Sealant composition for self-sealing pneumatic tire

By using the elastomer components of isobutylene and conjugated diene as well as granular fillers and organic peroxides in the sealant composition to form a partially depolymerized sealant layer, the fluidity and temperature difference problems of the existing sealant composition are solved , achieving better sealing performance and service life.

CN118725473APending Publication Date: 2024-10-01THE GOODYEAR TIRE & RUBBER CO
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410374360.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-03-28
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing sealant compositions tend to flow excessively after a tire is punctured, causing the tire to lose balance. They also have poor sealing performance over a wide temperature range and cannot effectively prevent air loss.

Method used

employing a sealant composition comprising at least 60 phr of an isobutylene-based elastomeric component, at least 5 phr of a conjugated diene-based elastomeric component, at least 5 phr of a particulate filler, and at least 0.5 phr of an organic peroxide, and Partially depolymerizes at appropriate temperatures to form a sealant layer to reduce flow and improve sealing performance.

Benefits of technology

Effectively reduces sealant flow and extends sealing performance, ensuring that the tire can maintain sealing performance for a longer period of time after being punctured, prevent air loss, and maintain effectiveness when temperatures change.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725473A_ABST
    Figure CN118725473A_ABST
Patent Text Reader

Abstract

The present invention relates to a sealant composition for a self-sealing pneumatic tire. A sealant composition suitable for forming a sealant layer in a tire comprises 100 phr of an elastomer, comprising at least 60 phr of an isobutylene-based elastomer component and at least 5 phr of a conjugated diene-based elastomer component. The sealant composition further includes at least 5 phr of a particulate filler, at least 0.5 phr of an organic peroxide, and optionally a colorant that provides a non-black color to the sealant.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] Aspects of the present invention are directed to sealant compositions suitable for sealing punctures in pneumatic tires, tires incorporating the compositions, and methods of manufacture. Background Art

[0002] Puncture seal tires are designed to delay or prevent air loss and subsequent deflation after a tire has been punctured by a sharp object, such as a nail, screw, or other object capable of piercing the tire.

[0003] A sealant composition ("sealant") is typically encapsulated or packaged between the layers of a tire. For example, the sealant may be arranged in a separate unit or sheet so that a puncturing object that penetrates the tread portion of the tire will penetrate enough of the sealant to seal the tire to prevent inflation air from escaping through the punctured hole.

[0004] Pneumatic tires with puncture sealing capabilities initially used unvulcanized rubber layers as sealants. (See, for example, U.S. Patents 1,419,470A, 1,601,013A, and 1,977,281A). Later, sealant compositions were developed to provide a longer service life for the tire after it was punctured. This allows the tire to continue to be used until it can be driven to a more convenient location for repair or replacement. For example, U.S. Patent 3,048,509A describes an unvulcanized synthetic rubber sealing composition containing 1,3-butadiene-styrene copolymer and a softener and a tackifier in the form of sheets separated by a covering sheet mainly comprising a vulcanized rubber compound.

[0005] Butyl rubber (a copolymer of isobutylene and isoprene) has also been used in sealant compositions. See, for example, U.S. Pat. Nos. 4,228,839A, 4,171,237A, 4,140,167A, and 4,426,468A and U.S. Publication No. 2005 / 0034799A1.

[0006] Sealant compositions incorporating dispersed particulate precured rubber materials have also been used, as described in U.S. Pat. No. 6,837,287 B2. Inorganic particulate materials have also been used in sealant compositions. U.S. Pat. No. 9,427,918 B2 describes a sealant composition comprising raw rubber, polybutene, treated silica, and peroxide. The raw rubber in the sealant composition may be natural rubber, butyl rubber, or a blend of natural rubber and butyl rubber. U.S. Pat. No. 9,802,446 B2 discloses a sealant comprising expandable graphene structures and microspheres.

[0007] Other sealant compositions and tires containing them are disclosed in U.S. Pat. Nos. 4,089,360A, 4,140,167A, 4,228,839A, 4,426,468A, 7,674,344B2, 8,221,849B2, 8,360,122B2, 9,677,025B2, 10,730,255B2 and U.S. Publication Nos. 20080115872A1, 20220097326A1, 20220111609A1 and 20220410516A1.

[0008] One drawback of many existing sealant compositions is that when a tire is punctured, the sealant composition continues to flow through the puncture. This can cause the tire to become unbalanced and can also create cleanup problems. In other cases, the sealant coating is inoperable or ineffective over a wide temperature range extending from hot summer days to cold winter days.

[0009] There remains a need for a sealant composition that is capable of self-sealing punctures in a tire that would otherwise result in air loss and eventual deflation of the tire while reducing excess flow of the sealant composition in the event of a puncture. Summary of the invention

[0010] According to one aspect of the exemplary embodiment, a sealant composition comprises 100 phr of an elastomer, wherein the elastomer comprises at least 60 phr of an isobutylene-based elastomer component and at least 5 phr of a conjugated diene-based elastomer component. The sealant composition further comprises at least 5 phr of a particulate filler and at least 0.5 phr of an organic peroxide.

[0011] The sealant composition may include a colorant that provides a non-black color to the sealant. The colorant may be selected from yellow pigments, yellow dyes, and mixtures thereof.

[0012] The isobutylene-based elastomeric component of the sealant composition may be selected from butyl rubber, polyisobutylene and mixtures thereof. The isobutylene-based elastomeric component may be at least 80% by weight of butyl rubber. The weight average molecular weight of the isobutylene-based elastomeric component may be at least 5000, or at least 30,000 and / or not more than 800,000. The sealant composition may include at least 75 phr of the isobutylene-based elastomer.

[0013] The conjugated diene-based elastomeric component of the sealant composition may be selected from natural rubber, synthetic polyisoprene, polybutadiene, styrene-butadiene copolymers, and mixtures and copolymers thereof. The conjugated diene-based elastomeric component may be at least 80% by weight of natural rubber. The sealant composition may include at least 8 phr of the conjugated diene-based elastomeric component.

[0014] The sealant composition may include up to 40 phr of a particulate filler. The particulate filler may include at least one of silica, titanium dioxide, calcium carbonate, and carbon black. The sealant composition may include at least 5 phr of silica. The sealant composition may contain a total of no more than 1 phr of a black reinforcing filler selected from carbon black, graphite, graphene, and mixtures thereof.

[0015] The organic peroxide in the sealant composition may be selected from diisopropylbenzene peroxide; 2,5-bis(tert-butylperoxy)-2,5-dimethylhexane; 1,1-di-tert-butylperoxy-3,3,5-trimethylcyclohexane; 2,5-dimethyl-2,5-di(tert-butylperoxy)hexyne-3; p-chlorobenzoyl peroxide; 2,4-dichlorobenzoyl peroxide; 2,2-bis-(tert-butylperoxy)-butane; tert-butylcumene peroxide; di-tert-butyl peroxide; benzoyl peroxide; 2,5-bis(tert-butylperoxy)-2,5-dimethylhexane; 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane; and mixtures thereof.

[0016] The sealant composition may further comprise at least 0.1 phr of a polyalkylene glycol.

[0017] According to another aspect of the exemplary embodiment, an uncured pneumatic tire includes a circumferential tread, a supporting carcass attached to the tread, a sealant layer including the sealant composition described above, and a containment layer disposed between the supporting carcass and the containment layer.

[0018] The containment layer of the uncured pneumatic tire may include a halobutyl rubber.

[0019] The cured pneumatic tire may be formed by curing the uncured pneumatic tire described above at a temperature sufficient for the organic peroxide to at least partially depolymerize the isobutylene-based elastomeric component.

[0020] According to another aspect of the exemplary embodiment, a method of forming a sealant layer includes forming a sealant composition comprising 100 phr of an elastomer, the elastomer comprising at least 60 phr of an isobutylene-based elastomer component and at least 5 phr of a conjugated diene-based elastomer component, a particulate filler, a colorant, and an organic peroxide. The method further includes treating the sealant composition to a sufficient temperature for a sufficient time to at least partially decompose the isobutylene-based elastomer component to form a sealant layer.

[0021] The method may further comprise, prior to treating the sealant composition, forming an uncured tire comprising a layer of the sealant composition.

[0022] According to another aspect of an exemplary embodiment, a method for manufacturing a pneumatic rubber tire having a puncture sealing feature includes constructing an unvulcanized tire, the unvulcanized tire including a circumferential rubber tread, a support carcass, a containment layer, and a sealant layer disposed between the support carcass and the containment layer. The sealant layer includes a sealant composition, the sealant composition including 100phr of an elastomer. The elastomer includes at least 60phr of an isobutylene-based elastomer component and at least 5phr of an elastomer component based on a conjugated diene. The sealant composition further includes a granular filler and an organic peroxide. The method further includes curing the unvulcanized tire at a sufficient temperature to at least partially depolymerize the isobutylene-based elastomer component, and producing a pneumatic rubber tire having a puncture sealing feature.

[0023] The present invention discloses the following embodiments:

[0024] 1. A sealant composition comprising:

[0025] 100 phr of an elastomer comprising:

[0026] at least 60 phr of an isobutylene-based elastomeric component, and

[0027] at least 5 phr of a conjugated diene-based elastomeric component;

[0028] at least 5 phr of particulate filler; and

[0029] At least 0.5 phr of organic peroxide.

