Surface protective film with release film
By using a polyethylene terephthalate film and a (meth)acrylate copolymer cross-linked adhesive layer in the surface protection film, combined with an amino-structured release layer, the non-silicone release layer is solved The problem of compression and contamination during the peeling process is eliminated, and a stable and safe peeling effect is achieved.
Patent Information
- Application Number
- CN202410371807.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-29
- Publication Date
- 2024-10-01
AI Technical Summary
Existing non-silicone release layers are prone to compression when the adhesive layer of the protective film is peeled off from the surface, resulting in difficulty in peeling and contamination of the adhesive layer.
A polyethylene terephthalate film is used as the first base material layer, the adhesive layer is a (meth)acrylate copolymer cross-linked, and the second base material layer of the release film contains an amino-structured release layer. The intensity of Si under fluorescent X-rays is below 0.5kcps, and the Tg is below +22°C. A melamine structure, acrylic acid, polyol and other components are added to the peeling layer to reduce the peeling force and inhibit the transfer of silicone components.
It effectively avoids the compression phenomenon during the peeling process, reduces the pollution of the adhesive layer, and improves the stability and use safety of the peeling film.
Smart Images

Figure CN118725756A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a surface protective film with a peeling film. Background Art
[0002] Surface protection films are used to protect the surfaces of optical components, electronic components, and the like.
[0003] For example, Patent Document 1 describes an optical surface protective film with a spacer, wherein the spacer is provided on the side of the adhesive layer opposite to the polyester film, wherein the Si-Kα ray intensity of the surface of the adhesive layer after the spacer is peeled off under fluorescent X-ray is 2.5 kcps or less. In addition, Patent Document 2 describes an optical surface protective film with a spacer, wherein the spacer has a substrate and a non-silicone release layer.
[0004] Patent Document 1: Japanese Patent Application Publication No. 2016-145341
[0005] Patent Document 2: Japanese Patent Application Publication No. 2017-31278 Summary of the invention
[0006] If a non-silicone release layer is used, compression is likely to occur when the release film is peeled off from the adhesive layer of the surface protective film. Here, compression (zipping) means that the release film cannot be peeled off from the adhesive layer of the surface protective film with a certain force, and as a result of slight vibration during peeling, peeling marks remain on the adhesive layer and peeling sounds are generated.
[0007] An object of the present invention is to provide a surface protection film with a release film which is less likely to be compressed.
[0008] The first embodiment of the present invention is a surface protective film with a release film, wherein the surface protective film comprises: a first substrate layer, which is composed of a polyethylene terephthalate film; and an adhesive layer, which is formed by cross-linking a (meth)acrylate copolymer, the surface protective film is a surface protective film for optical or electronic use, the release film comprises a second substrate layer and a release layer formed on one side of the second substrate layer, the release layer of the release film contains an amino structure, and the Si in the release layer of the release film is less than 0.5 kcps under fluorescent X-rays.
[0009] Second aspect: The surface protection film with a release film according to the first aspect, wherein the surface protection film has a Tg of +22° C. or less, and the release layer of the release film contains a component that does not chemically react with the amino structure.
[0010] Third aspect: The surface protection film with a release film according to the first aspect or the second aspect, wherein Tg of the surface protection film is +11° C. or less.
[0011] The fourth method: A surface protective film with a release film according to any one of the first to third methods, wherein when the instantaneous maximum value of the release force when the release film is peeled off at a peeling speed of 0.3 m / min and a peeling angle of 180 degrees is set to B, and the average release force when the release film is peeled off at a peeling speed of 0.3 m / min and a peeling angle of 180 degrees is set to C, the value A obtained by the formula: A=B / C is less than 1.5.
[0012] A fifth aspect: A surface protection film with a release film according to any one of the first to fourth aspects, wherein when an average release force when the release film is peeled off at a peeling speed of 0.3 m / min and a peeling angle of 180 degrees is defined as C, C is greater than 0.02 N / 25 mm.
[0013] Sixth aspect: The surface protection film with a release film according to any one of the first aspect to the fifth aspect, wherein the release layer of the release film contains a melamine structure.
[0014] Seventh aspect: The surface protection film with a release film according to any one of the first aspect to the sixth aspect, wherein the release layer contains any one of acrylic acid, polyol, and polyether.
[0015] According to the present invention, it is possible to provide a surface protection film with a release film which is not easily compressed and uses a non-silicone release layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 This is a cross-sectional view showing an example of a surface protection film with a release film.
