Antibacterial leather fabric and preparation method thereof
Through degreasing, retanning and fatliquoring, combined with agave and chitosan modified nano-hydroxyapatite antibacterial liquid, the problem of easy formation of plaque and mildew in animal leather has been solved, achieving efficient antibacterial effect and Washability extends the service life of leather fabrics.
Patent Information
- Application Number
- CN202411073045.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-08-06
AI Technical Summary
Animal leather is prone to plaque and mildew during use, and existing antibacterial agents are highly irritating to the skin and have poor washability, making them unable to meet high-quality demands.
Using degreasing, retanning and fatliquoring treatment methods, using 1-butyl-3-methylimidazole chloride, 1-butyl-3-methylimidazole hexafluorophosphate, decyl glucoside and animal fur waste to extract liquid for defatting, combined with dragon tongue The antibacterial solution of nano-hydroxyapatite modified with orchid and chitosan was soaked in antibacterial solution, and further retanned by acrylic retanning agent and modified montmorillonite, and finally using sulfite fish oil and polyethylene glycol 400 dioleic acid. The ester is fatliquified.
Significantly improves the antibacterial effect of leather fabrics, extends its service life, improves antibacterial properties and washability, and avoids the risk of skin irritation.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of fabric preparation, and particularly relates to an antibacterial leather fabric and a preparation method thereof. Background Art
[0002] Leather fabric is made by bonding animal leather with base fabric after degreasing and tanning. Animal leather such as cowhide, pigskin, sheepskin, etc. are the raw materials for people to make leather fabrics. They have good strength, durability, and natural patterns of animal leather. They are beautiful, waterproof and breathable, comfortable to use, and have a long service life. They are very popular. Due to the limited resources and high prices of animal leather, there are a large number of synthetic leathers on the market as a substitute for animal leather with low cost. However, synthetic leather has poor strength, is not waterproof, and is not breathable, and cannot meet people's high quality needs.
[0003] Compared with synthetic leather, animal leather has outstanding advantages, but it also has some problems. Antibacterial property is a major bottleneck that limits the application of animal leather. Animal leather contains oil and natural protein. During use, sweat, sebum, and metabolic products secreted by human sweat glands and sebaceous glands also become a nutrient source for microorganisms, leading to the growth and proliferation of microorganisms. Therefore, natural leather has high daily maintenance requirements. Once improperly cared for, bacterial plaques will form and mildew will occur, which will damage animal leather products on the one hand and affect human health on the other.
[0004] At present, people usually achieve antibacterial treatment of animal leather by adding antibacterial agents such as fatty alcohol polyoxyethylene ether, N-phenyl-2-naphthylamine, and cocamidopropyl betaine. However, the antibacterial activity is general and the washing resistance is poor. The antibacterial activity will disappear after loss. In addition, it is irritating to the skin and will also affect human health.
[0005] Patent CN108265136B discloses a leather care agent and its preparation method, which is made by mixing methylparaben, monoglyceride, white oil, stearic acid, lanolin, dimethyl silicone oil, sulfated castor oil, thyme essential oil, nanosilver, deionized water, vitamin A palmitate, triethanolamine borate, coconut oil fatty acid diethanolamide and the like as raw materials. This patented technology improves the antibacterial effect and ensures color fastness through the synergistic effect of vitamin A palmitate, triethanolamine borate and coconut oil fatty acid diethanolamide. Among them, vitamin A palmitate may cause allergic reactions in the human body; triethanolamine borate has certain harmfulness, and short-term contact may cause eye and skin irritation, burns and chemical burns, etc., and long-term contact may cause problems in the nervous system, respiratory system and other aspects. Summary of the invention
[0006] In view of the deficiencies in the prior art, the object of the present invention is to provide an antibacterial leather fabric and a preparation method thereof.
[0007] In order to achieve the above object, the present invention adopts the following technical solution: A method for preparing an antibacterial leather fabric, the specific steps are as follows: S1. First, the animal hide is degreased using a degreasing agent solution to obtain a degreased hide; S2. Wash once, neutralize, wash twice, and obtain a twice washed leather; S3 then completely immerses the secondary washed leather in the antibacterial liquid for immersion treatment to obtain antibacterial treated leather; S4. The antibacterial treated leather is then retanned using a retanning agent to obtain a retanned leather; S5. Finally, the retanned leather is fat-liquored using a fatliquor, dyed, and fixed to obtain the antibacterial leather fabric.
[0008] Preferably, in step S1, the animal hide is selected from any one of cow hide, pig hide and sheep hide.
[0009] Preferably, in step S1, the animal hide is washed and completely immersed in a degreasing agent solution of 12 to 15 times its weight, left to stand for 2 to 3 hours, the pH is adjusted to 2 to 3 using a 20 to 30% by mass formic acid aqueous solution, the drum is rotated for 2 to 3 hours, and the liquid is discharged.
[0010] Preferably, in step S1, the degreasing agent solution is prepared by mixing the following components in parts by weight: 3 to 4 parts of 1-butyl-3-methylimidazolium chloride, 4 to 5 parts of 1-butyl-3-methylimidazolium hexafluorophosphate, 8 to 10 parts of decyl glucoside, and 100 parts of animal fur waste extract.
[0011] Further preferably, the animal fur waste extract is prepared by the following method: first add the animal fur waste to a 1-2 mol / L sodium hydroxide solution, stir and heat at 95-100°C for 6-8 hours, filter and collect the filtrate while hot, naturally cool to 60-65°C, drop lauroyl chloride into the filtrate, control the pH to 9-10 with a 1-2 mol / L sodium hydroxide solution, stir for 3-4 hours after the addition is complete, and obtain the animal fur waste extract; wherein the amount ratio of animal fur waste, sodium hydroxide solution, and lauroyl chloride is 3-4 kg: 2-3 kg: 0.2-0.3 mL.
[0012] Preferably, in step S2, the first water washing is to wash the defatted leather 2 to 3 times with water of 2 to 3 times its mass to obtain the first water-washed leather; the neutralization is to add the first water-washed leather into 2 to 3 times its mass of water, then adjust the pH to 7, stir at 35 to 40° C. for 1 to 2 hours, drain, and obtain the neutralized water-washed leather; the second water washing is to wash the neutralized water-washed leather 2 to 3 times with water of 2 to 3 times its mass to obtain the second water-washed leather.
[0013] Preferably, in step S3, the mass ratio of the secondary washed leather to the antibacterial liquid is 1:5-6; and the process conditions for the immersion treatment are: 300-400W ultrasonic oscillation treatment for 40-50 minutes.
