Gold stamping base oil as well as preparation method and application thereof
Through the compounding of bisphenol A epoxy acrylate, hydroxy acrylic resin and amino resin, the alcohol resistance, water resistance and storage stability problems of UV screen printing ink are solved, the hot stamping effect and adhesion are improved, and it is suitable for glass bottles. print.
Patent Information
- Application Number
- CN202410966346.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-10-01
AI Technical Summary
Existing UV screen printing inks have problems such as high VOC emissions, long drying time, poor alcohol and water resistance, low storage stability and poor hot stamping effect.
By compounding bisphenol A epoxy acrylate with hydroxyl acrylic resin and amino resin, a dual-curing UV hot stamping base oil is prepared. Combined with an appropriate amount of additives, the alcohol resistance, water resistance and storage stability of the hot stamping base oil are improved. And improve the bronzing effect.
The hot stamping base oil has excellent liquor and water immersion resistance and good storage stability. It also improves the hot stamping properties and adhesion, and is suitable for printing graphics and text on glass bottles.
Smart Images

Figure BDA0004951880150000061 
Figure BDA0004951880150000071 
Figure BDA0004951880150000072
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of inks, and in particular to a hot stamping primer and a preparation method and application thereof. Background Art
[0002] At present, the requirements for screen printing inks on the market have gradually improved from functionalization to environmental protection and aesthetics. Traditional solvent-based screen printing inks have a large amount of solvent (VOC) volatilization emissions, which can easily cause serious environmental pollution, and the drying time is long, resulting in low preparation efficiency. UV screen printing inks have become an ideal choice for screen printing inks because of their low VOC emissions or no solvent emissions. However, the first generation of UV screen printing inks are composed of UV resins, reactive diluents, photoinitiators, fillers, pigments and additives. They are irradiated and cured by traditional mercury lamps. Although they can significantly reduce VOC emissions, the mercury lamp has a short service life and is not environmentally friendly. It also requires preheating and cooling, which is inefficient. The second generation of UV screen printing inks uses LED cold light sources for curing, which is more environmentally friendly, does not require preheating and cooling, and is more efficient. It has been widely used in the high-end wine bottle industry, but it still has defects such as poor alcohol and water resistance, low storage stability, and poor hot stamping effect.
[0003] For example, the prior art discloses an LED-cured water transfer primer, which uses phenolic epoxy polyurethane and acrylic resin as the main film-forming materials, can withstand high temperature hot stamping, and has good adhesion to glass. However, due to the lack of cross-linking reaction with amino resins and other resins in the later stage, the mask has poor alcohol and water resistance after film formation, and the phenolic epoxy is brittle, which is not conducive to the later water transfer operation. Another example is that the prior art uses polyester resin, polyester acrylate, appropriate monomers and amino resin, and combines photoinitiator, filler, leveling agent, defoamer, and inhibitor to prepare an LED-cured and heat-cured dual-cured water transfer hot stamping primer. Since the main film-forming material has poor temperature resistance and chemical resistance, the hot stamping effect and alcohol and water resistance are all poor. The prior art also discloses a UV-curing and heat-curing dual-curing water transfer hot stamping primer, whose main components are polyester acrylate, terpene resin, hydroxy acrylate, reactive diluent, amino resin, strong acid catalyst, photoinitiator, thixotropic agent, defoaming agent, and leveling agent. A strong acid catalyst is added to the water transfer hot stamping primer to reduce the later curing temperature, but the strong acid catalyst is sensitive to storage time and storage temperature. After partial or complete failure, its performance varies greatly, resulting in poor storage stability of the water transfer hot stamping primer. Summary of the invention
[0004] The present invention aims to solve at least one of the above-mentioned technical problems existing in the prior art. To this end, the purpose of the present invention is to provide a hot stamping primer, which improves the comprehensive performance of the dual-curing UV hot stamping primer by combining bisphenol A epoxy acrylate with a specific molecular weight with a hydroxyl acrylic resin and an amino resin.
[0005] The second aspect of the present invention is to provide a method for preparing a hot stamping primer.
[0006] A third aspect of the present invention is to provide a UV screen printing ink.
[0007] A fourth aspect of the present invention is to provide an application of hot stamping primer or UV screen printing ink.
[0008] In order to achieve the above object, the technical solution adopted by the present invention is:
[0009] The first aspect of the present invention provides a hot stamping primer, comprising the following components:
[0010] Bisphenol A epoxy acrylate, hydroxy acrylic resin, amino resin, additives;
[0011] The number average molecular weight of the bisphenol A epoxy acrylate is ≥1000.