[0017] (Explanation of Reference Numerals)
[0018] 10: Surface protection film with peel-off film
[0019] 11: Second substrate layer
[0020] 12: Peel off layer
[0021] 13: Adhesive layer
[0022] 14: First substrate layer
[0023] 15: Peeling film
[0024] 16: Surface protection film DETAILED DESCRIPTION
[0025] Hereinafter, the present invention will be described based on preferred embodiments.
[0026] like Figure 1 As shown, the surface protection film with a release film 10 according to the embodiment includes a release film 15 and a surface protection film 16 .
[0027] The surface protection film 16 includes a first base material layer 14 made of a polyethylene terephthalate (PET) film and an adhesive layer 13 formed by cross-linking a (meth)acrylic acid ester copolymer. The surface protection film 16 is a surface protection film for optical or electronic use.
[0028] The release film 15 includes a second base layer 11 and a release layer 12 formed on one surface of the second base layer 11. The release layer 12 of the release film 15 includes an amino structure. Si in the release layer 12 of the release film 15 is 0.5 kcps or less under fluorescent X-ray.
[0029] In the surface protection film with release film 10 of the embodiment, Si in the release layer 12 of the release film 15 is 0.5 kcps or less under fluorescent X-ray. The amount of Si in the release layer 12 can be quantified by the intensity (kcps) of Si-Kα rays using fluorescent X-ray analysis. The amount of Si in the release layer 12 is a value that does not include the amount of Si in the second substrate layer 11. After measuring the amount of Si in the release film 15 from the release layer 12 side, the amount of Si in the second substrate layer 11 without the release layer 12 is subtracted, so that the amount of Si in the release layer 12 can be obtained.
[0030] The small amount of Si in the peeling layer 12 can confirm that the content of silicone components such as organic silicone compounds in the peeling layer 12 is small. In the case where the peeling layer contains silicone components, there is a risk that the silicone components are transferred to the surface of the adhesive layer in large quantities when the peeling film and the surface protection film are attached. In addition, there is a risk that the silicone components transferred to the surface of the adhesive layer contaminate the surface of adherends such as optical components and electronic components. Therefore, by making the amount of Si in the peeling layer 12 within the above range, the surface contamination of the adhesive layer and the adherend can be suppressed.
[0031] In the surface protection film with release film 10 of the embodiment, the release film 15 includes an amino structure in the release layer 12. The release layer 12 including the amino structure may include a component having an amino structure. Specific examples include a structure consisting of one component having an amino structure, a structure consisting of two or more components having an amino structure, and a structure consisting of at least one component having an amino structure and at least one component not having an amino structure.
[0032] The release layer 12 may be composed of one component or two or more components. When the release layer 12 is composed of a composition containing two or more components, chemical reactions, chemical bonds, etc. may occur between the components contained in the composition.
[0033] The component having an amino structure is not particularly limited, and the release agent component contained in the release layer 12 may be a component having an amino structure. As the component having an amino structure, a component having no Si such as a silicone release agent is preferred. The component other than the silicone release agent may be a component other than a long-chain alkyl material. The release layer 12 may include a component having no long-chain alkyl and having an amino structure and a component having no amino structure and having a long-chain alkyl. The release agent component in the release layer 12 may be one or more than one.
[0034] Specific examples of components having an amino structure include amino resins such as melamine resins, amino alkyd resins, etc. The amino alkyd resin may include a mixture of an amino resin and an alkyd resin. The amino structure contained in the release layer 12 may be a melamine structure or an amino structure other than a melamine structure.
[0035] Amino resin is a resin produced by condensation of a compound having an amino group such as melamine, urea, benzoguanamine, aniline, etc. and a compound having an aldehyde group such as formaldehyde. Amino resin can be used as a thermosetting resin alone or in combination with an alkyd resin, an acrylic resin, an epoxy resin, etc.
[0036] The release film 15 preferably contains a melamine structure in the release layer 12. The release layer 12 containing a melamine structure may contain a component having a melamine structure. Specific examples include a structure composed of one component having a melamine structure, a structure composed of two or more components having a melamine structure, and a structure composed of at least one component having a melamine structure and at least one component not having a melamine structure.
[0037] The component having a melamine structure is not particularly limited, and the release agent component contained in the release layer 12 may be a component having a melamine structure. Specific examples of the component having a melamine structure include melamine resins.