[0014] Preferably, in step S3, the antibacterial solution is prepared by the following method: (A) first drying agave to a moisture content of less than 5wt%, and crushing to 80-100 mesh to obtain agave powder; (B) then stirring and dispersing the agave powder in 20 to 25 times its weight of water, irradiating with microwaves at 600 to 750 W for 10 to 12 minutes, and filtering to obtain the filtrate; (C) Finally, chitosan-modified nano-hydroxyapatite is added to the filtrate, and the filtrate is treated with ultrasonic oscillation at 300-400W for 30-40 minutes to obtain the antibacterial solution.
[0015] More preferably, the mass ratio of agave powder to chitosan-modified nano-hydroxyapatite is 10:5-6.
[0016] Further preferably, the chitosan modified nano hydroxyapatite is prepared by the following method: firstly, hydroxypropyltrimethylammonium chloride chitosan is stirred and dispersed in deionized water to obtain a chitosan aqueous solution, and then nano hydroxyapatite is added to the chitosan aqueous solution, and the chitosan aqueous solution is subjected to ultrasonic oscillation treatment at 200-300W for 50-60 minutes at 5-10°C, and the supernatant is obtained by centrifugation at room temperature, and the unbound material is removed by filtering with a microporous membrane to obtain the chitosan modified nano hydroxyapatite; wherein the dosage ratio of hydroxypropyltrimethylammonium chloride chitosan, nano hydroxyapatite and deionized water is 1 mg: 1-2 mg: 5-6 mL.
[0017] Preferably, in step S4, the specific method of retanning is: soak the antibacterial treated leather in 40-50°C water of 2-3 times its weight for 40-50 minutes, add retanning agent, rotate the drum for 2-3 hours, and drain the liquid; the mass ratio of the antibacterial treated leather to the retanning agent is 1:0.8-1.
[0018] Preferably, in step S4, the retanning agent is obtained by mixing an acrylic retanning agent (RG-BR02, Weifang Jintai Materials Factory) and modified montmorillonite in a mass ratio of 1:0.2-0.3.
[0019] Further preferably, the modified montmorillonite is prepared by the following method: firstly, sodium montmorillonite is stirred and dispersed in water, then L-tyrosine is added, pH is adjusted to 7, stirred and heated to 90°C, kept stirring for 3 hours, naturally cooled to room temperature, centrifuged to obtain a precipitate, washed with water, and dried to obtain the modified montmorillonite; wherein the mass ratio of sodium montmorillonite, water, and L-tyrosine is 4-5:100:6-7.
[0020] Preferably, in step S5, the mass ratio of the retanned leather to the fatliquor is 100:0.3-0.4; the specific method of fatliquor treatment is: soak the retanned leather in 60-65°C water of 2-3 times its weight for 20-30 minutes, add the fatliquor, rotate the drum for 2-3 hours, and drain the liquid.
[0021] Preferably, in step S5, the fatliquor is obtained by mixing sulfited fish oil, neat's foot oil, and polyethylene glycol 400 dioleate in a mass ratio of 1:1:0.3-0.4.
[0022] An antibacterial leather fabric is obtained by the above-mentioned preparation method.
[0023] Compared with the prior art, the present invention has the following beneficial effects: The present invention firstly degreases the animal hide with a degreasing agent solution to obtain degreased hide; washes once, neutralizes, and washes twice to obtain a second-washed hide; then completely immerses the second-washed hide in an antibacterial liquid, performs an immersion treatment, and obtains an antibacterial treated hide; then retans the antibacterial treated hide with a retanning agent to obtain a retanned hide; finally, the retanned hide is fat-liquored with a fatliquor, dyed, and fixed to obtain an antibacterial leather fabric. The leather fabric obtained by the present invention has an excellent antibacterial effect and prolongs the service life of the leather fabric.
[0024] The degreasing agent solution is prepared by mixing 1-butyl-3-methylimidazolium chloride, 1-butyl-3-methylimidazolium hexafluorophosphate, decyl glucoside, animal fur waste extract, etc. 1-butyl-3-methylimidazolium chloride and 1-butyl-3-methylimidazolium hexafluorophosphate in the degreasing agent solution are ionic liquids with excellent solubility in oils and fats; the animal fur waste extract has good compatibility with the protein components in animal hides, and thus synergizes with 1-butyl-3-methylimidazolium chloride, 1-butyl-3-methylimidazolium hexafluorophosphate, decyl glucoside, etc. to improve the degreasing effect, thereby providing a good basis for the full entry of the subsequent antibacterial solution and promoting further improvement of the antibacterial effect.
[0025] The antibacterial liquid is prepared using agave and chitosan-modified nano-hydroxyapatite as raw materials, combining the antibacterial components of agave with the antibacterial properties of chitosan and nano-hydroxyapatite. In addition, nano-hydroxyapatite also has good adsorption properties, further enhancing the overall antibacterial properties.
[0026] The retanning agent is obtained by mixing acrylic retanning agent with modified montmorillonite. The fatliquor is obtained by mixing sulfited fish oil, neat's foot oil and polyethylene glycol 400 dioleate. Through the corresponding retanning and fatliquor treatment, the uniform distribution of antibacterial components in the leather fabric is promoted, and the antibacterial effect is further improved. DETAILED DESCRIPTION
[0027] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] Unless otherwise specified, all commodities in this invention are purchased through market channels.
[0029] For the convenience of comparison, the animal hides in the embodiments and comparative examples are all cow hides from the same source.
[0030] Example 1 A method for preparing an antibacterial leather fabric, the specific steps are as follows: S1. First, the animal hide is degreased using a degreasing agent solution to obtain a degreased hide; S2. Wash once, neutralize, wash twice, and obtain a twice washed leather; S3 then completely immerses the secondary washed leather in the antibacterial liquid for immersion treatment to obtain antibacterial treated leather; S4. The antibacterial treated leather is then retanned using a retanning agent to obtain a retanned leather; S5. Finally, the retanned leather is fat-liquored with a fatliquor, dyed, and fixed to obtain an antibacterial leather fabric.
[0031] In step S1, the animal hide is washed and completely immersed in a degreasing agent solution of 12 times its weight, and allowed to stand for 2 hours. A 20% mass concentration of formic acid aqueous solution is used to adjust the pH to 2, and the drum is rotated for 2 hours to discharge the liquid.
[0032] In step S1, the degreasing agent solution is prepared by mixing the following components: 0.3 kg of 1-butyl-3-methylimidazolium chloride, 0.4 kg of 1-butyl-3-methylimidazolium hexafluorophosphate, 0.8 kg of decyl glucoside, and 10 kg of animal fur waste extract.
[0033] The animal fur waste extract is prepared by the following method: first, 30 kg of animal fur waste is added to 20 kg of 1 mol / L sodium hydroxide solution, heated with stirring at 95°C for 6 hours, the filtrate is filtered while hot, naturally cooled to 60°C, 2 mL of lauroyl chloride is added dropwise to the filtrate, the pH is controlled to 9 with 1 mol / L sodium hydroxide solution, and stirred for 3 hours after the addition is completed to obtain the animal fur waste extract.
