movement and make a model of the patient's dentition, and then hot-press the plate-shaped transparent polymer composite resin to manufacture the transparent orthodontic device for each planned tooth movement stage. Unlike orthodontic devices with fixed brackets, this type of transparent orthodontic treatment requires the use of hard materials to guide tooth arrangement in order to ensure aesthetics, which can easily cause pain to patients. In addition, when moving teeth, if the fit is not good, resulting in the incorrect sitting position of the transparent orthodontic device, it will be difficult to move the teeth according to the patient's wishes, and it may even tilt unintentionally; if the tooth tilt continues, it may cause a collision with the adjacent tooth roots, making the originally manufactured transparent orthodontic device no longer suitable, and then the transparent orthodontic correction device needs to be remanufactured, which will ultimately increase costs and increase the orthodontic treatment cycle.

[0005] In order to improve the orthodontic effect, the industry has proposed a solution of attaching additional accessories to the surface of transparent orthodontic devices. However, when this solution attaches multiple accessories to the teeth, the installation and removal of the entire transparent orthodontic device is more difficult. At the same time, the installation and removal process of the accessories may also cause deformation, making the attachments more likely to fall off, increasing the difficulty of orthodontic treatment.

[0006] In recent years, researchers have applied shape memory materials to orthodontic technology. For example, CN114848178A discloses a method for preparing a 3D printed shape memory dental mold, comprising the following steps: (1) providing a photosensitive 3D printed shape memory material, comprising 40-70 parts of a shape memory photosensitive polymer, 10-30 parts of an active diluent, 5-20 parts of a cross-linking agent, and 1-3 parts of a photoinitiator; wherein the shape memory photosensitive polymer is one or more of epoxy resin, polyurethane, polyimide, and polylactic acid; (2) determining the correction parameters of the orthodontic appliance according to the patient's oral data, and constructing a three-dimensional model data of the orthodontic appliance dental mold; (3) performing 3D printing on the photosensitive 3D printed shape memory material according to the three-dimensional model data of the orthodontic appliance dental mold to obtain a 3D printed shape memory dental mold. CN115537062A discloses a 3D printing ink material and a bracketless invisible orthodontic appliance with shape memory function. The 3D printing ink material comprises the following components: 39-49% photosensitive polymer, 18-24% thermosensitive polymer, 7-10% active diluent, 14-24% functional monomer, 0.45-1% photoinitiator, 0.04-0.1% inhibitor, and 4.9-5.51% curing agent; wherein the photosensitive polymer is one or more of epoxy vinyl ester resin, polyethylene, ethylene-vinyl acetate copolymer, and polyimide, and the thermosensitive polymer is bisphenol A epoxy resin.

[0007] The materials used to manufacture transparent orthodontic devices, while meeting the orthodontic treatment efficacy, usually need to meet the following performance requirements: on the one hand, they are suitable for 3D printing technology, and can use the convenient customization of 3D printing to quickly formulate treatment plans to respond to patients; on the other hand, they can introduce shape memory, anti-staining, and degradable properties into the materials, so that the manufactured orthodontic products are beautiful, easy to disassemble, safe and environmentally friendly when used. Although shape memory materials have been explored in orthodontic devices, there are obvious deficiencies in the degradability and safety and environmental protection of the materials, and it is difficult to take into account both shape memory performance and mechanical properties at the same time, and the correction force is poor, which limits its application in oral / dental materials. Therefore, the development of shape memory materials that are degradable, safe and environmentally friendly, suitable for 3D printing, and have excellent mechanical properties is an urgent problem to be solved in this field. Summary of the invention

[0008] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a photosensitive prepolymer, a photosensitive resin composition and applications thereof. By designing and compounding the raw materials, the photosensitive prepolymer has the characteristics of being degradable and having shape memory, is safe and environmentally friendly, and can be used to prepare a photosensitive resin composition suitable for 3D printing. The photosensitive prepolymer has excellent mechanical properties, can increase the corrective force, and has broad application prospects in oral and dental materials.

[0009] To achieve this object, the present invention adopts the following technical solutions:

[0010] In a first aspect, the present invention provides a photosensitive prepolymer, wherein the raw materials for preparing the photosensitive prepolymer include a combination of a polymer polyol, an alicyclic diisocyanate, a chain extender and a hydroxyl-containing acrylate; the chain extender includes a diol containing an alicyclic heterocyclic structure.

[0011] The photosensitive prepolymer provided by the present invention is obtained by reacting a polymer polyol, an alicyclic diisocyanate, a chain extender and a hydroxyl-containing acrylate; wherein the polymer polyol constructs a polymer soft segment, and the alicyclic diisocyanate and the chain extender participate in constructing a polymer hard segment. At the same time, the introduction of the chain extender can regulate the glass transition temperature and increase the response temperature of the shape memory, so that the photosensitive prepolymer can match the requirements of the shape memory change temperature when the tooth orthodontic product is used; and then by introducing a hydroxyl-containing acrylate for end-capping, the photosensitive prepolymer contains a reactive double bond group, which can meet the needs of light curing and 3D printing.

[0012] Specifically, the photosensitive prepolymer comprises carbamate (obtained by the reaction of alicyclic diisocyanate, polymer polyol and chain extender) and acrylate structure as the main chain, the photosensitive group (hydroxyl-containing acrylate) is bonded to the carbamate structure, and comprises a soft segment (polymer polyol) and a hard segment (chain extender reacts with alicyclic diisocyanate); the soft segment structure helps the photosensitive prepolymer to show flexibility, and the hard segment gives it strength and heat resistance. The hard carbon skeleton in the photosensitive prepolymer gives the material excellent physical properties such as thermal properties, strength, elastic modulus and tensile elongation, and the soft carbon skeleton allows the material to change shape by external force after heating. At the same time, the photosensitive prepolymer forms a specific segment structure based on the design of the raw materials for preparation, and there are two incompatible phases in the segment: a fixed phase that maintains the shape of the molded product and a transition phase that undergoes a reversible change from soft to hard with temperature; the fixed phase will restore the product to its original shape under the action of the recovery stress, thereby achieving shape memory.

[0013] Furthermore, the present invention introduces alicyclic diisocyanate and diol containing alicyclic heterocyclic structure as chain extenders to construct the hard segment. The two are compounded with each other. On the one hand, the photosensitive prepolymer and the photosensitive resin composition containing the same have excellent mechanical properties. On the other hand, compared with aromatic diisocyanates, the alicyclic structure has better stability and is not prone to yellowing. At the same time, it also avoids material degradation to produce aromatic diamine substances that are carcinogenic to the human body. At the same time, the diol containing alicyclic heterocyclic structure is safe and biodegradable, and can regulate (improve) the shape memory response temperature of the photosensitive prepolymer.