[0038] Examples of the melamine resin include alkylated melamine resins such as methylated melamine resins, ethylated melamine resins, and butylated melamine resins, and more specifically, full ether type methylated melamine resins and methylol type methylated melamine resins.
[0039] The thickness, additives, etc. of the release layer 12 can be appropriately designed. The release layer 12 may contain any one selected from a component that chemically reacts with an amino structure, a component that does not chemically react with an amino structure, and other components as a component other than the component having an amino structure.
[0040] The component that does not chemically react with the amino structure may be a transfer component that can be transferred from the release layer 12 to the adhesive layer 13. The transfer component may be added in a small amount compared to the release agent component. For example, the total amount of the release layer 12 is set to 100 parts by weight, and the release agent component may be added in a range of 60 parts by weight to 99 parts by weight and the transfer component may be added in a range of 1 part by weight to 40 parts by weight. The transfer component in the release layer 12 may be one type or two or more types.
[0041] The amount of the transfer component is not particularly limited, and may be 39 parts by weight or less based on 100 parts by weight of the total amount of the release layer 12. The transfer component may be 35 parts by weight or less, 30 parts by weight or less, 25 parts by weight or less, 20 parts by weight or less, 15 parts by weight or less, 10 parts by weight or less, 5 parts by weight or less, or even less.
[0042] When the release layer 12 contains components other than the release agent component and the transfer component, the components other than the release agent component and the transfer component may be 39 parts by weight or less based on the total amount of the release layer 12 being 100 parts by weight. The amount of the components other than the release agent component and the transfer component is not particularly limited, and may be 35 parts by weight or less, 30 parts by weight or less, 25 parts by weight or less, 20 parts by weight or less, 15 parts by weight or less, 10 parts by weight or less, 5 parts by weight or less, or less.
[0043] The release layer 12 preferably contains any one of acrylic acid, polyol, and polyether. More specifically, the release layer 12 preferably contains any one of acrylic acid, polyol, and polyether as at least one component. Any one of acrylic acid, polyol, and polyether may be a component without an amino structure, may be the above-mentioned transfer component, may be a component that chemically reacts with an amino structure, or may be a component that does not chemically react with an amino structure.
[0044] The release film 15 containing the transfer component in the release layer 12 is preferably a micro-transfer type that transfers a small amount to the adhesive layer. The release film 15 containing no transfer component in the release layer 12 is a non-transfer type that does not transfer to the adhesive layer.
[0045] The non-transfer type and the micro-transfer type can both suppress the occurrence of compression. The micro-transfer type release film 15 is harder than the non-transfer type release film 15, and can suppress the occurrence of compression (zipping) even when combined with the surface protection film 16 having the adhesive layer 13 with a high Tg, so it is more preferred.
[0046] The acrylic acid may be any component having an acrylic structure, and examples thereof include acrylic compounds, acrylic polymers, and acrylic resins.
[0047] The polyol may be any component having a polyol structure, and examples thereof include polyol compounds.
[0048] The polyether may be any component having a polyether structure, and examples thereof include polyether compounds.
[0049] The release layer 12 may contain a polyol compound having a polyether structure, such as polyethylene glycol and polypropylene glycol.
[0050] As required, additives may be added to the release layer 12. Examples of additives include stabilizers, antioxidants, ultraviolet absorbers, antistatic agents, thickeners, lubricants, foaming agents, defoamers, inorganic particles, and organic particles. In addition, the release layer 12 may be formed without containing these additives. Examples of lubricants include, but are not particularly limited to, fatty acid esters.
[0051] Sulfonic acid such as p-toluenesulfonic acid can be used as an additive for the release layer 12. Sulfonic acid can be a catalyst for the curing reaction of melamine resin. When curing the melamine resin, the coating film applied on the second substrate layer 11 can be treated under heating conditions as needed.
[0052] By curing the amino resin (component having an amino structure) such as melamine resin contained in the peeling layer 12, the transfer from the peeling layer 12 to the adhesive layer 13 is suppressed. In addition, since the component that chemically reacts with the amino structure is also in a state of being bonded to the cured resin, the transfer to the adhesive layer 13 can be suppressed. Therefore, it is suitable for a peeling layer 12 of a micro-transfer type or a non-transfer type.
[0053] The second substrate layer 11 of the release film 15 is not particularly limited, and a polyester resin film such as polyethylene terephthalate (PET) film can be used. The thickness, additives, etc. of the second substrate layer 11 can be appropriately designed. The second substrate layer 11 can contain silicon (Si) compounds such as silicon dioxide (SiO2), silicates, clay minerals, and zeolites as anti-blocking agents, fillers, etc.
