Composite material, preparation method and application thereof, and decorative product
By combining modified cellulose nanofibers with polypropylene, combined with compatibilizers and stabilizers, the problem of traditional automotive interior door panel materials being difficult to balance between low odor and mechanical properties is solved, achieving a composite of low odor and high tensile strength. Material, suitable for decorative products, and more environmentally friendly.
Patent Information
- Application Number
- CN202410745527.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-11
- Publication Date
- 2024-10-01
AI Technical Summary
When traditional car interior door panel materials are modified with talc powder, it is difficult to achieve both low odor and excellent mechanical properties, and the deodorants used are chemical raw materials, which is not conducive to low-carbon and environmental protection.
Modified cellulose nanofibers are used to replace the inorganic filler talc, combined with polypropylene, compatibilizers, heat stabilizers, antioxidants and light stabilizers, and the specific ratio of modified cellulose nanofibers and polypropylene through silane coupling agents , reducing the odor of composite materials while maintaining good mechanical properties.
The composite material has excellent low odor and mechanical properties, meets the requirements of decorative products for low odor and high tensile strength, and the material is more environmentally friendly.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of polymer composite materials, and in particular to a composite material, a preparation method and application thereof, and a decorative product. Background Art
[0002] With the development of the national economy and the transportation industry, the number of cars has increased rapidly, and the pursuit of cars has gradually upgraded. Healthy and environmentally friendly interior space has become a new consumer demand. Customers are particularly concerned about the smell in the cab; the proportion of bio-based materials used in cars needs to be gradually increased.
[0003] Car interior door panels are mostly made of polypropylene, most of which are modified with talcum powder filler. Talc comes from the processing of natural stone, which is not conducive to low carbon and environmental protection, and it is difficult to take into account both low odor and excellent mechanical properties of plastic products.
[0004] Therefore, the traditional technology still needs to be improved. Summary of the invention
[0005] Based on this, it is necessary to provide a composite material and its preparation method, application and product, which composite material not only has excellent comprehensive mechanical properties but also has low odor.
[0006] This application is implemented through the following technical solutions:
[0007] In one aspect of the present application, a composite material is provided, wherein the raw materials for preparing the composite material include the following components in parts by weight:
[0008] Polypropylene 55 to 90 parts;
[0009] 5 to 20 parts of modified cellulose nanofibers;
[0010] 2~5 parts of compatibilizer;
[0011] 3~5 parts of heat stabilizer;
[0012] 0.1 to 0.6 parts of antioxidant;
[0013] Light stabilizer 0.2~0.5 parts;
[0014] The method for preparing the modified cellulose nanofibers comprises the following steps:
[0015] The cellulose nanofibers, the silane coupling agent and the solvent are mixed to prepare the modified cellulose nanofibers;
[0016] The weight ratio of the polypropylene to the modified cellulose nanofiber is (2.75-18):1.
[0017] The above-mentioned composite material of the present application introduces a silane coupling agent into the cellulose nanofiber for modification, and at the same time, the modified cellulose nanofiber and polypropylene, a compatibilizer, a heat stabilizer, an antioxidant and a light stabilizer act together. By controlling the specific ratio of each preparation raw material and the specific weight percentage of polypropylene and the modified cellulose nanofiber, the components act synergistically, which promotes the addition of the modified cellulose nanofiber and the compatibilizer, while reducing the odor of the composite material, maintaining good mechanical properties, so that the composite material has both excellent low odor and mechanical properties, so that it can meet the requirements of decorative products for low odor and high tensile strength performance.
[0018] In some embodiments, the mixing temperature is 70°C to 110°C; and / or
[0019] The mixing time is 30 min to 50 min; and / or
[0020] The silane coupling agent includes one or more of KH550, KH540 and KH791.
[0021] In some embodiments, the solvent comprises ethanol.
[0022] In some embodiments, the raw materials for preparation include the following components by weight:
[0023] Polypropylene 60~80 parts;
[0024] 10-20 parts of modified cellulose nanofibers;
[0025] 2~5 parts of compatibilizer;
[0026] 3~5 parts of heat stabilizer;
[0027] 0.1 to 0.6 parts of antioxidant;
[0028] Light stabilizer 0.2~0.5 parts.
