Rubber compositions incorporating preformed natural rubber-carbon black composites
By using a combination of preformed natural rubber-carbon black composite material with conjugated diene elastomer and sulfur curing agent in the tire tread, the difficulty in balancing rolling resistance and tear properties of tire tread compositions in the prior art is solved. problem, achieving more efficient performance improvements and cost reductions.
Patent Information
- Application Number
- CN202410366872.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-28
- Publication Date
- 2024-10-01
AI Technical Summary
Existing tire tread compositions have difficulty balancing rolling resistance and tear properties when improving wear and mileage performance, and adding tread layers increases manufacturing costs or time.
Using a rubber composition containing at least 20 phr of preformed natural rubber-carbon black composite, at least 3 phr of conjugated diene elastomer and sulfur-based curing agent, blended with fillers such as silica at above 115°C to form Cured rubber composition with multi-phase morphology to improve tire rolling resistance and tear resistance.
It is possible to improve the rolling resistance and tear resistance of the tire without adding a tread layer, and at the same time reduce the tread wear, and the process can shorten the manufacturing time and reduce the cost.
Smart Images

Figure BDA0004764487910000171 
Figure BDA0004764487910000201 
Figure BDA0004764487910000221
Abstract
Description
Technical Field
[0001] Aspects of the exemplary embodiments are directed to compositions suitable for use in a variety of tire components, such as in tire treads, bases, and wire coatings, and particularly to compositions that incorporate a preformed natural rubber-carbon black composite in addition to natural rubber in conventional forms. Background Art
[0002] Tire treads are typically formed from natural rubber or other elastomers, which are compounded with various additives such as fillers and curing aids prior to the addition of a sulfur-based curative such as elemental sulfur. Such compounding ingredients are typically selected to improve performance indicators related to tread wear and tire mileage. Typically, there is a tradeoff between improvements in tread wear and mileage and other parameters such as tear and rolling resistance.
[0003] U.S. Patent No. 8536262B2 describes the inner tread rubber layer of a tire formed of rubber, the rubber comprising a small amount of syndiotactic-1,2-polybutadiene and a major amount of isoprene and / or 1,3-butadiene polymer or copolymer and a copolymer of styrene and isoprene and / or 1,3-polybutadiene. The composition further includes a blend of a rubber reinforced carbon black filler having an iodine absorption value (ASTM D2515) of about 20 to about 50 g / kg and 100 to about 300 g / kg, respectively. The inner tread rubber layer is located between the tire cap and the carcass, and is designed to promote tire handling while substantially maintaining the hysteresis properties of the rubber, reducing the tendency of internal heat accumulation during tire use. Although beneficial, adding an additional tread layer will increase the cost or time of manufacturing the tire.
[0004] Recently, elastomeric composites containing natural rubber latex and carbon black have been developed for use in tire compositions, such as described in U.S. Pat. Nos. 9,156,955 B2 and 10,767,028 B2. For example, the composites can be compounded with curing agents and other additives to produce a composition suitable for forming a tire tread. However, such composites tend to provide a limited range of properties.
[0005] There remains a need for a rubber composition formed from a composite material that can maintain the rolling resistance and tear properties of a tire formed from a cured composition without unduly affecting treadwear. Summary of the invention
[0006] According to one aspect of the exemplary embodiment, the rubber composition comprises at least 20 phr of a composite material, at least 3 phr of a conjugated diene elastomer, a curing activator and a sulfur-based curing agent. The composite material comprises reinforcing carbon black dispersed in natural rubber. The composite material and the conjugated diene elastomer together provide at least 90 phr of a vulcanizable elastomer in the rubber composition.
[0007] The rubber composition may further include a reinforcing filler other than carbon black. The reinforcing filler may include silica. The rubber composition may include at least 5 phr, or at least 8 phr, or at most 30 phr, or at most 18 phr of silica.
[0008] The composite material may provide at least 20 phr of reinforcing carbon black, or at least 30 phr, or at most 80 phr, or at most 55 phr of reinforcing carbon black to the rubber composition. The composite material may provide at least 50 phr of natural rubber, or at least 70 phr, or at most 95 phr, or at most 90 phr of natural rubber to the rubber composition. The composite material may be solid at 21° C. and atmospheric pressure.
[0009] The conjugated diene elastomer may comprise at least one of natural rubber and synthetic polyisoprene.The rubber composition may comprise at least 5 phr of the conjugated diene elastomer, or at least 10 phr, or at most 50 phr, or at most 30 phr of the conjugated diene elastomer.
[0010] The curing activator may be selected from fatty acids, zinc oxide and mixtures thereof.
[0011] The rubber composition may further comprise at least 0.1 phr of at least one processing aid selected from the group consisting of resins, oils, and mixtures thereof.
[0012] The rubber composition may further include at least 1 phr of at least one of an antioxidant and an antiozonant, and / or at least 0.5 phr of a cure accelerator, and / or at least 0.05 phr of a cure retarder.
[0013] The composite material and the conjugated diene elastomer may together provide at least 98 phr of vulcanizable elastomer in the rubber composition.
[0014] In another aspect of the exemplary embodiment, an article is formed from the rubber composition of any of the above aspects. The article may include a tire tread.
[0015] In another aspect of the exemplary embodiment, the method of forming the rubber composition includes blending a composite material with a conjugated diene elastomer at a temperature of at least 115° C. to form a mixture. The composite material comprises reinforcing carbon black dispersed in natural rubber. The composite material and the conjugated diene elastomer together provide at least 90 phr of a total of 100 phr of a vulcanizable elastomer. The mixture is blended with a sulfur-based curing agent to form the rubber composition.
[0016] In the method, the mixture may further include silicon dioxide.
[0017] The method may further include curing the rubber composition to form a shaped article.
[0018] The present invention discloses the following scheme:
[0019] Solution 1. A rubber composition comprising:
[0020] at least 20 phr of a composite material comprising reinforcing carbon black dispersed in natural rubber;
[0021] at least 3 phr of a conjugated diene elastomer, said composite and conjugated diene elastomer together providing at least 90 phr of a vulcanizable elastomer in said rubber composition;
[0022] Cure activator, and
[0023] Sulfur based curing agent.
[0024] Aspect 2. The rubber composition according to aspect 1, further comprising a reinforcing filler other than carbon black.
[0025] Aspect 3. The rubber composition according to aspect 2, wherein the reinforcing filler comprises silica.
[0026] Option 4. The rubber composition according to Option 3, wherein the rubber composition comprises at least 5 phr of silica.
[0027] Option 5. The rubber composition according to Option 1, wherein the composite material provides at least 20 phr of reinforcing carbon black to the rubber composition.
[0028] Option 6. The rubber composition according to Option 1, wherein the composite material provides at least 50 phr of natural rubber to the rubber composition.
[0029] Aspect 7. The rubber composition according to aspect 1, wherein the composite material is solid.
[0030] Aspect 8. The rubber composition according to aspect 1, wherein the conjugated diene elastomer comprises at least one of natural rubber and synthetic polyisoprene.
[0031] Aspect 9. The rubber composition of aspect 1, wherein the rubber composition comprises at least 5 phr of the conjugated diene elastomer.
[0032] Aspect 10. The rubber composition according to aspect 1, wherein the curing activator is selected from the group consisting of fatty acids, zinc oxide, and mixtures thereof.
[0033] Aspect 11. The rubber composition according to aspect 1, further comprising at least 0.1 phr of a processing aid selected from the group consisting of resins, oils, and mixtures thereof.
[0034] Aspect 12. The rubber composition according to aspect 1, further comprising at least 1 phr of at least one of an antioxidant and an antiozonant.