[0034] In step S2, the first water washing is to wash the defatted leather twice with water twice as much as its weight to obtain the first water washed leather; the neutralization is to add the first water washed leather into water twice as much as its weight, then adjust the pH to 7, stir at 35°C for 1 hour, drain, and obtain the neutralized water washed leather; the second water washing is to wash the neutralized water washed leather twice with water twice as much as its weight to obtain the second water washed leather.
[0035] In step S3, the mass ratio of the secondary washed leather to the antibacterial liquid is 1:5; and the process conditions for the immersion treatment are: 300W ultrasonic oscillation treatment for 40 minutes.
[0036] In step S3, the antibacterial solution is prepared by the following method: (A) drying agave to a moisture content of less than 5 wt %, and crushing to 80 mesh to obtain agave powder; (B) then stirring and dispersing the agave powder in 20 times its weight of water, irradiating with 600W microwaves for 10 minutes, and filtering to obtain the filtrate; (C) Finally, chitosan-modified nano-hydroxyapatite was added to the filtrate and treated with 300W ultrasonic oscillation for 30 minutes to obtain the antibacterial solution.
[0037] The mass ratio of agave powder to chitosan-modified nano-hydroxyapatite is 10:5.
[0038] Chitosan modified nano hydroxyapatite is prepared by the following method: first, 1 g of hydroxypropyltrimethylammonium chloride chitosan is stirred and dispersed in 5 L of deionized water to obtain a chitosan aqueous solution, then 1 g of nano hydroxyapatite is added to the chitosan aqueous solution, and ultrasonic oscillation is performed at 200 W for 50 minutes at 5°C, and the supernatant is obtained by centrifugation at room temperature, and unbound materials are removed by filtering with a microporous filter membrane.
[0039] In step S4, the specific method of retanning is: soak the antibacterial treated leather in 40°C water twice its weight for 40 minutes, add retanning agent, rotate the drum for 2 hours, and drain the liquid; the mass ratio of the antibacterial treated leather to the retanning agent is 1:0.8.
[0040] In step S4, the retanning agent is obtained by mixing an acrylic retanning agent (RG-BR02, Weifang Jintai Material Factory) and modified montmorillonite in a mass ratio of 1:0.2.
[0041] The modified montmorillonite is prepared by the following method: first, 40g of sodium montmorillonite is stirred and dispersed in 1kg of water, then 60g of L-tyrosine is added, the pH is adjusted to 7, and the mixture is stirred and heated to 90°C, kept stirring for 3 hours, naturally cooled to room temperature, centrifuged to obtain the precipitate, washed with water, and dried to obtain the modified montmorillonite.
[0042] In step S5, the mass ratio of the retanned leather to the fatliquor is 100:0.3; the specific method of fatliquor treatment is: soak the retanned leather in 60°C water twice its weight for 20 minutes, add the fatliquor, rotate the drum for 2 hours, and drain the liquid.
[0043] In step S5, the fatliquor is obtained by mixing sulfited fish oil, neat's foot oil, and polyethylene glycol 400 dioleate in a mass ratio of 1:1:0.3.
[0044] Example 2 A method for preparing an antibacterial leather fabric, the specific steps are as follows: S1. First, the animal hide is degreased using a degreasing agent solution to obtain a degreased hide; S2. Wash once, neutralize, wash twice, and obtain a twice washed leather; S3 then completely immerses the secondary washed leather in the antibacterial liquid for immersion treatment to obtain antibacterial treated leather; S4. The antibacterial treated leather is then retanned using a retanning agent to obtain a retanned leather; S5. Finally, the retanned leather is fat-liquored with a fatliquor, dyed, and fixed to obtain an antibacterial leather fabric.
[0045] In step S1, the animal hide is washed and completely immersed in a degreasing agent solution of 15 times its weight, and allowed to stand for 3 hours. A 30% mass concentration of formic acid aqueous solution is used to adjust the pH to 3, and the drum is rotated for 3 hours to discharge the liquid.
[0046] In step S1, the degreasing agent solution is prepared by mixing the following components: 0.4 kg of 1-butyl-3-methylimidazolium chloride, 0.5 kg of 1-butyl-3-methylimidazolium hexafluorophosphate, 1 kg of decyl glucoside, and 10 kg of animal fur waste extract.
[0047] The animal fur waste extract is prepared by the following method: first, 40 kg of animal fur waste is added to 30 kg of 2 mol / L sodium hydroxide solution, heated with stirring at 100°C for 8 hours, the filtrate is filtered while hot, naturally cooled to 65°C, 3 mL of lauroyl chloride is added dropwise to the filtrate, the pH is controlled to 10 with 2 mol / L sodium hydroxide solution, and stirred for 4 hours after the addition is completed to obtain the animal fur waste extract.
[0048] In step S2, the first water washing is to wash the defatted leather three times with water of three times its mass to obtain the first water washed leather; the neutralization is to add the first water washed leather into water of three times its mass, then adjust the pH to 7, stir at 40°C for 2 hours, drain, and obtain the neutralized water washed leather; the second water washing is to wash the neutralized water washed leather three times with water of three times its mass to obtain the second water washed leather.
[0049] In step S3, the mass ratio of the secondary washed leather to the antibacterial liquid is 1:6; and the process conditions for the immersion treatment are: 400W ultrasonic oscillation treatment for 50 minutes.
[0050] In step S3, the antibacterial solution is prepared by the following method: (A) drying agave to a moisture content of less than 5 wt %, and crushing to 100 mesh to obtain agave powder; (B) then stirring and dispersing the agave powder in 25 times its weight of water, irradiating with 750W microwaves for 12 minutes, and filtering to obtain the filtrate; (C) Finally, chitosan-modified nano-hydroxyapatite was added to the filtrate and treated with 400W ultrasonic oscillation for 40 minutes to obtain the antibacterial solution.
[0051] The mass ratio of agave powder to chitosan-modified nano-hydroxyapatite is 10:6.
[0052] Chitosan modified nano hydroxyapatite is prepared by the following method: first, 1 g of hydroxypropyltrimethylammonium chloride chitosan is stirred and dispersed in 6 L of deionized water to obtain a chitosan aqueous solution, then 2 g of nano hydroxyapatite is added to the chitosan aqueous solution, and the solution is ultrasonically oscillated at 300 W for 60 minutes at 10°C, and the supernatant is obtained by centrifugation at room temperature, and unbound materials are removed by filtering with a microporous membrane.
[0053] In step S4, the specific method of retanning is: soak the antibacterial treated leather in 50°C water of 3 times its weight for 50 minutes, add retanning agent, rotate the drum for 3 hours, and drain the liquid; the mass ratio of the antibacterial treated leather to the retanning agent is 1:1.