[0014] In summary, the present invention designs and mutually compounded raw materials such as polymer polyols, alicyclic diisocyanates, chain extenders, and hydroxyl-containing acrylates, so that the photosensitive prepolymer has the characteristics of thermal shape memory, and its shape memory response temperature can meet the requirements of shape memory change temperature when used in orthodontic products; at the same time, the photosensitive prepolymer is biodegradable, safe and environmentally friendly, and has an appropriate viscosity, which can maintain a viscosity suitable for 3D printing and exhibit physical properties that can be used as dental / oral materials. The photosensitive resin composition suitable for 3D printing can obtain a 3D printing material with shape memory function, safety and degradability. As an oral support, it has excellent mechanical properties, can effectively increase the correction force, and can change and restore the shape under temperature changes, providing excellent correction effects and improving user comfort.

[0015] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. Through the following preferred technical solutions, the objectives and beneficial effects of the present invention can be better achieved and realized.

[0016] Preferably, the polymer polyol comprises a degradable polymer diol.

[0017] Preferably, the polymer polyol comprises polyester diol and / or polyether diol.

[0018] Preferably, the polyester diol includes any one of polycaprolactone diol, polybutylene carbonate, polyhexylene carbonate, polybutylene succinate, polyhexylene succinate, polybutylene adipate, and polyhexylene adipate, or a combination of at least two thereof;

[0019] Preferably, the polyether diol comprises polypropylene glycol and / or polytetramethylene glycol.

[0020] As a preferred technical solution of the present invention, the polymer polyol adopts a degradable polymer diol, including polyester diol and / or polyether diol, further preferably polyester diol, and further preferably polycaprolactone diol and / or polycarbonate diol, which provide a polymer soft segment to make the photosensitive prepolymer biodegradable, while regulating the polymer chain segment structure and shape memory properties to obtain an ideal shape memory function.

[0021] Preferably, the number average molecular weight of the polymer polyol is 500-5000, for example, it can be 800, 1000, 1200, 1500, 1800, 2000, 2200, 2500, 2800, 3000, 3200, 3500, 3800, 4000, 4200, 4500 or 4800, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0022] Preferably, the hydroxyl value of the polymer polyol is 20-220 mg KOH / g, for example, it can be 30 mg KOH / g, 40 mg KOH / g, 50 mg KOH / g, 60 mg KOH / g, 80 mg KOH / g, 100 mg KOH / g, 120 mg KOH / g, 150 mg KOH / g, 180 mg KOH / g, 200 mg KOH / g or 210 mg KOH / g, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0023] In the present invention, the "alicyclic diisocyanate" refers to a class of compounds containing an alicyclic structure and two NCO groups; the alicyclic structure preferably contains 4-20 (e.g., 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 18, etc.) ring carbon atoms, and the alicyclic structure includes a single ring, a bridged ring, or a condensed ring. Of course, the molecular structure of the alicyclic diisocyanate may also contain an optional chain alkyl group.

[0024] Preferably, the alicyclic diisocyanate includes any one or a combination of at least two of 1,3-cyclohexane diisocyanate, 1,4-cyclohexane diisocyanate, 1,3-diisocyanate-2-methylcyclohexane, 2,4-diisocyanate-1-methylcyclohexane, isophorone diisocyanate (IPDI), 1,4-cyclohexane dimethyl diisocyanate, 4,4'-dicyclohexylmethane diisocyanate (HMDI), 1,5-decahydronaphthalene diisocyanate, and norbornane dimethylene diisocyanate.

[0025] As a preferred technical solution of the present invention, the chain extender is a diol containing a fatty heterocyclic structure, preferably a bio-based small molecule diol. On the one hand, it can participate in the construction of the polymer hard segment, regulate the glass transition temperature of the photosensitive prepolymer, and increase the response temperature of the shape memory. On the other hand, the chain extender is biodegradable and can further enhance the biodegradability of the photosensitive prepolymer.

[0026] Preferably, the chain extender comprises a diol containing a tetrahydrofuran structure, more preferably 2,5-dihydroxymethyltetrahydrofuran Isosorbide Isomanitol Isoidol Anhydroerythritol Any one or a combination of at least two of the following.

[0027] Based on the consideration of industrialization and large-scale low-cost availability, the chain extender is further preferably 2,5-dihydroxymethyltetrahydrofuran and / or isomannide.

[0028] As a preferred technical solution of the present invention, the chain extender (containing aliphatic heterocyclic structure, bio-based small molecule diol) can be converted from monosaccharides, such as isosorbide, isomannide, and isoelditol can be converted from hexose dehydration, anhydroerythritol can be converted from erythritol, and 2,5-dihydroxymethyltetrahydrofuran can be converted from hexose dicarboxylic acid dehydration to 2,5-furan dicarboxylic acid, and then hydrogenated to obtain the product.

[0029] Preferably, the hydroxyl-containing acrylate includes any one of 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, 3-hydroxypropyl acrylate, 4-hydroxybutyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, 3-hydroxypropyl methacrylate, and 4-hydroxybutyl methacrylate, or a combination of at least two thereof.

[0030] Preferably, the total molar number of hydroxyl groups in the polymer polyol and the chain extender is n1, the molar number of NCO groups in the alicyclic diisocyanate is n2, and n1:n2=1:(1.1-3), for example, it can be 1:1.15, 1:1.2, 1:1.25, 1:1.3, 1:1.35, 1:1.4, 1:1.45, 1:1.5, 1:1.6, 1:1.7, 1:1.8, 1:1.9, 1:2, 1:2.1, 1:2.2, 1:2.3, 1:2.4, 1:2.5, 1:2.6, 1:2.7, 1:2.8 or 1:2.9, etc.

[0031] Preferably, the total molar number of hydroxyl groups in the polymer polyol, chain extender and hydroxyl-containing acrylate is n H The molar number of NCO groups in the alicyclic diisocyanate is n2, n H :n2=(1-1.15):1, for example, it can be 1:1, 1.02:1, 1.05:1, 1.08:1, 1.1:1, 1.12:1 or 1.14:1, etc.

[0032] Preferably, the molar ratio of the polymer polyol to the chain extender is 1:(1-10), for example, it can be 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5, 1:4, 1:4.5, 1:5, 1:5.5, 1:6, 1:6.5, 1:7, 1:.7.5, 1:8, 1:8.5, 1:9 or 1:9.5, etc.

[0033] Preferably, the molar ratio of the polymer polyol to the hydroxyl-containing acrylate is 1:(0.5-8), for example, it can be 1:0.6, 1:0.8, 1:1, 1:1.2, 1:1.5, 1:1.8, 1:2, 1:2.2, 1:2.5, 1:2.8, 1:3, 1:3.2, 1:3.5, 1:3.8, 1:4, 1:4.2, 1:4.5, 1:4.8, 1:5, 1:5.2, 1:5.5, 1:5.8, 1:6, 1:6.2, 1:6.5, 1:6.8, 1:7, 1:7.2, 1:7.5 or 1:7.8, etc.