[0035] Aspect 13. The rubber composition according to aspect 1, further comprising at least 0.5 phr of a curing accelerator.
[0036] Aspect 14. The rubber composition according to aspect 1, further comprising at least 0.05 phr of a cure retarder.
[0037] Embodiment 15. The rubber composition of embodiment 1, wherein the composite material and the conjugated diene elastomer together provide at least 98 phr of the vulcanizable elastomer in the rubber composition.
[0038] Embodiment 16. An article formed from the composition described in Embodiment 1.
[0039] Embodiment 17. The article according to embodiment 16, comprising a tire tread.
[0040] Embodiment 18. A method for forming a rubber composition, comprising:
[0041] blending a composite material comprising reinforcing carbon black dispersed in natural rubber with a conjugated diene elastomer, the composite material and the conjugated diene elastomer together providing at least 90 phr of a total of 100 phr of vulcanizable elastomer, at a temperature of at least 115° C. to form a mixture; and
[0042] The mixture is then blended with a sulfur-based curing agent to form the rubber composition.
[0043] Option 19. A method according to Option 18, wherein the mixture further comprises silicon dioxide.
[0044] Embodiment 20. The method according to embodiment 18, further comprising curing the rubber composition to form a shaped article. DETAILED DESCRIPTION
[0045] Aspects of the exemplary embodiments relate to rubber compositions suitable for forming molded or extruded articles, and to articles formed from the compositions, such as tire treads. The compositions comprise a preformed composite material, a conjugated diene-based elastomer, a reinforcing filler (e.g., silica), a sulfur-based curing agent, and optionally one or more processing aids (e.g., oils and waxes), coupling agents, antioxidants, antiozonants, other components of a sulfur based cure package (e.g., cure activators, cure accelerators, and cure retarders), and other additives known in the art.
[0046] An exemplary composite material comprises natural rubber and carbon black as major components. The combination of the composite material and the conjugated diene-based rubber alone produces a cured rubber composition having a multiphase morphology in which the carbon black is unevenly dispersed in the rubber composition, which provides good rolling resistance and tear properties of the tire without excessively affecting tread wear.
[0047] In the present specification, the term "phr" refers to the parts of the corresponding material per 100 parts by weight of rubber or elastomer. The term "phf" refers to the parts per hundred parts by weight of filler. By convention, the uncured rubber used in the sealant composition totals 100 phr.
[0048] Unless otherwise specified, the terms "rubber" and "elastomer" are used interchangeably. Unless otherwise specified, the terms "cured" and "vulcanized" are used interchangeably.
[0049] As used herein, Mooney viscosity (ML 1+4) is measured in MU at 100° C. according to ASTM D1646-19a, “Standard Test Methods for Rubber—Viscosity, Stress Relaxation, and Pre-Vulcanization Characteristics (Mooney Viscometer)”.
[0050] As referred to herein, the glass transition temperature (Tg) of an elastomer or an elastomeric composition refers to the glass transition temperature(s) of the corresponding elastomer or elastomeric composition in its uncured state or, in the case of an elastomeric composition, in a cured state. The Tg value referred to herein is measured as the peak midpoint by a differential scanning calorimeter (DSC) at a heating rate of 10°C / min, according to ASTM D3418-21 "Standard Test Method for Transition Temperatures and Enthalpies of Fusion and Crystallization of Polymers by Differential Scanning Calorimetry".
[0051] Composite Materials
[0052] The composite material comprises natural rubber and reinforcing carbon black dispersed in the natural rubber. In one embodiment, the natural rubber and the carbon black together constitute at least 90 wt %, or at least 95 wt %, or at least 98 wt %, or at most 100 wt % of the composite material.
[0053] In one embodiment, the composite material has a Mooney viscosity of no more than 100 M.U., or no more than 85 M.U., or at least 60 M.U. The composite material may be a solid or pourable liquid at room temperature (21° C.) and atmospheric pressure. In another embodiment, the composite material may be a solid material at room temperature, for example in the form of strips or crumbs.
[0054] The composite material is unvulcanized and does not contain a sulfur-based curing agent and an organic peroxide curing agent. The composite material may also be free of reinforcing fillers other than carbon black, and free of a curing accelerator, a curing activator, and a curing retardant, examples of which are described below.
[0055] Composite material can be used in rubber composition, and its amount is at least 20phr, or at least 30phr, or at least 50phr, or at least 80phr, or at least 100phr, or at most 160phr, or at most 150phr, or at most 140phr.The elastomer content (mainly natural rubber) in composite material contributes (contribute) the total 100phr of elastomer in rubber composition.Therefore, the maximum phr of composite material in rubber composition depends at least in part on its rubber content.For example, composite material can provide at least 10phr, or at least 20phr, or at least 50phr, or at least 60phr, or at least 70phr, or at least 80phr, or at most 95phr, or at most 90phr of total elastomer in rubber composition.
[0056] The composite material may contribute at least 10 phr, or at least 15 phr, or at least 20 phr, or at least 30 phr, or at least 40 phr, or up to 80 phr, or up to 60 phr, or up to 50 phr of carbon black to the rubber composition.
[0057] The weight ratio of carbon black to natural rubber in the composite may be at least 20:80, or at least 30:70, or at most 50:50, or at most 40:60, such as about 35:65.
[0058] The carbon black in the composite material can be a single reinforcing carbon black or can include two or more different types of carbon black.
[0059] Carbon black used in composite materials can have 15m 2 / g to 300m 2 / g, or at least 40m 2 The nitrogen surface area (NSA) of carbon black (wt. %) is measured according to ASTM D6556-21 "Standard Test Method for Carbon Black—Total and External Surface Area by Nitrogen Adsorption". Exemplary carbon blacks include the ASTM designations N110, N121, N134, N220, N231, N234, N242, N293, N299, N315, N326, N330, N332, N339, N343, N347, N351, N358, N375, N539, N550, N582, N630, N642, N650, N683, N754, N762, N765, N774, N787, N907, N908, N990, and N991 as specified in ASTM D1765-21 "Standard Classification System for Carbon Blacks Used in Rubber Products."
[0060] A mixture of two or more forms of carbon black can be used. An example of a composite material suitable for use herein is described in U.S. Patent No. 10767028B2, which includes two types of carbon black. Other composite materials with different carbon blacks are described in U.S. Patent Publication No. 20100071817A1.
[0061] In one embodiment, the carbon black is pretreated, for example with silicon, prior to forming the composite material. An example of a silicon-treated carbon black is available from Cabot Corporation as CRX TM 2000
[0062] Exemplary composite materials including carbon black and natural rubber are available from Engineered Elastomer Composites (E2C TM ), such as E2C TM DX9620 and E2C TM DX 9640. E2C TM DX9620 has a Mooney viscosity ML (1+4) of about 69 M.U at 100°C, a 300% modulus of about 17.0 MPa, a tensile strength of about 29.8 MPa, an elongation at break of about 528%, and a tan δ of about 0.130 at 60°C. E2C TM DX9640 has a Mooney viscosity of about 84 MU, a 300% modulus of about 18.5 MPa, a tensile strength of about 30.1 MPa, an elongation at break of about 473%, and a tan delta of about 0.15 at 60°C.
[0063] When two or more forms of carbon are used, the first carbon black in the composite may be heat treated at a temperature between 1100°C and 1800°C to provide a more crystalline structure than the second carbon black. The partially crystalline first carbon black may have a carbon structure of 120 cm 3 / 100g to 200cm 3 / 100g OAN structure, measured according to ASTM D2414-22 "Standard Test Method for Carbon Black—Oil Absorption Number (OAN)", and to The Raman crystallite planar size (La) is measured according to the method of Gruber et al., "Raman Studies of Heat-Treated Carbon Blacks", Carbon, Vol. 32 (7), pp. 1377, pp. 1382 (1994).