[0054] In step S4, the retanning agent is obtained by mixing an acrylic retanning agent (RG-BR02, Weifang Jintai Material Factory) and modified montmorillonite in a mass ratio of 1:0.3.
[0055] The modified montmorillonite is prepared by the following method: first, 50g of sodium montmorillonite is stirred and dispersed in 1kg of water, then 70g of L-tyrosine is added, the pH is adjusted to 7, and the mixture is stirred and heated to 90°C, kept stirring for 3 hours, naturally cooled to room temperature, centrifuged to obtain the precipitate, washed with water, and dried to obtain the modified montmorillonite.
[0056] In step S5, the mass ratio of the retanned leather to the fatliquor is 100:0.4; the specific method of fatliquor treatment is: soak the retanned leather in 65°C water of 3 times its weight for 30 minutes, add the fatliquor, rotate the drum for 3 hours, and drain the liquid.
[0057] In step S5, the fatliquor is obtained by mixing sulfited fish oil, neat's foot oil, and polyethylene glycol 400 dioleate in a mass ratio of 1:1:0.4.
[0058] Example 3 A method for preparing an antibacterial leather fabric, the specific steps are as follows: S1. First, the animal hide is degreased using a degreasing agent solution to obtain a degreased hide; S2. Wash once, neutralize, wash twice, and obtain a twice washed leather; S3 then completely immerses the secondary washed leather in the antibacterial liquid for immersion treatment to obtain antibacterial treated leather; S4. The antibacterial treated leather is then retanned using a retanning agent to obtain a retanned leather; S5. Finally, the retanned leather is fat-liquored with a fatliquor, dyed, and fixed to obtain an antibacterial leather fabric.
[0059] In step S1, the animal hide is washed and completely immersed in a degreasing agent solution of 13 times its weight, and allowed to stand for 2 hours. The pH value is adjusted to 3 using a 25% formic acid aqueous solution, and the drum is rotated for 2 hours to discharge the liquid.
[0060] In step S1, the degreasing agent solution is prepared by mixing the following components: 0.35 kg of 1-butyl-3-methylimidazolium chloride, 0.45 kg of 1-butyl-3-methylimidazolium hexafluorophosphate, 0.9 kg of decyl glucoside, and 10 kg of animal fur waste extract.
[0061] The animal fur waste extract is prepared by the following method: first, 35 kg of animal fur waste is added to 25 kg of 1.5 mol / L sodium hydroxide solution, heated with stirring at 98°C for 7 hours, the filtrate is filtered while hot, naturally cooled to 62°C, 3 mL of lauroyl chloride is added dropwise to the filtrate, and the pH is controlled to 9 with 2 mol / L sodium hydroxide solution. After the addition is completed, the extract is stirred for 3 hours to obtain the animal fur waste extract.
[0062] In step S2, the first water washing is to wash the defatted leather three times with water twice its mass to obtain the first water washed leather; the neutralization is to add the first water washed leather into water twice its mass, then adjust the pH to 7, stir at 38°C for 1.5 hours, drain, and obtain the neutralized water washed leather; the second water washing is to wash the neutralized water washed leather three times with water twice its mass to obtain the second water washed leather.
[0063] In step S3, the mass ratio of the secondary washed leather to the antibacterial liquid is 1:5; and the process conditions for the immersion treatment are: 400W ultrasonic oscillation treatment for 45 minutes.
[0064] In step S3, the antibacterial solution is prepared by the following method: (A) drying agave to a moisture content of less than 5 wt %, and crushing to 90 mesh to obtain agave powder; (B) then stirring and dispersing the agave powder in 22 times its weight of water, irradiating with 700W microwaves for 11 minutes, and filtering to obtain the filtrate; (C) Finally, chitosan-modified nano-hydroxyapatite was added to the filtrate and treated with 400W ultrasonic oscillation for 35 minutes to obtain the antibacterial solution.
[0065] The mass ratio of agave powder to chitosan-modified nano-hydroxyapatite is 10:5.5.
[0066] Chitosan modified nano hydroxyapatite is prepared by the following method: first, 1 g of hydroxypropyltrimethylammonium chloride chitosan is stirred and dispersed in 5.5 L of deionized water to obtain a chitosan aqueous solution, then 1.5 g of nano hydroxyapatite is added to the chitosan aqueous solution, and ultrasonic oscillation is performed at 300 W for 55 minutes at 8°C, and the supernatant is obtained by centrifugation at room temperature, and unbound materials are removed by filtering with a microporous filter membrane.
[0067] In step S4, the specific method of retanning is: soak the antibacterial treated leather in 45°C water of 3 times its weight for 45 minutes, add retanning agent, rotate the drum for 2.5 hours, and drain the liquid; the mass ratio of the antibacterial treated leather to the retanning agent is 1:0.9.
[0068] In step S4, the retanning agent is obtained by mixing an acrylic retanning agent (RG-BR02, Weifang Jintai Material Factory) and modified montmorillonite in a mass ratio of 1:0.25.
[0069] The modified montmorillonite is prepared by the following method: first, 45g of sodium montmorillonite is stirred and dispersed in 1kg of water, then 65g of L-tyrosine is added, the pH is adjusted to 7, and the mixture is stirred and heated to 90°C, kept stirring for 3 hours, cooled naturally to room temperature, centrifuged to obtain the precipitate, washed with water, and dried to obtain the modified montmorillonite.
[0070] In step S5, the mass ratio of the retanned leather to the fatliquor is 100:0.35; the specific method of fatliquor treatment is: soak the retanned leather in 62°C water twice its weight for 20 to 30 minutes, add the fatliquor, rotate the drum for 3 hours, and drain the liquid.
[0071] In step S5, the fatliquor is obtained by mixing sulfited fish oil, neat's foot oil, and polyethylene glycol 400 dioleate in a mass ratio of 1:1:0.35.
[0072] Comparative Example 1 A method for preparing an antibacterial leather fabric, the specific steps are as follows: S1. First, the animal hide is degreased using a degreasing agent solution to obtain a degreased hide; S2. Wash once, neutralize, wash twice, and obtain a twice washed leather; S3 then completely immerses the secondary washed leather in the antibacterial liquid for immersion treatment to obtain antibacterial treated leather; S4. The antibacterial treated leather is then retanned using a retanning agent to obtain a retanned leather; S5. Finally, the retanned leather is fat-liquored with a fatliquor, dyed, and fixed to obtain an antibacterial leather fabric.
[0073] In step S1, the animal hide is washed and completely immersed in a degreasing agent solution of 12 times its weight, and allowed to stand for 2 hours. A 20% mass concentration of formic acid aqueous solution is used to adjust the pH to 2, and the drum is rotated for 2 hours to discharge the liquid.