[0054] The surface protection film 16 of the example in the figure has an adhesive layer 13 on one side of the first substrate layer 14. The adhesive layer 13 is formed by crosslinking a (meth) acrylic acid ester copolymer. As the (meth) acrylic acid ester copolymer, there can be cited a copolymer formed by copolymerizing two or more monomers including a (meth) acrylic acid monomer or a (meth) acrylic acid ester, (meth) acrylamide, or a (meth) acrylic acid derivative monomer. The thickness, additives, etc. of the adhesive layer 13 can be appropriately designed.
[0055] In the present specification, (meth)acrylate refers to acrylate and / or methacrylate. (Meth)acrylic acid, (meth)acrylate, (meth)acrylamide, etc. also refer to acrylic acid and / or methacrylic acid and derivatives thereof.
[0056] In order to crosslink the (meth)acrylate copolymer, an ultraviolet curing agent, an electron beam curing agent, a crosslinking agent, etc. can be used. The crosslinking agent may be a radical crosslinking agent such as a peroxide, or a reactive crosslinking agent such as an isocyanate compound or an epoxy compound.
[0057] The reactive crosslinking agent can react with polar functional groups such as hydroxyl groups and carboxyl groups contained in the (meth)acrylate copolymer to crosslink the copolymer. The (meth)acrylate copolymer having a polar functional group can be obtained by copolymerizing a (meth)acrylate monomer having a polar functional group with the (meth)acrylate copolymer.
[0058] The Tg of the surface protection film 16 is preferably +22° C. or lower, and more preferably +11° C. or lower. The Tg of the surface protection film 16 can be measured by attaching the surface protection film 16 having the first base material layer 14 and the adhesive layer 13 to a viscoelasticity measuring device.
[0059] Tg generally refers to the glass transition temperature. The glass transition temperature (Tg) is a type of transition temperature and can be measured using various methods such as differential scanning calorimetry (DSC), differential thermal analysis (DTA), and dynamic viscoelasticity measurement (DMA).
[0060] When the temperature dependence of the loss tangent tanδ is measured by dynamic viscoelasticity measurement, the glass transition temperature (Tg) is detected from the peak temperature rather than from the inflection point or baseline displacement, so that the measurement becomes easy. Therefore, even for a laminate of heterogeneous materials such as the surface protection film 16, the Tg of the surface protection film 16 can be obtained by observing the apparent peak.
[0061] The Tg of the surface protection film 16 is not limited to the glass transition of the adhesive layer 13 and the first substrate layer 14 at the same temperature, as long as the Tg value can be measured by the above method. The glass transition temperature (Tg) of the polyethylene terephthalate film constituting the first substrate layer 14 and the glass transition temperature (Tg) of the crosslinked product of the (meth) acrylic acid ester copolymer constituting the adhesive layer 13 do not necessarily need to be the same.
[0062] In the design of acrylic adhesives, the glass transition temperature (Tg) of the (meth)acrylic acid ester copolymer before crosslinking is usually controlled. The glass transition temperature (Tg) of the (meth)acrylic acid ester copolymer is not particularly limited, but in order to obtain a soft adhesive layer 13, it is preferably less than -30°C, and can also be -70°C or more and -40°C or less.
[0063] According to the surface protection film with release film 10 of the embodiment, a wide range of Tg can be selected, and therefore, a (meth)acrylate copolymer used in the adhesive layer 13 can be selected with a relatively low Tg as in the past, or a higher Tg than in the past. The (meth)acrylate copolymer can be appropriately designed according to the application and performance of the surface protection film 16.
[0064] A polyethylene terephthalate (PET) film can be used as the first substrate layer 14 of the surface protection film 16. The thickness, additives, etc. of the first substrate layer 14 can be appropriately designed. The first substrate layer 14 can contain silicon (Si) compounds such as silicon dioxide (SiO2), silicates, clay minerals, and zeolites as anti-blocking agents, fillers, and the like.
[0065] In this specification, the instantaneous maximum value of the peeling force (instantaneous maximum peeling force) when the release film 15 is peeled off at a peeling speed of 0.3 m / min and a peeling angle of 180 degrees is referred to as B, and the average peeling force when the release film 15 is peeled off at a peeling speed of 0.3 m / min and a peeling angle of 180 degrees is referred to as C. These peeling forces are measured by peeling the release film 15 from the adhesive layer 13 of the surface protection film 16.