[0064] In one embodiment, the carbon black has a carbon black content of at least 95 m / s as measured by STSA. 2 / g of external surface area and greater than 80mL / 100g of dibutyl phthalate adsorption, and the composite material contains at least 65phr of carbon black. In another specific embodiment, the carbon black has at least 75m / 100g of external surface area as measured by STSA. 2 / g surface area and greater than 60mL / 100g dibutyl phthalate adsorption, and the composite material contains at least 70phr of carbon black. In another specific embodiment, the carbon black is present in the composite material in an amount satisfying L≥-0.26*S+94, where L is the amount of carbon black in the composite material, in phr, and S is the surface area of the carbon black measured by STSA, in m 2 These and other suitable composite materials are described, for example, in U.S. Patent Publication No. 20150105491A1.
[0065] Although the composite material may consist essentially of carbon black and natural rubber (e.g., these two materials total at least 95% by weight, or at least 98% by weight, or up to 100% by weight of the composite material), it is also contemplated that the composite material may include other components. For example, in one embodiment, 2 to 25% by weight, or up to 15% by weight, or up to 8% by weight of the composite material may include other rubber-forming elastomers. These other elastomers may include other conjugated diene elastomers, such as synthetic cis-1,4-polyisoprene, polybutadiene, butadiene copolymers, isoprene copolymers, and mixtures of these elastomers. Suitable copolymers may be selected from butadiene / styrene copolymers, isoprene / butadiene copolymers, isoprene-styrene copolymers, and copolymers of isoprene / butadiene / styrene.
[0066] Composite materials can be formed by mixing carbon black with natural rubber at a suitable temperature (e.g., at least 100° C., or at least 120° C.) for a sufficient time to obtain a highly dispersed mixture. In one embodiment, carbon black is added to natural rubber as a slurry, and the mixture is coagulated using a coagulant (e.g., an acid). This method is described in U.S. Patent No. 9156955B2. Slurry can be formed by mixing carbon black and water, which can be ground to improve dispersibility, such as described in U.S. Patent Publication No. 20150105491A1.
[0067] Conjugated diene based elastomers
[0068] The conjugated diene-based elastomer (which does not form part of the composite) may be present in the rubber composition in an amount of at least 3 phr, or at least 5 phr, or at least 6 phr, or at least 8 phr, or at least 10 phr, at least 12 phr, and / or at most 90 phr, or at most 80 phr, or at most 60 phr, or at most 40 phr, or at most 30 phr, or at most 20 phr, or at most 16 phr, for example in an amount of 10 to 30 phr.
[0069] In one embodiment, the weight ratio of conjugated diene-based elastomer to natural rubber present in the composite is at least 5:95, or at least 6:94, or at least 10:90, or at least 12:88, or at most 30:70, or at most 25:75, or at most 20:80.
[0070] Elastomers based on conjugated dienes are composed of one or more elastomers derived from conjugated dienes alone or primarily (e.g., at least 60 wt %, or at least 90 wt %, or at least 95 wt %). For example, elastomers based on conjugated dienes can be selected from natural rubber, synthetic polyisoprene, polybutadiene, and mixtures and copolymers thereof. These elastomers all contain double bonds in each monomer unit.
[0071] Natural rubber is primarily derived from isoprene (2-methyl-1,3-butadiene) and is therefore primarily (e.g., at least 99% by weight) polyisoprene. As used herein, the term "natural rubber" refers to naturally occurring rubber, such as can be harvested from sources such as Hevea rubber trees and non-Hevea sources (e.g., guayule shrubs and dandelions such as TKS). In other words, the term "natural rubber" should be interpreted as excluding synthetic polyisoprene. Natural rubber produced from the rubber plantation gel (cup gel) of the Hevea brasiliensis tree is a common form of natural rubber. For example, technical graded rubber or block rubber (TSR) is a natural rubber available from Indonesia, where it may be referred to as standard Indonesian rubber (SIR), standard Malaysian rubber (SMR), and standard Thai rubber (STR). It is available in a variety of grades, including TSR 10 and TSR 20, with the TSR 10 grade having a higher purity.
[0072] In one embodiment, the conjugated diene based elastomer is at least 60 wt% natural rubber, or at least 80 wt%, or at least 90 wt%, or at least 95 wt%, or up to 100 wt% natural rubber.
[0073] In some embodiments, synthetic polyisoprene, particularly cis-1,4-polyisoprene having a cis content of at least 94 weight percent, or at least 96 weight percent, can be used in the conjugated diene-based elastomer. The Tg of the synthetic polyisoprene can be between -60°C and -70°C. In one embodiment, a mixture of synthetic polyisoprene and natural rubber is used as the conjugated diene-based elastomer.
[0074] Other conjugated diene-based elastomers may optionally be present in small amounts (e.g., up to 10 phr, or up to 5 phr, or up to 2 phr in total), which may include one or more of butadiene rubber (BR), isoprene-isobutylene copolymers, and halogenated butyl rubbers (e.g., bromobutyl rubber and chlorobutyl rubber).
[0075] Other vulcanizable elastomers
[0076] In addition to the natural rubber and the conjugated diene-based elastomer present in the composite material, other vulcanizable elastomers may be present in the rubber composition in small amounts (e.g., up to 10 phr, or up to 5 phr, or up to 2 phr in total) and may be selected from nitrile rubber, liquid rubber, polynorbornene copolymer, ethylene-propylene-diene rubber, chloroprene rubber, acrylate rubber, fluororubber, silicone rubber, polysulfide rubber, epichlorohydrin rubber, styrene-isoprene-butadiene terpolymer, hydrated acrylonitrile-butadiene rubber, isoprene-butadiene copolymer, butyl rubber , hydrogenated styrene-butadiene rubber, butadiene-acrylonitrile rubber, terpolymers formed from ethylene monomers, propylene monomers and / or ethylene propylene diene monomer (EPDM), isoprene-based block copolymers, butadiene-based block polymers, styrene block copolymers, styrene-butadiene-styrene block copolymers (SBS), styrene-ethylene / butylene-styrene block copolymers (SEBS), styrene-[ethylene-(ethylene / propylene)]-styrene block polymers (SEEPS), random styrene copolymers, hydrogenated styrene block copolymers, Styrene-butadiene copolymers, polyisobutylene, ethylene-vinyl acetate (EVA) polymers, polyolefins, amorphous polyolefins, semi-crystalline polyolefins, alpha-polyolefins, reactor-ready polyolefins, acrylates, metallocene-catalyzed polyolefin polymers and elastomers, reactor-made thermoplastic polyolefin elastomers, olefin block copolymers, copolyester block copolymers, polyurethane block copolymers, polyamide block copolymers, thermoplastic polyolefins, thermoplastic vulcanizates, ethylene vinyl acetate copolymers , ethylene n-butyl acrylate copolymer, ethylene methyl acrylate copolymer, chloroprene rubber, acrylic resin, polyurethane, poly (acrylate), ethylene acrylic acid copolymer, polyether ether ketone, polyamide, atactic polypropylene, polyethylene (including atactic polypropylene), ethylene-propylene polymer, propylene-hexene polymer, ethylene-butene polymer, ethylene-octene polymer, propylene-butene polymer, propylene-octene polymer, metallocene-catalyzed polypropylene polymer, metallocene-catalyzed polyethylene polymer, ethylene-propylene-butene terpolymer, composed of propylene, ethylene, C4-C 10Copolymers prepared from α-olefin monomers, polypropylene polymers, maleated polyolefins, polyester copolymers, copolyester polymers, ethylene acrylic acid copolymers and / or polyvinyl acetate, and / or wherein the polymers are optionally modified and / or functionalized at pendant positions of the polymer chain and / or within the polymer and mixtures thereof to include one or more selected from hydroxyl-, ethoxy-, epoxy-, siloxane-, amine-, aminosiloxane-, carboxyl-, phthalocyanine- and silane-sulfide groups.