[0029] In some of the embodiments, the weight ratio of the polypropylene to the modified cellulose nanofibers is (3-15):1.
[0030] In some embodiments, the compatibilizer comprises a maleic anhydride grafted compatibilizer; and / or
[0031] The heat stabilizer includes one or more of a zinc stabilizer and an amine stabilizer.
[0032] In some embodiments, the antioxidant includes a primary antioxidant and a secondary antioxidant, and the weight ratio of the primary antioxidant to the secondary antioxidant is (1-3): 1;
[0033] The primary antioxidant includes antioxidant 1010;
[0034] The secondary antioxidant includes one or more of antioxidant 168 and antioxidant 618; and / or
[0035] The light stabilizer includes an ultraviolet absorber and a free radical scavenger, and the weight ratio of the ultraviolet absorber to the free radical scavenger is (1-5):1.
[0036] On the other hand, the present application also provides a method for preparing a composite material, comprising the following steps:
[0037] The raw materials for preparing the composite material are mixed and extruded into shape.
[0038] On the other hand, the present application also provides the use of the above composite material in the preparation of decorative products.
[0039] The present application also provides a decorative product, which comprises the composite material mentioned above or a composite material prepared by the method for preparing the composite material mentioned above. DETAILED DESCRIPTION
[0040] For ease of understanding of the present application, the present application will be described more fully below, and preferred embodiments of the present application are provided. However, the present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present application more thorough and comprehensive.
[0041] The implementation of this application is described in detail below in combination with some implementation methods and examples. This example is implemented based on the technical solution of this application, and provides a detailed implementation method and specific operation process, but the protection scope of this application is not limited to the following examples.
[0042] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.
[0043] the term
[0044] Unless otherwise specified or incompatible herewith, the terms and phrases used herein shall have the following meanings:
[0045] In the present application, "plurality", "multiple" and the like, unless otherwise specified, refer to a number greater than or equal to 2. For example, "one or more" means one or greater than or equal to two.
[0046] In the present application, the terms "further", "particularly" and the like are used for descriptive purposes to indicate differences in content, but should not be construed as limiting the scope of protection of the present application.
[0047] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.
[0048] In the present application, when it comes to a numerical interval (i.e., a numerical range), unless otherwise specified, the distribution of the optional numerical values in the numerical interval is considered to be continuous, and includes the two numerical endpoints (i.e., the minimum value and the maximum value) of the numerical interval, and each numerical value between the two numerical endpoints. Unless otherwise specified, when the numerical interval only refers to the integers in the numerical interval, it includes the two endpoint integers of the numerical range, and each integer between the two endpoints, which is equivalent to directly listing each integer. When multiple numerical ranges are provided to describe features or characteristics, these numerical ranges can be combined. In other words, unless otherwise specified, the numerical range disclosed herein should be understood to include any and all sub-ranges included therein. The "numerical value" in the numerical interval can be any quantitative value, such as a number, a percentage, a ratio, etc. "Numerical interval" allows broadly including numerical interval types such as percentage intervals, ratio intervals, and ratio intervals.
[0049] In the present application, the term "room temperature" generally refers to 4°C to 35°C, preferably 20°C±5°C. In some embodiments of the present application, room temperature refers to 20°C to 30°C.
[0050] In this application, unless otherwise specified, the temperature parameter is allowed to be either a constant temperature treatment or to vary within a certain temperature range. It should be understood that the constant temperature treatment allows the temperature to fluctuate within the accuracy range controlled by the instrument. Fluctuations within the range of ±5°C, ±4°C, ±3°C, ±2°C, and ±1°C are allowed.
[0051] In this application, when referring to the unit of a data range, if there is a unit only after the right endpoint, it means that the units of the left and right endpoints are the same. For example, 2~5h means that the units of the left endpoint "2" and the right endpoint "5" are both h (hours).
[0052] As shown in the background technology, in the traditional technology, the car interior door panels are mostly made of polypropylene materials, most of which are modified by talcum powder fillers. One of the low-odor, low-VOC and scratch-resistant polypropylene interior materials for cars uses talcum powder to strengthen the polypropylene matrix in the formula, and uses a deodorant to reduce the odor and VOC content, but the deodorant is still a chemical raw material. Another method for preparing a nanocellulose polypropylene masterbatch is to use a common filler in PP plastic as a medium, load nanocellulose on it, and then make a masterbatch with PP, which prevents the aggregation of nanocellulose through the mutual repulsion between charges.