[0034] Preferably, the number average molecular weight of the photosensitive prepolymer is 1000-10000, for example, it can be 2000, 3000, 4000, 5000, 6000, 7000, 8000 or 9000, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0035] In a second aspect, the present invention provides a method for preparing the photosensitive prepolymer as described in the first aspect, the preparation method comprising:

[0036] The polymer polyol, alicyclic diisocyanate and chain extender are polymerized to obtain a polyurethane intermediate terminated with an NCO group;

[0037] The polyurethane intermediate is subjected to a capping reaction with a hydroxyl-containing acrylate to obtain the photosensitive prepolymer.

[0038] Preferably, the polymer polyol, chain extender and other components are dehydrated to prevent moisture from affecting the polymerization reaction.

[0039] Preferably, the polymerization reaction is carried out in the presence of a solvent.

[0040] In the preparation method of the photosensitive prepolymer, as the polymerization reaction proceeds, the molecular weight of the product increases continuously and the viscosity increases. As the viscosity increases, the heat of reaction generated by the polymerization reaction is not easy to diffuse, resulting in a rapid increase in the system temperature, which accelerates the polymerization reaction and causes the oligomer to gel before reaching a sufficient molecular weight, and cannot be used as a material. Therefore, in the preparation process of the photosensitive prepolymer, in order to avoid the polyurethane intermediate from gelling before reaching a sufficient molecular weight, it is preferred to react in a solvent. The solvent does not participate in the reaction (the solvent must not have functional groups such as hydroxyl, amino, isocyanate, etc. that can react with carbamate), and is used to control the reaction rate of the material to prevent the viscosity from increasing rapidly and gelling due to the increase in molecular weight.

[0041] Preferably, the solvent may be a conventional organic solvent, such as any one of ketone solvents (such as acetone, butanone), ester solvents (such as ethyl acetate, butyl acetate), and aromatic solvents (such as toluene, xylene), or a combination of at least two thereof; however, such organic solvents need to be removed when preparing the photosensitive resin composition or the 3D printing material.

[0042] In order to facilitate the application of the photosensitive prepolymer and the preparation of the photosensitive resin composition, the solvent used in the polymerization reaction is preferably a diluent monomer, thereby avoiding the need for an additional step of removing the organic solvent before compounding the photosensitive resin composition.

[0043] Preferably, the diluent monomer comprises an acrylate and / or methacrylate containing one unsaturated double bond, such as cyclotrimethylolpropane methylal acrylate, cyclotrimethylolpropane methylal methacrylate, 3,3,5-trimethylcyclohexyl acrylate, tetrahydrofurfuryl acrylate, tetrahydrofurfuryl methacrylate, benzyl methacrylate, 2-tetrahydropyranyl acrylate, 2-tetrahydropyranyl methacrylate, menthyl acrylate, menthyl methacrylate, glyceryl acetonate acrylate, glyceryl acetonate methacrylate, fenchyl acrylate, cyclohexyl acrylate, cyclomethacrylate, and the like. Preferably, the present invention comprises any one of 4-tert-butylcyclohexyl acrylate, 4-tert-butylcyclohexyl methacrylate, 1-adamantane acrylate, 1-adamantane methacrylate, and dicyclopentenyl acrylate, and any one of 4-tert-butylcyclohexyl acrylate, 4-tert-butylcyclohexyl methacrylate, 1-adamantane acrylate, 1-adamantane methacrylate, and dicyclopentenyl acrylate, and any one of cyclotrimethylolpropane formal acrylate, 3,3,5-trimethylcyclohexyl acrylate, menthyl acrylate, menthyl methacrylate, glyceryl acetone acrylate, glyceryl acetone methacrylate, fenchyl acrylate, 4-tert-butylcyclohexyl acrylate, and 4-tert-butylcyclohexyl methacrylate, or a combination of at least two thereof.

[0044] Preferably, the amount of the solvent (diluting the monomer) used in the polymerization reaction is sufficient to regulate the reaction rate and control the photosensitive prepolymer product to have a suitable viscosity.

[0045] Preferably, the mass ratio of the polymer polyol to the solvent is 1:(0.2-5), for example, it can be 1:0.5, 1:0.6, 1:0.8, 1:1, 1:1.2, 1:1.5, 1:1.8, 1:2, 1:2.2, 1:2.5, 1:2.8, 1:3, 1:3.2, 1:3.5, 1:3.8, 1:4, 1:4.2, 1:4.5 or 1:4.8, etc.

[0046] Preferably, the viscosity of the photosensitive prepolymer (room temperature / normal temperature) is 800-8000 mPa·s, for example, it can be 1000 mPa·s, 1500 mPa·s, 2000 mPa·s, 2500 mPa·s, 3000 mPa·s, 3500 mPa·s, 4000 mPa·s, 4500 mPa·s, 5000 mPa·s, 5500 mPa·s, 6000 mPa·s, 6500 mPa·s, 7000 mPa·s or 7500 mPa·s, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0047] In order to prevent the diluent monomer used as a solvent from being polymerized, the polymerization reaction is preferably carried out in the presence of a polymerization inhibitor.

[0048] Preferably, the inhibitor comprises a phenolic compound, illustratively including but not limited to: any one or a combination of at least two of hydroquinone, p-methoxyphenol, 6-tert-butyl-2,4-dimethylphenol, 2,6-di-tert-butyl-p-methylphenol, vitamin E, tea polyphenols, tert-butyl-4-hydroxyanisole, and N,N'-bis(β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl)hydrazine (antioxidant 1024).

[0049] Preferably, based on the mass of the polymer polyol as 100%, the mass of the inhibitor is ≤2%, for example, it can be 0, 0.01%, 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.2%, 1.5% or 1.8%, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range, and 0-1% is further preferred.

[0050] Preferably, the polymerization reaction is carried out in the presence of a catalyst.

[0051] Preferably, the catalyst includes any one of an amine catalyst, a tin catalyst, a titanium catalyst, a zinc catalyst, and a bismuth catalyst, or a combination of at least two of them.

[0052] Preferably, the amine catalyst includes any one of triethylamine, triethylenediamine, N-ethylmorpholine, triethylenediamine, N,N-dimethylcyclohexylamine, and pentamethyldiethylenetriamine, or a combination of at least two thereof.

[0053] Preferably, the tin-based catalyst includes any one of trimethyltin laurate, dibutyltin dilaurate, and stannous octoate, or a combination of at least two thereof.

[0054] Preferably, the titanium-based catalyst is a titanium-based organic metal salt, such as tetrabutyl titanate and / or tetraisopropyl titanate.

[0055] Preferably, the zinc-based catalyst is a zinc-based organic metal salt, such as any one of zinc octoate, zinc isooctanoate, and zinc 2-ethylhexanoate, or a combination of at least two thereof.

[0056] Preferably, the bismuth-based catalyst is a bismuth-based organic metal salt, such as bismuth isooctanoate and / or bismuth 2-ethylhexanoate.