[0030] 2. The sealant composition of embodiment 1, further comprising a colorant that provides a non-black color to the sealant.

[0031] 3. The sealant composition according to embodiment 2, wherein the colorant is selected from the group consisting of yellow pigments, yellow dyes, and mixtures thereof.

[0032] 4. The sealant composition of embodiment 1, wherein the isobutylene-based elastomeric component is selected from the group consisting of butyl rubber, polyisobutylene, and mixtures thereof.

[0033] 5. The sealant composition of embodiment 3, wherein the isobutylene-based elastomeric component is at least 80% by weight butyl rubber.

[0034] 6. The sealant composition of embodiment 1, wherein the isobutylene-based elastomeric component comprises a butyl rubber having a weight average molecular weight of at least 5,000 and / or no more than 800,000.

[0035] 7. The sealant composition of embodiment 1, wherein the sealant composition comprises at least 75 phr of the isobutylene-based elastomer.

[0036] 8. The sealant composition of embodiment 1, wherein the conjugated diene-based elastomeric component is selected from the group consisting of natural rubber, synthetic polyisoprene, polybutadiene, styrene-butadiene copolymers, and mixtures and copolymers thereof.

[0037] 9. The sealant composition of embodiment 8, wherein the conjugated diene-based elastomeric component is at least 80% by weight natural rubber.

[0038] 10. The sealant composition of embodiment 1, wherein the sealant composition comprises at least 8 phr of the conjugated diene-based elastomeric component.

[0039] 11. The sealant composition according to embodiment 1, wherein the sealant composition comprises up to 40 phr of the particulate filler.

[0040] 12. The sealant composition of embodiment 1, wherein the particulate filler comprises at least one of silica, titanium dioxide, calcium carbonate, and carbon black.

[0041] 13. The sealant composition according to embodiment 12, wherein the sealant composition comprises at least 5 phr of silica.

[0042] 14. A sealant composition according to embodiment 1, wherein the organic peroxide is selected from diisopropylbenzene peroxide; 2,5-bis(tert-butylperoxy)-2,5-dimethylhexane; 1,1-di-tert-butylperoxy-3,3,5-trimethylcyclohexane; 2,5-dimethyl-2,5-di(tert-butylperoxy)hexyne-3; p-chlorobenzoyl peroxide; 2,4-dichlorobenzoyl peroxide; 2,2-bis-(tert-butylperoxy)-butane; tert-butylcumene peroxide; di-tert-butyl peroxide; benzoyl peroxide; 2,5-bis(tert-butylperoxy)-2,5-dimethylhexane; 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane; and mixtures thereof.

[0043] 15. The sealant composition according to embodiment 1, further comprising at least 0.1 phr of a polyalkylene glycol.

[0044] 16. An uncured pneumatic tire comprising:

[0045] Circumferential tread;

[0046] a support carcass attached to the tread;

[0047] a sealant layer comprising the sealant composition of embodiment 1; and

[0048] A containment layer, the sealant layer is disposed between the supporting carcass and the containment layer.

[0049] 17. The uncured pneumatic tire of embodiment 16, wherein the containment layer comprises a halogenated butyl rubber.

[0050] 18. A cured pneumatic tire formed by curing the uncured pneumatic tire of embodiment 17 at a temperature sufficient to cause the organic peroxide to at least partially depolymerize the isobutylene-based elastomeric component.

[0051] 19. A method of forming a sealant layer, comprising:

[0052] forming a sealant composition comprising 100 phr of an elastomer comprising at least 60 phr of an isobutylene-based elastomeric component and at least 5 phr of a conjugated diene-based elastomeric component; a particulate filler; a colorant; and an organic peroxide; and

[0053] The sealant composition is treated to a sufficient temperature and for a sufficient time to at least partially decompose the isobutylene-based elastomeric component to form the sealant layer.

[0054] 20. The method of embodiment 19, further comprising, prior to treating the sealant composition, forming an uncured tire comprising a layer of the sealant composition.

[0055] 21. A method of manufacturing a pneumatic rubber tire having a puncture sealing feature, comprising:

[0056] constructing an unvulcanized tire comprising a circumferential rubber tread, a supporting carcass, a containment layer, and a sealant layer disposed between the supporting carcass and the containment layer, the sealant layer comprising a sealant composition comprising 100 phr of an elastomer comprising at least 60 phr of an isobutylene-based elastomeric component and at least 5 phr of a conjugated diene-based elastomeric component; a particulate filler; and an organic peroxide; and

[0057] The uncured tire is cured at a temperature sufficient to at least partially depolymerize the isobutylene-based elastomeric component and produce a pneumatic rubber tire having puncture sealing characteristics. BRIEF DESCRIPTION OF THE DRAWINGS

[0058] Figure 1 is a cross-sectional view of a tire according to one aspect of an exemplary embodiment, wherein a sealant layer is disposed between an inner liner and a carcass of the tire;

[0059] Figure 2 is a cross-sectional view of a tire according to another aspect of the exemplary embodiment, wherein a sealant layer is disposed between first and second innerliner layers;

[0060] Figure 3 is a cross-sectional view of a tire according to another aspect of an exemplary embodiment wherein a sealant layer is disposed between a containment layer and a carcass of the tire. DETAILED DESCRIPTION

[0061] Described herein are sealant compositions (or "sealants") suitable for use in the enclosure of a pneumatic tire. The sealant seals punctures in the tire by flowing to fill voids while minimizing excess sealant flow out of the enclosure and maintaining sealing properties over an extended period of time.

[0062] In the present specification, the term "phr" refers to the parts of the corresponding material per 100 parts by weight of rubber or elastomer. The term "phf" refers to the parts per hundred parts by weight of filler. By convention, the unreacted rubber used in the sealant composition (i.e., excluding any pre-cured rubber particles used as filler) totals 100 phr.

[0063] Unless otherwise specified, the terms "rubber" and "elastomer" are used interchangeably.

[0064] As used herein, Mooney viscosity is measured at 125° C. according to ASTM D1646-19a “Standard Test Methods for Rubber-Viscosity, Stress Relaxation, and Pre-Vulcanization Characteristics (Mooney Viscometer)”.

[0065] The glass transition temperature (Tg) of an elastomer or elastomeric composition, wherein as used herein, means the glass transition temperature(s) of the corresponding elastomer or elastomeric composition in its unreacted state or, in the case of an elastomeric composition, possibly in a reacted state. The Tg value referred to herein is the peak midpoint measured by differential scanning calorimetry (DSC) at a heating rate of 10°C / min according to ASTM D3418-21 "Standard Test Method for Transition Temperatures and Enthalpies of Fusion and Crystallization of Polymers by Differential Scanning Calorimetry".

[0066] Hereinafter, sealant compositions, methods of preparation, and exemplary tires incorporating the sealant compositions are described.

[0067] Sealant composition

[0068] An exemplary sealant composition is formed by curing a mixture comprising an isobutylene-based elastomer having a low degree of unsaturation, a conjugated diene-based elastomer having a high degree of unsaturation, and a peroxide, such as an organic peroxide that generates free radicals. The butene-based elastomer of the sealant composition can be partially depolymerized in situ in the tire by the organic peroxide that generates free radicals. The sealant may incorporate one or more granular filler materials, such as silica and clay. One or more colorants may be present in the sealant composition to contrast with the black color of the tire to help identify punctures in the tire. Processing oils and / or polyoxyalkylene polymers, such as polyethylene glycol, may also be present in the sealant composition. It should be understood that the sealant composition is not limited to these components.

[0069] The sealant composition is used to provide a built-in sealant layer (or two or more layers) for a pneumatic tire. Each sealant layer is obtained by (partial) depolymerization of the butene units of the butene-based elastomer in the sealant composition. Depending on the position of the built-in sealant layer, one or more sealant layers may be positioned inside the tread of the tire. The sealant layer can be built into the tire to form a tire assembly in a suitable mold or on a core. The butene units of the butene-based elastomer of the sealant composition can be depolymerized during the subsequent curing of the tire at an elevated temperature to form a tire with the resulting built-in sealant layer.

[0070] Although not fully understood, it is believed that the conjugated diene-based elastomeric component forms a matrix in the reactive sealant that entraps the lower molecular weight butyl chains derived by depolymerization of the isobutylene-based elastomeric component. This creates a reactive sealant layer in the tire that is able to flow to only a limited extent when the tire is punctured (enough to be noticeable), while allowing the pressure within the tire to be maintained at a drivable level for an extended period of days or weeks.

[0071] 1. Elastomer

[0072] An exemplary sealant composition comprises two elastomeric components, an isobutylene-based elastomeric component and a conjugated diene-based elastomeric component. The two elastomeric components together may be at least 80 phr, or at least 90 phr, or at least 95 phr or 100 phr in the sealant composition.

[0073] A. Isobutylene-based Elastomer Components

[0074] The isobutylene-based elastomeric component may be at least 60 phr, at least 70 phr, at least 75 phr, or at least 80 phr in the sealant composition, and / or at most 95 phr, at most 92 phr, or at most 90 phr. The isobutylene-based elastomeric component is composed of one or more elastomers derived from isobutylene. For example, the isobutylene-based elastomeric component may be selected from butyl rubber, polyisobutylene, and mixtures thereof. In one embodiment, the isobutylene-based elastomer is at least 80 wt %, or at least 90 wt %, or at least 95 wt %, or 100 wt % butyl rubber.