[0074] In step S1, the degreasing agent solution is prepared by mixing the following components: 0.3 kg of 1-butyl-3-methylimidazolium chloride, 0.4 kg of 1-butyl-3-methylimidazolium hexafluorophosphate, 0.8 kg of decyl glucoside, and 10 kg of animal fur waste extract.
[0075] The animal fur waste extract is prepared by the following method: first, 30 kg of animal fur waste is added to 20 kg of 1 mol / L sodium hydroxide solution, heated with stirring at 95°C for 6 hours, the filtrate is filtered while hot, naturally cooled to 60°C, 2 mL of lauroyl chloride is added dropwise to the filtrate, the pH is controlled to 9 with 1 mol / L sodium hydroxide solution, and stirred for 3 hours after the addition is completed to obtain the animal fur waste extract.
[0076] In step S2, the first water washing is to wash the defatted leather twice with water twice as much as its weight to obtain the first water washed leather; the neutralization is to add the first water washed leather into water twice as much as its weight, then adjust the pH to 7, stir at 35°C for 1 hour, drain, and obtain the neutralized water washed leather; the second water washing is to wash the neutralized water washed leather twice with water twice as much as its weight to obtain the second water washed leather.
[0077] In step S3, the mass ratio of the secondary washed leather to the antibacterial liquid is 1:5; and the process conditions for the immersion treatment are: 300W ultrasonic oscillation treatment for 40 minutes.
[0078] In step S3, the antibacterial solution is prepared by the following method: (A) drying agave to a moisture content of less than 5 wt %, and crushing to 80 mesh to obtain agave powder; (B) The agave powder is then stirred and dispersed in 20 times its weight of water, irradiated with 600W microwaves for 10 minutes, and the filtrate is filtered to obtain the antibacterial solution.
[0079] In step S4, the specific method of retanning is: soak the antibacterial treated leather in 40°C water twice its weight for 40 minutes, add retanning agent, rotate the drum for 2 hours, and drain the liquid; the mass ratio of the antibacterial treated leather to the retanning agent is 1:0.8.
[0080] In step S4, the retanning agent is obtained by mixing an acrylic retanning agent (RG-BR02, Weifang Jintai Material Factory) and modified montmorillonite in a mass ratio of 1:0.2.
[0081] The modified montmorillonite is prepared by the following method: first, 40g of sodium montmorillonite is stirred and dispersed in 1kg of water, then 60g of L-tyrosine is added, the pH is adjusted to 7, and the mixture is stirred and heated to 90°C, kept stirring for 3 hours, naturally cooled to room temperature, centrifuged to obtain the precipitate, washed with water, and dried to obtain the modified montmorillonite.
[0082] In step S5, the mass ratio of the retanned leather to the fatliquor is 100:0.3; the specific method of fatliquor treatment is: soak the retanned leather in 60°C water twice its weight for 20 minutes, add the fatliquor, rotate the drum for 2 hours, and drain the liquid.
[0083] In step S5, the fatliquor is obtained by mixing sulfited fish oil, neat's foot oil, and polyethylene glycol 400 dioleate in a mass ratio of 1:1:0.3.
[0084] Comparative Example 2 A method for preparing an antibacterial leather fabric, the specific steps are as follows: S1. First, the animal hide is degreased using a degreasing agent solution to obtain a degreased hide; S2. Wash once, neutralize, wash twice, and obtain a twice washed leather; S3 then completely immerses the secondary washed leather in the antibacterial liquid for immersion treatment to obtain antibacterial treated leather; S4. The antibacterial treated leather is then retanned using a retanning agent to obtain a retanned leather; S5. Finally, the retanned leather is fat-liquored with a fatliquor, dyed, and fixed to obtain an antibacterial leather fabric.
[0085] In step S1, the animal hide is washed and completely immersed in a degreasing agent solution of 12 times its weight, and allowed to stand for 2 hours. A 20% mass concentration of formic acid aqueous solution is used to adjust the pH to 2, and the drum is rotated for 2 hours to discharge the liquid.
[0086] In step S1, the degreasing agent solution is prepared by mixing the following components: 0.4 kg of 1-butyl-3-methylimidazolium hexafluorophosphate, 0.8 kg of decyl glucoside, and 10 kg of animal fur waste extract.
[0087] The animal fur waste extract is prepared by the following method: first, 30 kg of animal fur waste is added to 20 kg of 1 mol / L sodium hydroxide solution, heated with stirring at 95°C for 6 hours, the filtrate is filtered while hot, naturally cooled to 60°C, 2 mL of lauroyl chloride is added dropwise to the filtrate, the pH is controlled to 9 with 1 mol / L sodium hydroxide solution, and stirred for 3 hours after the addition is completed to obtain the animal fur waste extract.
[0088] In step S2, the first water washing is to wash the defatted leather twice with water twice as much as its weight to obtain the first water washed leather; the neutralization is to add the first water washed leather into water twice as much as its weight, then adjust the pH to 7, stir at 35°C for 1 hour, drain, and obtain the neutralized water washed leather; the second water washing is to wash the neutralized water washed leather twice with water twice as much as its weight to obtain the second water washed leather.
[0089] In step S3, the mass ratio of the secondary washed leather to the antibacterial liquid is 1:5; and the process conditions for the immersion treatment are: 300W ultrasonic oscillation treatment for 40 minutes.
[0090] In step S3, the antibacterial solution is prepared by the following method: (A) drying agave to a moisture content of less than 5 wt %, and crushing to 80 mesh to obtain agave powder; (B) then stirring and dispersing the agave powder in 20 times its weight of water, irradiating with 600W microwaves for 10 minutes, and filtering to obtain the filtrate; (C) Finally, chitosan-modified nano-hydroxyapatite was added to the filtrate and treated with 300W ultrasonic oscillation for 30 minutes to obtain the antibacterial solution.
[0091] The mass ratio of agave powder to chitosan-modified nano-hydroxyapatite is 10:5.
[0092] Chitosan modified nano hydroxyapatite is prepared by the following method: first, 1 g of hydroxypropyltrimethylammonium chloride chitosan is stirred and dispersed in 5 L of deionized water to obtain a chitosan aqueous solution, then 1 g of nano hydroxyapatite is added to the chitosan aqueous solution, and ultrasonic oscillation is performed at 200 W for 50 minutes at 5°C, and the supernatant is obtained by centrifugation at room temperature, and unbound materials are removed by filtering with a microporous filter membrane.
[0093] In step S4, the specific method of retanning is: soak the antibacterial treated leather in 40°C water twice its weight for 40 minutes, add retanning agent, rotate the drum for 2 hours, and drain the liquid; the mass ratio of the antibacterial treated leather to the retanning agent is 1:0.8.