[0057] As a preferred technical solution of the present invention, the catalyst is added to make the polymerization reaction proceed faster. Even without the catalyst, the polymerization reaction can proceed. From the perspective of the application safety of dental / oral materials, it is preferred not to add a catalyst.

[0058] Preferably, based on the mass of the polymer polyol as 100%, the mass of the catalyst is ≤2%, for example, it can be 0, 0.01%, 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.2%, 1.5% or 1.8%, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range, and 0-1% is further preferred.

[0059] Preferably, the temperature of the polymerization reaction is 20-100°C, for example, it can be 30°C, 35°C, 38°C, 40°C, 42°C, 45°C, 48°C, 50°C, 52°C, 55°C, 58°C, 60°C, 65°C, 68°C, 70°C, 72°C, 75°C, 78°C, 80°C, 90°C or 95°C, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0060] In order to avoid the polymerization of the diluent monomer used as a solvent and to prevent the system from gelling, the polymerization temperature is preferably ≤ 60°C, more preferably 30-60°C.

[0061] Preferably, the polymerization reaction time is 1-8h, for example, it can be 1.5h, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, 5h, 5.5h, 6h, 6.5h, 7h or 7.5h, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively enumerates the specific point values ​​included in the range, and 2-6h is further preferred.

[0062] In the present invention, the polyurethane intermediate can be prepared by a one-step method or a two-step method. Specifically, the one-step method comprises: putting polymer polyol, alicyclic diisocyanate and chain extender into a reaction device, and performing polymerization reaction in the presence of an optional solvent, an optional inhibitor and an optional catalyst to obtain the polyurethane intermediate. The two-step method comprises: putting polymer polyol and alicyclic diisocyanate into a reaction device, and performing a first stage reaction in the presence of an optional solvent, an optional inhibitor and an optional catalyst, and then adding a chain extender to perform a second stage reaction to obtain the polyurethane intermediate.

[0063] Preferably, the temperature of the end-capping reaction is 20-100°C, for example, it can be 30°C, 35°C, 38°C, 40°C, 42°C, 45°C, 48°C, 50°C, 52°C, 55°C, 58°C, 60°C, 65°C, 68°C, 70°C, 72°C, 75°C, 78°C, 80°C, 90°C or 95°C, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range, and 30-60°C is further preferred.

[0064] Preferably, the end-capping reaction time is 0.5-6 h, for example, it can be 1 h, 1.5 h, 2 h, 2.5 h, 3 h, 3.5 h, 4 h, 4.5 h, 5 h or 5.5 h, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively enumerates the specific point values ​​included in the range, and 1-5 h is further preferred.

[0065] In addition, the polymerization reaction and the end-capping reaction are carried out under stirring conditions, and the stirring speeds of the polymerization reaction and the end-capping reaction are each independently 100-600 rpm, for example, 150 rpm, 200 rpm, 250 rpm, 300 rpm, 350 rpm, 400 rpm, 450 rpm, 500 rpm or 550 rpm, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0066] In a third aspect, the present invention provides a photosensitive resin composition, comprising a combination of the photosensitive prepolymer and an initiator as described in the first aspect.

[0067] Preferably, the mass percentage of the photosensitive prepolymer in the photosensitive resin composition is 10%-45%, for example, it can be 12%, 15%, 18%, 20%, 22%, 25%, 28%, 30%, 32%, 35%, 38%, 40%, 42% or 44%, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the said range.

[0068] Preferably, the mass percentage of the initiator in the photosensitive resin composition is 0.5%-5%, for example, it can be 0.8%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4% or 4.5%, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0069] Preferably, the initiator is a free radical initiator.

[0070] Preferably, the initiator comprises a photoinitiator and optionally a thermal initiator.

[0071] Preferably, the mass percentage of the photoinitiator in the photosensitive resin composition is 0.5%-5%, for example, it can be 0.8%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5% or 4.8%, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the said range.

[0072] Preferably, the photoinitiator includes 2-hydroxy-2-methylpropiophenone (photoinitiator 184), 1-hydroxycyclohexyl phenyl ketone (photoinitiator 1173), methyl benzoylformate (photoinitiator MBF), benzoin dimethyl ether (photoinitiator 651), 2-hydroxy-2-methyl-p-hydroxyethyl ether phenyl-1-propanone (photoinitiator 2959), 4,4'-bis(diethylamino)benzophenone (photoinitiator EAB), difunctional ketone sulfone (photoinitiator 1001M), 2,4-diethylthiazolone (photoinitiator DETX) , 2-methyl-2-(4-morpholinyl)-1-(4-(methylthio)phenyl)-1-propanone (photoinitiator 907), 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone (photoinitiator 369), ethyl 2,4,6-trimethylbenzoylphenylphosphonate (photoinitiator TPO-L), diphenyl (2,4,6-trimethylbenzoyl)phosphine oxide (photoinitiator TPO), phenyl bis (2,4,6-trimethylbenzoyl)phosphine oxide (photoinitiator 819), any one or a combination of at least two thereof.

[0073] Preferably, the thermal initiator includes any one of dicumyl peroxide, benzoyl peroxide, and azobisisobutyronitrile, or a combination of at least two thereof.

[0074] Preferably, the photosensitive resin composition further comprises a diluent monomer.

[0075] Preferably, the mass percentage of the diluted monomer in the photosensitive resin composition is 54%-75%, for example, it can be 55%, 56%, 58%, 60%, 62%, 65%, 68%, 70%, 72% or 74%, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the said range.

[0076] Preferably, the diluent monomer includes an acrylate monomer containing one unsaturated double bond; the glass transition temperature (Tg) of the homopolymer of the diluent monomer (acrylate monomer) is 15-150°C, for example, it can be 20°C, 30°C, 40°C, 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C or 140°C, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the said range.

[0077] As a preferred technical solution of the present invention, by making the Tg value of the homopolymer of the diluent monomer within the temperature range of daily use of the product, the photosensitive prepolymer is diluted and the viscosity of the photosensitive resin composition is reduced while ensuring the function of the thermal shape memory characteristics of the photosensitive prepolymer.

[0078] Preferably, the diluent monomer comprises acrylate and / or methacrylate, and further preferably cyclotrimethylolpropane formal acrylate, cyclotrimethylolpropane formal methacrylate, 3,3,5-trimethylcyclohexyl acrylate, tetrahydrofurfuryl acrylate, tetrahydrofurfuryl methacrylate, benzyl methacrylate, 2-tetrahydropyranyl acrylate, 2-tetrahydropyranyl methacrylate, menthyl acrylate, menthyl methacrylate, glyceryl acetonate acrylate, glyceryl acetonate methacrylate, fenchyl acrylate, cyclohexyl acrylate, cyclohexyl methacrylate, Any one or a combination of at least two of 4-tert-butylcyclohexyl acrylate, 4-tert-butylcyclohexyl methacrylate, 1-adamantane acrylate, 1-adamantane methacrylate, and dicyclopentenyl acrylate, and more preferably any one or a combination of at least two of cyclotrimethylolpropane formal acrylate, 3,3,5-trimethylcyclohexyl acrylate, menthyl acrylate, menthyl methacrylate, glyceryl acetonate acrylate, glyceryl acetonate methacrylate, fenchyl acrylate, 4-tert-butylcyclohexyl acrylate, and 4-tert-butylcyclohexyl methacrylate.