[0075] Butyl rubber is a copolymer of isobutylene and a conjugated diene, particularly isoprene. In one embodiment, isobutylene-derived units comprise the majority of the units in the copolymer, while isoprene-derived units comprise the minority of the units. For example, the ratio of isobutylene-derived units to isoprene-derived units may be at least 90:10, or at least 95:5, or at least 98:2, or at least 98.5:1.5, or at least 99:1, or at most 99.5:0.5. The use of butyl rubber having a low unsaturation content (e.g., a ratio of isobutylene-derived units to isoprene-derived units of at most 2) promotes more efficient depolymerization of the organic peroxide. When the depolymerization process reaches the double bond unsaturation in the butyl rubber, the presence of the double bonds in the butyl rubber tends to terminate its depolymerization, thereby allowing partial but incomplete depolymerization to occur. Since the butyl rubber is at least partially depolymerized by the organic peroxide present in the sealant composition, a byproduct of this depolymerization is isobutylene.

[0076] The butyl rubber may have a weight average molecular weight Mw of at least 30,000, or at least 40,000, such as up to 800,000, or up to 600,000, or up to 400,000. The butyl rubber may have a relatively high Mooney viscosity at 125°C, such as 25 to 60, or at least 40, or up to 60.

[0077] Example rubbers include those from ExxonMobil Company marketed as Exxon 068 TM Butyl rubber, which is a copolymer of isobutylene and isoprene, is sold having less than 1% of units derived from isoprene and a Mooney viscosity of about 51 at 25°C.

[0078] Polyisobutylene (PIB) is a homopolymer of isobutylene, i.e., formed in the absence of unsaturated monomers such as isoprene. Polyisobutylene suitable for use in the isobutylene-based elastomeric component may have a weight average molecular weight Mw of at least 5,000, or at least 10,000, or at least 30,000, or at least 40,000, or at least 50,000, such as up to 800,000, or up to 600,000, or up to 400,000, or up to 150,000. In addition, the polyisobutylene may have a polydispersity (Mw / Mn) in the range of 1.6 to 4.0 and a glass transition temperature in the range of -55°C to -70°C, such as in the range of -62°C to -66°C, or in the range of -63°C to -65°C. The polyisobutylene elastomer may optionally be stabilized with a small amount of an antioxidant, for example 100 ppm to 1000 ppm of an antioxidant, or 300 ppm to about 700 ppm of an antioxidant.A variety of antioxidants may be used, such as butylated hydroxytoluene (BHT).

[0079] Examples of polyisobutylenes suitable for use are available from BASF as B10, B12 and B15. B10 has a weight average molecular weight Mw of 53,000, a viscosity average molecular weight Mv of 40,000, and a glass transition temperature (Tg) of -64°C; B12 has a weight average molecular weight of 70,000, a viscosity average molecular weight of 55,000, and a glass transition temperature (Tg) of -64°C; and B15 has a weight average molecular weight of 108,000, a viscosity average molecular weight of 85,000, and a glass transition temperature (Tg) of -64°C.

[0080] In one embodiment, the sealant composition is free or substantially free (less than 1 phr) of polybutene, particularly low molecular weight polybutene (Mw less than 8000). Polybutene is a polymer formed from a mixture of 1-butene, 2-butene and isobutylene.

[0081] B. Conjugated Diene-Based Elastomer Components

[0082] In the sealant composition, the rubber component based on conjugated dienes may be at least 5 phr, at least 6 phr or at least 8 phr, and / or at most 40 phr, at most 25 phr, at most 20 phr or at most 15 phr. The elastomeric component based on conjugated dienes is composed of one or more elastomers derived from conjugated dienes alone or mainly (at least 60 wt %, or at least 80 wt %, or at least 90 wt % or at least 95 wt %). The elastomeric component based on conjugated dienes can be selected from natural rubber, synthetic polyisoprene, polybutadiene, styrene-butadiene copolymers and mixtures and copolymers thereof. In one embodiment, the elastomeric component based on conjugated dienes is at least 80 wt % of natural rubber.

[0083] Natural rubber is primarily derived from isoprene (2-methyl-1,3-butadiene) and is therefore primarily (e.g., at least 99% by weight) polyisoprene. As used herein, the term "natural rubber" refers to naturally occurring rubber, such as can be harvested from sources such as Hevea brasiliensis rubber trees and non-Hevea brasiliensis sources (e.g., guayule shrubs and dandelions such as TKS). In other words, the term "natural rubber" should be interpreted as excluding synthetic polyisoprene. Natural rubber produced from the rubber plantation gel (cup gel) of the Hevea brasiliensis tree is a common form of natural rubber. For example, technical graded rubber or block rubber (TSR) is a natural rubber available from Indonesia, where it can be referred to as standard Indonesian rubber (SIR), standard Malaysian rubber (SMR), and standard Thai rubber (STR). It is available in a variety of grades, including TSR 10 and TSR 20, with the TSR 10 grade having a higher purity.

[0084] In one embodiment, the conjugated diene-based elastomeric component is at least 80% by weight natural rubber, or at least 90% by weight, or up to 100% by weight natural rubber.

[0085] Synthetic polyisoprene, particularly cis-1,4-polyisoprene having a cis content of at least 94 weight percent is also suitable. The cis-1,4-content of the synthetic polyisoprene may be at least 96 weight percent. The Tg of the synthetic polyisoprene may be between -60°C and -70°C.

[0086] The weight ratio of the conjugated diene-based elastomeric component (especially natural rubber) to the isobutylene-based elastomeric component (especially butyl rubber) in the sealant composition may be at least 5:95, or at least 10:90, or at least 15:85, or at least 17:83, or at least 20:80, or at least 25:75, or at most 40:60, or at most 30:70.

[0087] 2. filler

[0088] Particulate fillers may be included in the sealant composition. In the following, fillers which are not present in the sealant composition are said to still be present in trace amounts, for example as commonly found as impurities in other particulate fillers.

[0089] The particulate filler(s) may be present in the sealant composition in a total amount of at least 5 phr, or at least 10 phr, or at least 15 phr or at least 20 phr, or at most 75 phr, or at most 60 phr, or at most 50 phr, or at most 40 phr, or at most 30 phr, or at most 25 phr or at most 20 phr.

[0090] Exemplary particulate fillers useful herein include silica, calcium carbonate (CaCO 3 ), titanium dioxide, hydrated aluminum silicate clay, 2:1 layered silicate clay and organophilic clay formed therefrom, calcium silicate, carbon black, graphite, graphene, carbon nanotubes, wollastonite, talc, diatomaceous earth, starch, lignin, alumina, polymer fillers and mixtures thereof.

[0091] In one embodiment, the filler comprises silica particles, such as amorphous (e.g., precipitated) silica and / or crystalline silica. The term "silica" is used herein to refer to silicon dioxide, SiO 2 (It may contain small amounts of impurities, typically less than 1% by weight, resulting from the process by which the silica is formed.) The term "precipitated silica" is used to refer to synthetic amorphous silica, typically obtained by a process in which a silicate is precipitated with an acidifying agent.

[0092] Precipitated silica can be prepared by digesting amorphous silica (such as that present in rice husks or other biowaste) with sodium hydroxide to form sodium silicate and precipitating silica from the sodium silicate by reaction with an acidifying agent (such as sulfuric acid or carbon dioxide). The resulting silica precipitate is washed and filtered. Methods for preparing precipitated silica are disclosed in U.S. Pat. Nos. 5,587,416A, 5,800,608A, 5,882,617A, 6,107,226A, 6,180,076B1, 6,221,149B1, 6,268,424B1, 6,335,396B1, 7,585,481B2, 9,334,169B2, 9,359,215B2, U.S. Publication Nos. 20020081247A1, 20030118500A1, 20040062701A1, 20050032965A1, and EP0647591A1. Precipitated silica can also be formed from silica gel, such as described in US Pat. Nos. 5,708,069 A, 7,550,610 Bl, and 5,789,514 A. For example, silica gel can be derivatized by hydrophobizing a silica hydrogel with, for example, organomercaptosilanes and alkylsilanes and drying the product.

[0093] The precipitated silica may have a nitrogen (BET) surface area of ​​100-350 m 2 The BET (nitrogen) surface area of ​​precipitated silica is determined according to ASTM D 1993-18 "Standard Test Method for Precipitated Silica-Surface Area by Multipoint BET Nitrogen Adsorption", which is related to the traditional theory described by Brunauer, Emmett and Teller in the Journal of the American Chemical Society, Vol. 60, p. 309 (1938).

[0094] Example precipitated silicas include Hi-Sil® from PPG Industries TM 532 and Hi-Sil TM 532 EP; Hubersil from JMHuber Company TM 4155; Zeosil TM, from Solvay under the trade names 115GR, 125GR, 165GR, 175GR, 185GR, 195GR, 1085GR, 1165MP, 1115MP, HRS1200MP, Premium MP, Premium200MP, Premium SW and 195HR; Ultrasil TM , from Evonik under the trade names VN2, VN3, VN3GR, 5000GR, 7000GR, 9000GR; Zeopol TM , from Evonik trade names 8755LS and 8745; Newsil TM , from Wuxi Quechen Silicon Chemical Co., Ltd. under the trade names 115GR and 2000MP; and Tokusil from Maruo Calcium Co., Ltd. TM 315.