[0053] Based on this, after a large number of creative experimental studies, the applicant has made the composite material in this application reinforced by replacing the inorganic filler talc with modified bio-based cellulose nanofibers (CNF), and has a good dispersion effect when used in combination with a compatibilizer. The addition of polypropylene, a compatibilizer, a heat stabilizer, an antioxidant and a light stabilizer works together to reduce the odor of the composite material while maintaining good mechanical properties, so that the composite material has both excellent low odor and mechanical properties.
[0054] An embodiment of the present application provides a composite material, wherein the raw materials for preparing the composite material include the following components by weight:
[0055] Polypropylene 55 to 90 parts;
[0056] 5 to 20 parts of modified cellulose nanofibers;
[0057] 2~5 parts of compatibilizer;
[0058] 3~5 parts of heat stabilizer;
[0059] 0.1 to 0.6 parts of antioxidant;
[0060] Light stabilizer 0.2~0.5 parts;
[0061] The method for preparing the modified cellulose nanofibers comprises the following steps:
[0062] The cellulose nanofibers, the silane coupling agent and the solvent are mixed to prepare the modified cellulose nanofibers.
[0063] During the mixing process, the cellulose nanofibers and the silane coupling agent generate physical interaction forces, so that the surface of the cellulose nanofibers can be loaded with the silane coupling agent to prepare modified cellulose nanofibers.
[0064] The weight ratio of the polypropylene to the modified cellulose nanofiber is (2.75-18):1.
[0065] It should be noted that the value range of polypropylene is "55 parts to 90 parts", which means the minimum and maximum values of the range of 55 parts to 90 parts, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values in the embodiments and the following point values: 55 parts, 56 parts, 57 parts, 58 parts, 59 parts, 60 parts, 61 parts, 62 parts, 63 parts, 64 parts, 65 parts, 66 parts, 67 parts, 68 parts, 69 parts, 70 parts, 71 parts, 72 parts, 73 parts, 74 parts, 75 parts, 76 parts, 77 parts, 78 parts, 79 parts, 80 parts, 81 parts, 82 parts, 83 parts, 84 parts, 85 parts, 86 parts, 87 parts, 88 parts, 89 parts or 90 parts; or a range composed of any two of these values, as an example, including: 60 parts to 85 parts.
[0066] The value range of the modified cellulose nanofiber is "5 parts to 20 parts", that is, the minimum and maximum values of the range of 5 parts to 20 parts, and each value between the minimum and maximum values. Specific examples include but are not limited to the point values in the embodiments and the following point values: 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, 16 parts, 17 parts, 18 parts, 19 parts or 20 parts; or a range composed of any two of these values, as an example, including: 6 parts to 15 parts.
[0067] The range of the compatibilizer is "2 parts to 5 parts", which means the minimum and maximum values of the range of 2 parts to 5 parts, and every value between the minimum and maximum values. Specific examples include, but are not limited to, the point values in the embodiments and the following point values: 2 parts, 2.5 parts, 3 parts, 3.5 parts, 4 parts, 4.5 parts or 5 parts; or a range consisting of any two of these values, including, as an example, 3 parts to 5 parts.
[0068] The value range of the heat stabilizer is "3 parts to 5 parts", that is, the minimum and maximum values of the range of 3 parts to 5 parts, and each value between the minimum and maximum values. Specific examples include but are not limited to the point values in the embodiment and the following point values: 3 parts, 3.5 parts, 4 parts, 4.5 parts or 5 parts; or a range composed of any two of these values, as an example, including: 4 parts to 5 parts.
[0069] The range of antioxidant is "0.1 part to 0.6 part", that is, the minimum and maximum values of the range of 0.1 part to 0.6 part, and each value between the minimum and maximum values. Specific examples include but are not limited to the point values in the embodiment and the following point values: 0.1 part, 0.2 part, 0.3 part, 0.4 part, 0.5 part or 0.6 part; or a range composed of any two of these values, as an example, including: 0.1 part to 0.5 part.