[0012] The invention obtains a UV-curing and heat-curing dual-curing UV hot stamping primer by compounding bisphenol A epoxy acrylate, hydroxyl acrylic resin and amino resin. The dual-curing UV hot stamping primer has the characteristics of excellent resistance to liquor and water immersion and good storage stability.
[0013] The molecular weight of the bisphenol A epoxy acrylate used in the present invention is not less than 1000, which is beneficial to the improvement of the alcohol resistance and water resistance of the hot stamping base oil, as well as the storage stability. At the same time, the bisphenol A epoxy acrylate is compounded with hydroxy acrylic resin and amino resin, which can improve the temperature resistance of the hot stamping base oil during hot stamping, and the hot stamping property is good. The addition of hydroxy acrylic resin can increase the crosslinking density of the hot stamping base oil during baking and curing, improve its adhesion after film formation, and simultaneously improve alcohol resistance and water resistance. In addition, the introduction of amino resin is also conducive to improving the adhesion of the hot stamping base oil after film formation.
[0014] In some embodiments of the present invention, the additives include reactive diluents, photoinitiators, inhibitors, defoamers, leveling agents, and adhesion promoters.
[0015] In some embodiments of the present invention, the molecular weight of the bisphenol A epoxy acrylate is 1000-2000.
[0016] In some embodiments of the present invention, the molecular weight of the bisphenol A epoxy acrylate is 1500-2000.
[0017] In some embodiments of the present invention, the molecular weight of the hydroxy acrylic resin is 1000-3000.
[0018] In some embodiments of the present invention, the hot stamping primer comprises the following components in parts by mass:
[0019] 30-50 parts of bisphenol A epoxy acrylate, 10-20 parts of hydroxy acrylic resin, 3-10 parts of amino resin, and 24-44 parts of additives.
[0020] In some embodiments of the present invention, the additives include the following components, measured by mass: 20 to 30 parts of active diluent, 2 to 5 parts of photoinitiator, 0.1 to 0.5 parts of inhibitor, 1 to 2 parts of defoaming agent, 0.5 to 1 part of leveling agent, and 0.5 to 1 part of adhesion promoter.
[0021] In some specific embodiments of the present invention, the hot stamping primer comprises the following components in parts by mass:
[0022] 30-50 parts of bisphenol A epoxy acrylate,
[0023] 10-20 parts of hydroxy acrylic resin,
[0024] 3-10 parts of amino resin,
[0025] 20-30 parts of active diluent,
[0026] 2 to 5 parts of photoinitiator,
[0027] 0.1 to 0.5 parts of polymerization inhibitor,
[0028] 1-2 parts of defoaming agent,
[0029] 0.5 to 1 part of leveling agent,
[0030] Adhesion promoter 0.5 to 1 part.
[0031] By adjusting the dosage of each component, it is helpful to further improve the flexibility and temperature resistance of the hot stamping base oil and improve its hot stamping properties.
[0032] In some examples of the present invention, the hot stamping primer comprises the following components by weight:
[0033] 35-45 parts of bisphenol A epoxy acrylate,
[0034] 10-15 parts of hydroxy acrylic resin,
[0035] 3-10 parts of amino resin,
[0036] Active diluent 25-35 parts,
[0037] 2 to 4 parts of photoinitiator,
[0038] 0.1 to 0.5 parts of polymerization inhibitor,
[0039] 1 to 1.5 parts of defoaming agent,
[0040] 0.5 to 1 part of leveling agent,
[0041] Adhesion promoter 0.5 to 1 part.
[0042] In some specific embodiments of the present invention, the mass fraction of bisphenol A epoxy acrylate in the hot stamping primer is 38 to 42 parts.
[0043] In some examples of the present invention, the mass percentage of bisphenol A epoxy acrylate in the hot stamping primer is 38-42%.
[0044] In some embodiments of the present invention, the bisphenol A epoxy acrylate is prepared by a preparation method comprising the following steps:
[0045] The epoxy resin and bisphenol A are subjected to chain extension reaction, acrylic monomer and catalyst are added, and when the acid value is less than 1 mg KOH / g, an active diluent is added to obtain bisphenol A epoxy acrylate.
[0046] In some embodiments of the present invention, after the chain extension reaction, the temperature is maintained at 100-120° C., and acrylic acid monomer and catalyst are added.