[0095] The silica may have been surface treated, for example with a coupling agent and / or polyoxyalkylene, such as polyethylene glycol, prior to incorporating the pretreated silica into the sealant composition to enhance dispersibility and / or adhesion to the elastomer. The coupling agent and / or polyoxyalkylene may also help inhibit the tendency of associated hydration water or hydroxyl groups on the silica to cause premature decomposition of the organic peroxide intended to depolymerize the butyl rubber in the sealant composition. In another embodiment, the silica may be treated in situ with a coupling agent and / or polyoxyalkylene within the sealant composition prior to the addition of the organic peroxide.

[0096] Polyalkylene glycols useful for pretreatment or in-situ use in the sealant composition are described in more detail below.

[0097] Suitable coupling agents generally include a first part that reacts with hydroxyl groups (e.g., silanol groups) present on the surface of precipitated silica and a second part that can react with a diene-based elastomer. The two parts are connected by a linking group (e.g., a hydrocarbon group or a sulfur bridge) so that the precipitated silica is chemically bonded to the elastomer. Examples of silica coupling agents include those containing the following groups: for example, alkyl, alkoxy, mercapto, blocked mercapto, sulfide-containing (e.g., alkoxy-containing based on monosulfide, alkoxy-containing based on disulfide, alkoxy-containing based on tetrasulfide), amino, vinyl, epoxy, and combinations thereof. The silica coupling agent may be present in an amount sufficient to provide a ratio of at least 0.1:100 or at most 1:5 of the total amount of coupling agent to the silica filler, by weight, such as the following ratio: at least 1:100, or at least 1:50, or at most 1:20, or at most 1:10.

[0098] In one embodiment, silica is present in the sealant composition at 1 phr or more, such as at least 2 phr, or at least 5 phr, or at least 6 phr, or at least 7 phr, or up to 20 phr, or up to 18 phr, or up to 15 phr, or up to 14 phr, or up to 12 phr, or up to 10 phr. The silica may be at least 10 phr, or at least 20 phr, or at least 30 phr, or up to 100 phr, or up to 99 phr, or up to 95 phr of the particulate filler.

[0099] In one embodiment, the ratio of silica to natural rubber is at least 0.4:1, and may be up to 1:1. In one embodiment, the ratio of silica to butyl rubber is at least 0.7:10, and may be up to 1.1:10.

[0100] Silicate clays useful in sealant compositions include layered silicate clays and organophilic clays derived therefrom. Exemplary layered silicate clays include montmorillonite, bentonite, hectorite, saponite, nontronite, beidellite, fluorohectorite, stevensite, volkonskoite, sauconite laponite, and physical blends thereof. Useful organophilic clays are silicate clays that have been chemically modified to render them compatible with organic materials. Silicate clays used as starting materials may include one or more of montmorillonite, hectorite, saponite, attapulgite, and sepiolite. These clays contain exchangeable cationic species, such as sodium, potassium, or calcium ions, on their surfaces and between clay galleries or layers. During the process of making the organophilic clay, at least a portion of these exchangeable cationic species are replaced with organic cations such as quaternary amines, organophosphorus ions, and the like.

[0101] Silicate clay may be absent from the sealant composition, or may be present in the sealant mixture at 0.5 to 20 phr, such as at least 1 phr, or at least 2 phr, or at least 5 phr, or up to 10 phr.

[0102] Calcium carbonate may also be used as a filler, for example in combination with silica. The benefit of using calcium carbonate over silica is to provide an improved degree of reinforcement, which can aid in processing of the sealant composition and, together with silica, help provide suitable stiffness and associated dimensional integrity to the partially depolymerized sealant composition.

[0103] In one embodiment, calcium carbonate may be used as a carrier for the organic peroxide.

[0104] Calcium carbonate may not be present in the sealant composition, or may be present in the sealant composition at 0.5 phr or more, such as at least 5 phr, or at least 10 phr, or at least 15 phr, or at least 18 phr, or up to 30 phr, or up to 25 phr, for example as a carrier for an organic peroxide. The ratio of calcium carbonate to organic peroxide may be at least 20:80, or at least 30:70, or up to 70:20, or up to 60:40, or up to 50:50.

[0105] When used in the sealant composition, the carbon black may have a CTAB of at least 100, or at least 102, or at least 104, or at most 120, or at most 118, or at most 116 m 2 Exemplary carbon blacks include ASTM trade names N110, N121, N134, N220, N231, N234, N242, N293, N299, N315, N326, N330, N332, N339, N343, N347, N351, N358, N375, N539, N550, N582, N630, N642, N650, N683, N754, N762, N765, N774, N787, N907, N908, N990 and N991 as specified in ASTM D 1765-21 "Standard Classification System for Carbon Blacks Used in Rubber Products".

[0106] In one embodiment, the sealant composition is free or substantially free (no more than 1 phr) of carbon black. In another embodiment, carbon black is present in the sealant composition at 2 to 20 phr, or at most 10 phr, or at most 5 phr.

[0107] When used in sealant compositions, graphene is generally a single-atom-thick carbon crystal form in which carbon atoms are held together by σ bonds arranged in a two-dimensional honeycomb lattice. More specifically, graphene is a crystalline allotrope of carbon with a two-dimensional nature. The carbon atoms in graphene are closely packed in a regular atomic-scale hexagonal (chicken wire) pattern. Each atom has four bonds, one σ bond connected to each of its three neighboring atoms, and one π bond facing out of the plane. The distance between adjacent carbon atoms in graphene is about 0.142 nanometers. Graphene used as a granular filler can have a Z-type (zig-zag), armchair (armchair), K-zone, gulf (gulf), bay (bay), canyon (cove) and / or fjord (fjord) edge configuration. At least 50%, at least 60%, at least 70% or at least 80% of the carbon-carbon bonds on the edge of the graphene structure can be one of a Z-type configuration, an armchair configuration and a bay configuration. For example, among the carbon-carbon bonds on the edge of the graphene structure, at least 40%, 50% or 60% may be in a zigzag configuration, less than 40% or less than 30% may be in a canyon configuration, and less than 20% may be in a fjord configuration.

[0108] Exemplary graphene that can be used as granular filler is peeled off into nano-scale graphene plate (NGP) material, which is basically a single single-sheet graphene sheet or multiple graphite plane sheets. Each graphite plane is generally a two-dimensional hexagonal structure of carbon atoms. Each plane has a length and width parallel to the graphite plane and a thickness orthogonal to the graphite plane, so that at least one of the values ​​of length, width and thickness is 100 nanometers (nm) or less. Typically, each of the length, width and thickness values ​​is less than 100nm. This NGP material can be produced by the method described in, for example, U.S. Patent No. 7,071,258B1.

[0109] In one embodiment, the sealant composition is free or substantially free (no more than 1 phr) of graphene. In another embodiment, graphene is present in the sealant composition at 2 to 20 phr, or at most 10 phr, or at most 5 phr.

[0110] In a specific embodiment, black particulate filler derived from one form or carbon (eg, carbon black, graphite, graphene, and / or carbon nanotubes) is present in the sealant composition at no more than 5 phr, or no more than 1 phr.

[0111] Titanium dioxide, when used as a filler, can also be used as a colorant. Titanium dioxide useful herein can have an average particle size of at least 0.1 micrometers (μm), such as at least 0.2 μm, or at most 5 μm, or at most 4 μm. The scattering of light by titanium dioxide is maximized in particles having a diameter of 0.2 to 0.3 μm. Therefore, in order to be used as a colorant, at least 50% by weight of the particles can be within this range.

[0112] In one embodiment, the sealant composition contains no or substantially no (no more than 0.1 phr) titanium dioxide. In another embodiment, titanium dioxide is present in the sealant composition at least 0.1 phr, for example, at least 1 phr, or at most 10 phr, or at most 5 phr, or at most 3 phr.

[0113] Exemplary polymeric fillers in particulate form useful herein include polypropylene, precured rubber, and mixtures thereof. Typically, particles of such fillers may have an average size of less than 10 micrometers (μm).

[0114] The polypropylene suitable for use as a filler may be low molecular weight. Such low molecular weight polypropylene may have a weight average molecular weight (MW) of at least 4000, or at least 6000, or at least 8000, or at least 10,000, or at most 40,000, or at most 25,000, or at most 20,000, or at most 15,000. w Polypropylene can be used as a substitute or partial substitute for carbon black and / or mineral fillers, where lower levels (eg, 30-40 wt % less) than would be used with these other fillers.

[0115] In one embodiment, no polymeric filler is present in the sealant composition. In another embodiment, the polymeric filler is present in the sealant composition in a total amount of at least 1 phr, or at most 15 phr.

[0116] 3. Processing oil

[0117] The sealant composition may optionally include one or more process oils. Suitable process oils include aromatic oils, paraffinic oils, naphthenic oils, triglyceride oils and low polycyclic aromatic hydrocarbons (PCA) oils, such as mild extract solvates (MES), treated distillate aromatic extracts (TDAE), special residual aromatic extracts (SRAE) and heavy naphthenic oils and mixtures thereof. Suitable low PCA oils may include those oils having a polycyclic aromatic hydrocarbon content of less than 3% by weight as determined by the IP346 method. A description of the IP346 method can be found in Standard Methods for Analysis & Testing of Petroleum and Related Products and British Standard 2000 Parts, 2003, 62nd edition, published by Institute of Petroleum, UK. Suitable naphthenic process oils and paraffinic process oils having a maximum aromatic content of less than 15% by weight are exemplary. Such process oils may have a naphthenic content of 35 to 45 wt %, a paraffinic content of 45 to 55 wt %, and an aromatic content of less than 15 wt %, such as 10 to 14 wt %.