[0066] When the ratio obtained by the formula: A=B / C is defined as A, the value of A is preferably 1.5 or less, more preferably 1.2 or less. When the ratio A of the instantaneous maximum peel force / average peel force is small, the release film 15 is less likely to be compressed when being peeled from the surface protection film 16 .
[0067] The value of the average peel force C is preferably greater than 0.02 N / 25 mm, and more preferably greater than 0.04 N / 25 mm. When the value of the average peel force C is small, the release film 15 is easily peeled from the surface protection film 16 .
[0068] In the surface protection film with release film 10, release film 15 is overlapped on surface protection film 16 in a state where release layer 12 and adhesive layer 13 face each other. Surface protection film 16 is used to protect the surface of the protection object in a state where release film 15 is peeled off from surface protection film with release film 10. At this time, adhesive layer 13 is used to adhere surface protection film 16 to the surface of the protection object.
[0069] The object to be protected by the surface protection film 16 is not particularly limited to optical components and electronic components, and examples thereof include optical films, optical glass, polarizing plates, phase difference plates, display panels, touch panels, etc. Examples of optical films include polarizing films, phase difference films, anti-reflection films, anti-glare (anti-glare) films, ultraviolet absorption films, infrared absorption films, optical compensation films, and brightness enhancement films.
[0070] If the surface protection film 16 is colorless and transparent, the state of the protected object can be visually confirmed even if the surface protection film 16 is attached, so it is preferred. The release film 15 can be colorless and transparent. As the second substrate layer 11, the release layer 12, the adhesive layer 13 and the first substrate layer 14, colorless and transparent materials can be selected.
[0071] The surface protection film 16 may be used only in the manufacturing process of the protected object, or may remain attached to the protected object after the protected object is shipped. In order for the surface protection film 16 to continuously protect the surface of the protected object, it is preferred that the surface protection film 16 has a moderate adhesive force to the protected object. When the surface protection film 16 is peeled off from the protected object, it is preferred that the adhesive force of the surface protection film 16 to the protected object is not too high.
[0072] As mentioned above, although this invention was demonstrated based on the suitable embodiment, this invention is not limited to the said embodiment, Various changes are possible within the range which does not deviate from the summary of this invention.
[0073] [Example]
[0074] Hereinafter, the present invention will be specifically described with reference to examples.
[0075] <Method for producing release film>
[0076] The following coating material for forming a release layer was applied to a 38 μm-thick PET film (DIAHOIL (registered trademark) T100 manufactured by Mitsubishi Chemical Corporation) and dried to prepare four types of release films. “Parts” means parts by weight.
[0077] In release film 1 (hereinafter referred to as "RF-1"), a coating material was used in which 3 parts of a curing agent "Arracourt (registered trademark) RA2000" manufactured by Arakawa Chemical Industries, Ltd. were added to 100 parts of a main agent "Arracourt (registered trademark) RL900" manufactured by Arakawa Chemical Industries, Ltd.
[0078] The coating material used in RF-1 contains a component having an amino structure (melamine), a component that chemically reacts with the amino structure (polyol), and a component that does not chemically react with the amino structure (acrylic acid). Among them, the component that contributes to the peeling property is acrylic acid.
[0079] Release film 2 (hereinafter referred to as "RF-2") was prepared by adding 10 parts of polypropylene glycol (weight average molecular weight 1000) and 3 parts of p-toluenesulfonic acid to 90 parts of CYMEL (registered trademark) 303LF, a fully ether type methylated melamine resin manufactured by Allnex.
[0080] The coating material used in RF-2 contains a component having an amino structure (melamine), a component that does not chemically react with the amino structure (polypropylene glycol), and other components (p-toluenesulfonic acid). Among them, the component that contributes to the peeling property is polypropylene glycol.
[0081] In release film 3 (hereinafter referred to as "RF-3"), a coating material was used in which 30 parts of an acrylic polymer (manufactured by Fujimori Industries, Ltd., hydroxyl value 59.8 mgKOH / g) and 3 parts of p-toluenesulfonic acid were added to 70 parts of methylol type methylated melamine resin "CYMEL (registered trademark) 370" manufactured by Allnex.
[0082] The coating material used in RF-3 contains a component having an amino structure (melamine), a component that chemically reacts with the amino structure (acrylic polymer), and other components (p-toluenesulfonic acid). Among them, the component that contributes to the peeling property is the acrylic polymer.
