Technological method for eccentric electric arc furnace return method smelting

By adopting the return method smelting process in the eccentric electric arc furnace smelting process, including deoxidation, oxygen blowing, fluxing and pre-reduction operations, the problems of low steel material recovery rate and oxidation and burning loss of alloy elements are solved, and the recovery rate is improved and the beneficial effects of retention are achieved. Elemental effects.

CN118726697APending Publication Date: 2024-10-01SINOSTEEL XINGTAI MACHINERY & MILL ROLL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410807265.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

During the smelting process of the eccentric electric arc furnace, the steel material recovery rate is low and the alloying elements are oxidized and burned, and the Cr and Mn elements cannot be effectively recovered, resulting in poor economic efficiency.

Method used

The eccentric electric arc furnace return method smelting process is adopted, including the steps: releasing oxidized slag before leaving the furnace, adding deoxidizer for deoxidation, loading carbon scrap steel and high alloy materials, sending electricity for smelting and blowing oxygen for fluxing, and adding slag after sampling and analysis agent and fluorspar, rapidly raise the temperature to decarburize and preserve chromium, and perform pre-reduction operations to recover chromium elements.

Benefits of technology

It improves the recovery rate of steel materials, removes C and part of P, retains Cr and Mn elements, achieves the purpose of decarburization and chromium preservation, and improves the economy of the smelting process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118726697A_ABST
    Figure CN118726697A_ABST
Patent Text Reader

Abstract

The invention discloses an eccentric electric arc furnace return method smelting process method, which belongs to the technical field of casting, and comprises the following steps: discharging most oxidizing slag in an eccentric electric arc furnace before feeding and tapping, remaining a predetermined amount of molten steel in the furnace after tapping, and adding a deoxidizing agent into the furnace for deoxidizing; after deoxidation is completed, loading is conducted, carbon scrap steel is loaded firstly, briquetting scrap steel is selected to increase the filling power of the furnace bottom, and then all the remaining high-alloy return scraps are added; power transmission smelting is carried out after charging is completed, middle-gear power transmission is used, the melting condition of molten steel in the furnace is observed, small-pressure oxygen blowing fluxing is carried out when the molten steel is melted to 80%, lime is added, and lime is supplemented in time according to the slag condition subsequently; after all the materials are melted down, sampling and analyzing, supplementing a slagging agent and fluorite, and then rapidly raising the temperature to perform decarburization and chromium protection operation; after sampling analysis is qualified, a calcium deoxidizing agent and silicon iron are added into the furnace for pre-reduction; differentiation treatment is carried out on main problems of all stages of steel making of the eccentric electric arc furnace, decarburization and chromium protection are achieved, and the steel and iron material recovery rate is increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of casting, in particular to a process for smelting using an eccentric electric arc furnace return method. Background Art

[0002] As the main equipment for molten steel smelting in the special steel industry, electric arc furnaces generally use the oxidation method for smelting. The oxidation method of electric arc furnace smelting adopts a model method of supplying oxygen throughout the smelting process, which has the characteristics of oxygen blowing to assist melting, decarburization and phosphorus reduction. However, during the oxygen blowing process, oxygen reacts with Fe, Si, C, Mn, Cr, V, and P elements in the steel material to produce oxides of different forms that precipitate into the slag and are eventually removed with the slag. Among the above elements, except for C and P, the other elements are beneficial elements for steelmaking. Since most of the silicon, manganese, and chromium elements in the charge will be oxidized and burned during the oxygen blowing process, the recovery rate of steel materials is low.

[0003] Some of the electric arc furnaces currently in use are eccentric electric arc furnaces. The steel outlet is located in the lower part of the furnace shell. The smelting mode is to leave steel and slag in the furnace. Steel and slag cannot be mixed out during the furnace discharge process. The function of this type of electric arc furnace equipment is designed to only undertake the melting period and oxidation period in the molten steel smelting process. It does not have the return oxygen blowing method and cannot recover the alloy elements in the steel material. The actual steel material recovery rate is about 86%-88%, and the economy is poor. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a process method for smelting by the return method of an eccentric electric arc furnace. In view of the problems of low steel material recovery rate and high oxidation and burning loss of alloy elements in the production process of an eccentric electric arc furnace, the return method of an eccentric electric arc furnace is adopted for smelting, and differentiated treatment is performed on the main problems in each stage of steelmaking in an eccentric arc furnace, so as to achieve the purpose of decarburization and chromium preservation and improving the recovery rate of steel materials.