[0118] Example naphthenic process oils include Hyprene from Ergon Refining, Inc. TM 100 and Tufflo 100 from BartonSolvent Company TM .

[0119] Triglyceride oils that can be used include vegetable oils, including vegetable oil, castor oil, soybean oil, canola oil (rapeseed oil), corn oil, cottonseed oil, olive oil, palm oil, safflower oil, sunflower oil, coconut oil and peanut oil. Castor oil is a triglyceride oil containing about 87% by weight of ricinoleic acid, 7% by weight of oleic acid, 3% by weight of linoleic acid, 2% by weight of palmitic acid and 1% by weight of stearic acid.

[0120] Relatively low concentrations of processing oil may aid in mixing the ingredients of the sealant composition and / or facilitate processing of the sealant composition.

[0121] Processing oil may be absent from the sealant composition, or may be used in the sealant composition at 0.1 phr or more, or at least 1 phr, or at least 2 phr, or at least 4 phr, or at least 5 phr, or up to 40 phr, or up to 20 phr, or up to 10 phr, or up to 8 phr.

[0122] 4. Polyoxyalkylene

[0123] Polyoxyalkylenes suitable for use in sealant compositions include polyethylene glycol, polypropylene glycol, and mixtures thereof. In one embodiment, the polyoxyalkylene is polyethylene glycol. The polyoxyalkylene may have a weight average molecular weight Mw of at least 500, such as at least 2,000, or at least 4,000, or at most 15,000, or at most 12,000, or at most 10,000, or at most 8,500. The polyoxyalkylene may not be present in the sealant composition. Where a polyoxyalkylene (e.g., polyethylene glycol) is used, it may be included in an amount of at least 0.1 phr, such as at least 0.2 phr, or at least 0.3 phr, or at most 5 phr, or at most 3 phr, or at most 2 phr, or at most 1 phr, or at most 0.6 phr.

[0124] Examples of commercially available polyethylene glycols include Carbowax TM PEG 3350 and Carbowaw TM PEG 8000, where the numbers represent the approximate weight average molecular weight. Other polyoxyalkylene polymers may be used, as described, for example, in US Pat. Nos. 6,322,811 Bl and 4,082,703A.

[0125] 5. Colorants

[0126] The sealant composition may include one or more colorants in the form of pigments and / or dyes. Both organic and inorganic colorants may be used. By including one or more non-black colorants in the sealant composition, the fact that the tire is punctured is obvious and the location of the puncture can be more easily identified. A wide variety of colors may be used for this purpose, with light or bright colors being suitable, which stand out from the typical black color of the tire tread. For example, white, red, orange, yellow, green or blue colorants may be included. Red iron pigments may be used to impart a bright red color, or yellow pigments may be used to impart a bright yellow color. The colorant may be used in an amount of 0.1 phr to 5 phr, such as at least 0.2 phr or at most 4 phr.

[0127] Some representative examples of pigments that can be used include Pigment Yellow 1 (CAS No. 2512-29-0), Pigment Yellow 110 (CAS No. 5590-18-1), Pigment Yellow 12 (CAS No. 15541-56-7), Pigment Yellow 126 (CAS No. 90268-23-8), Pigment Yellow 127 (CAS No. 68610-86-6), Pigment Yellow 13 (CAS No. 5102-83-0), Pigment Yellow 138 (CAS No. 30125-47-4), Pigment Yellow 14 (CAS No. 5 468-75-7), Pigment Yellow 150 (CAS No. 68511-62-6), Pigment Yellow 151 (CAS No. 31837-42-0), Pigment Yellow 154 (CAS No. 68134-22-5), Pigment Yellow 168 (CAS No. 71832-85-4), Pigment Yellow 17 (CAS No. 4531-49-1), Pigment Yellow 174 (CAS No. 78952-72-4), Pigment Yellow 180 (CAS No. 77804-81-0), Pigment Yellow 183 (CAS No. 652 12-77-3), Pigment Yellow 191 (CAS No. 129423-54-7), Pigment Yellow 3 (CAS No. 6486-23-3), Pigment Yellow 34 (CAS No. 1344-37-2), Pigment Yellow 42 (CAS No. 51274-00-1), Pigment Yellow 65 (CAS No. 6528-34-3), Pigment Yellow 74 (CAS No. 6358-31-2), Pigment Yellow 75 (CAS No. 52320-66-8), Pigment Yellow 81 (CAS No. 22094-93-5), Pigment Yellow 83 (CAS No. 5567-15-7), CI Pigment Yellow 42 (Iron Oxide), CI Pigment Yellow 34 (Lead Chromate), CI Pigment Yellow 184 (Bismuth Vanadate), CI Pigment Yellow 53 (Nickel Antimony), CI Pigment Orange 20 (Cadmium Sulfide), CI Pigment Red 101 (Iron Oxide), CI Pigment Red 104, CI Pigment Red 29 (Ultramarine Pigment), CI Pigment Blue 29 (Ultramarine Pigment), CI Pigment Blue 28, CI Pigment Blue 36, CI Pigment Violet 15 (Ultramarine Pigment), CI Pigment Violet 16 (Manganese Violet), Pigment Green 17 (Chromium Oxide Green), CI Pigment Green 19 (Cobalt-based Mixed Metal Oxide), CI Pigment Green 26 (Cobalt-based Mixed Metal Oxide), and CI Pigment Green 50 (Cobalt-based Mixed Metal Oxide). Some other inorganic pigments that can be used include Ultramarine Blue, Persian Blue, Cobalt Blue (CAS No. 1345-16-0), Azure Blue, Egyptian Blue, Han Blue (BaCuSi 4 O 10 )、Azurite blue(Cu 3 (CO 3 ) 2 (OH) 2), Prussian blue (CAS No. 14038-43-8), YInMn blue (yttrium indium manganese blue), realgar red (α-As 4 S 4 ), cadmium red (Cd 2 SSe), cerium sulfide red, Venetian red (Fe 2 O 3 ), red ochre (anhydrous Fe 2 O 3 ), burnt ochre red, red lead (Pb 3 O 4 ), vermilion, cinnabar red, ultramarine purple, Han purple (BaCuSi 2 O 6 ), cobalt violet (CO 3 (PO 4 ) 2 ), manganese violet (NH 4 MnP 2 O 7 ), Cassius Purple, Primrose Yellow (BiVO 4 ), cadmium yellow (CdS), chrome yellow (PbCrO 4 ), cobalt yellow (K 3 Co(NO 2 ) 6 ), yellow ocher color (Fe 2 O 3 ·H 2 O), Naples yellow, titanium yellow (NiO·Sb 2 O 3 ·20TiO 2 ), zinc yellow (ZnCrO 4 ) and chrome orange (PbCrO 4 · PbO). Mixtures of colorants may be used.

[0128] In one embodiment, the sealant composition includes a white mineral pigment, such as titanium dioxide, and / or a yellow or other non-white pigment or dye. However, for purposes of calculating phr and phf, titanium dioxide is considered a filler, not a colorant.

[0129] 6. Organic peroxides

[0130] Organic peroxides (organic peroxides) are typically present in sealant compositions and serve as depolymerizing agents for the isobutylene-based elastomeric component.

[0131] The organic peroxide used may be one of those commonly used for crosslinking rubbery polymers. Peroxide compounds that decompose only at relatively high temperatures (e.g., above 75° C. or above 80° C.) may be used. Suitable organic peroxides include dialkyl peroxides having the same or different groups, such as dialkylbenzene peroxides and alkyl peresters. The organic peroxide may contain two peroxide groups. Typically, the peroxide groups are attached to a tert-butyl group. The basic groups of the two peroxide groups hanging thereon may be aliphatic, cycloaliphatic, or aromatic groups.

[0132] Examples of suitable organic peroxides include bis(α,α-dimethylbenzyl) peroxide (more commonly known as dicumyl peroxide); tert-butyl peroxybenzoate; 2,5-bis(tert-butylperoxy)-2,5-dimethylhexane; 1,1-di-tert-butylperoxy-3,3,5-trimethylcyclohexane; 2,5-dimethyl-2,5-di(tert-butylperoxy)-hexyne-3; p-chlorobenzoyl peroxide; 2,4-dichlorobenzoyl peroxide; 2,2-bis-(tert-butylperoxy)-butane; tert-butylcumyl peroxide; di-tert-butyl peroxide; benzoyl peroxide; 2,5-bis(tert-butylperoxy)-2,5-dimethylhexane; 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane; and mixtures thereof.

[0133] In one embodiment, the first organic peroxide acts as a depolymerization initiator and the second organic peroxide acts as a depolymerization propagator. The first organic peroxide is activated at a lower temperature than the second organic peroxide, but tends to decompose faster. For example, the organic peroxide may contain a small amount of n-butyl 4,4-di(tert-butylperoxy)valerate as a depolymerization initiator and a large amount of diisopropylbenzene peroxide as a depolymerization propagator.