[0047] In some embodiments of the present invention, the amount of the acrylic monomer added is equal to the molar amount of the epoxy group.
[0048] In some embodiments of the present invention, after the reactive diluent is added, the solid content of the resin is ≥70%.
[0049] In some embodiments of the present invention, the catalyst comprises a triphenylphosphine catalyst.
[0050] In some embodiments of the present invention, the hydroxy acrylic resin is prepared by a preparation method comprising the following steps:
[0051] In a solvent and an initiator, methyl methacrylate, acrylic acid, hydroxyethyl methacrylate and butyl acrylate are subjected to a reflux reaction, the solvent is removed, and an active diluent is added to obtain a hydroxy acrylic resin.
[0052] In some embodiments of the present invention, the hydroxylated acrylic resin comprises the following components in parts by mass:
[0053] 38-42 parts of solvent, 3-5 parts of initiator, 25-30 parts of methyl methacrylate, 4-6 parts of acrylic acid, 6-10 parts of butyl acrylate, and 13-18 parts of hydroxyethyl methacrylate.
[0054] In some embodiments of the present invention, the solvent includes butyl acetate.
[0055] In some embodiments of the present invention, the initiator comprises dibenzoyl peroxide (BPO).
[0056] In some embodiments of the present invention, the temperature of the reflux reaction is 120-130°C.
[0057] In some embodiments of the present invention, the method of removing the solvent is distillation under reduced pressure.
[0058] In some embodiments of the present invention, the amino resin comprises a fully methylated amino resin.
[0059] In some embodiments of the present invention, the fully methylated amino resin includes Cytec 308 fully methylated amino resin and / or Sanmu 5747 fully methylated amino resin.
[0060] In some embodiments of the present invention, the reactive diluent includes at least one of 2-phenoxyethyl acrylate (PHEA), diethylene glycol monophenyl ether acrylate (PH2EA), isobornyl acrylate (IBOA), tetrahydrofuran acrylate (THFA), and trimethylolpropane triacrylate (TMPTA).
[0061] In some embodiments of the present invention, the active diluent includes at least three of 2-phenoxyethyl acrylate (PHEA), diethylene glycol monophenyl ether acrylate (PH2EA), isobornyl acrylate (IBOA), tetrahydrofuran acrylate (THFA), and trimethylolpropane triacrylate (TMPTA).
[0062] In some specific embodiments of the present invention, the active diluent includes at least one of the following combinations: 2-phenoxyethyl acrylate (PHEA), diethylene glycol monophenyl ether acrylate (PH2EA) and isobornyl acrylate (IBOA); 2-phenoxyethyl acrylate (PHEA), trimethylolpropane triacrylate (TMPTA) and isobornyl acrylate (IBOA).
[0063] In some embodiments of the present invention, the photoinitiator includes at least two of 1-hydroxycyclohexyl phenyl ketone, 2,4,6 (trimethylbenzoyl) diphenyl phosphine oxide, 2-methyl-1-[4-(methylthio) phenyl] -2-(4-morpholinyl) -1-propanone, and isopropylthioxanthone.
[0064] In some embodiments of the present invention, the photoinitiator includes 1-hydroxycyclohexyl phenyl ketone, 2,4,6 (trimethylbenzoyl) diphenyl phosphine oxide, 2-methyl-1-[4-(methylthio)phenyl]-2-(4-morpholinyl)-1-propanone and isopropylthioxanthone.
[0065] In some specific embodiments of the present invention, the mass ratio of each component in the photoinitiator is: 1-hydroxycyclohexyl phenyl ketone: 2,4,6 (trimethylbenzoyl) diphenyl phosphine oxide: 2-methyl-1-[4-(methylthio) phenyl] -2-(4-morpholinyl) -1-propanone: isopropylthioxanthone = (30-40): (30-40): (15-25): (5-15).
[0066] In some embodiments of the present invention, the defoaming agent is BYK1799 or a commercially available product of the same type.
[0067] In some embodiments of the present invention, the leveling agent is BYK333 or a commercially available product of the same type.
[0068] In some embodiments of the present invention, the adhesion promoter is a phosphate type adhesion promoter.
[0069] In some embodiments of the present invention, the adhesion promoter is Sartomer CD9051 or a commercially available product of the same type.
[0070] In some embodiments of the present invention, the inhibitor is MEHQ.