[0077] In one embodiment, the rubber composition is free of such other vulcanizable elastomers.
[0078] Reinforcement filler
[0079] In addition to the carbon black found in the composite material, one or more reinforcing fillers may be present in the rubber composition. Examples of such reinforcing fillers include silicon dioxide, calcium carbonate (CaCO ), titanium dioxide, hydrated aluminum silicate clay, 2:1 layered silicate clay and organophilic clays formed therefrom, calcium silicate, graphite, graphene, carbon nanotubes, wollastonite, talc, diatomaceous earth, starch, lignin, aluminum oxide, another carbon black (e.g., different from the carbon black present in the composite material) and mixtures thereof.
[0080] The reinforcing filler(s) may be present in the rubber composition in an amount of 0 to 150 phr, for example at least 2 phr, or at least 4 phr, or at least 6 phr, or at least 8 phr, or at most 100 phr, or at most 80 phr, or at most 50 phr, or at most 20 phr, or at most 15 phr, at most 10 phr, for example 5 to 15 phr.
[0081] In one embodiment, the reinforcing filler comprises or consists of silica particles, such as amorphous (e.g., precipitated) silica and / or crystalline silica. The term "silica" is used herein to refer to silicon dioxide, SiO2 (which may contain small amounts of impurities, typically less than 1% by weight, resulting from the process of forming the silica). The term "precipitated silica" is used to refer to synthetic amorphous silica, typically obtained by a process of precipitating a silicate with an acidifying agent.
[0082] Silica can be present in the rubber composition in an amount of at least 2 phr, or at least 4 phr, or at least 6 phr, at least 8 phr, or up to 100 phr, or up to 80 phr, or up to 50 phr, or up to 20 phr, or up to 18 phr, or up to 15 phr, up to 10 phr, for example 5 to 15 phr.
[0083] Silica can be prepared by various methods. Precipitated silica can be prepared by digesting amorphous silica (e.g., amorphous silica present in rice husks or other biowaste) with sodium hydroxide to form sodium silicate, and precipitating silica from the sodium silicate by reacting with an acidulant (e.g., sulfuric acid or carbon dioxide). The resulting silica precipitate is washed and filtered. Methods for preparing precipitated silica are disclosed in U.S. Patents Nos. 5587416A, 5800608A, 5882617A, and 9359215B2, and U.S. Publication Nos. 20020081247A1 and 20050032965A1. Precipitated silica can also be formed from silica gel, such as described in U.S. Patents Nos. 5708069, 7550610, and 5789514. For example, silica gel can be derived by hydrophobizing silica hydrogel with, for example, organic mercaptosilanes and alkylsilanes and drying the product.
[0084] A variety of methods can be used to determine the surface area of silica. In the test method of ASTM D6845-20 "Standard Test Method for Silica, Precipitated, Hydrated—CTAB (Cetyltrimethylammonium Bromide) Surface Area", the measurement of the specific surface area of silica does not include the area contained in the micropores that are too small to accommodate CTAB molecules. This test method is applicable to characterizing all types of rubber-grade silica.
[0085] According to ASTM D6845-20, the silica used in the reinforcing filler may have a 2 / g, or at least 140m 2 / g, or at least 220m 2 / g, or at least 240m 2 / g CTAB specific surface area. Silica can have a surface area of up to 500 m 2 / g, or up to 400m 2 / g, or up to 300m 2 / g CTAB specific surface area.
[0086] Examples of precipitated silica suitable for use herein include Hi-Sil® from PPG Industries. TM 532.Hi-Sil TM 532EP and HiSil TM EZ 160G; Hubersil by JMHuber Company TM 4155; Zeosil TM, from Solvay, the names are 115GR, 125GR, 165GR, 175GR, 185GR, 195GR, 1085GR, 1165MP, 1115MP, HRS1200MP, Premium MP, Premium 200MP, Premium SW and 195HR; Ultrasil TM , from Evonik with the names VN2, VN3, VN3GR, 5000GR, 6000GR, 7000GR and 9000GR; Zeopol TM , from Evonik, the names are 8755LS and 8745; Newsil TM , 115GR and 2000MP from Wuxi Quechen Silicon Chemical Co., Ltd; and Tokusil from Maruo Calcium Co., Ltd TM 315, and mixtures thereof.
[0087] In one embodiment, the silica is present in the rubber composition in an amount of 1 phr or more, such as at least 2 phr, or at least 5 phr, or at least 6 phr, or at least 7 phr, or up to 20 phr, or up to 18 phr, or up to 15 phr, or up to 14 phr, or up to 12 phr, or up to 10 phr. The silica can be at least 2 phf, or at least 4 phf, or at least 8 phf, or at least 12 phf, or up to 25 phf, or up to 20 phf, or up to 18 phf of the reinforcing filler.
[0088] In one embodiment, the weight ratio of silica to total elastomer (eg, natural rubber) in the rubber composition is at least 4:100, or at least 6:100, and may be up to 20:100, or up to 15:100.
[0089] In one embodiment, the weight ratio of silica to carbon black in the rubber composition is at least 4:100, or at least 7:100, or at least 12:100, or at least 15:100, and may be at most 3:10, or at most 2:10.
[0090] In one embodiment, the silica may be surface treated, for example, with a coupling agent and / or polyalkylene oxide, such as polyethylene glycol, before the pretreated silica is incorporated into the rubber composition. Pretreatment may be used to enhance the dispersion and / or adhesion of the silica to the elastomer. In another embodiment, the silica may be treated in situ with a coupling agent and / or polyalkylene oxide in the rubber composition, typically prior to the addition of a curing agent.
[0091] Polyalkylene glycols that can be used for silica pretreatment or in-situ for rubber compositions include polyethylene glycol, polypropylene glycol and mixtures thereof. In one embodiment, polyalkylene oxide is polyethylene glycol. Polyalkylene oxide can have at least 500, for example at least 2000 or at least 4000 or at most 15000 or at most 12000 or at most 10000 or at most 8500 weight average molecular weight Mw. Polyalkylene oxide may not be present in the rubber composition. When using polyalkylene oxide (such as polyethylene glycol), it can be included in an amount of at least 0.1phr, for example at least 0.2phr or at least 0.3phr or at most 5phr or at most 3phr or at most 2phr or at most 1phr or at most 0.6phr.
[0092] Examples of commercially available polyethylene glycols include Carbowax TM PEG 3350 and Carbowaw TM PEG 8000, where the numbers represent the approximate weight average molecular weight. Other polyalkylene oxide polymers may be used, as described, for example, in US Pat. Nos. 6,322,811 and 4,082,703.
[0093] Suitable coupling agents generally include a first part that reacts with a hydroxyl group (e.g., silanol group) present on the surface of the precipitated silica and a second part that can react with a diene-based elastomer. The two parts are connected by a linking group (e.g., a hydrocarbon group or a sulfur bridge) so that the precipitated silica is bonded to the elastomer. Examples of silica coupling agents include those containing groups such as alkyl, alkoxy, sulfhydryl, end-capped sulfhydryl, sulfide-containing (e.g., containing monosulfide-based alkoxy, containing disulfide-based alkoxy, containing tetrasulfide-based alkoxy), amino, vinyl, epoxy, and combinations thereof. The amount of the silica coupling agent present can be sufficient to provide a ratio of the total amount of the coupling agent to the silica filler of at least 0.1:100 or at most 1:5, by weight, such as at least 1:100, or at least 1:50, or at most 1:20, or at most 1:10.