[0134] Suitable peroxides include those having an active oxygen content (AOC) of at least 2. The active oxygen content is determined by dividing the weight of the active oxygen atoms in the compound by its total molecular weight (this is done on the basis of one active oxygen atom for each peroxide group (-OO-) in the compound). For example, tert-butyl cumyl peroxide has one active oxygen atom (molecular weight of 16) and a total molecular weight of 208. Thus, the active oxygen content of tert-butyl cumyl peroxide is 16 / 208 (7.7%). Peroxides having an active oxygen content greater than 7%, 8%, 9% or even 10% are particularly suitable. This is because they generate less gas during the tire curing process than peroxides with lower active oxygen contents.

[0135] The organic peroxide may be added to the sealant composition in pure form (100% active peroxide), or may be supported on an inert, free-flowing mineral carrier, or dispersed in an oil (e.g., silicone oil). Calcium carbonate is an inert mineral carrier that is often used for this purpose. Another carrier is a combination of calcium carbonate and calcium silicate.

[0136] An example peroxide is in the form of a composite of dicumyl peroxide on precipitated calcium carbonate (40.5% active) which can be used as 40C is available from Arkema Inc. Another example hydrogen peroxide is in the form of a composite material of n-butyl 4,4-di-(tert-butylperoxy)valerate with a combination of calcium carbonate and calcium silicate as a mineral carrier, which is available as Trigonox 17-40B pd T M Obtained from Nouryon, the weight ratio of organic peroxide to carrier is 40 / 60.

[0137] Desirably, the isobutylene-based elastomeric component (e.g., butyl rubber) of the sealant composition is depolymerized by free radicals (generated by the organic peroxide) to the extent that the resulting sealant layer has a storage modulus (G') of at least 50 kPa, or at least 60 kPa, or at least 80 kPa, or at least 90 kPa, or at most 200 kPa, or at most 180 kPa, or at most 170 kPa as measured by a Rubber Process Analyzer (RPA) (measured at 40°C, 1 Hz, and 5% strain) after exposure to 170°C for 5 minutes. The appropriate storage modulus (G') may depend to some extent on the type of tire, including tire size and expected tire usage conditions, to improve the sealant efficiency of the built-in tire sealant, thereby improving the ability to effectively seal against various puncturing objects (e.g., nails).

[0138] The natural rubber in the sealant composition tends to react with the organic peroxide, thereby reducing the amount available for depolymerization of the isobutylene-based elastomeric component (e.g., butyl rubber). Therefore, the amount of organic peroxide added to the composition is selected to be sufficient to cause partial depolymerization of the isobutylene-based elastomeric component in situ in the tire. The organic peroxide may be added to the sealant composition in an amount of at least 0.1 phr (expressed as active peroxide), such as at least 0.5 phr, or at least 1 phr, or at least 2 phr, or at least 4 phr, or at most 20 phr, or at most 10 phr, or at most 8 phr.

[0139] Exemplary sealant compositions do not include sulfur-based vulcanizing (curing) agents.

[0140] In one embodiment, the organic peroxide is activated with an activator such as a 2,2,6,6-tetraalkylpiperidinyl hindered amine. Examples of such hindered amines are, for example, poly[[6-[1,1,3,3,-tetramethylbutyl]amino]-s-triazine-2,4-diyl][2,2,6,6,-tetramethyl-4-piperidinyl)imino]hexamethylene[(2,2,6,6-tetramethyl-4-piperidinyl)imino]] compounds, such as described in U.S. Pat. No. 7,674,344 B2.

[0141] Exemplary sealant compositions (expressed in phr) are shown in Table 1.

[0142] Table 1: Sealant composition

[0143]

[0144]

[0145] It will be appreciated that combinations of the above-mentioned ranges may be employed.

[0146] Forming a sealant composition

[0147] The various components of the sealant layer can be mixed together using convenient rubber mixing equipment (such as an internal rubber mixer). Typically, the elastomers, such as butyl rubber and natural rubber, are blended in at least one continuous preliminary or non-productive mixing stage in the absence of an organic peroxide, followed by a final or productive mixing step in which the organic peroxide (and possibly one or more additional ingredients) is added.

[0148] In one embodiment, in one or more first non-productive stages, the components except the organic peroxide are stirred in a mixer, which is set at a suitable temperature, such as at least 100°C, or at least 110°C, or at most 180°C. The temperature of the mixture increases as the mixture is stirred. When the temperature reaches a desired value, the mixture is dripped from the mixer and cooled before being returned to the mixer. In a second productive stage, the mixture is returned to the mixer together with the organic peroxide. The mixer is set at a temperature lower than the decomposition temperature of the organic peroxide, such as 70°C, or below, such as about 60°C. The mixture drips from the mixer when the maximum temperature of about 85°C is to minimize the premature decomposition of the peroxide.

[0149] Tire structure

[0150] The sealant layer formed by the sealant composition described above can be built into an uncured tubeless pneumatic rubber tire before vulcanization. When building the tire, the sealant composition can be encapsulated in one or more layers in one or more envelopes within the tire. The one or more envelopes can be at least partially defined by one or more containment layers formed of hard rubber, which makes it relatively easy to handle the sealant composition and build it into the tire.

[0151] In one embodiment, the tire includes a generally annular supporting carcass, a peripheral tread, and an internal containment layer, such as an inner liner (or "innerliner"). As used herein, the term "tread" refers to both the portion of the tire that contacts the road under normal inflation and load, and any subtread. The inner liner is an air barrier that prevents air or other gases used to inflate the tire (such as nitrogen) from escaping through the tire structure by diffusion. The inner liner can be formed of halogenated butyl rubber or some other suitable material with a high degree of gas permeation resistance. A sealant layer can be positioned between the supporting carcass and the inner liner or other containment layer. In another embodiment, two or more inner liners act as containment layers for the sealant.

[0152] In one embodiment, if Figure 1 As shown, the sealant layer is located between the supporting carcass and the tire innerliner, and optionally in direct contact with the supporting carcass and the tire innerliner. In another embodiment, the sealant layer formulation is positioned between two innerliner layers, and optionally in direct contact with the two innerliner layers, such as Figure 2 In this case, the sealant layer is sandwiched between first and second innerliners and is separated from the tire carcass and tread by the first and second innerliners, respectively. As an alternative to one or more of the one or more innerliners, one or more other containment layers may be employed. In another embodiment, the tire does not include any innerliners, and the sealant composition is built (extruded) into the tire between different types of containment layers supporting the carcass and the tire, such as Figure 3 As will be appreciated, a plurality of sealant layers may be provided, wherein each pair of adjacent sealant layers is separated by an intermediate containment layer. The carcass and / or tread may include one or more reinforcing plies formed from fabric, polyethylene sheet and / or metal.

[0153] exist Figure 1In the embodiment of the present invention, a tubeless type self-sealing pneumatic rubber tire 2 is shown. The tire has a sidewall 3, a supporting carcass 4, an inextensible bead 5, an inner liner (air barrier layer) 6, a sealant layer 7, and a peripheral tread (tread portion) 8 extending from the sidewall. Each sidewall 3 extends radially inward from the axial outer edge of the tread portion 8 to engage each inextensible bead 5. The supporting carcass 4 serves as a support structure for the tread portion 8 and the sidewall 3. The sealant layer 7 is disposed on the inner side of the supporting carcass 4 and on the outer side of the inner liner 6. The peripheral tread 8 is adapted to contact the ground when the tire is in use.

[0154] exist Figure 2 In the embodiment of the invention, a self-sealing pneumatic rubber tire 10 is shown. The pneumatic tire is of the tubeless type and includes a tread portion 11, a crown region 12, a sidewall 13, a supporting carcass 14, an inextensible bead 15, an inner liner composed of an inner layer and an outer layer 16A, 16B, and a sealant layer 17. In this embodiment, the sealant layer 17 is sandwiched between the two layers 16A, 16B of the inner liner. Thus, the sealant layer 17 is disposed radially inward from one layer 16A of the inner liner and radially outward from the other layer 16B of the inner liner. Both the inner liner layer 16 and the sealant layer 17 are disposed radially inward from the supporting carcass 14.

[0155] exist Figure 3 In the embodiment of the present invention, a tubeless self-sealing pneumatic rubber tire 22 is shown, which has no inner liner. The self-sealing pneumatic rubber tire 22 includes a sidewall 23, a support carcass 24, an inextensible bead 25, a containment layer 26, a sealant layer 27 and a peripheral tread (tread portion) 28. Each sidewall 23 extends radially inward from the axial outer edge of the tread portion 28 to engage each inextensible bead 25. The support carcass 24 serves as a support structure for the tread portion 28 and the sidewall 23. The sealant layer 27 is disposed on the inner side of the support carcass 24 and on the outer side of the containment layer 26. In particular, the sealant layer 25 is sandwiched between the support carcass 24 and the containment layer 26. The peripheral tread 28 is suitable for contacting the ground when the tire is in use. In this embodiment, the containment layer 26 is disposed on the inner side of the sealant layer 27 and is the innermost layer of the tire 22.

[0156] The sealant layer 7, 17, 27 may extend at least from one sidewall of the tire to the other sidewall, in other words it may have a length surrounding the tread area 8, 11, 28 of the tire.

[0157] In an uncured puncture sealant tire, the thickness of the sealant layer can be varied widely. In one embodiment, the thickness of the sealant layer is from 0.2 mm to 8.5 mm, such as at least 3 mm, or at least 4 mm, or at most 6 mm, or at most 5 mm. In a passenger car tire, a thickness of about 4.5 mm can be used.