[0071] The second aspect of the present invention provides a method for preparing the hot stamping primer according to the first aspect of the present invention, comprising the following steps:
[0072] Bisphenol A epoxy acrylate, hydroxyl acrylic resin, amino resin and additives are mixed and dispersed to obtain hot stamping base oil.
[0073] In some embodiments of the present invention, the mixing and dispersing is stirring and dispersing.
[0074] A third aspect of the present invention provides a UV silk screen printing ink, wherein the UV silk screen printing ink comprises the hot stamping primer described in the first aspect of the present invention.
[0075] The fourth aspect of the present invention provides an application of the hot stamping primer described in the first aspect of the present invention or the UV screen printing ink described in the third aspect of the present invention in the field of glass bottle printing.
[0076] In some embodiments of the present invention, the UV screen printing ink or hot stamping primer is used for screen printing.
[0077] In some embodiments of the present invention, the glass bottle comprises a wine bottle.
[0078] In some embodiments of the present invention, the printing on the glass bottle body is printing of graphics and text on the glass bottle body.
[0079] Compared with the prior art, the present invention has the following beneficial effects:
[0080] (1) The present invention obtains a dual-curing UV hot stamping primer by compounding bisphenol A epoxy acrylate, hydroxyl acrylic resin, and amino resin, which has the characteristics of excellent resistance to liquor and water immersion and good storage stability. Among them, the molecular weight of bisphenol A epoxy acrylate is not less than 1000, which is conducive to improving the alcohol resistance and water resistance and storage stability of the hot stamping primer, and the compounding of bisphenol A epoxy acrylate with hydroxyl acrylic resin and amino resin can improve the temperature resistance of the hot stamping primer during hot stamping, and the hot stamping performance is good. Amino resin and hydroxyl acrylic resin can increase the crosslinking density of the hot stamping primer during baking and curing, improve its adhesion after film formation, and further improve alcohol resistance and water resistance.
[0081] (2) The hot stamping primer obtained by the present invention has good drying properties, excellent adhesion, good flexibility, good hot stamping properties, excellent alcohol and water immersion resistance, and good storage stability. It can be used as a UV screen printing ink and applied to the printing of glass bottle graphics, text, etc. DETAILED DESCRIPTION
[0082] The present invention is further described in detail below by specific examples. Unless otherwise specified, the raw materials, reagents or devices used in the examples and comparative examples can be obtained from conventional commercial sources or can be obtained by prior art methods. Unless otherwise specified, the experiments or test methods are conventional methods in the art.
[0083] Some of the raw materials used in the following examples and comparative examples of the present invention are described as follows:
[0084] Bisphenol A epoxy acrylate: commercially available E51 epoxy resin and bisphenol A are put into a reactor according to the designed ratio of E51 epoxy group molar amount: bisphenol A molar amount = 1.37:1.54 for chain extension reaction (the epoxy group molar amount is calculated based on the actually measured epoxy value). After the reaction is complete, the temperature is maintained at 100° C., an acrylic acid monomer in an amount equal to the epoxy group molar amount is added, and then a triphenylphosphine catalyst is added in batches until the acid value is less than 1 mgKOH / g, and then an active diluent PHEA is added and diluted to a resin solid content of 60% in the active diluent to obtain bisphenol A epoxy acrylate with a molecular weight of 1500 to 2000.
[0085] Hydroxylated acrylic resin: According to the formula shown in Table 1, butyl acetate is used as a solvent and BPO is used as an initiator. Methyl methacrylate, acrylic acid, hydroxyethyl methacrylate and butyl acrylate are mixed and reacted under reflux conditions. The reflux temperature reaches the boiling point of the butyl acetate solvent (126°C ± 2°C). After the conversion rate reaches 98% or above, the solvent butyl acetate is removed by reduced pressure distillation, and then the temperature is lowered to below 80°C, and an active diluent PHEA is added to obtain a hydroxylated acrylic resin with a molecular weight of 1000 to 3000.
[0086] Table 1 Reference formula of hydroxyl acrylic resin
[0087] Raw material name Amount (parts by mass) Butyl acetate 39~41 BPO 3.9~4.1 Methyl Methacrylate 29~30 acrylic acid 5~6 Butyl acrylate 8~10 Hydroxyethyl Methacrylate 15~16
[0088] Amino resin: Cyanotec 308 fully methylated amino resin, which is commercially available. The Cyanotec 308 fully methylated amino resin in the following examples and comparative examples is of the same kind; Sanmu 5747 fully methylated amino resin, which is commercially available.