[0094] Additional reinforcing fillers other than silica and carbon black may be used, for example, in a total amount of up to 30 phr, or up to 20 phr, or up to 10 phr, or up to 1 phr, or may not be used. Examples of such additional reinforcing fillers include alumina, aluminum hydroxide, clay (reinforcing grade), magnesium hydroxide, boron nitride, aluminum nitride, titanium dioxide, reinforcing zinc oxide, and combinations thereof.
[0095] In one embodiment, the components of the rubber composition other than natural rubber, carbon black and silica are present in the rubber composition in a total amount of no more than 40 phr, or no more than 30 phr, or no more than 20 phr, or no more than 15 phr.
[0096] Processing Aids
[0097] Processing aids may be used in the rubber composition in amounts totaling from 1 to 20.0 phr, or up to 10 phr, or up to 5 phr, and may include one or more of resins and liquid plasticizers such as oils.
[0098] Examples of resins that can be used in the rubber composition include tackifying resins such as non-reactive phenolic resins and rigid resins such as reactive phenolic resins and resorcinol or resorcinol and hexamethylenetetramine, benzoxazine resins, hydrocarbon resins such as aromatic, aliphatic and alicyclic resins.
[0099] Examples of hydrocarbon resins may have a Tg of at least 30°C, or at most 50°C. The hydrocarbon resin Tg may be determined by DSC according to the procedure described above for elastomer Tg measurements. The hydrocarbon resin may have a softening point of at least 70°C, or at most 100°C. The softening point of a hydrocarbon resin is generally related to the Tg. The Tg is generally lower than its softening point, and the lower the Tg, the lower the softening point.
[0100] Examples of aliphatic resins include C5 fraction homopolymer and copolymer resins.Examples of cycloaliphatic resins include cyclopentadiene ("CPD") homopolymer or copolymer resins, dicyclopentadiene ("DCPD") homopolymer or copolymer resins, and combinations thereof.
[0101] Examples of aromatic resins include aromatic homopolymer resins and aromatic copolymer resins.Aromatic copolymer resins refer to hydrocarbon resins comprising one or more aromatic monomers in combination with one or more other (non-aromatic) monomers, wherein the majority by weight of all monomers are typically aromatic.
[0102] The specific example of aromatic resin includes coumarin-indene resin, alkyl-phenol resin and vinyl aromatic homopolymer or copolymer resin. The example of alkyl-phenol resin includes alkyl-phenol acetylene resin such as p-tert-butylphenol-acetylene resin, alkylphenol-formaldehyde resin (for example, resin with low polymerization degree). Vinyl aromatic resin can include one or more of the following monomers: α-methyl styrene, styrene, o-methyl styrene, m-methyl styrene, p-methyl styrene, vinyl toluene, p-(tert-butyl) styrene, methoxy styrene, chlorostyrene, hydroxystyrene, vinyl mesitylene, divinylbenzene, vinyl naphthalene etc. The example of vinyl aromatic copolymer resin includes vinyl aromatic / terpene copolymer resin (for example, limonene / styrene copolymer resin), vinyl aromatic / C5 fraction resin (for example, C5 fraction / styrene copolymer resin), vinyl aromatic / aliphatic copolymer resin (for example, CPD / styrene copolymer resin and DCPD / styrene copolymer resin).
[0103] In the case of an aromatic resin based on one or more of the above-mentioned vinyl aromatic monomers (e.g., styrene, α-methylstyrene), at least 80 wt. %, or at least 85 wt. %, or at least 90 wt. %, at least 95 wt. %, or up to 100 wt. % of the monomers in the aromatic resin may be aromatic monomers.
[0104] Other aromatic resins include terpene resins such as α-pinene resins, β-pinene resins, limonene resins (e.g., L-limonene, D-limonene, dipentene as a racemic mixture of L- and D-isomers), β-phellandrene, δ-3-carene, δ-2-carene, and combinations thereof.
[0105] In one embodiment, the hydrocarbon resin comprises a combination of aromatic and aliphatic / cycloaliphatic hydrocarbons. In this case, the total amount of any aliphatic and / or cycloaliphatic resins used in combination with the aromatic resins may be no more than 5 phr, or less than 4 phr, or less than 3 phr, or greater than 20 wt%, or no more than 15 wt%, or no more than 10 wt% of the total amount of hydrocarbon resins.
[0106] The aromatic resin may have a Mw of at least 1000 g / mole and / or at most 4000 g / mole.
[0107] The total amount of resin in the rubber composition may be at least 1 phr, or at least 2 phr, or at most 20 phr, or at most 10 phr, or at most 5 phr, or may be absent.
[0108] The term liquid plasticizer refers to a plasticizer component that is liquid at room temperature (i.e., liquid at 25°C and above), and includes oils and non-oils. In contrast to liquid plasticizers, hydrocarbon resins are generally solid at room temperature. Typically, the Tg of a liquid plasticizer will be below 0°C, typically much lower, such as below -30°C, or below -40°C, or below -50°C, such as a Tg of 0°C to -100°C.
[0109] Suitable liquid plasticizers include oils (e.g., petroleum and plant-derived oils) and non-oil liquid plasticizers, such as ether plasticizers, ester plasticizers, phosphate plasticizers, and sulfonate plasticizers. Liquid plasticizers can be added as tackifier oils (for filling rubber) during or after compounding. Petroleum-based oils can include aromatic, cycloparaffinic, low polycyclic aromatic (PCA) oils and mixtures thereof. Vegetable oils can include oils obtained from vegetables, nuts, seeds, and mixtures thereof, such as triglycerides. The Tg of the oil or oils used can be -40°C to -100°C.
[0110] When present, the rubber composition may include at least 1 phr of liquid plasticizer, or up to 20 phr, or up to 10 phr, or up to 5 phr of liquid plasticizer. In one embodiment, no liquid plasticizer is used.
[0111] In addition to one or more of the above processing aids, the rubber composition may also include a peptizing agent, such as pentachlorothiophenol, dibenzamide diphenyl disulfide, or mixtures thereof. If used, typical amounts of peptizing agents may range from 0.1 phr to 1 phr.
[0112] Antidegradants (antioxidants, antiozonants)
[0113] The rubber composition may include one or more antidegradants, such as antiozonants and / or antioxidants. These compounds help protect the tire from oxidation and ozonation. Representative antidegradants include amine-based antioxidants, such as monophenols, bisphenols, thiobisphenols, polyphenols, polymer hindered phenols, hydroquinone derivatives, phosphites, phosphate blends, thioesters, naphthylamines, diphenolamines and other diarylamine derivatives, p-phenylenediamine (PPD), quinolines and blended amines. Exemplary amine-based antioxidants include diphenyl-p-phenylenediamine, N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine (6PPD), oligomeric 2,2,4-trimethylquinoline (TMQ) and others such as those disclosed in The Vanderbilt Rubber Handbook (1978), pages 344-347. The antioxidant may be at least 0.1 phr, or at least 0.3 phr, or at least 1 phr, or at least 2 phr, or at most 10 phr, or at most 5 phr of the rubber composition.