[0158] The tread, sidewall and carcass may each be formed from a sulfur-curable rubber composition, which may be the same or different. Exemplary elastomers for forming the rubber compositions used in these components may include natural rubber, synthetic polyisoprene, natural polyisoprene, styrene-butadiene copolymer, solution polymerized styrene-butadiene (SSBR), emulsion polymerized styrene-butadiene rubber (ESBR), butadiene rubber (BR), halogenated butyl rubber, bromobutyl rubber, chlorobutyl rubber, nitrile rubber, liquid rubber, polynorbornene copolymer, isoprene-isobutylene copolymer, ethylene propylene rubber, chloroprene rubber, acrylate rubber, fluorine-containing rubber, silicone-containing rubber, polysulfide rubber, epichlorohydrin rubber, styrene-isoprene-butadiene terpolymer, hydrated acrylonitrile-butadiene rubber, isoprene-butadiene copolymer, butyl rubber, hydrogenated styrene-butadiene rubber, butadiene-acrylonitrile rubber, Terpolymers formed by ethylene monomer, propylene monomer and / or ethylene propylene diene monomer (EPDM), isoprene-based block copolymers, butadiene-based block copolymers, styrene block copolymers, styrene-butadiene-styrene block copolymers (SBS), styrene-ethylene / butylene-styrene block copolymers (SEBS), styrene-[ethylene-(ethylene / propylene)]-styrene block copolymers (SEEPS), styrene-isoprene-styrene block copolymers (SIS), random styrene copolymers, hydrogenated styrene block copolymers, styrene-butadiene copolymers, polyisobutylene, ethylene-vinyl acetate (EVA) polymers, polyolefins, amorphous polyolefins, semi-crystalline polyolefins, α-polyolefins, reactor-ready polyolefins (reactor-ready polyolefin), acrylates, metallocene-catalyzed polyolefin polymers and elastomers, reactor-made thermoplastic polyolefin elastomers, olefin block copolymers, copolyester block copolymers, polyurethane block copolymers, polyamide block copolymers, thermoplastic polyolefins, thermoplastic vulcanizates, ethylene vinyl acetate copolymers, ethylene n-butyl acrylate copolymers, ethylene methyl acrylate copolymers, chloroprene rubber, acrylic resins, polyurethanes, poly(acrylates), ethylene acrylic acid copolymers, polyetheretherketones, polyamides, atactic polypropylene, polyethylene (including atactic polypropylene), ethylene-propylene polymers, propylene-hexene polymers, ethylene-butene polymers, ethylene-octene polymers, propylene-butene polymers, propylene-octene polymers, metallocene-catalyzed polypropylene polymers, metallocene-catalyzed polyethylene polymers, ethylene-propylene-butene terpolymers, propylene, ethylene, C 4 -C 10Copolymers prepared from α-olefin monomers, polypropylene polymers, maleated polyolefins, polyester copolymers, copolyester polymers, ethylene acrylic acid copolymers and / or polyvinyl acetate, and / or wherein the polymers are optionally modified and / or functionalized at the polymer chain ends and / or at side chain positions within the polymer to include one or more of the following: hydroxyl-, ethoxy-, epoxy-, siloxane-, amine-, aminosiloxane-, carboxyl-, phthalocyanine- and silane-sulfide groups.

[0159] As an example, a tire tread rubber composition includes 100 phr of an elastomeric component, such as a mixture of styrene-butadiene rubber and polybutadiene, optionally with natural rubber, polyisoprene, or a combination thereof.

[0160] In one embodiment, the rubber composition used to form the tread, sidewall, carcass and / or housing layer(s) contains no butyl rubber or contains no more than 5 phr of butyl rubber.

[0161] In addition to the elastomer, the rubber composition used to form the tread, sidewall and carcass may include one or more reinforcing fillers; one or more processing aids, such as liquid plasticizers (e.g., oils), resins, waxes, antioxidants, antidegradants and / or antiozonants; and a cure package including a sulfur-based vulcanizing agent. The cure package may further include one or more curing accelerators and / or activators, which act as catalysts for the vulcanizing agent.

[0162] The reinforcing filler in a total amount of at least 1 phr or at most 200 phr may include one or more of silica, carbon black, aluminum oxide, aluminum hydroxide, clay (reinforced grade), magnesium hydroxide, boron nitride, aluminum nitride and titanium dioxide. Suitable silica and carbon black can be used in the sealant composition as described above. Silica can be present in the rubber composition in an amount of 1 to 200 phr, such as at least 3 phr or at least 10 phr. Carbon black can be present in an amount of 5 phr to 200 phr, such as at least 10 phr or at most 80 phr, or at most 50 phr.

[0163] Examples of sulfur-based vulcanizing agents include elemental sulfur (free sulfur), insoluble polymer sulfur, soluble sulfur, sulfur-donating vulcanizing agents, such as amine disulfides, polymer polysulfides or sulfur-olefin adducts and mixtures thereof. The sulfur vulcanizing agent can be used in the following amounts: 0.1 to 10 phr, such as at least 0.5 phr, or at least 1 phr, or at most 8 phr, or at most 5 phr. In other embodiments, the sulfur vulcanizing agent is not present in the rubber composition.

[0164] Examples of curing activators include zinc oxide and fatty acids (e.g., stearic acid) and combinations thereof. Examples of curing accelerators include amines, disulfides, guanidines, thioureas, thiazoles, thiurams, sulfenamides, dithiocarbamates / salts, xanthates / salts and combinations thereof.

[0165] An exemplary composition for forming a tread includes a mixture of an elastomer, a filler consisting of silica and carbon black, stearic acid, a processing oil, zinc oxide, an antioxidant, a paraffin wax, and optionally a silane coupling agent.

[0166] When used, the tire innerliner can be a halobutyl rubber-based layer formed from a halobutyl rubber composition containing a sulfur curing agent of a halobutyl rubber (e.g., chlorobutyl rubber or bromobutyl rubber). The innerliner may also contain one or more sulfur-curable diene-based elastomers, such as cis-1,4-polyisoprene natural rubber, cis-1,-4-polybutadiene rubber, and styrene / butadiene rubber, and mixtures thereof, particularly a combination of one or more halobutyl rubbers and one or more diene-based elastomers.

[0167] Incorporating the sealant composition into a tire

[0168] The sealant composition, for example in the form of a strip of material, is incorporated into the uncured tire.The components of the tire may be assembled in a mold or on a core and then cured.

[0169] In one embodiment, the tire is formed in a mold. In another embodiment, the tire is formed on a toroidal core or tire blank. When formed on the core, the tire can be gradually formed in layers starting from the innermost layer, starting from the innermost layer, which can be an inner liner or other containment layer. The inner liner / other containment layer can be applied by an extruder using a rubber strip or in sheet form or by other suitable methods. Optional tire beads, such as column beads of one or more wires, can be applied in the tire bead area above the inner liner / containment layer. Then apply a layer of unreacted sealant, optionally followed by a second inner liner. Finally, build the carcass, sidewalls and tread. As will be understood, the two layers of inner liners incorporated into the sealant composition can be applied to the core as one piece. When formed in a mold, the tire can be constructed from the outside to the inside, i.e. in the opposite order. The formation of the unvulcanized tire is not limited to any particular method, as long as the sealant layer is enclosed therein.

[0170] In one embodiment, the sealant layer is located between the carbon black reinforced rubber innerliner of the tire and the tire carcass, or between two carbon black reinforced tire rubber innerliners.The tire may have a rubber tread and rubber sidewalls containing rubber reinforced carbon black.

[0171] After the uncured tire is built to include a layer of unreacted sealant formulation, it is vulcanized. This may include heating the tire to a temperature of at least 80°C to partially depolymerize the butyl rubber. Higher temperatures are then used to cure the rubber compositions of the tread, carcass, and sidewalls.

[0172] The vulcanization of the uncured tire can be carried out in a wide temperature range, for example, a temperature in the range of 100° C. to 200° C., for example, at least 130° C., or at least 140° C., or at most 170° C., or at most 165° C. In one embodiment, the tire can reach a maximum curing temperature of 160° C. to 165° C. The curing cycle for curing the uncured tire can have a duration of 4 minutes to 240 minutes, for example, 10 minutes to 25 minutes, or 10 minutes to 17 minutes, or 11 minutes to 13 minutes. Any suitable vulcanization method can be used, for example, heating in a press or mold and / or heating with superheated steam or hot air.

[0173] At least partial depolymerization of the isobutylene-based elastomeric component of a sealant composition layer built into the tire (e.g., between the tire innerliner and the tire carcass) occurs during the curing of the tire itself at elevated temperatures by an organic peroxide. In practice, a major portion of the isobutylene-based elastomeric component of the sealant composition depolymerizes in the presence of the active organic peroxide when the tire assembly is cured under conditions of elevated temperature. Thus, the unreacted sealant layer is converted into a puncture sealant layer during the curing process of the tire. The sealant layer may be bonded to adjacent layers of the tire during the process.