[0083] Release film 4 (hereinafter referred to as "RF-4") was prepared by adding 3 parts of p-toluenesulfonic acid solution "DRYER 900" manufactured by Resonac Co., Ltd. to 100 parts of long-chain alkyl-modified amino alkyd resin "Tesfine (registered trademark) 303" manufactured by Resonac Co., Ltd.
[0084] The coating used in RF_4 contains a component having an amino structure, a component that chemically reacts with the amino structure (alkyd acid), and other components (p-toluenesulfonic acid). Among them, the component that contributes to the peeling property is the alkyd acid.
[0085] Furthermore, as a release film 5 (hereinafter referred to as “RF-5”), a release film “DIAHOIL (registered trademark) MRF” (base material thickness: 38 μm) manufactured by Mitsubishi Chemical Corporation was used.
[0086] Among RF-1 to RF-4, RF-1 and RF-2 are micro-transfer types, and these "components that do not chemically react with the amino structure" are transfer components. RF-3 and RF-4 are non-transfer types that do not use transfer components. RF-5 is a type in which components such as silicone are transferred in large quantities from the release layer to the adhesive layer.
[0087] <Production of (meth)acrylic acid ester copolymer>
[0088] Nitrogen was introduced into a reaction apparatus equipped with a stirrer, a thermometer, a reflux condenser, and a nitrogen inlet pipe to replace the air in the reaction apparatus with nitrogen. Then, 90 parts by weight of the monomers (A) to (C) shown in Table 1 and a solvent (ethyl acetate) were added to the reaction apparatus. Then, 0.1 parts by weight of dimethyl azobisisobutyrate as a polymerization initiator was added dropwise over 2 hours, and the mixture was reacted at 65° C. for 6 hours to obtain a (meth)acrylate copolymer.
[0089] Hereinafter, the obtained five types of (meth)acrylate copolymers are referred to as "AP-A", "AP-B", "AP-C", "AP-D" and "AP-E", respectively. It should be noted that, although the measurement results are not particularly shown, the weight average molecular weight of the obtained (meth)acrylate copolymers is in the range of 100,000 to 1,000,000.
[0090] The monomers used are 2-ethylhexyl acrylate (2EHA), dimethylacrylamide (DMAA), and 4-hydroxybutyl acrylate (4HBA). The values in parentheses in Table 1 (A) to (C) are parts by weight of each monomer.
[0091]
Table 1
[0092] (A) (B) (C) Tg(℃) AP-A 2EHA(100) - 4HBA(4.5) -68.6 AP-B 2EHA(91) DMAA(9) 4HBA(4.5) -59.9 AP-C 2EHA(82) DMAA(18) 4HBA(4.5) -50.4 AP-D 2EHA(73) DMAA(27) 4HBA(4.5) -40.0 AP-E 2EHA(65) DMAA(35) 4HBA(4.5) -30.0
[0093] <Calculation of Tg of (meth)acrylic acid ester copolymer>
[0094] The Tg (° C.) of the (meth)acrylic acid ester-based copolymer is calculated from the glass transition temperature Tgn (° C.) of the homopolymer of each monomer and the value of the weight fraction Wn of each monomer using the following formula.
[0095] 1 / (Tg+273)=Σ[Wn / (Tgn+273)]
[0096] The Tgn of the homopolymers was -70°C for 2EHA, +119°C for DMAA, and -32°C for 4HBA based on literature values. Σ represents the sum of the values of the term [Wn / (Tgn+273)] obtained for each monomer. The results are shown in Table 1 above.
[0097] <Manufacturing of Adhesive Composition and Surface Protective Film>
[0098] The crosslinking agent TKA-100 (isocyanurate of hexamethylene diisocyanate compound, manufactured by Asahi Kasei Corporation) shown in (F) of Table 2 was added to the (meth)acrylate copolymer shown in (E) of Table 2, and stirred and mixed to obtain an adhesive composition. The values shown in parentheses in (E) to (F) of Table 2 are the weight parts of the (meth)acrylate copolymer and the crosslinking agent, respectively.
[0099] The obtained PSA composition was applied onto a 38 μm thick PET film (DIAHOIL (registered trademark) T100 manufactured by Mitsubishi Chemical Corporation) and then dried at 120° C. to remove the solvent, thereby obtaining a surface protection film having a 15 μm thick PSA layer.
[0100] Hereinafter, the 10 types of surface protection films obtained are respectively referred to as "PF-A1", "PF-A2", "PF-B1", "PF-B2", "PF-C1", "PF-C2", "PF-D1", "PF-D2", "PF-E1", and "PF-E2".