[0114] Exemplary antiozonants include physical protectants, such as waxes. Suitable waxes include paraffin waxes and microcrystalline waxes, which may be of the type described in the Vanderbilt Rubber Handbook (1978), pages 346 and 347. The wax (or waxes) may be present in 0.1 phr or more, such as at least 0.3 phr, or at least 0.5 phr, or at most 5 phr, or at most 2 phr.
[0115] Curing packaging
[0116] Vulcanizing agent
[0117] An exemplary cure package includes a vulcanizing (curing) agent and one or more of a cure accelerator, a cure activator, and a cure inhibitor. The cure package may be used in the rubber composition at 0.5 to 20 phr, or at least 5 phr, or at most 10 phr.
[0118] The vulcanization of the rubber composition can be carried out in the presence of a sulfur-based vulcanizing agent. Examples of suitable sulfur-based vulcanizing agents include elemental sulfur (free sulfur), insoluble polymer sulfur, soluble sulfur, and sulfur-donating vulcanizing agents, such as amine disulfide, polymeric polysulfide, or sulfur-olefin adducts and mixtures thereof.
[0119] In the rubber composition, the sulfur vulcanizing agent may be used in an amount of 0.1 to 10 phr, such as at least 0.3 phr, or at least 0.4 phr, or at least 0.5 phr, or at least 0.7 phr, or at most 5 phr, or at most 3 phr.
[0120] Curing accelerator, curing activator, curing retardant
[0121] Curing accelerator acts as a catalyst for vulcanizing agent. Suitable curing accelerators include amines, disulfides, guanidines, thioureas, thiazoles, thiurams, sulfenamides, dithiocarbamates and xanthates. Examples of thiazole curing accelerators include 2-mercaptobenzothiazole and 2,2'-disulfide bis(benzothiazole) (MBTS). Examples of sulfenamide curing accelerators include benzothiazole sulfenamides, such as N-cyclohexyl-2-benzothiazole sulfenamide (CBS) and N-tert-butyl-2-benzothiophene sulfenamide (TBBS). Guanidine curing accelerators include diphenylguanidine (DPG).
[0122] Curing accelerators with a fast vulcanization initiation time (referred to as "t0") of less than 3 minutes are referred to as super accelerators. Examples of super accelerators that can be used include 1,6-bis(N,N'-dibenzylthiocarbamoyldithio)hexane (BDBZTH), tetrabenzylthiuram disulfide (TBzTD), tetramethylthiuram monosulfide (TMTM), tetramethylthiuram disulfide (TMTD), tetraethylthiuram disulfide (TETD), tetraisobutylthiuram disulfide (TiBTD), dipentamethylenethiuram tetrasulfide (DPTT), zinc dibutyldithiocarbamate (ZDBC), zinc diethyldithiocarbamate, zinc dimethyldithiocarbamate, copper dimethyldithiocarbamate, diethyldithiocarbamate, and diethyldithiocarbamate. Tellurium carbamate (TDEC), zinc dibenzyl dithiocarbamate (ZBED), zinc diisononyl dithiocarbamate, zinc pentamethylene dithiocarbamate, zinc dibenzyl dithiocarbamate (ZBEC), zinc isopropyl xanthate (ZIX), zinc butyl xanthate (ZBX), sodium ethyl xanthate (SEX), sodium isobutyl xanthate (SIBX), sodium isopropyl xanthate (SIPX), sodium n-butyl xanthate (SNBX), sodium amyl xanthate (SAX), potassium ethyl xanthate (PEX), potassium amyl xanthate (PAX), zinc 2-ethylhexyl dithiophosphate (ZDT / S), and mixtures thereof.
[0123] In some cases, a combination of accelerators is used, one of which acts faster than another.
[0124] The curing accelerator can be incorporated into the rubber composition in an amount of 0.1 to 10 phr, or at least 0.5 phr, or at least 1 phr, or at least 2 phr, or at most 8 phr, or at most 5 phr. The amount of the curing accelerator can be selected to provide an acceptable curing time, for example, below 90 minutes.
[0125] Cure activators are additives used to support vulcanization. Cure activators include inorganic and organic cure activators. Zinc oxide is a widely used inorganic cure activator, and when used, zinc oxide can be present at 1 phr to 10 phr, such as at least 2 phr, or at most 5 phr.
[0126] Organic curing activators include stearic acid, palmitic acid, lauric acid, mixtures thereof, zinc salts of each of the foregoing, and thiourea compounds such as thiourea, and dialkylthioureas such as dialkylthioureas and diarylthioureas, and mixtures thereof. Specific thiourea compounds include N, N'-diphenylthiourea, trimethylthiourea, N, N'-diethylthiourea (DEU), N, N'-dimethylthiourea, N, N'-dibutylthiourea, ethylenethiourea, N, N'-diisopropylthiourea, N, N'-diisopropylthiourea-dicyclohexylthiourea, 1,3-di(o-tolyl)thiourea, 1,3-di(p-tolyl)thiourea, 1,1-diphenyl-2-thiourea, 2,5-dithiourea, guanosinethiourea, 1-(1-naphthyl)-2-thiourea, 1-phenyl-2-thiourea, p-tolylthiourea, and o-tolylthiourea. One commonly used organic curing activator is a blend of stearic acid, palmitic acid, and oleic acid, with stearic acid being the major component of the blend.
[0127] When used, the total amount of organic curing activator(s) may be from 0.1 to 6 phr, such as at least 0.5 phr, or at least 1 phr, or up to 4 phr.
[0128] Curing agents are used to control the vulcanization process and generally delay or inhibit vulcanization until the desired time and / or temperature is reached. Examples of cure retarders include cyclohexylthiophthalimide.
[0129] When used, the amount of cure retarders may be at least 0.1 phr, or at most 3 phr, or at most 2 phr.
[0130] Composition Examples
[0131] Table 1 shows exemplary rubber compositions according to aspects of the exemplary embodiments.
[0132] Table 1: Rubber composition examples
[0133]
[0134] Preparation of rubber composition
[0135] The rubber composition may be prepared by mixing the composite material, natural rubber and / or (if used) other vulcanizable elastomers, silica and other rubber compounding ingredients (excluding the curative) with at least one mechanical mixer in at least one sequential mixing stage, generally referred to as a "non-productive" mixing stage, or stage(s), at elevated temperatures under high shear rubber mixing conditions, followed by a final "productive" mixing stage wherein a sulfur-based curing package, such as a sulfur-based curative and a cure accelerator, is added to the mix and mixed at a lower mixing temperature to avoid unnecessary pre-curing of the rubber mixture during the mixing stage.
[0136] The ingredients can be mixed for a few minutes in a non-productive mixing stage at a temperature of 115°C to 150°C, such as about 124°C. Once the curing package is added, the subsequent productive mixing step can be carried out at a temperature below the vulcanization (curing) temperature to avoid undesirable pre-curing of the rubber composition, such as below 180°C, or no more than 160°C, or no more than 120°C, such as at least 40°C, at least 60°C, such as at a temperature of 100-115°C for 2 minutes. Mixing can be carried out by kneading the ingredients together, such as in a Banbury mixer or on a rolling roller. Between each mixing stage, the rubber composition can be cooled to a temperature below 40°C. For example, the rubber composition can be poured from the mixer after each mixing step, taken out from an open mill, and cooled to below 40°C after each mixing step.
[0137] When the curing package is fully mixed, the rubber composition can be extruded, molded or otherwise shaped to form an article, such as a tire tread. The temperature of the mixture can be raised to achieve curing. The curing of the pneumatic tire or its part can be carried out at a temperature of 120° C. to 200° C., such as at least 140° C. or at most 180° C., about 150° C. Any conventional vulcanization method can be used, such as heating in a press or mold, or heating with superheated steam or hot air. Such tires can be constructed, shaped, molded and cured by various known methods, which methods are apparent to those skilled in the art.