[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is: A process for smelting by an eccentric arc furnace return method comprises the following steps: Step 1, before tapping the eccentric electric arc furnace, most of the oxidized slag in the furnace is released, a predetermined amount of molten steel remains in the furnace after tapping, and a deoxidizer is added into the furnace for deoxidation; Step 2: After deoxidation, loading is performed. First, carbon scrap steel is loaded, and briquette scrap steel is selected to increase the fluffiness of the furnace bottom, and then all the remaining high-alloy return materials are added; Step 3: After the loading is completed, start the power supply for smelting. Use the middle gear to supply power and observe the melting of the molten steel in the furnace. When the molten steel is melted to 80%, blow oxygen at a low pressure to assist melting and add lime. Add lime in time according to the slag condition later. Step 4: After all the materials are melted, samples are taken for analysis, slag-removing agent and fluorite are added, and then the temperature is quickly raised to perform decarburization and chromium preservation operations; The following two situations require sampling and analysis at any time: a. Observe the color change of the smelting smoke on the furnace top and take samples after the smoke turns white; b. Calculate the decarburization rate of each oxygen blowing tube by 0.07% and take samples when the target carbon requirement is reached; Step 5: After the sampling and analysis are qualified, calcium deoxidizer and ferrosilicon are added into the furnace for pre-reduction.

[0006] The technical solution of the present invention is further improved in that: in step 1, most of the oxidized slag in the eccentric arc furnace is released before steel is discharged, and P is less than 0.005% before discharge; after discharge, 7-9 tons of molten steel remain in the furnace, and 300 kg of deoxidizer is added to the furnace for deoxidation in advance.

[0007] A further improvement of the technical solution of the present invention is that the deoxidizer includes silicon-calcium alloy, calcium deoxidizer and carbon ferromanganese; the amount of silicon-calcium alloy added is 150kg, the amount of calcium deoxidizer added is 50kg, and the amount of carbon ferromanganese added is 100kg.

[0008] A further improvement of the technical solution of the present invention is that in step 2, all the furnace materials need to be added at one time, and no charging is performed during the smelting process.

[0009] A further improvement of the technical solution of the present invention is that in step 3, the middle gear is gear 8; the amount of white ash added is 500 kg; the subsequent timely addition of white ash according to the slag condition specifically refers to observing the slag condition in the furnace according to the power supply of the graphite electrode. If the slag cannot cover the arc, it means that the slag is too thin and white ash needs to be added for slag making.

[0010] A further improvement of the technical solution of the present invention is that in step 4, the amount of slagging agent added is 12-18 kg / t, the amount of fluorite added is 10 kg / t, the temperature is quickly raised to 1580°C-1600°C for decarburization and chromium preservation operation, and the oxygen pressure during decarburization is greater than 10 MPa.

[0011] A further improvement of the technical solution of the present invention is that the composition of the slagging agent includes at least 50% sodium fluoride.

[0012] A further improvement of the technical solution of the present invention is that in step 5, 5-7 kg / t of calcium deoxidizer and 100 kg of ferrosilicon are added into the furnace for pre-reduction operation to recover the chromium element in the slag to the greatest extent.

[0013] A further improvement of the technical solution of the present invention is that the components of the calcium deoxidizer at least include: Ca 25%-30%, Al 2%-5%, SiO 2 20%-25%.