[0070] The value range of the light stabilizer is "0.2 parts to 0.5 parts", which means the minimum and maximum values of the range of 0.2 parts to 0.5 parts, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values in the embodiment and the following point values: 0.2 parts, 0.3 parts, 0.4 parts or 0.5 parts; or a range composed of any two of these values, as an example, including: 0.3 parts to 0.5 parts.
[0071] The weight ratio of the polypropylene to the modified cellulose nanofiber may be 2.75:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, 11:1, 12:1, 13:1, 14:1, 15:1, 16:1, 17:1 or 18:1.
[0072] The above-mentioned composite material of the present application introduces a silane coupling agent into the cellulose nanofiber for modification, and at the same time, the modified cellulose nanofiber and polypropylene, a compatibilizer, a heat stabilizer, an antioxidant and a light stabilizer act together. By controlling the specific ratio of each preparation raw material and the specific weight percentage of polypropylene and the modified cellulose nanofiber, the components act synergistically, which promotes the addition of the modified cellulose nanofiber and the compatibilizer, while reducing the odor of the composite material, maintaining good mechanical properties, so that the composite material has both excellent low odor and mechanical properties, so that it can meet the requirements of decorative products for low odor and high tensile strength performance.
[0073] In some embodiments, the solvent includes ethanol.
[0074] In some embodiments, the temperature of the mixing process is 70°C to 110°C.
[0075] In some embodiments, the mixing time is 30 min to 50 min.
[0076] In some embodiments, the mixing process is performed under stirring conditions.
[0077] In some embodiments, the silane coupling agent includes one or more of KH550, KH540 and KH791.
[0078] In some embodiments, the raw materials for preparation include the following components by weight:
[0079] Polypropylene 60~80 parts;
[0080] 10-20 parts of modified cellulose nanofibers;
[0081] 2~5 parts of compatibilizer;
[0082] 3~5 parts of heat stabilizer;
[0083] 0.1 to 0.6 parts of antioxidant;
[0084] Light stabilizer 0.2~0.5 parts.
[0085] The ratio range of the raw materials used in the preparation is further controlled, and the composite material has lower odor and better tensile properties.
[0086] In some of the embodiments, the weight ratio of the polypropylene to the modified cellulose nanofiber is (3-15):1.
[0087] The ratio range of the raw materials used in the preparation is further controlled, and the composite material has lower odor and better tensile properties.
[0088] In some embodiments, the compatibilizer includes PP-g-MAH.
[0089] In some embodiments, the thermal stabilizer includes one or more of a zinc stabilizer and an amine stabilizer.
[0090] In some embodiments, the antioxidant includes a primary antioxidant and a secondary antioxidant, and the weight ratio of the primary antioxidant to the secondary antioxidant is (1-3):1.
[0091] In some embodiments, the primary antioxidant includes antioxidant 1010 .
[0092] In some embodiments, the secondary antioxidant includes one or more of antioxidant 168 and antioxidant 618 .
[0093] In some embodiments, the light stabilizer comprises an ultraviolet absorber and a free radical scavenger, and the weight ratio of the ultraviolet absorber to the free radical scavenger is 1-5:1;
[0094] In some embodiments, the ultraviolet absorber includes UV-24;
[0095] In some embodiments, the free radical scavenger comprises HALS.
[0096] An embodiment of the present application provides a method for preparing a composite material. The preparation method comprises the following steps:
[0097] The raw materials for preparing the composite material are mixed and extruded into shape.
[0098] In some embodiments, the mixing time is 2 min to 4 min.
[0099] In some embodiments, the extrusion temperature is 160°C to 250°C.
[0100] It will be appreciated that the melt extrusion step may be carried out in a single screw extruder or a twin screw extruder.
[0101] In some specific examples, in the method for preparing the composite material, the melt extrusion step is carried out in a twin-screw extruder.
[0102] In some of the embodiments, the vacuum degree in the extrusion process is -0.9 bar to -0.8 bar.
[0103] In addition, the composite material obtained by this preparation method also has higher fluidity, which is more conducive to injection molding; and the preparation method of the above composite material is simple, the processing is convenient, and the production adaptability is wide.
[0104] After the extrusion step, an injection molding process is also included, in which the product is placed in a hot air baking at 60° C. to 90° C. for 30 min to 90 min to prepare a composite material.