[0138] In one embodiment, a tire is provided, the tire having a tread formed at least in part by an exemplary rubber composition. Other parts of the tire, such as a tire sidewall or a wire coating, may additionally or alternatively be formed at least in part by a rubber composition as described herein. The tire may be a pneumatic tire for a road vehicle (such as a car or truck), or a tire for an off-road vehicle, an aircraft, etc. The tire tread may have a tread depth of at least 20 mm, such as 22-28 mm, which is suitable for use in a truck.
[0139] The rubber composition is not limited to use in tires, but can be used in rubber gloves, surgical instruments, and the like.
[0140] Nature of the product
[0141] The use of the rubber composition in a tire, for example in a tire tread, can provide the tire with improved or desirable tread properties. These improved or desirable properties may include tear resistance and elongation at break. The rubber composition may also improve the properties of wire coatings and base formulations.
[0142] These improvements have been made in part through laboratory research, plant-scale testing, and commercial composite materials from Cabot Corporation, E2C TM Field evaluation of DX9640 has demonstrated that replacing part of the natural rubber in a rubber composition with a composite natural rubber and carbon black material can significantly enhance compound properties (particularly stiffness and wear resistance) that contribute to improved mileage.
[0143] Without intending to limit the scope of the exemplary embodiments, the following examples illustrate the preparation of exemplary rubber compositions using the composite materials and their properties.
[0144] Example
[0145] Table 1 Tire tread cap formulations were prepared with the goal of achieving comparable or better tread wear (e.g., as shown in the Grosch test of a medium radial truck (MRT) tire), improved rolling resistance (as shown using rebound at 100°C), and comparable or better tear resistance (as shown by original and aged Strebler adhesion at 100°C) when using the composites. Tire base and wire coating formulations were also prepared with the goal of achieving rolling resistance and tear resistance.
[0146] Example 1
[0147] Rubber compositions suitable for truck tire tread caps were prepared using the formulations shown in Table 2.
[0148] Examples A, B and C were prepared using ASTM N121 grade carbon black and natural rubber, without the use of composite materials. Example A was formulated as a baseline tread composition suitable for a radial medium truck tire. Example B added silica to the baseline composition, and Example C used a modified cure package.
[0149] For these three examples, in the first mixing stage, the natural rubber was mixed with part of the carbon black (30 phr) until the mixture reached 160°C. It was then dripped from the mixer and cooled. In the second mixing stage, the remaining carbon black (18 phr), silica (if used), wax and antioxidant were added. In the productive mixing stage, sulfur, accelerator and cure retarder were added and the mixture was dripped from the mixer at a temperature below the cure temperature.
[0150] Examples D, E and F were prepared using natural rubber and a composite material (a material containing about 64.5% by weight natural rubber and 35.5% by weight carbon black). The amounts of carbon black and natural rubber in these three compositions were about the same as those in the benchmark formulations A, B and C. Silica was used in each of these examples. Example E used a modified curing package, and Example F used a higher surface area silica than Examples D and E.
[0151] To prepare Example D, E and F, in a single non-productive stage, the composition was mixed until the temperature reached 124 ° C and dripped from the mixer. In the productive stage, sulfur, accelerator and cure retarder were added, and the mixture composition was mixed in the mixer until it reached 104 ° C and dripped from the mixer. In this stage, the rotor speed remained constant at 50 rpm. Mixing at a lower temperature in the non-productive and productive stages helps to maintain the polymer filler network in the composite material, thereby maintaining performance indicators. In the curing stage, the rubber composition was heated to a temperature of 150 ° C for 32 minutes.
[0152] Table 2: Rubber composition formulation (in phr)
[0153]
[0154] 1 E2C from Cabot Corporation TM DX9640 Carbon Black Masterbatch
[0155] 2 Carbon Black from Birla Carbon ASTM N121
[0156] 3 Amorphous precipitated silica from Evonik 6100GR, which has about 160m 2 / g of BET nitrogen surface area.
[0157] 4 Amorphous precipitated silica, obtained from Solvay as Premium SW, having a density of about 250 m 2 / g of CTAB surface area.
[0158] 5 A blend of microcrystalline wax and paraffin wax.
[0159] 6 Predominantly stearic acid (at least 90% stearic acid) such as a blend of stearic acid, palmitic acid and oleic acid.
[0160] 7 Blends of p-phenylenediamine and quinoline.
[0161] 8 Elemental sulfur.
[0162] 9 N-tert-Butylbenzothiazolesulfenamide (TBBS).
[0163] 10 N-(Cyclohexylthio)phthalimide (CTP).
[0164] The performance tests of the cured samples were carried out as follows:
[0165] Specific gravity: measured according to ASTM D297-21 "Standard Test Methods for Rubber Products—Chemical Analysis".
[0166] Cured stiffness: Storage modulus G' was determined by a rubber process analyzer (RPA 500). Storage modulus values were measured at a temperature of 40°C on uncured samples after curing at 10% strain and at 10% and 50% strain (in MPa). Measurements on cured samples indicate the ride and handling properties of tires using the rubber composition in the tread. Tan delta values (ratio of G' to G') at 10% strain were also obtained.
[0167] Tensile properties: The loop tensile modulus (MPa), tensile strength (MPa) and elongation at break (%) of the samples before and after aging were measured using an Instron Corporation instrument at 300% strain.
[0168] Rolling resistance predictor: The rebound percentage is measured on cured samples at a given temperature using a ZwickRoell 5109 Rebound Elastometer as an indicator of the tire's wet braking ability, with higher values being better, according to ASTM D7121-05 (2018) "Standard Test Method for Rubber Property—Resilience Using Schob Type Rebound Pendulum". Rebound is a measure of the hysteresis of a compound when subjected to a load. Generally, the higher the measured rebound, the lower the rolling resistance.
[0169] Strebler Adhesion Steady State Average Load is determined at 100°C on cured samples before and after aging. This is a peel test that determines interfacial adhesion by pulling one rubber composition away from another rubber composition at right angles with an untorn test specimen, and the two ends of the rubber composition pulled apart at 180° from each other.
[0170] Crack Growth: DeMattia notch growth (mm / min) was measured on aged samples at 95°C according to ASTM D813-07 (2019) “Standard Test Method for Rubber Deterioration—Crack Growth”. In Table 3, the higher the notch growth rate, the greater the resistance of the tread groove to surface crack growth.
[0171] Wear resistance: Indicates the tread wear condition, determined by the Grosch wear rate, in mg / km of rubber worn. When the test rubber sample moves a given distance on a rotating abrasive disc, it is placed under a constant load (Newton) at a certain slip angle. Medium and high wear severity tests are performed. The main difference between the two tests is the load and the slip angle. The high severity Grosch is the average of two samples run at a load of 70N and a 12 degree angle, while the medium severity is the average of two tests run at loads of 70N and 40N and at angles of 12 and 6 degrees respectively.
[0172] The results are shown in Table 3. The results were normalized and the result of Example A was set to 100. All parameters were generally better as higher as possible.
[0173] Table 3: Results
[0174]
[0175] The results in Table 3 show that Examples D and E have higher aged Strebler adhesion values and better wear resistance at high severity, and better wear resistance at reduced medium severity wear resistance. By replacing part of the natural rubber in the formulation with a composite material, an improved balance of performance indicators is achieved. Example F shows similar improvements in Strebler values as Examples D and E, with a compromise in wear resistance at low and high severity.