[0079] As a preferred technical solution of the present invention, the diluent monomer is more preferably cyclotrimethylolpropane methyl acrylate, menthyl acrylate, menthyl methacrylate, acetone glycerol acrylate, acetone glycerol methacrylate, etc., and the diluent monomer with low odor or no irritating odor is selected to avoid the strong irritating odor caused by the selection of diluent monomers such as isobornyl acrylate and / or isobornyl methacrylate, thereby improving the user experience of the photosensitive resin composition during the printing and molding process.

[0080] Preferably, the photosensitive resin composition further comprises a cross-linking monomer.

[0081] Preferably, the mass percentage of the cross-linking monomer in the photosensitive resin composition is ≤5%, for example, it can be 0, 0.1%, 0.2%, 0.5%, 0.6%, 0.8%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4% or 4.5%, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the said range.

[0082] Preferably, the cross-linking monomer is an acrylic acid ester compound having at least 2 (eg, 2, 3, 4, 5, 6, etc.) unsaturated double bonds in its molecular structure.

[0083] Preferably, the viscosity of the cross-linking monomer is ≤500 mPa·s.

[0084] Preferably, the cross-linking monomer includes any one of triethylene glycol dimethacrylate, 1,4-butanediol dimethacrylate, 1,4-cyclohexanediol diacrylate, 1,4-cyclohexanediol dimethacrylate, tricyclodecane dimethanol diacrylate, tricyclodecane dimethanol dimethacrylate, neopentyl glycol diacrylate, trimethylolpropane triacrylate, trimethylolpropane trimethacrylate, ethoxylated trimethylolpropane triacrylate, ditrimethylolpropane tetraacrylate, trihydroxyethyl isocyanurate triacrylate, and trihydroxyethyl isocyanurate trimethacrylate, or a combination of at least two thereof.

[0085] Preferably, the photosensitive resin composition further comprises additives, and the additives include any one or a combination of at least two of a polymerization inhibitor, an ultraviolet absorber, a defoamer, a thickener, a leveling agent, and a stabilizer.

[0086] Preferably, the mass percentage of the additive in the photosensitive resin composition is ≤5%, for example, it can be 0, 0.1%, 0.2%, 0.5%, 0.6%, 0.8%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4% or 4.5%, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0087] Preferably, the inhibitor comprises a phenolic compound, and further preferably any one or a combination of at least two of hydroquinone, p-methoxyphenol, 6-tert-butyl-2,4-dimethylphenol, 2,6-di-tert-butyl-p-methylphenol, vitamin E, tea polyphenols, tert-butyl-4-hydroxyanisole, and N,N'-bis(β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl)hydrazine (antioxidant 1024).

[0088] In the present invention, the ultraviolet absorber is not particularly limited, and any conventional ultraviolet absorber that can be used in a polymer system is applicable to the present invention.

[0089] Preferably, the ultraviolet absorber includes any one of UV-1, UV-O, UV-9, BP-6, BP-4, UV-531, UV-P, UVP-327, UV-328, UV-329, UV-360, UV-571, triazine-5, UV-1164, UV-1577, UV-627, and UV-1600, or a combination of at least two thereof.

[0090] In the present invention, the defoamer, thickener, and leveling agent are not particularly limited, and conventional defoamers, thickeners, leveling agents, etc. that can be used in polymer systems are applicable to the present invention. Exemplarily, the defoamer includes an organosilicon defoamer; and / or, the thickener includes silicon dioxide (e.g., fumed silica); and / or, the leveling agent includes a polyether-modified polysiloxane leveling agent.

[0091] Preferably, the stabilizer includes any one of free tertiary amine, hindered amine, and organic phosphate, or a combination of at least two or three thereof, to stabilize the photosensitive resin composition. Exemplarily, the free tertiary amine includes diethylethanolamine and / or trihexylamine.

[0092] In the present invention, the introduction of the additives (such as inhibitors, UV absorbers, defoamers, thickeners, leveling agents, stabilizers) can improve the thermal stability, oxidation stability, storage stability, surface properties, flow properties and processing properties of the photosensitive resin composition.

[0093] In addition, the photosensitive resin composition may further include other additives that may be added by those skilled in the art, such as any one of a pigment, a filler, and an organic solvent, or a combination of at least two of them.

[0094] In the present invention, the photosensitive resin composition is in a liquid state and can be cured by light exposure; the light exposure includes UV (ultraviolet) light exposure, but it is not limited to UV light and can also be applied to other light exposures. The photosensitive resin composition is in a liquid state before light exposure and initiates a curing crosslinking reaction under light exposure to form a polymer system with a network structure.

[0095] In the present invention, the preparation method of the photosensitive resin composition comprises: uniformly mixing a photosensitive prepolymer, an initiator, a diluent monomer, an optional cross-linking monomer and an optional additive to obtain the photosensitive resin composition.

[0096] In a fourth aspect, the present invention provides a use of the photosensitive resin composition as described in the third aspect in biomedical materials.

[0097] Preferably, the photosensitive resin composition is applied to oral materials.

[0098] On the other hand, the present invention provides a 3D printing material, the raw materials for preparing the 3D printing material include the photosensitive resin composition as described in the third aspect.

[0099] In the present invention, the term "3D printing" refers to the process of manufacturing three-dimensional objects by layering materials using 3D digital data. In this specification, 3D printing technology is mainly described as digital light processing (DLP), stereolithography equipment (SLA) and PolyJet technology, but it is understood that it also includes other 3D printing technologies.

[0100] Preferably, the method for preparing the 3D printing material comprises: placing the photosensitive resin composition in a 3D printer for 3D printing to obtain the 3D printing material.

[0101] Preferably, the 3D printing further includes a secondary curing step.

[0102] Preferably, the secondary curing is performed under conditions of light (eg UV light) and / or heating.

[0103] Preferably, the heating temperature is 40-80°C, for example, it can be 45°C, 48°C, 50°C, 52°C, 55°C, 58°C, 60°C, 62°C, 65°C, 68°C, 70°C, 72°C, 75°C or 78°C, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range, and 50-65°C is further preferred.

[0104] Preferably, the secondary curing time is 5-30 min, for example, 6 min, 8 min, 10 min, 12 min, 15 min, 18 min, 20 min, 22 min, 25 min or 28 min, as well as specific point values ​​between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0105] In a fifth aspect, the present invention provides an oral support, wherein the raw materials for preparing the oral support include the photosensitive resin composition as described in the third aspect.