[0105] One embodiment of the present application is the use of the composite material in preparing decorative products.
[0106] An embodiment of the present application provides a decorative product, which is made of the above-mentioned composite material.
[0107] Optionally, the decorative product comprises an automobile interior door panel.
[0108] In order to make the purpose, technical solutions and advantages of the present application more concise and clear, the present application is described with the following specific embodiments, but the present application is by no means limited to these embodiments. The embodiments described below are only preferred embodiments of the present application and can be used to describe the present application, and cannot be understood as limiting the scope of the present application. It should be pointed out that any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.
[0109] In order to better illustrate the present application, the contents of the present application are further described below in conjunction with embodiments.
[0110] Example 1
[0111] (1) Provide the following raw materials by weight: 80 parts of polypropylene, 10 parts of modified cellulose nanofibers, 4 parts of a compatibilizer, 5 parts of a heat stabilizer, 0.5 parts of an antioxidant, and 0.5 parts of a light stabilizer. For details, refer to Table 1.
[0112] The polypropylene model is copolymer polypropylene derived from LyondellBasell RP348RX B, the cellulose nanofiber model is carboxylated cellulose nanofiber derived from Hebei Yufei Chemical, the silane coupling agent model is KH550 derived from Chenguang, the compatibilizer model is maleic anhydride grafted compatibilizer PP-g-MAH derived from Kangjin Chemical, the antioxidant is a mixture of a main antioxidant and a secondary antioxidant, and the antioxidant is selected from antioxidant 1010 and antioxidant 168 in a weight ratio of 3:1; the light stabilizer is a mixture of an ultraviolet absorber and a free radical scavenger, and the light stabilizer is selected from an ultraviolet absorber UV-24 and a free radical scavenger HALS in a weight ratio of 5:1.
[0113] (2) Polypropylene, modified cellulose nanofibers, a compatibilizer, a heat stabilizer, an antioxidant, and a light stabilizer are mixed according to weight proportions and stirred at high speed for 4 minutes using a mixing device at a rotation speed of 110 rpm to obtain a mixture.
[0114] The preparation method of modified cellulose nanofibers includes the following steps: placing 100 parts of cellulose nanofibers and 4 parts of silane coupling agents into a 40% ethanol aqueous solution at a temperature of 90°C, stirring and mixing for 50 minutes, and drying to obtain modified cellulose nanofibers.
[0115] (3) The above mixture is fed into the main feed of an extruder, and the extrusion temperature is set to 250°C and the vacuum degree is -0.9 bar. Melt extrusion granulation is performed to obtain pellets. The pellets are fed into an injection molding machine for injection molding. After the pellets are taken out, they are baked at 90°C hot air for 90 minutes to obtain a composite material.
[0116] (4) Testing: The composite materials prepared above were subjected to tensile strength and odor tests, as follows:
[0117] 1: Tensile strength: tested according to the method specified in the national standard GB-T 1040.1-2018 Determination of tensile properties of plastics Part 1: General principles.
[0118] 2: Odor: Add 50 ml of distilled water to the container, use a metal stand to support the sample, and ensure that the sample does not contact water. Store it in a sealed container at (80±2)℃ for (2±0.1) hours, and evaluate the odor. The odor evaluation score is shown in Table 2.
[0119] Please see Table 3 for specific test results.
[0120] Embodiment 2~5
[0121] Other Examples 2 to 5 are basically the same as Example 1, except that the preparation raw materials in Table 1 are different. Please see Table 1 for details.
[0122] The other steps and conditions are the same as those in Example 1.
[0123] Example 6
[0124] The other embodiment 6 is basically the same as the embodiment 1, and the only difference is that the temperature and time of drying in step (3) are different, specifically: the pellets are put into the injection molding machine for injection molding, and after taking out the parts, they are baked with hot air at 80°C for 60 minutes to obtain the composite material.
[0125] Comparative Examples 1 to 4
[0126] Comparative Examples 1 to 4 are substantially the same as Example 1, except that the raw materials for preparation in Table 1 are different. For details, please see Table 1.
[0127] The other steps and conditions are the same as those in Example 1.