[0014] Due to the adoption of the above technical solution, the technical progress achieved by the present invention is: The essence of the return smelting method provided by the present invention is to decarburize and retain chromium. At a certain metallurgical temperature, the affinity of carbon and oxygen is greater than that of other elements, so as to carry out targeted decarburization and retain most of the alloy elements. At the same time, the pre-reduction operation before the furnace is carried out to reduce the chromium oxide and manganese oxide elements in the slag to the molten steel, so as to finally achieve the purpose of removing C and part of P in the smelting process while retaining the Cr and Mn elements. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art are briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those of ordinary skill in the art, other drawings can be obtained based on these drawings without creative work. Figure 1 It is a flow chart of a process method for smelting by an eccentric arc furnace return method provided in an embodiment of the present invention. DETAILED DESCRIPTION

[0016] It should be noted that the terms "including" and "having" and any variations thereof in the specification and claims of the present invention and the above-mentioned drawings are intended to cover non-exclusive inclusions. For example, a process, method, system, product or apparatus comprising a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or apparatus.

[0017] The present invention is further described in detail below with reference to the accompanying drawings and embodiments: There are two biggest difficulties in the eccentric electric arc furnace smelting return method. First, in order to improve the smelting efficiency, the eccentric furnace adopts the operation of leaving steel and slag in the furnace. Simply understood, there is strong oxidizing molten steel in the furnace at any time. If the return method is used for smelting, the remaining strong oxidizing molten steel in the furnace will react chemically with the easily oxidized alloy elements in the later steel material, affecting the yield; second, the eccentric electric arc furnace adopts the furnace bottom tapping technology, which cannot mix the steel slag, and it is impossible to further recover the Cr and Mn elements in the slag, which affects the return method smelting effect. The present invention performs differentiated treatment on the main problems of each stage of steelmaking in the eccentric electric arc furnace to achieve the purpose of decarburization and chromium preservation and improving the recovery rate of steel materials.

[0018] like Figure 1 As shown, a process for smelting by an eccentric arc furnace return method comprises the following steps: Step 1: Pretreatment of oxidized molten steel in the furnace Before tapping the eccentric electric arc furnace, most of the oxidized slag in the furnace is discharged, and P is less than 0.005% before tapping. After tapping, about 8 tons of molten steel (7-9 tons) are left in the furnace. Deoxidizers are added to the furnace for deoxidation in advance. Considering the high Si content in the bonding layer chips, the deoxidizers include silicon-calcium alloy, calcium deoxidizer and carbon ferromanganese; the amount of silicon-calcium alloy added is 150kg, the amount of calcium deoxidizer added is 50kg, and the amount of carbon ferromanganese added is 100kg.

[0019] Among them, the components of the calcium deoxidizer include at least: Ca (calcium) 25%-30%, Al (aluminum) 2%-5%, and SiO2 (silicon dioxide) 20%-25%.

[0020] Step 2: Steel material selection and fabrication requirements After deoxidation is completed, loading operation is carried out. First, carbon scrap steel is loaded, and briquette scrap steel is selected to increase the fluffiness of the furnace bottom. Then all the remaining high-alloy return materials are added. All the furnace materials are added at one time, and no loading is carried out during the smelting process.

[0021] Step 3: Power transmission curve requirements for smelting process After the loading is completed, start the power smelting, use the middle gear (8th gear) to supply power, observe the melting of molten steel in the furnace, blow oxygen at a small pressure to assist melting when it melts to 80%, and add 500kg of lime. Subsequently, add more lime in time according to the slag conditions.

[0022] When adding lime, it is necessary to observe the slag in the furnace according to the power supply of the graphite electrode. If the slag cannot cover the arc, it means that the slag is too thin and lime needs to be added for slag making.

[0023] Step 4: Sampling and analysis After all the materials are melted, samples are taken for analysis, and 12-18 kg / t of slag-removing agent (preferably 15 kg / t) and 10 kg / t of fluorite are added. The temperature is quickly raised to 1580℃-1600℃ for decarburization and chromium preservation. The oxygen pressure during decarburization is >10Mpa.

[0024] The ingredients of the slagging agent include at least: 50% sodium fluoride.

[0025] Sampling and analysis shall be carried out at any time in the following two situations: a. Observe the color change of the smelting smoke on the furnace top, and take samples after the smoke turns white; b. Calculate the decarburization rate of each oxygen blowing tube by 0.07%, and take samples when the target carbon requirement is reached.