[0176] Example E is the same as Example D except that it contains slightly less sulfur, accelerator, and cure retarder. Example E improves the rolling resistance index by 10% over Example A, while also improving the composite tear resistance index and high severity Grosch wear resistance, while maintaining stiffness and elongation at break within the general guidelines for long-distance driving applications.
[0177] In the samples containing composites, an increase in the dispersion percentage based on a higher 300% to 100% tensile modulus ratio (i.e., better filler-polymer interaction) was observed. In this case, an additional non-productive mixing step can further improve the dispersion and processing indicators.
[0178] Example 2
[0179] Rubber compositions suitable for use as truck tire tread bases were prepared using the formulations shown in Table 4.
[0180] Examples G, H and I were prepared using ASTM N347 grade carbon black and natural rubber, without using composite materials. Example G was formulated as a baseline tread base composition suitable for a medium-duty truck radial tire. Compared to the baseline composition, Example H partially replaced the carbon black with silica, and Example I used a modified cure package.
[0181] For these three examples, in the first mixing stage, natural rubber is mixed with part of the carbon black (up to 17.1 phr), silica (up to 9.7 phr), oil and curing activator until the mixture reaches 155°C. It is then dripped from the mixer and cooled. In the second mixing stage, silica (up to 5.5 phr) and silane are mixed at a temperature of 145°C. After cooling, the remaining carbon black (up to 5 phr), silica (up to 1.8 phr), wax and antioxidant are mixed in the third mixing stage. In the productive mixing stage, sulfur, accelerator and curing retarder are added and the mixture is dripped from the mixer at a temperature below the curing temperature.
[0182] Examples J and K were prepared using natural rubber and a composite material (a material containing about 64.5% by weight natural rubber and 35.5% by weight carbon black). The amounts of carbon black and natural rubber in these three compositions were approximately the same as those in the benchmark formulations G, H, and I. Silica was used in each of these examples. Example K used the same curing package as Example I.
[0183] In order to prepare Example J and K, the first non-productive stage is similar to the first non-productive stage of Example H and I. The difference is that the content of natural rubber is lower in the first non-productive stage of Example J and K. The second non-productive stage of Example J and K corresponds to the non-productive stage of Example H and I. In the third non-productive stage, the composite material in Example J and K and the remaining amount of silica (1.8phr) and weathering protective agent are added and mixed until the temperature reaches 124°C. In the productive stage, sulfur, accelerator and curing retarder are added, and the mixture composition is mixed in a mixer until it reaches 104°C and drips out from the mixer. At this stage, the rotor speed remains constant at 50rpm. In the curing stage, the rubber composition is heated to a temperature of 150°C for 32 minutes.
[0184] Table 4: Rubber composition formulation (in phr)
[0185] Components Example G Example H Embodiment 1 Example J Example K <![CDATA[Composite material 1 > 0 0 0 48.2 48.2 Natural rubber (in composites) 0 0 0 31.1 31.1 Carbon black (in composites) 0 0 0 17.1 17.1 Natural rubber (additional) 90 90 90 58.9 58.9 Synthetic polyisoprene (additional) 10 10 10 10 10 <![CDATA[Carbon black (loose) 2 > 20 17.1 17.1 0 0 <![CDATA[Silicon dioxide 3 > 13.5 16.4 16.4 16.4 16.4 Silica coupling agent 1.36 1.36 1.36 1.36 1.36 Oil 1.8 1.8 1.8 1.8 1.8 <![CDATA[Stearic acid 4 > 1 1 1 1 1 <![CDATA[Antioxidants and antiozonants 5 > 3.5 3.5 3.5 3.5 3.5 <![CDATA[Sulfur 6 > 3.13 3.13 3.92 3.13 3.92 <![CDATA[Accelerator 7 > 1.15 1.15 1.18 1.15 1.18 <![CDATA[Curing retarder 8 > 0.1 0 0.1 0.06 0.16 Total phr 149.54 149.44 150.36 149.50 150.42
[0186] 1 E2C from Cabot Corporation TM DX9640 Carbon Black Masterbatch
[0187] 2 Carbon Black ASTM N347 from Orion Engineered Carbons
[0188] 3 Amorphous precipitated silica from Evonik 6100GR
[0189] 4 Predominantly stearic acid (at least 90% stearic acid) such as a blend of stearic acid, palmitic acid and oleic acid.
[0190] 5 Blends of p-phenylenediamine and quinoline.
[0191] 6 80% oil treated sulfur (90% insoluble)
[0192] 7 N-tert-Butylbenzothiazolesulfenamide (TBBS).
[0193] 8 N-(Cyclohexylthio)phthalimide (CTP).
[0194] The results for these formulations are shown in Table 5.
[0195] Table 5: Results
[0196]
[0197] Example K improves Bose fatigue and RPA 500tan(δ) values while maintaining Strebler, DeMattia and elongation at break results above the minimum acceptable values defined in the General Guidelines for MTR Tread Base Compounds. Improvements in cured stiffness (G') and tensile properties were also observed.
[0198] The results of Examples 1 and 2, as well as other evaluations not reported herein, indicate that improvements in tread wear and tire mileage can be achieved using the exemplary compositions without significant compromises in other parameters, such as tear and rolling resistance / hysteresis, typically experienced when modifying rubber compositions. This suggests that the exemplary compositions can expand the "performance triangle" of rolling resistance, tear, and tread wear, thereby overcoming challenges commonly faced during the development of new composite formulations for tire programs.
[0199] Each of the above-mentioned files is incorporated herein by reference.Except in the embodiment or otherwise clearly indicated, all numerical values of the amount, reaction conditions, molecular weight, carbon number, etc. of the specified material in this specification are understood to be modified by the word "about".Unless otherwise stated, each chemical substance or composition mentioned herein should be interpreted as commercial grade material, which may contain isomers, by-products, derivatives and other such materials generally understood to be present in commercial grade.However, unless otherwise stated, the amount of each chemical component does not include any solvent or diluent oil generally present in commercial materials.It should be understood that the upper and lower limits, scopes and ratios described herein can be independently combined.Similarly, the scope and amount of each element of the present invention can be used together with the scope or amount of any other element.
[0200] It should be understood that the above disclosed variants and other features and functions, or alternatives thereof, may be incorporated into many other different systems or applications. Those skilled in the art may subsequently make various currently unforeseen or unanticipated substitutions, modifications, variations or improvements thereto, which are also intended to be covered by the appended claims.
Claims
1. A rubber composition, characterized in that: A composite material of at least 20 phr characterized by reinforcing carbon black dispersed in natural rubber; at least 3 phr of a conjugated diene elastomer, said composite material and the conjugated diene elastomer together providing at least 90 phr of a vulcanizable elastomer in said rubber composition; Cure activator, and Sulfur based curing agent.
2. The rubber composition according to claim 1, characterized in that The rubber composition comprises at least 5 phr of silica.
3. The rubber composition according to claim 1, characterized in that The composite material provides at least 20 phr of reinforcing carbon black to the rubber composition.
4. The rubber composition according to claim 1, characterized in that The composite material provides at least 50 phr of natural rubber to the rubber composition.
5. The rubber composition according to claim 1, characterized in that The composite material is solid.
6. The rubber composition according to claim 1, characterized in that The conjugated diene elastomer includes at least one of natural rubber and synthetic polyisoprene.
7. The rubber composition according to claim 1, characterized in that The rubber composition comprises at least 5 phr of a conjugated diene elastomer.
8. The rubber composition of claim 1 further characterized by at least 1 phr of at least one of an antioxidant and an antiozonant.
9. An article formed from the composition of claim 1.
10. The product according to claim 9, characterized in that Tire tread.