[0128] Comparative Example 5
[0129] The raw materials for preparation of Comparative Example 5 are the same as those of Example 1, except that the steps for preparing the composite material are as follows:
[0130] (1) mechanically mixing the polypropylene, cellulose nanofibers, silane coupling agent, compatibilizer, heat stabilizer, antioxidant and light stabilizer, and stirring at high speed for 4 minutes using a mixing device to obtain a mixture;
[0131] (2) The above mixture is fed into the main feed of an extruder, and the extrusion temperature is set to 250°C and the vacuum degree is -0.9 bar, and melt extrusion granulation is performed to obtain pellets; the pellets are fed into an injection molding machine for injection molding, and after the pellets are taken out, they are baked at 90°C hot air for 90 minutes to obtain a composite material.
[0132] The other steps and conditions are the same as those in Example 1. The raw materials for the preparation of each example and comparative example are shown in Table 1. Wherein, T1 represents the weight ratio of the primary antioxidant to the secondary antioxidant, and T2 represents the weight ratio of the ultraviolet absorber to the free radical scavenger.
[0133] Table 1
[0134]
[0135] The odor evaluation score levels are shown in Table 2.
[0136] Table 2
[0137]
[0138] The test results of each embodiment and comparative example are shown in Table 3 below:
[0139] Table 3
[0140]
[0141] By comparing and analyzing the test data of Examples 1 to 6 and Comparative Examples 1 to 5 in Table 3, it can be seen that the composite material of the present application has both excellent low odor and mechanical properties, and can meet the practical application of the product.
[0142] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0143] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be construed as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent application shall be subject to the attached claims.
Claims
1. A composite material, It is characterized in that The raw materials for preparing the composite material include the following components by weight: Polypropylene 55 to 90 parts; 5 to 20 parts of modified cellulose nanofibers; 2~5 parts of compatibilizer; 3~5 parts of heat stabilizer; 0.1 to 0.6 parts of antioxidant; Light stabilizer 0.2~0.5 parts; The method for preparing the modified cellulose nanofibers comprises the following steps: The cellulose nanofibers, the silane coupling agent and the solvent are mixed to prepare the modified cellulose nanofibers; The weight ratio of the polypropylene to the modified cellulose nanofiber is (2.75-18):
1.
2. The composite material according to claim 1, It is characterized in that The mixing temperature is 70°C to 110°C; and / or The mixing time is 30 min to 50 min; and / or The silane coupling agent includes one or more of KH550, KH540 and KH791.
3. The composite material according to claim 1, It is characterized in that The solvent includes ethanol.
4. The composite material according to any one of claims 1 to 3, It is characterized in that The raw materials for its preparation include the following components by weight: Polypropylene 60~80 parts; 10-20 parts of modified cellulose nanofibers; 2~5 parts of compatibilizer; 3~5 parts of heat stabilizer; 0.1 to 0.6 parts of antioxidant; Light stabilizer 0.2~0.5 parts.
5. The composite material according to any one of claims 1 to 3, It is characterized in that The weight ratio of the polypropylene to the modified cellulose nanofiber is (3-15):
1.
6. The composite material according to any one of claims 1 to 3, It is characterized in that The compatibilizer comprises a maleic anhydride grafted compatibilizer; and / or The heat stabilizer includes one or more of a zinc stabilizer and an amine stabilizer.
7. The composite material according to any one of claims 1 to 3, It is characterized in that The antioxidant comprises a primary antioxidant and a secondary antioxidant, and the weight ratio of the primary antioxidant to the secondary antioxidant is (1-3):1; The primary antioxidant includes antioxidant 1010; The secondary antioxidant includes one or more of antioxidant 168 and antioxidant 618; and / or The light stabilizer includes an ultraviolet absorber and a free radical scavenger, and the weight ratio of the ultraviolet absorber to the free radical scavenger is (1-5):
1.
8. A method for preparing a composite material, It is characterized in that The steps include: The raw materials for preparing the composite material according to any one of claims 1 to 7 are mixed and extruded into a mold.
9. Use of the composite material according to any one of claims 1 to 7 in the preparation of decorative products.
10. A decorative product, It is characterized in that The decorative article comprises the composite material according to any one of claims 1 to 7 or a composite material prepared by the method for preparing a composite material according to claim 8.