[0026] Step 5: Pre-reduction system before leaving the furnace After the sampling and analysis are qualified, 5-7 kg / t (preferably 6 kg / t) of calcium deoxidizer and 100 kg of ferrosilicon are added into the furnace for pre-reduction operation to recover the chromium element in the slag to the greatest extent. Other deoxidizers can be added according to the changes in the composition, and aluminum deoxidizers are prohibited from being added in the later stage. The purpose of removing C and part of P in the smelting process is finally achieved, while retaining Cr and Mn elements.

[0027] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A process for smelting by an eccentric arc furnace return method, characterized in that: The following steps are involved: Step 1, before tapping the eccentric electric arc furnace, most of the oxidized slag in the furnace is released, a predetermined amount of molten steel remains in the furnace after tapping, and a deoxidizer is added into the furnace for deoxidation; Step 2: After deoxidation, loading is performed. First, carbon scrap steel is loaded, and briquette scrap steel is selected to increase the fluffiness of the furnace bottom, and then all the remaining high-alloy return materials are added; Step 3: After the loading is completed, start the power supply for smelting. Use the middle gear to supply power and observe the melting of the molten steel in the furnace. When the molten steel is melted to 80%, blow oxygen at a low pressure to assist melting and add lime. Add lime in time according to the slag condition later. Step 4: After all the materials are melted, samples are taken for analysis, slag-removing agent and fluorite are added, and then the temperature is quickly raised to perform decarburization and chromium preservation operations; The following two situations require sampling and analysis at any time: a. Observe the color change of the smelting smoke on the furnace top and take samples after the smoke turns white; b. Calculate the decarburization rate of each oxygen blowing tube by 0.07% and take samples when the target carbon requirement is reached; Step 5: After the sampling and analysis are qualified, calcium deoxidizer and ferrosilicon are added into the furnace for pre-reduction.

2. The eccentric arc furnace return smelting process according to claim 1, characterized in that: In step 1, most of the oxidized slag in the eccentric electric arc furnace is released before tapping the steel, and P is less than 0.005% before tapping. After tapping the steel, 7-9 tons of molten steel remain in the furnace, and 300 kg of deoxidizer is added into the furnace for deoxidation in advance.

3. The eccentric arc furnace return smelting process according to claim 2 is characterized in that: The deoxidizer includes silicon-calcium alloy, calcium deoxidizer and carbon ferromanganese; the amount of silicon-calcium alloy added is 150kg, the amount of calcium deoxidizer added is 50kg, and the amount of carbon ferromanganese added is 100kg.

4. The eccentric arc furnace return smelting process according to claim 1 is characterized in that: In step 2, all the charges must be added at once, and no charging is performed during the smelting process.

5. The eccentric arc furnace return smelting process according to claim 1, characterized in that: In step 3, the middle gear is gear 8; the amount of white ash added is 500 kg; the subsequent timely addition of white ash according to the slag condition specifically refers to observing the slag condition in the furnace according to the power supply of the graphite electrode. If the slag cannot cover the arc, it means that the slag is too thin and white ash needs to be added for slag making.

6. The eccentric arc furnace return smelting process according to claim 1, characterized in that: In step 4, the amount of slagging agent added is 12-18 kg / t, the amount of fluorite added is 10 kg / t, and the temperature is quickly raised to 1580°C-1600°C for decarburization and chromium preservation operation. During decarburization, the oxygen pressure is greater than 10 MPa.

7. The eccentric arc furnace return smelting process according to claim 6, characterized in that: The slagging agent contains at least 50% sodium fluoride.

8. The eccentric arc furnace return smelting process according to claim 1, characterized in that: In step 5, 5-7 kg / t of calcium deoxidizer and 100 kg of ferrosilicon are added into the furnace for pre-reduction operation to recover the chromium element in the slag to the greatest extent.

9. The eccentric arc furnace return smelting process according to any one of claims 3 or 8, characterized in that: The components of the calcium deoxidizer include at least: Ca 25%-30%, Al 2%-5%, and SiO 2 20%-25%.