[0094] In step S4, the retanning agent is obtained by mixing an acrylic retanning agent (RG-BR02, Weifang Jintai Material Factory) and modified montmorillonite in a mass ratio of 1:0.2.
[0095] The modified montmorillonite is prepared by the following method: first, 40g of sodium montmorillonite is stirred and dispersed in 1kg of water, then 60g of L-tyrosine is added, the pH is adjusted to 7, and the mixture is stirred and heated to 90°C, kept stirring for 3 hours, naturally cooled to room temperature, centrifuged to obtain the precipitate, washed with water, and dried to obtain the modified montmorillonite.
[0096] In step S5, the mass ratio of the retanned leather to the fatliquor is 100:0.3; the specific method of fatliquor treatment is: soak the retanned leather in 60°C water twice its weight for 20 minutes, add the fatliquor, rotate the drum for 2 hours, and drain the liquid.
[0097] In step S5, the fatliquor is obtained by mixing sulfited fish oil, neat's foot oil, and polyethylene glycol 400 dioleate in a mass ratio of 1:1:0.3.
[0098] Comparative Example 3 A method for preparing an antibacterial leather fabric, the specific steps are as follows: S1. First, the animal hide is degreased using a degreasing agent solution to obtain a degreased hide; S2. Wash once, neutralize, wash twice, and obtain a twice washed leather; S3 then completely immerses the secondary washed leather in the antibacterial liquid for immersion treatment to obtain antibacterial treated leather; S4. The antibacterial treated leather is then retanned using a retanning agent to obtain a retanned leather; S5. Finally, the retanned leather is fat-liquored with a fatliquor, dyed, and fixed to obtain an antibacterial leather fabric.
[0099] In step S1, the animal hide is washed and completely immersed in a degreasing agent solution of 12 times its weight, and allowed to stand for 2 hours. A 20% mass concentration of formic acid aqueous solution is used to adjust the pH to 2, and the drum is rotated for 2 hours to discharge the liquid.
[0100] In step S1, the degreasing agent solution is prepared by mixing the following components: 0.3 kg of 1-butyl-3-methylimidazolium chloride, 0.8 kg of decyl glucoside, and 10 kg of animal fur waste extract.
[0101] The animal fur waste extract is prepared by the following method: first, 30 kg of animal fur waste is added to 20 kg of 1 mol / L sodium hydroxide solution, heated with stirring at 95°C for 6 hours, the filtrate is filtered while hot, naturally cooled to 60°C, 2 mL of lauroyl chloride is added dropwise to the filtrate, the pH is controlled to 9 with 1 mol / L sodium hydroxide solution, and stirred for 3 hours after the addition is completed to obtain the animal fur waste extract.
[0102] In step S2, the first water washing is to wash the defatted leather twice with water twice as much as its weight to obtain the first water washed leather; the neutralization is to add the first water washed leather into water twice as much as its weight, then adjust the pH to 7, stir at 35°C for 1 hour, drain, and obtain the neutralized water washed leather; the second water washing is to wash the neutralized water washed leather twice with water twice as much as its weight to obtain the second water washed leather.
[0103] In step S3, the mass ratio of the secondary washed leather to the antibacterial liquid is 1:5; and the process conditions for the immersion treatment are: 300W ultrasonic oscillation treatment for 40 minutes.
[0104] In step S3, the antibacterial solution is prepared by the following method: (A) drying agave to a moisture content of less than 5 wt %, and crushing to 80 mesh to obtain agave powder; (B) then stirring and dispersing the agave powder in 20 times its weight of water, irradiating with 600W microwaves for 10 minutes, and filtering to obtain the filtrate; (C) Finally, chitosan-modified nano-hydroxyapatite was added to the filtrate and treated with 300W ultrasonic oscillation for 30 minutes to obtain the antibacterial solution.
[0105] The mass ratio of agave powder to chitosan-modified nano-hydroxyapatite is 10:5.
[0106] Chitosan modified nano hydroxyapatite is prepared by the following method: first, 1 g of hydroxypropyltrimethylammonium chloride chitosan is stirred and dispersed in 5 L of deionized water to obtain a chitosan aqueous solution, then 1 g of nano hydroxyapatite is added to the chitosan aqueous solution, and ultrasonic oscillation is performed at 200 W for 50 minutes at 5°C, and the supernatant is obtained by centrifugation at room temperature, and unbound materials are removed by filtering with a microporous filter membrane.
[0107] In step S4, the specific method of retanning is: soak the antibacterial treated leather in 40°C water twice its weight for 40 minutes, add retanning agent, rotate the drum for 2 hours, and drain the liquid; the mass ratio of the antibacterial treated leather to the retanning agent is 1:0.8.
[0108] In step S4, the retanning agent is obtained by mixing an acrylic retanning agent (RG-BR02, Weifang Jintai Material Factory) and modified montmorillonite in a mass ratio of 1:0.2.
[0109] The modified montmorillonite is prepared by the following method: first, 40g of sodium montmorillonite is stirred and dispersed in 1kg of water, then 60g of L-tyrosine is added, the pH is adjusted to 7, and the mixture is stirred and heated to 90°C, kept stirring for 3 hours, naturally cooled to room temperature, centrifuged to obtain the precipitate, washed with water, and dried to obtain the modified montmorillonite.
[0110] In step S5, the mass ratio of the retanned leather to the fatliquor is 100:0.3; the specific method of fatliquor treatment is: soak the retanned leather in 60°C water twice its weight for 20 minutes, add the fatliquor, rotate the drum for 2 hours, and drain the liquid.
[0111] In step S5, the fatliquor is obtained by mixing sulfited fish oil, neat's foot oil, and polyethylene glycol 400 dioleate in a mass ratio of 1:1:0.3.
[0112] Comparative Example 4 A method for preparing an antibacterial leather fabric, the specific steps are as follows: S1. First, the animal hide is degreased using a degreasing agent solution to obtain a degreased hide; S2. Wash once, neutralize, wash twice, and obtain a twice washed leather; S3 then completely immerses the secondary washed leather in the antibacterial liquid for immersion treatment to obtain antibacterial treated leather; S4. The antibacterial treated leather is then retanned using a retanning agent to obtain a retanned leather; S5. Finally, the retanned leather is fat-liquored with a fatliquor, dyed, and fixed to obtain an antibacterial leather fabric.
[0113] In step S1, the animal hide is washed and completely immersed in a degreasing agent solution of 12 times its weight, and allowed to stand for 2 hours. A 20% mass concentration of formic acid aqueous solution is used to adjust the pH to 2, and the drum is rotated for 2 hours to discharge the liquid.
[0114] In step S1, the degreasing agent solution is prepared by mixing the following components: 0.3 kg of 1-butyl-3-methylimidazolium chloride, 0.4 kg of 1-butyl-3-methylimidazolium hexafluorophosphate, and 10 kg of animal fur waste extract.