[0106] Preferably, the cured product of the photosensitive resin composition and the 3D printing material (oral support) have excellent mechanical properties, with a bending strength of ≥145MPa, which can be 148-172MPa; a bending elastic modulus of ≥3470MPa, which can be 3470-3804MPa; a tensile strength of ≥95MPa, which can be 95-114MPa; and an elongation of ≤35%, which can be 15-31%.

[0107] Preferably, the oral support comprises any one of an artificial tooth, a transparent orthodontic device, a surgical guide, and a splint.

[0108] In the present invention, the photosensitive resin composition can be used to prepare oral supports through 3D printing technology, and can output transparent orthodontic devices that conform to the patient's oral structure style, such as orthodontic appliances, orthodontic retainers, dental arch expanders, etc., which have excellent mechanical properties, can improve the correction force, and can also change and restore the shape when heated, improve the user's comfort, and can also provide a variety of customized dental products (such as artificial teeth, surgical guides, splints). Since the transparent orthodontic device is different from the patient's current tooth structure, it is not easy to wear even if it is inserted into the teeth, and even if it is worn, it will not cause much pain.

[0109] Specifically, the photosensitive resin composition can be used to print a transparent orthodontic device customized according to the patient's oral structure, which can increase the correction force. At a higher temperature (50-100°C, such as immersed in warm water or boiling water), the transparent orthodontic device is easily deformed after being subjected to force, and the shape automatically returns to its original state after the external force is removed; but when the transparent orthodontic device immersed in warm water or boiling water and deformed by force is placed in the oral environment for use, due to the change in body temperature (body temperature is lower than the temperature at which it can be deformed), its shape is fixed and can exert a correction force. Further, because it has plasticity under the condition of 50-100°C, that is, under the condition of 50-60°C hot water (the temperature that the oral cavity can withstand), the transparent orthodontic device can be molded and easy to remove; such as in warm boiled water, the external force is removed, and the shape returns to the original printed shape; such as the deformed resin is kept under external force and cooled to room temperature, the shape remains unchanged in the stressed shape, and has shape memory characteristics. After the transparent orthodontic device is cleaned with warm water and placed in the mouth, the temperature of the device gradually drops to body temperature. During this process, the device spontaneously returns to its original shape (3D printed shape suitable for orthodontics). After it is completely fixed, it gradually exerts its orthodontic effect.

[0110] Compared with the prior art, the present invention has the following beneficial effects:

[0111] (1) The photosensitive prepolymer provided by the present invention has the characteristics of thermal shape memory through the design and mutual compounding of the preparation raw materials such as polymer polyol, alicyclic diisocyanate, chain extender, hydroxyl-containing acrylate, etc., and its shape memory response temperature can meet the requirements of shape memory change temperature when used in dental orthodontic products; at the same time, the photosensitive prepolymer is degradable, safe and environmentally friendly, has appropriate viscosity, and is suitable for 3D printing photosensitive resin composition. It can obtain 3D printing materials with shape memory function, safety and degradability, which can be used as oral support, has excellent mechanical properties, can increase the correction force, and can change and restore the shape under temperature changes, providing excellent correction effect.

[0112] (2) The photosensitive resin composition provided by the present invention can be cured and molded using 3D printing technology to output orthodontic products that conform to the oral structure style, so that the product has a bending strength of ≥148MPa, a bending elastic modulus of ≥3470MPa, a tensile strength of ≥95MPa, and an elongation of ≤35%. It has excellent mechanical properties, increases the correction force, and has a shape memory function. It can change and restore the shape when heated to improve the user's comfort; moreover, the 3D printing material and oral support made of the photosensitive resin composition have excellent degradable properties, and are particularly suitable for orthodontic devices that are used in short cycles (e.g., 14-30 days) and are replaced relatively frequently. The photosensitive prepolymer and photosensitive resin composition provided by the present invention can provide a variety of customized dental products and have broad application prospects. DETAILED DESCRIPTION

[0113] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0114] In the present invention, the features defined as "first" or "second" may include one or more of the features explicitly or implicitly, and are used to distinguish and describe the features, without distinction of order or importance. In the description of the present invention, unless otherwise specified, "plurality" means two or more.

[0115] As used herein, the terms "comprises," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus comprising the listed elements is not necessarily limited to only those elements but may also include other elements not expressly listed or inherent to such composition, process, method, article.

[0116] "Optionally" or "either" means that the subsequently described matter or event can or cannot occur, and that the description includes instances where the event occurs and instances where it does not.

[0117] In the following specific embodiments of the present invention, the materials, reagents, etc. used can all be conventional commercially available raw materials obtained from commercial channels. Among them, the material information of the polymer polyol is as follows:

[0118] Polycaprolactone diol: number average molecular weight 2000, hydroxyl value 53-59 mg KOH / g, brand PCL220N, purchased from Daicel Japan;

[0119] Polytetrahydrofuran diol: number average molecular weight of 2000, hydroxyl value of 54.7-57.5 mg KOH / g, brand PTMG2000, purchased from Hyosung, South Korea;

[0120] Poly(hexanediol carbonate): number average molecular weight is 2000, hydroxyl value is 51-61 mg KOH / g, brand name is Duonail TM T5652, purchased from Asahi Kasei, Japan;

[0121] Polypropylene glycol: number average molecular weight of 600, hydroxyl value of 170-208 mg KOH / g, brand PPG-600, purchased from Shandong Dongda Chemical;

[0122] Polybutylene adipate: number average molecular weight of 5000, hydroxyl value of 20-24 mg KOH / g, brand T-5044, purchased from Huada Chemical;

[0123] Poly(hexanediol adipate): number average molecular weight is 1500, hydroxyl value is 71-79 mg KOH / g, brand name Unipol-6515, purchased from Changxing, China.

[0124] The photosensitive prepolymer and the preparation method thereof of the present invention will be described in detail below by taking a plurality of embodiments as examples, but the photosensitive prepolymer and the preparation method thereof of the present invention are not limited to these embodiments.

[0125] Example 1

[0126] A photosensitive prepolymer, the preparation raw materials include polymer polyol (polycaprolactone diol), alicyclic diisocyanate (isophorone diisocyanate, IPDI), chain extender (2,5-dihydroxymethyltetrahydrofuran) and hydroxyl-containing acrylate (2-hydroxyethyl acrylate), the molar ratio of polycaprolactone diol, isophorone diisocyanate, 2,5-dihydroxymethyltetrahydrofuran and 2-hydroxyethyl acrylate is 1:5:3:2; the specific preparation method includes the following steps:

[0127] (1) After nitrogen replacement of the reaction apparatus, polymer polyol and chain extender were added according to the above molar ratio, and solvent (cyclotrimethylolpropane formal acrylate) and polymerization inhibitor (p-methoxyphenol) were added at the same time, so that the mass ratio of polymer polyol, solvent and polymerization inhibitor was 1:1:0.003, and the above materials were mixed and dispersed uniformly under stirring conditions, and vacuum dehydrated for 1 hour;

[0128] (2) adding alicyclic diisocyanate to the reaction system of step (1), heating to 45° C. with stirring at 300 rpm, adding a catalyst (dibutyltin dilaurate, the mass ratio of which to the polymer polyol is 0.003:1), reacting for 4 h, and obtaining a polyurethane intermediate terminated with an NCO group;

[0129] (3) maintaining the temperature and stirring rate of step (2) unchanged, adding hydroxyl-containing acrylate to carry out end-capping reaction, cooling to 25° C. after 3 hours, discharging the material, and obtaining the photosensitive prepolymer.