[0089] Photoinitiator: 1-hydroxycyclohexyl phenyl ketone (184), 2,4,6 (trimethylbenzoyl) diphenyl phosphine oxide (TPO), 2-methyl-1-[4-(methylthio)phenyl]-2-(4-morpholinyl)-1-propanone (907) and isopropylthioxanthone (2, 4 isomer mixture) (ITX) were mixed in a mass ratio of 35:35:20:10.
[0090] The following is described in detail with reference to the embodiments and comparative examples:
[0091] Embodiments 1 to 5
[0092] Examples 1 to 5 provide a hot stamping primer, and the specific formula is shown in Table 2.
[0093] Table 2 Hot stamping base oil formula table of Examples 1 to 5 (parts by mass)
[0094]
[0095]
[0096] The preparation method of the hot stamping primer of the above embodiments 1 to 5 can refer to the following steps:
[0097] According to the formula ratio, bisphenol A epoxy acrylate, hydroxy acrylic resin, amino resin, active diluent, defoaming agent, leveling agent, adhesion promoter, polymerization inhibitor and photoinitiator are stirred and dispersed uniformly to obtain hot stamping base oil.
[0098] Comparative Examples 1 to 3
[0099] Comparative Examples 1 to 3 provide a hot stamping primer, and the formula is shown in Table 3.
[0100] Table 3 Formula of hot stamping base oil of comparative examples 1 to 3 (parts by mass)
[0101]
[0102] In Table 3, the commercially available E51 epoxy ester is an epoxy ester synthesized from Nan Ya 128 epoxy resin and acrylic acid, and has a weight average molecular weight of about 520; the commercially available E20 epoxy ester is an epoxy ester synthesized from Nan Ya 901 epoxy resin and acrylic acid, and has a weight average molecular weight of about 1140.
[0103] The preparation methods of the hot stamping primers of Comparative Examples 1 to 3 are the same as those of Example 1.
[0104] Results
[0105] The film-forming steps of the hot stamping primer of the above-mentioned embodiment and comparative example are as follows: add active diluent PHEA to the hot stamping primer obtained in the above-mentioned embodiment and comparative example to adjust the viscosity to a non-stick screen, let it stand until the bubbles are eliminated, and then screen print it on water transfer paper. After screen printing, use an LED UV machine to irradiate and cure it 1 to 2 times, then perform hot stamping at 100 to 120°C, and then transfer print it to a glass bottle, and bake it at 180°C for 15 to 20 minutes to form a film.
[0106] The specific performance test of the hot stamping primer of the above embodiment and comparative example was carried out according to the following method:
[0107] Dryness: After screen printing the hot stamping primer, cure it twice with an LED UV machine and touch it with your hand to see if it is sticky.
[0108] Silk screen printing: Silk screen the gold-stamping primer, and observe whether the board surface is flat and clear after silk screen printing, whether the silk screen mesh is blocked, and whether it sticks to the silk screen.
[0109] Hot stamping: Use the hot stamping machine to hot stamp the UV-cured hot stamping primer and observe whether the board surface is bright and flawless.
[0110] Flexibility: Observe whether the gold-stamped primer is easily broken when it is silk-screened and then transferred to the glass bottle.
[0111] Adhesion: Transfer the UV-cured hot stamping primer to the glass bottle, bake it at 180℃ for 15-20 minutes, and use the hundred-grid method to test the adhesion after cooling. 5B is 100% adhesion, 4B is 80% adhesion, 3B is 60% adhesion, and 0B is no adhesion.
[0112] Alcohol resistance: Soak in 50-degree liquor for 30 minutes: Transfer the UV-cured hot stamping primer to the glass bottle, bake at 180°C for 15-20 minutes, leave it at room temperature for 2 hours, then completely soak the printed hot stamping primer in 50-degree liquor. After soaking for 30 minutes, observe that there is no abnormality on the board surface. Test the adhesion after returning to room temperature for 1 hour.
[0113] Water resistance: Soak in 40℃ hot water for 30 minutes: Transfer the UV-cured hot stamping primer to the glass bottle, bake at 180℃ for 15-20 minutes, leave it at room temperature for 2 hours, then completely soak the printed hot stamping primer in 40℃ hot water. After soaking for 30 minutes, observe that there is no abnormality on the board surface. Test the adhesion after returning to room temperature for 1 hour.