[0115] The animal fur waste extract is prepared by the following method: first, 30 kg of animal fur waste is added to 20 kg of 1 mol / L sodium hydroxide solution, heated with stirring at 95°C for 6 hours, the filtrate is filtered while hot, naturally cooled to 60°C, 2 mL of lauroyl chloride is added dropwise to the filtrate, the pH is controlled to 9 with 1 mol / L sodium hydroxide solution, and stirred for 3 hours after the addition is completed to obtain the animal fur waste extract.
[0116] In step S2, the first water washing is to wash the defatted leather twice with water twice as much as its weight to obtain the first water washed leather; the neutralization is to add the first water washed leather into water twice as much as its weight, then adjust the pH to 7, stir at 35°C for 1 hour, drain, and obtain the neutralized water washed leather; the second water washing is to wash the neutralized water washed leather twice with water twice as much as its weight to obtain the second water washed leather.
[0117] In step S3, the mass ratio of the secondary washed leather to the antibacterial liquid is 1:5; and the process conditions for the immersion treatment are: 300W ultrasonic oscillation treatment for 40 minutes.
[0118] In step S3, the antibacterial solution is prepared by the following method: (A) drying agave to a moisture content of less than 5 wt %, and crushing to 80 mesh to obtain agave powder; (B) then stirring and dispersing the agave powder in 20 times its weight of water, irradiating with 600W microwaves for 10 minutes, and filtering to obtain the filtrate; (C) Finally, chitosan-modified nano-hydroxyapatite was added to the filtrate and treated with 300W ultrasonic oscillation for 30 minutes to obtain the antibacterial solution.
[0119] The mass ratio of agave powder to chitosan-modified nano-hydroxyapatite is 10:5.
[0120] Chitosan modified nano hydroxyapatite is prepared by the following method: first, 1 g of hydroxypropyltrimethylammonium chloride chitosan is stirred and dispersed in 5 L of deionized water to obtain a chitosan aqueous solution, then 1 g of nano hydroxyapatite is added to the chitosan aqueous solution, and ultrasonic oscillation is performed at 200 W for 50 minutes at 5°C, and the supernatant is obtained by centrifugation at room temperature, and unbound materials are removed by filtering with a microporous filter membrane.
[0121] In step S4, the specific method of retanning is: soak the antibacterial treated leather in 40°C water twice its weight for 40 minutes, add retanning agent, rotate the drum for 2 hours, and drain the liquid; the mass ratio of the antibacterial treated leather to the retanning agent is 1:0.8.
[0122] In step S4, the retanning agent is obtained by mixing an acrylic retanning agent (RG-BR02, Weifang Jintai Material Factory) and modified montmorillonite in a mass ratio of 1:0.2.
[0123] The modified montmorillonite is prepared by the following method: first, 40g of sodium montmorillonite is stirred and dispersed in 1kg of water, then 60g of L-tyrosine is added, the pH is adjusted to 7, and the mixture is stirred and heated to 90°C, kept stirring for 3 hours, naturally cooled to room temperature, centrifuged to obtain the precipitate, washed with water, and dried to obtain the modified montmorillonite.
[0124] In step S5, the mass ratio of the retanned leather to the fatliquor is 100:0.3; the specific method of fatliquor treatment is: soak the retanned leather in 60°C water twice its weight for 20 minutes, add the fatliquor, rotate the drum for 2 hours, and drain the liquid.
[0125] In step S5, the fatliquor is obtained by mixing sulfited fish oil, neat's foot oil, and polyethylene glycol 400 dioleate in a mass ratio of 1:1:0.3.
[0126] Comparative Example 5 A method for preparing an antibacterial leather fabric, the specific steps are as follows: S1. First, the animal hide is degreased using a degreasing agent solution to obtain a degreased hide; S2. Wash once, neutralize, wash twice, and obtain a twice washed leather; S3 then completely immerses the secondary washed leather in the antibacterial liquid for immersion treatment to obtain antibacterial treated leather; S4. The antibacterial treated leather is then retanned using a retanning agent to obtain a retanned leather; S5. Finally, the retanned leather is fat-liquored with a fatliquor, dyed, and fixed to obtain an antibacterial leather fabric.
[0127] In step S1, the animal hide is washed and completely immersed in a degreasing agent solution of 12 times its weight, and allowed to stand for 2 hours. A 20% mass concentration of formic acid aqueous solution is used to adjust the pH to 2, and the drum is rotated for 2 hours to discharge the liquid.
[0128] In step S1, the degreasing agent solution is prepared by mixing the following components: 0.3 kg of 1-butyl-3-methylimidazolium chloride, 0.4 kg of 1-butyl-3-methylimidazolium hexafluorophosphate, 0.8 kg of decyl glucoside, and 10 kg of animal fur waste extract.
[0129] The animal fur waste extract is prepared by the following method: first, 30 kg of animal fur waste is added to 20 kg of 1 mol / L sodium hydroxide solution, heated with stirring at 95°C for 6 hours, the filtrate is filtered while hot, naturally cooled to 60°C, 2 mL of lauroyl chloride is added dropwise to the filtrate, the pH is controlled to 9 with 1 mol / L sodium hydroxide solution, and stirred for 3 hours after the addition is completed to obtain the animal fur waste extract.
[0130] In step S2, the first water washing is to wash the defatted leather twice with water twice as much as its weight to obtain the first water washed leather; the neutralization is to add the first water washed leather into water twice as much as its weight, then adjust the pH to 7, stir at 35°C for 1 hour, drain, and obtain the neutralized water washed leather; the second water washing is to wash the neutralized water washed leather twice with water twice as much as its weight to obtain the second water washed leather.
[0131] In step S3, the mass ratio of the secondary washed leather to the antibacterial liquid is 1:5; and the process conditions for the immersion treatment are: 300W ultrasonic oscillation treatment for 40 minutes.
[0132] In step S3, the antibacterial solution is prepared by the following method: (A) drying agave to a moisture content of less than 5 wt %, and crushing to 80 mesh to obtain agave powder; (B) then stirring and dispersing the agave powder in 20 times its weight of water, irradiating with 600W microwaves for 10 minutes, and filtering to obtain the filtrate; (C) Finally, chitosan-modified nano-hydroxyapatite was added to the filtrate and treated with 300W ultrasonic oscillation for 30 minutes to obtain the antibacterial solution.
[0133] The mass ratio of agave powder to chitosan-modified nano-hydroxyapatite is 10:5.
[0134] Chitosan modified nano hydroxyapatite is prepared by the following method: first, 1 g of hydroxypropyltrimethylammonium chloride chitosan is stirred and dispersed in 5 L of deionized water to obtain a chitosan aqueous solution, then 1 g of nano hydroxyapatite is added to the chitosan aqueous solution, and ultrasonic oscillation is performed at 200 W for 50 minutes at 5°C, and the supernatant is obtained by centrifugation at room temperature, and unbound materials are removed by filtering with a microporous filter membrane.