[0130] Examples 2-9, Comparative Examples 1-4

[0131] A photosensitive prepolymer, which differs from Example 1 only in that the raw materials for preparation are different, as shown in Table 1; in Table 1, "molar ratio" represents the molar ratio of polymer polyol, diisocyanate, chain extender and hydroxyl-containing acrylate; in Table 1, the usage ratio of catalyst (if any), inhibitor and solvent is the same as that in Example 1; the preparation method is the same as that in Example 1.

[0132] Table 1

[0133]

[0134]

[0135]

[0136] The molecular weight of the photosensitive prepolymers provided in Examples 1-9 and Comparative Examples 1-4 was tested by gel chromatography (GPC) with tetrahydrofuran as the mobile phase, and the rotational viscosity of the photosensitive prepolymers (containing solvent) was tested according to the method in standard GB / T 22235. The obtained data are shown in Table 2:

[0137] Table 2

[0138]

[0139]

[0140] The photosensitive resin composition, 3D printing material and oral support (transparent orthodontic appliance) of the present invention will be described in detail below using multiple application examples.

[0141] Application Example 1-9, Comparative Application Example 1-4

[0142] A photosensitive resin composition, the types and amounts of each component are shown in Table 3; the photosensitive resin composition is used to prepare a 3D printing material, and the method includes:

[0143] Mix the components evenly according to the formula shown in Table 3 to obtain the photosensitive resin composition; pour the photosensitive resin composition into the resin tank of the 3D printer (model CPD-100, light source wavelength 405nm), set the layer thickness to 0.1mm, and the exposure time of each layer to 8s. After printing, place it in an ultrasonic cleaner, clean the uncured resin on the surface with anhydrous ethanol, and blow dry the residual ethanol with a high-pressure air gun, and then place the printed model in a UV curing light box for secondary curing. The temperature in the UV curing light box is 60°C, and the secondary curing time is 15min. The 3D printing material is obtained as a test sample for subsequent performance testing.

[0144] Table 3

[0145]

[0146]

[0147]

[0148] The following performance tests were performed on the aforementioned 3D printing materials:

[0149] (1) Flexural strength and flexural modulus: tested according to the method in standard ISO 20795-2;

[0150] (2) Tensile strength and elongation: tested according to the method in standard ASTM D638;

[0151] (3) Shape memory performance: The shape of the transparent orthodontic appliance is formed by a computer program, and the corresponding transparent orthodontic appliance is printed using a 3D printer. In order to confirm its shape memory properties, thermal deformation and shape recovery experiments were carried out. Specifically, the sample to be tested was immersed in 60°C water, and then an external force was applied to change the shape to determine whether the deformation was fixed at 37°C. The deformed shape was then immersed in 60°C water to determine whether it could be restored to its original shape. If deformation, fixation and recovery can be achieved, it means that the shape memory property is present.

[0152] The test results are shown in Table 4:

[0153] Table 4

[0154]

[0155]

[0156] According to the above performance test results, the photosensitive prepolymer provided by the present invention is used to prepare a photosensitive resin composition, which can meet the requirements of 3D printing and obtain a 3D printing material with excellent mechanical properties, and its bending strength is 148-172MPa, the bending elastic modulus is 3470-3804MPa, the tensile strength is 95-114MPa, and the elongation is 15-31%; the excellent mechanical properties exhibited by the 3D printing material enable it to fully meet the performance requirements of dental / oral products such as transparent orthodontic devices and increase the correction force.

[0157] Furthermore, the 3D printed material (transparent orthodontic appliance) sample can change its shape when an external force is applied at a temperature of 50-100°C, and be fixed in the deformed shape; if an external force is applied when immersed in an environment of 50-100°C again, the shape will be restored, thereby exhibiting an excellent shape memory function; therefore, the photosensitive resin composition can be used to 3D print a transparent orthodontic appliance through DLP, and the orthodontic device can be pasted on the back of the patient's orthodontic teeth during treatment, so as to exert an orthodontic retention effect.

[0158] The photosensitive resin composition prepared using the photosensitive resin A-D1 provided in Comparative Example 1 and the photosensitive resin A-D4 provided in Comparative Example 4 does not have a shape memory function under the set conditions, and the mechanical properties are relatively poor, which cannot meet the basic performance requirements of orthodontic materials. The photosensitive resin composition prepared using the photosensitive resin A-D2 of Comparative Example 2, although it has a shape memory function and similar mechanical properties under the set conditions, the introduction of the non-bio-based chain extender 1,4-cyclohexanedimethanol increases the difficulty of material degradation, and it is not preferably used in orthodontic devices that are used in a short period (14-30 days) and replaced relatively frequently. The photosensitive resin composition prepared using the photosensitive resin A-D3 of Comparative Example 3, although it also has a shape memory function and similar mechanical properties under the set conditions, the introduction of aromatic isocyanates such as MDI makes the material prone to produce carcinogenic substances such as aromatic amines during degradation, and it is not recommended for use in oral materials.

[0159] The applicant declares that the present invention uses the above embodiments to illustrate the photosensitive prepolymer, photosensitive resin composition and its application, but the present invention is not limited to the above embodiments, that is, it does not mean that the present invention must rely on the above embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A photosensitive prepolymer, characterized in that: The raw materials for preparing the photosensitive prepolymer include a combination of polymer polyol, alicyclic diisocyanate, a chain extender and hydroxyl-containing acrylate; the chain extender includes a diol containing an alicyclic heterocyclic structure.

2. The photosensitive prepolymer according to claim 1, characterized in that: The polymer polyol comprises polyester diol and / or polyether diol, preferably polyester diol; Preferably, the polyester diol includes any one of polycaprolactone diol, polybutylene carbonate, polyhexylene carbonate, polybutylene succinate, polyhexylene succinate, polybutylene adipate, and polyhexylene adipate, or a combination of at least two thereof; Preferably, the polyether diol comprises polypropylene glycol and / or polytetramethylene glycol; Preferably, the number average molecular weight of the polymer polyol is 500-5000.