[0101]
Table 2
[0102] (E) (F) Tg(℃) PF-A1 AP-A(100) TKA-100(1.2) -19 PF-A2 AP-A(100) TKA-100(2.4) -19 PF-B1 AP-B(100) TKA-100(1.2) -7 PF-B2 AP-B(100) TKA-100(2.4) -5 PF-C1 AP-C(100) TKA-100(1.2) -1 PF-C2 AP-C(100) TKA-100(2.4) +4 PF-D1 AP-D(100) TKA-100(1.2) +18 PF-D2 AP-D(100) TKA-100(2.4) +20 PF-E1 AP-E(100) TKA-100(1.2) +23 PF-E2 AP-E(100) TKA-100(2.4) +29
[0103] <Method for measuring Tg of surface protection film>
[0104] The surface protection film is clamped on a solid shearing fixture which is an option installed in a viscoelasticity measuring device (product name "Rheogel-E4000", manufactured by UBM Co., Ltd.). The set temperature of the device is raised from -50°C to +100°C at a heating rate of 2°C / min, and the storage modulus and loss modulus are measured in shear mode at a deformation amount of 1% and a frequency of 1Hz. From the result, the loss tangent tanδ of the surface protection film per 1°C is calculated. The temperature at which the loss tangent value reaches a maximum value is set to the Tg of the surface protection film. The results are shown in Table 2 above.
[0105] The Tg of the surface protection film is measured by actually manufacturing a surface protection film with a release film by the manufacturing method described later, peeling off the release film, and then attaching it to a viscoelasticity measuring device. However, the Tg of the surface protection film varies depending on the release film, so the results are shown for each surface protection film without distinguishing the type of release film.
[0106] <Method for measuring the amount of Si contained in the peeling layer>
[0107] The amount of Si present in the peeling layer of the peeling film was defined as F (kcps) and measured by fluorescent X-ray analysis. The fluorescent X-ray analysis was performed using an XRF device manufactured by Rigaku Corporation, model "ZSX (registered trademark) PrimsTVi", with a measurement range of 30 mm in diameter, detection X-ray: Si-Kα, output: 30 kV, 100 mA, and spectroscopic crystal PETH.
[0108] As a blank, the amount of Si present in an area equivalent to a 30 mm circle of the base film used in the release film was defined as A (kcps), and measured by fluorescent X-ray analysis under the same conditions as the above F (kcps). The value obtained by subtracting the above A (kcps) from the above F (kcps) was defined as the amount of Si (kcps) contained in the above release layer.
[0109]
Table 3
[0110] Frequency(kcps) RF-1 0.0 RF-2 0.2 RF-3 0.0 RF-4 0.0 RF-5 55.9
[0111] <Method for producing a surface protective film with a release film and method for measuring release force>
[0112] Any one of the 5 release films shown in Table 3 was bonded onto any one of the 10 surface protection films shown in Table 2. Thus, a total of 50 types of surface protection films with release films were produced.
[0113] The surface protective film with a release film was cut into 25 mm wide and 150 mm long to prepare a test piece. The surface protective film side of the test piece was fixed to the test device, and the release film was clamped and peeled off to measure the peeling force (N / 25 mm). The peeling speed was set to 0.3 m / min and the peeling angle was set to 180°.
[0114] The test machine used was a table-type precision universal testing machine (manufactured by Shimadzu Corporation, Autoplotter (registered trademark) AGS-X), and peeling was performed with a length of 120 mm, and the peeling force was measured at a frequency of 60 times per second. Based on the measurement results, the peeling force when the maximum value was instantaneously displayed was set as B, and the average value of the peeling force was set as C. Furthermore, the value of A=B / C was calculated.
[0115] As for the results, the measured values of B (instantaneous maximum value) are shown in Table 4, the measured values of C (average value) are shown in Table 5, and the values of A=B / C are shown in Table 6.