[0135] In step S4, the specific method of retanning is: soak the antibacterial treated leather in 40°C water twice its weight for 40 minutes, add retanning agent, rotate the drum for 2 hours, and drain the liquid; the mass ratio of the antibacterial treated leather to the retanning agent is 1:0.8.
[0136] In step S4, the retanning agent is obtained by mixing an acrylic retanning agent (RG-BR02, Weifang Jintai Material Factory) and sodium montmorillonite in a mass ratio of 1:0.2.
[0137] In step S5, the mass ratio of the retanned leather to the fatliquor is 100:0.3; the specific method of fatliquor treatment is: soak the retanned leather in 60°C water twice its weight for 20 minutes, add the fatliquor, rotate the drum for 2 hours, and drain the liquid.
[0138] In step S5, the fatliquor is obtained by mixing sulfited fish oil, neat's foot oil, and polyethylene glycol 400 dioleate in a mass ratio of 1:1:0.3.
[0139] The performance tests were conducted on the leather fabrics obtained in Examples 1 to 3 and Comparative Examples 1 to 5, respectively, using GB / T20944.3-2008 "Evaluation of antimicrobial properties of textiles Part 3: Oscillation method" to test the antibacterial properties against Staphylococcus aureus, Escherichia coli and Candida albicans. The results are shown in Table 1.
[0140] Table 1. Comparison of antibacterial activity
[0141] It can be seen from Table 1 that the leather fabrics obtained in Examples 1 to 3 have good antibacterial properties against Staphylococcus aureus, Escherichia coli and Candida albicans.
[0142] The antibacterial liquid of Comparative Example 1 omitted chitosan-modified nano-hydroxyapatite, Comparative Example 2 omitted 1-butyl-3-methylimidazolium chloride, Comparative Example 3 omitted 1-butyl-3-methylimidazolium hexafluorophosphate, Comparative Example 4 omitted decyl glucoside, and Comparative Example 5 did not modify the montmorillonite. The antibacterial activity was significantly deteriorated, and the water washing resistance was also deteriorated, indicating that the antibacterial components of agave and chitosan-modified nano-hydroxyapatite synergistically improved the antibacterial activity, and the chitosan-modified nano-hydroxyapatite loaded the antibacterial components of agave, making it more resistant to water washing, and the degreasing and retanning treatments further improved the water resistance.
[0143] The present invention illustrates the technical concept of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned embodiments, that is, it does not mean that the present invention must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of individual raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing an antibacterial leather fabric, characterized in that: The specific steps are as follows: S1. First, the animal hide is degreased using a degreasing agent solution to obtain a degreased hide; S2. Wash once, neutralize, wash twice, and obtain a twice washed leather; S3 then completely immerses the secondary washed leather in the antibacterial liquid for immersion treatment to obtain antibacterial treated leather; S4. The antibacterial treated leather is then retanned using a retanning agent to obtain a retanned leather; S5. Finally, the retanned leather is fat-liquored using a fatliquor, dyed, and fixed to obtain the antibacterial leather fabric.
2. The preparation method according to claim 1, characterized in that: In step S1, the animal hide is selected from any one of cow hide, pig hide and sheep hide.
3. The preparation method according to claim 1, characterized in that: In step S1, the animal hide is washed and completely immersed in a degreasing agent solution of 12 to 15 times its weight, and allowed to stand for 2 to 3 hours. A 20 to 30% mass concentration of formic acid aqueous solution is used to adjust the pH to 2 to 3, and the drum is rotated for 2 to 3 hours to discharge the liquid.
4. The preparation method according to claim 1, characterized in that: In step S1, the degreasing agent solution is prepared by mixing the following components in parts by weight: 3-4 parts of 1-butyl-3-methylimidazolium chloride, 4-5 parts of 1-butyl-3-methylimidazolium hexafluorophosphate, 8-10 parts of decyl glucoside, and 100 parts of animal fur waste extract.
5. The preparation method according to claim 1, characterized in that: In step S2, the first water washing is to wash the defatted leather 2 to 3 times with water of 2 to 3 times its mass to obtain the first water-washed leather; the neutralization is to add the first water-washed leather into 2 to 3 times its mass of water, then adjust the pH value to 6 to 7 with 1 to 2 mol / L sodium bicarbonate aqueous solution, stir at 35 to 40° C. for 1 to 2 hours, drain and obtain the neutralized water-washed leather; the second water washing is to wash the neutralized water-washed leather 2 to 3 times with water of 2 to 3 times its mass to obtain the second water-washed leather.
6. The preparation method according to claim 1, characterized in that: In step S3, the mass ratio of the secondary washed leather to the antibacterial liquid is 1:5-6; the process conditions of the immersion treatment are: 300-400W ultrasonic oscillation treatment for 40-50 minutes.
7. The preparation method according to claim 1, characterized in that: In step S3, the antibacterial solution is prepared by the following method: (A) first drying agave to a moisture content of less than 5wt%, and crushing to 80-100 mesh to obtain agave powder; (B) then stirring and dispersing the agave powder in 20 to 25 times its weight of water, irradiating with microwaves at 600 to 750 W for 10 to 12 minutes, and filtering to obtain the filtrate; (C) Finally, chitosan-modified nano-hydroxyapatite is added to the filtrate, and the filtrate is treated with ultrasonic oscillation at 300-400W for 30-40 minutes to obtain the antibacterial solution.
8. The preparation method according to claim 1, characterized in that: In step S4, the specific method of retanning is: soak the antibacterial treated leather in 40-50°C water of 2-3 times its weight for 40-50 minutes, add retanning agent, rotate the drum for 2-3 hours, and drain the liquid; the mass ratio of the antibacterial treated leather to the retanning agent is 1:0.8-1.
9. The preparation method according to claim 1, characterized in that: In step S5, the mass ratio of the retanned leather to the fatliquor is 100:0.3-0.4; the specific method of fatliquor treatment is: soak the retanned leather in 60-65°C water of 2-3 times its weight for 20-30 minutes, add the fatliquor, rotate the drum for 2-3 hours, and drain the liquid.
10. An antibacterial leather fabric obtained by the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Manufacturing method for lasting bacterium resisting and inhibiting type leather
CN106222328A
Antibacterial and antiviral agent, antibacterial, mildew-proof and antiviral leather as well as preparation method and application thereof
CN111700080A
Leather degreasing agent based on ionic liquid and preparation method thereof
CN111944935A
Wear-resistant and scratch-resistant leather fabric
CN114015818A
Processing technology and application of washable and waterproof sheep leather
CN116397056A