[0114] Storage stability: Place the hot stamping primer in a light-proof and sealed container and store it in a 50°C oven for 7 days. After storage, compare the rotational viscosity with that before storage (tested in accordance with GB / T 10247-2008) to determine whether it has thickened. The viscosity increase should not exceed 1000mPa.S / 25°C as the standard.
[0115] The test results are shown in Tables 4 and 5.
[0116] Table 4 Performance test results of the hot stamping primer in the embodiment
[0117]
[0118]
[0119] Table 5 Performance test results of hot stamping primer of comparative example
[0120]
[0121] It can be seen from Table 4 and Table 5 that the hot stamping primer obtained by the present invention has better comprehensive performance, good drying property, excellent adhesion, good flexibility, good hot stamping property, excellent resistance to liquor and water immersion, and good storage stability.
[0122] In Comparative Examples 1 and 2, conventional commercially available low molecular weight epoxy resins were used to replace bisphenol A epoxy acrylate, and the obtained hot stamping primer had poor temperature resistance and could not be hot stamped. In addition, the alcohol resistance and water resistance after film formation also decreased, and all tests failed.
[0123] Comparative Example 3 lacks hydroxyl acrylic resin, and the cross-linking density is insufficient during the baking and curing process after screen printing. The alcohol resistance and water resistance after film formation are unqualified, and the adhesion is reduced to only 3B, making it difficult to print graphics on the glass bottle.
[0124] In summary, in the hot stamping base oil of the present invention, the molecular weight of bisphenol A epoxy acrylate is not less than 1000, which is conducive to the improvement of alcohol resistance, water resistance and storage stability of the hot stamping base oil, and bisphenol A epoxy acrylate is compounded with hydroxy acrylic resin and amino resin, which can improve the temperature resistance of the hot stamping base oil during hot stamping, and the hot stamping property is good. Amino resin and hydroxy acrylic resin can improve the crosslinking density of the hot stamping base oil during baking and curing, improve its adhesion after film formation, and further improve alcohol resistance and water resistance. Therefore, the hot stamping base oil obtained by the present invention has good dryness, excellent adhesion, good flexibility, good hot stamping property, excellent alcohol resistance and water immersion resistance, and good storage stability, and can be used as UV silk screen ink for printing of glass bottle graphics, text, etc.
[0125] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A hot stamping primer, characterized in that: The components include: Bisphenol A epoxy acrylate, hydroxy acrylic resin, amino resin, additives; The number average molecular weight of the bisphenol A epoxy acrylate is ≥1000.
2. The hot stamping primer according to claim 1, characterized in that: The additives include active diluent, photoinitiator, polymerization inhibitor, defoamer, leveling agent and adhesion promoter.
3. The hot stamping primer according to claim 1 or 2, characterized in that: The molecular weight of the bisphenol A epoxy acrylate is 1000 to 2000; And / or, the molecular weight of the hydroxy acrylic resin is 1000-3000.
4. The hot stamping primer according to claim 1 or 2, characterized in that: Calculated by mass, it includes the following components: 30-50 parts of bisphenol A epoxy acrylate, 10-20 parts of hydroxy acrylic resin, 3-10 parts of amino resin, and 24-44 parts of additives.
5. The hot stamping primer according to claim 4, characterized in that: The additives include the following components by weight: 20 to 30 parts of active diluent, 2 to 5 parts of photoinitiator, 0.1 to 0.5 parts of inhibitor, 1 to 2 parts of defoamer, 0.5 to 1 parts of leveling agent, and 0.5 to 1 parts of adhesion promoter.
6. The hot stamping primer according to claim 1 or 2, characterized in that: The active diluent includes at least one of 2-phenoxyethyl acrylate, diethylene glycol monophenyl ether acrylate, isobornyl acrylate, tetrahydrofuran acrylate, and trimethylolpropane triacrylate.
7. The hot stamping primer according to claim 1 or 2, characterized in that: The photoinitiator includes at least two of 1-hydroxycyclohexyl phenyl ketone, 2,4,6 (trimethylbenzoyl) diphenyl phosphine oxide, 2-methyl-1-[4-(methylthio) phenyl]-2-(4-morpholinyl)-1-propanone, and isopropylthioxanthone.
8. A method for preparing the hot stamping primer according to any one of claims 1 to 7, characterized in that: The steps include: Bisphenol A epoxy acrylate, hydroxyl acrylic resin, amino resin and additives are mixed and dispersed to obtain hot stamping base oil.
9. A UV screen printing ink, characterized in that: The silk screen printing ink comprises the hot stamping primer according to any one of claims 1 to 7.