[0116]
Table 4
[0117] B is the maximum value at instant RF-1 RF-2 RF-3 RF-4 RF-5 PF-A1 0.086 0.145 0.126 0.164 0.032 PF-A2 0.061 0.068 0.073 0.101 0.027 PF-B1 0.178 0.373 0.286 0.393 0.054 PF-B2 0.126 0.183 0.186 0.240 0.043 PF-C1 0.407 1.582 0.934 1.639 0.082 PF-C2 0.290 0.620 0.561 0.766 0.062 PF-D1 0.684 4.173 2.257 6.160 0.100 PF-D2 0.446 2.744 1.897 0.829 0.098 PF-E1 0.379 7.050 1.592 2.233 0.087 PF-E2 0.288 1.859 0.642 1.202 0.073
[0118]
Table 5
[0119] C average value RF-1 RF-2 RF-3 RF-4 RF-5 PF-A1 0.078 0.134 0.119 0.157 0.029 PF-A2 0.053 0.064 0.067 0.093 0.023 PF-B1 0.170 0.344 0.274 0.380 0.049 PF-B2 0.121 0.170 0.177 0.232 0.039 PF-C1 0.386 1.339 0.895 1.562 0.075 PF-C2 0.278 0.518 0.536 0.746 0.059 PF-D1 0.653 3.704 0.978 1.977 0.094 PF-D2 0.427 2.521 0.510 0.312 0.077 PF-E1 0.115 0.700 0.225 0.714 0.080 PF-E2 0.109 0.257 0.097 0.213 0.066
[0120]
Table 6
[0121] A=B / C RF-1 RF-2 RF-3 RF-4 RF-5 PF-A1 1.1 1.1 1.1 1.0 1.1 PF-A2 1.2 1.1 1.1 1.1 1.1 PF-B1 1.0 1.1 1.0 1.0 1.1 PF-B2 1.0 1.1 1.0 1.0 1.1 PF-C1 1.1 1.2 1.0 1.0 1.1 PF-C2 1.0 1.2 1.0 1.0 1.1 PF-D1 1.0 1.1 2.3 3.1 1.1 PF-D2 1.0 1.1 3.7 2.7 1.3 PF-E1 3.3 10.1 7.1 3.1 1.1 PF-E2 2.6 7.2 6.6 5.6 1.1
[0122] In RF-1 to RF_4, the amount of Si contained in the peeling layer was 0.5 kcps or less under fluorescent X-ray.
[0123] In RF-1 and RF-2, the value of A=B / C becomes small in each of the eight types of PF-A1 to PF-D2, and compression can be suppressed.
[0124] In RF-3 and RF-4, the value of A=B / C becomes small in each of the six types of PF-A1 to PF-C2, and compression can be suppressed.
[0125] In RF-5, the value of A=B / C was small among all 10 types of surface protection films, and compression was suppressed, but a large amount of Si was contained in the release layer.
[0126] In the combination of RF-1 or RF-2 and PF-A1 to PF-D2, the Tg of the surface protective film is below +22°C, and the release layer of the release film contains a component having an amino structure and a component that does not chemically react with the amino structure. In addition, in the combination of RF-1 to RF_4 and PF-A1 to PF-C2, the Tg of the surface protective film is below +11°C, and the release layer of the release film contains an amino structure.
Claims
1. A surface protective film with a release film, wherein: The surface protection film comprises: a first substrate layer composed of a polyethylene terephthalate film; and an adhesive layer formed by cross-linking a (meth)acrylate copolymer. The surface protection film is an optical or electronic surface protection film. The release film comprises a second base material layer and a release layer formed on one side of the second base material layer. The release layer of the release film contains an amino structure, The Si in the release layer of the release film is 0.5 kcps or less under fluorescent X-ray.
2. The surface protection film with a release film according to claim 1, wherein The surface protection film has a Tg of +22° C. or less, and the release layer of the release film contains a component that does not chemically react with the amino structure.
3. The surface protection film with a release film according to claim 1, wherein The surface protection film has a Tg of +11° C. or less.
4. The surface protection film with a release film according to claim 2 or 3, wherein When the instantaneous maximum value of the peeling force when the peeling film is peeled off at a peeling speed of 0.3 m / min and a peeling angle of 180 degrees is set to B, and the average peeling force when the peeling film is peeled off at a peeling speed of 0.3 m / min and a peeling angle of 180 degrees is set to C, the value A obtained by the formula: A=B / C is less than 1.
5.
5. The surface protection film with a release film according to claim 2 or 3, wherein When an average peeling force when the release film is peeled off at a peeling speed of 0.3 m / min and a peeling angle of 180 degrees is defined as C, the C is greater than 0.02 N / 25 mm.
6. The surface protection film with a release film according to claim 2 or 3, wherein The release layer of the release film includes a melamine structure.
7. The surface protection film with a release film according to claim 2 or 3, wherein The release layer contains any one of acrylic acid, polyol, and polyether.