3. The photosensitive prepolymer according to claim 1 or 2, characterized in that: The alicyclic diisocyanate includes any one of 1,3-cyclohexane diisocyanate, 1,4-cyclohexane diisocyanate, 1,3-diisocyanate-2-methylcyclohexane, 2,4-diisocyanate-1-methylcyclohexane, isophorone diisocyanate, 1,4-cyclohexane dimethyl diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, 1,5-decahydronaphthalene diisocyanate, and norbornane dimethylene diisocyanate, or a combination of at least two thereof; Preferably, the chain extender comprises a diol containing a tetrahydrofuran structure, and more preferably any one or a combination of at least two of 2,5-dihydroxymethyltetrahydrofuran, isosorbide, isomannide, isoidide, and dehydrated erythritol; Preferably, the hydroxyl-containing acrylate includes any one of 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, 3-hydroxypropyl acrylate, 4-hydroxybutyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, 3-hydroxypropyl methacrylate, and 4-hydroxybutyl methacrylate, or a combination of at least two thereof.

4. The photosensitive prepolymer according to any one of claims 1 to 3, characterized in that: The total number of moles of hydroxyl groups in the polymer polyol and the chain extender is n1, the number of moles of NCO groups in the alicyclic diisocyanate is n2, and n1:n2=1:(1.1-3); Preferably, the molar ratio of the polymer polyol to the chain extender is 1:(1-10); Preferably, the number average molecular weight of the photosensitive prepolymer is 1000-10000.

5. A method for preparing a photosensitive prepolymer according to any one of claims 1 to 4, characterized in that: The preparation method comprises: The polymer polyol, alicyclic diisocyanate and chain extender are polymerized to obtain a polyurethane intermediate terminated with an NCO group; The polyurethane intermediate is subjected to a capping reaction with a hydroxyl-containing acrylate to obtain the photosensitive prepolymer.

6. The preparation method according to claim 5, characterized in that: The polymerization reaction is carried out in the presence of a solvent; Preferably, the polymerization reaction is carried out in the presence of a catalyst; Preferably, the catalyst comprises any one or a combination of at least two of an amine catalyst, a tin catalyst, a titanium catalyst, a zinc catalyst, and a bismuth catalyst; Preferably, the polymerization reaction temperature is 20-100°C, more preferably 30-60°C; Preferably, the polymerization reaction time is 1-8h, more preferably 2-6h; Preferably, the temperature of the end-capping reaction is 20-100°C, more preferably 30-60°C; Preferably, the end-capping reaction time is 0.5-6 h, more preferably 1-5 h.

7. A photosensitive resin composition, characterized in that: The photosensitive resin composition comprises a combination of the photosensitive prepolymer according to any one of claims 1 to 4 and an initiator.

8. The photosensitive resin composition according to claim 7, characterized in that: The mass percentage of the photosensitive prepolymer in the photosensitive resin composition is 10%-45%; Preferably, the mass percentage of the initiator in the photosensitive resin composition is 0.5%-5%; Preferably, the initiator comprises a photoinitiator and optionally a thermal initiator; Preferably, the photoinitiator includes any one of 2-hydroxy-2-methylpropiophenone, 1-hydroxycyclohexyl phenyl ketone, methyl benzoylformate, benzoin dimethyl ether, 2-hydroxy-2-methyl-p-hydroxyethyl ether phenyl-1-propanone, 4,4'-bis(diethylamino)benzophenone, difunctional ketone sulfone, 2,4-diethylthiazolone, 2-methyl-2-(4-morpholinyl)-1-(4-(methylthio)phenyl)-1-propanone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone, ethyl 2,4,6-trimethylbenzoylphenylphosphonate, diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, and phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, or a combination of at least two thereof; Preferably, the thermal initiator comprises any one of dicumyl peroxide, benzoyl peroxide, and azobisisobutyronitrile, or a combination of at least two thereof; Preferably, the photosensitive resin composition further comprises a diluent monomer; Preferably, the mass percentage of the diluent monomer in the photosensitive resin composition is 54%-75%; Preferably, the diluent monomer comprises acrylate and / or methacrylate, and further preferably cyclotrimethylolpropane formal acrylate, cyclotrimethylolpropane formal methacrylate, 3,3,5-trimethylcyclohexyl acrylate, tetrahydrofurfuryl acrylate, tetrahydrofurfuryl methacrylate, benzyl methacrylate, 2-tetrahydropyranyl acrylate, 2-tetrahydropyranyl methacrylate, menthyl acrylate, menthyl methacrylate, glyceryl acetonate acrylate, glyceryl acetonate methacrylate, fenchyl acrylate, cyclohexyl acrylate, cyclohexyl methacrylate, Any one of 4-tert-butylcyclohexyl acrylate, 4-tert-butylcyclohexyl methacrylate, 1-adamantane acrylate, 1-adamantane methacrylate, and dicyclopentenyl acrylate, or a combination of at least two thereof; more preferably any one of cyclotrimethylolpropane formal acrylate, 3,3,5-trimethylcyclohexyl acrylate, menthyl acrylate, menthyl methacrylate, glyceryl acetonate acrylate, glyceryl acetonate methacrylate, fenchyl acrylate, 4-tert-butylcyclohexyl acrylate, and 4-tert-butylcyclohexyl methacrylate, or a combination of at least two thereof; Preferably, the photosensitive resin composition further comprises a cross-linking monomer; Preferably, the mass percentage of the crosslinking monomer in the photosensitive resin composition is ≤5%; Preferably, the crosslinking monomer includes any one of triethylene glycol dimethacrylate, 1,4-butanediol dimethacrylate, 1,4-cyclohexanediol diacrylate, 1,4-cyclohexanediol dimethacrylate, tricyclodecane dimethanol diacrylate, tricyclodecane dimethanol dimethacrylate, neopentyl glycol diacrylate, trimethylolpropane triacrylate, trimethylolpropane trimethacrylate, ethoxylated trimethylolpropane triacrylate, ditrimethylolpropane tetraacrylate, trihydroxyethyl isocyanurate triacrylate, and trihydroxyethyl isocyanurate trimethacrylate, or a combination of at least two thereof; Preferably, the photosensitive resin composition further comprises an additive, wherein the additive comprises any one or a combination of at least two of an inhibitor, an ultraviolet absorber, a defoamer, a thickener, a leveling agent, and a stabilizer; Preferably, the mass percentage of the additive in the photosensitive resin composition is ≤5%.

9. Use of the photosensitive resin composition according to claim 7 or 8 in biomedical materials; Preferably, the photosensitive resin composition is applied to oral materials.

10. An oral support, characterized in that: The raw material for preparing the oral support comprises the photosensitive resin composition according to claim 7 or 8; Preferably, the oral support comprises any one of an artificial tooth, a transparent orthodontic device, a surgical guide, and a splint.

Citation Information

Cited By

  • 3D printing appliance step-by-step curing method based on gray level regulation and control

    CN119795549A

  • 3D printing biodegradable high-toughness polycaprolactone photosensitive resin and preparation method thereof

    CN119899332A

  • 3D printing photosensitive resin, preparation method and 3D printing elastomer