[0174] In one embodiment, the sealant composition is incorporated into the uncured tire in the form of one or more material strips. One or more strips can be prepared using conventional equipment such as a calender, an extruder or a combination thereof, and the sealant composition strips are assembled into the tire. The thickness of the sealant composition layer can be at least 1mm, or 12mm at the most. For passenger car tires, the sealant composition layer can have a thickness of 2-5mm, and for truck tires, a thickness of 5-9mm can be used. The width of the sealant layer can be enough to extend at least the width of the tire tread, for example at least 5cm or at least 10cm.

[0175] Without intending to limit the scope of the present invention, the following examples illustrate the preparation and evaluation of sealant compositions.

[0176] Example

[0177] Sealant compositions were prepared using different ratios of butyl rubber to natural rubber, different amounts of peroxide, and different amounts of silica to demonstrate that the viscosity and hysteresis of the sealant composition upon reaction can be improved to reduce excess bleed compared to compositions not containing natural rubber. In the examples below, it is also shown that hysteresis can be reduced by reducing the amount of filler and / or the amount of peroxide. However, since natural rubber tends to crosslink with peroxide, sufficient amounts of peroxide are used to ensure decomposition of the butyl rubber.

[0178] The unreacted sealant compositions shown in Table 2 were prepared in two stages. In the non-productive stage, the components other than the peroxide were mixed in a mixer set at 120°C and about 100 rpm. The temperature was raised to about 160°C and the mixture was dripped out after about 4 minutes. In the productive stage, the mixture was returned to the mixer set at about 60°C and about 60 rpm. The mixture was dripped out at a maximum temperature of 85°C (to minimize decomposition of the peroxide).

[0179] Example 1 is a comparative sealant composition. Two batches of Example 1 were prepared for evaluation of reproducibility. Examples 2-4 are exemplary compositions containing a mixture of butyl rubber and natural rubber. Examples 5 and 6 are comparative compositions containing no natural rubber.

[0180] All components are expressed in parts by weight per hundred parts of rubber (phr).

[0181] Table 2: Sealant composition

[0182]

[0183] 1 -TSR 20, made from rubber plantation gel (cup gel) from the Hevea brasiliensis tree grown in Indonesia.

[0184] 2 -Exxon TM Butyl 068, obtained from ExxonMobil Chemical. It contains a non-staining antioxidant as an additive. The Mooney viscosity is about 51 according to ASTM D1646-19a.

[0185] 3 -HI-SIL TM 532EP synthetic amorphous silica, surface area (BET) is about 60m 2 / g, from PPG Industries, Inc.

[0186] 4-From KaMin Performance Industries HG90 kaolin (hydrated aluminum silicate), surface area (BET) is about 21m 2 / g.

[0187] 5 -Cotiox TM KA-100 titanium dioxide, particle size about 0.25-0.35μ, from Cosmo Chemical Co., Ltd.

[0188] 6 -Hyprene TM 100 naphthenic process oil, with a viscosity of about 22.3 cSt at 40°C according to ASTM D445, from Ergon Refining, Inc.

[0189] 7 - Polyethylene glycol Carbowax TM PEG 8000, weight average molecular weight about 8000, from Univar.

[0190] 8 -Akrosperse E-6837 TM Yellow pigment 12, contains EPR (ethylene / propylene rubber) (50% / 50%) from Akrochem Company.

[0191] 9 - 40C Dicumyl Peroxide on Precipitated Calcium Carbonate (40.5% active ingredient) from Arkema Inc.

[0192] Note: The levels shown in Table 1 are active dicumyl peroxide levels.

[0193] Sample evaluation

[0194] After the production stage, the samples were ground to a thickness of less than 0.5 cm. After cooling, the samples were molded using a die cutter to a size suitable for RPA testing.

[0195] Rubber Process Analyzer (RPA) RPA2000 was used to characterize the samples. After loading the samples, they were exposed to a temperature of 170°C for 5 minutes. Dynamic mechanical analysis was performed and the storage modulus G' values ​​at 1%, 3% and 5% strain (MPa) were obtained at a temperature of 40°C. Tan δ values ​​(ratio of G' to G') were also obtained.

[0196] The RPA results are shown in Table 3.

[0197] Table 3: Rubber Process Analyzer Results

[0198]

[0199]

[0200] Example 5, prepared with lower levels of filler and organic peroxide than Example 1, has comparable G' values, but has lower hysteresis, as shown by the lower tan delta result. Example 6, with the same filler level as Example 5, but an even lower level of organic peroxide, shows a further decrease in tan delta with a slight increase in G'. Examples 2, 3, and 4, which contain natural rubber, also exhibit lower hysteresis than Example 1.

[0201] Sealing

[0202] To evaluate the ability of the example compositions to seal punctures, simulated tire assemblies were prepared in which a 3 mm thick pressed sealant layer was positioned between a 5 mm "tread" layer and 2 layers of material of 1 mm each (on one side of the sealant layer) and a 1 mm inner liner (on the other side of the sealant layer). The assembly was sealed along its edges and cured at 170°C for 11-12 minutes. After cooling, the sample was mounted on a test fixture and an air pressure of 138 kPa was applied to the inner liner side of the assembly.

[0203] Each specimen was punctured with two small nails (2.5 mm diameter), two medium nails (3.4 mm diameter), and two large nails (5 mm diameter), taking care to ensure that the nails passed completely through the test specimen but left enough protruding from the specimen to allow it to be pulled out during testing.

[0204] The sample is pressurized to 241 kPa and kept at this pressure for several minutes. The nail is then pulled out. The sealing index is calculated, which takes into account:

[0205] 1. Puncture hole sealing: The number of puncture holes sealed is weighted (the larger the nail, the greater the recorded weight).

[0206] 2. Sealing efficiency: whether the puncture hole is sealed immediately.

[0207] Therefore, the sealing index generally gives higher values ​​for samples showing better sealing properties. Table 4 shows the results obtained.

[0208] Table 4: Sealing index

[0209]

[0210] Example 4 is not a direct comparison because it was evaluated in a tire seal test where the cured tire was mounted and inflated and punctured with 36 nails (9 nails of each size). All samples performed relatively well, with Example 5 showing the worst seal index.

[0211] After the seal test was completed, the samples were re-inflated and monitored for two days, and any small leaks in the samples were repaired by reinserting the nails. All samples were then re-inflated and monitored for another 7 days. The samples were then visually inspected. All samples containing natural rubber completely maintained air pressure, with essentially no sealant flowing out of the puncture hole. For the samples without natural rubber, significant leakage of sealant and a decrease in pressure were observed.

[0212] It was concluded that the natural rubber network plays an important role in containing the sealant in the cladding and maintaining pressure during the experiments.

[0213] Unexpectedly, significant differences in the long-term behavior of compositions with comparable RPA properties and similar sealing indicators were observed. The compositions containing natural rubber kept the sealant in the samples during the one-week experiment, and they also subsequently retained the full air pressure.

[0214] The results indicate that the natural rubber containing composition can seal nail puncture holes in tires by flowing to fill the voids but does not exhibit continuous flow out of the envelope and into the tire cavity or onto the tread.

[0215] Each of the above-mentioned files is incorporated herein by reference.Except in the examples or otherwise clearly indicated, all numerical values ​​of the amount, reaction conditions, molecular weight, carbon number, etc. of the specified material in this specification should be understood to be modified by the word "about".Unless otherwise stated, each chemical substance or composition mentioned herein should be interpreted as commercial grade material, which may contain isomers, by-products, derivatives and other such materials generally understood to be present in commercial grade.However, unless otherwise stated, the amount of each chemical component is represented by not including any solvent or diluent oil that may be generally present in commercial materials.It should be understood that the upper and lower limits, range limits and ratio limits described herein can be independently combined.Similarly, the scope and amount of each element of the present invention can be used together with the scope or amount of any other element.

[0216] It should be understood that the above disclosed variants and other features and functions, or alternatives thereof, may be incorporated into many other different systems or applications. Various currently unforeseen or unanticipated substitutions, modifications, variations or improvements may be subsequently made by those skilled in the art, which are also intended to be covered by the following claims.

Claims

1. A sealant composition, characterized in that: 100phr elastomer, characterized by: at least 60 phr of an isobutylene-based elastomeric component, and at least 5 phr of a conjugated diene-based elastomeric component; at least 5 phr of particulate filler; and At least 0.5 phr of organic peroxide.

2. The sealant composition of claim 1 further characterized by a colorant, said colorant providing a non-black color to said sealant.

3. The sealant composition according to claim 1, characterized in that The isobutylene-based elastomeric component is selected from the group consisting of butyl rubber, polyisobutylene, and mixtures thereof.

4. The sealant composition according to claim 3, characterized in that The isobutylene-based elastomeric component is at least 80% by weight butyl rubber.

5. The sealant composition according to claim 1, characterized in that The isobutylene-based elastomeric component comprises a butyl rubber having a weight average molecular weight of at least 5,000 and / or not more than 800,000.

6. The sealant composition according to claim 1, characterized in that The sealant composition comprises at least 75 phr of the isobutylene-based elastomer.

7. The sealant composition according to claim 1, characterized in that The sealant composition comprises at least 8 phr of the conjugated diene-based elastomeric component.

8. An uncured pneumatic tire, characterized in that: Circumferential tread; a support carcass attached to the tread; A sealant layer, characterized by the sealant composition according to claim 1; and A containment layer, the sealant layer is disposed between the supporting carcass and the containment layer.

9. The uncured pneumatic tire according to claim 16, characterized in that The containment layer comprises halogenated butyl rubber.