Insulator-covered soft magnetic powder, dust core, magnetic element, and electronic device
By covering the surface of soft magnetic particles with an inorganic insulating film and an organic film, the problem of reduced insulation caused by moisture absorption of the insulating film is solved, efficient magnetic properties and mechanical strength are achieved in a humid environment, and the high magnetic permeability of the dust core is ensured. and withstand voltage.
Patent Information
- Application Number
- CN202410352718.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2024-03-26
- Publication Date
- 2024-10-01
AI Technical Summary
The insulating film in existing soft magnetic particles has high hygroscopicity, which reduces the insulation and fluidity between particles and affects the insulation and density of the powder magnetic core.
An inorganic insulating film is used to cover the surface of the soft magnetic particles, and an organic film with hydrophobic functional groups is formed on it to ensure the moisture resistance and fluidity of the insulating film. The moisture content is measured to be above 30 ppm and below 400 ppm by the Karl-Fischer method. , ensuring the stability of the soft magnetic powder covered by the insulator.
It realizes a dust core that maintains insulation and fluidity in a humid environment, improves the magnetic properties and mechanical strength, and ensures the high magnetic permeability and withstand voltage of the dust core.
Smart Images

Figure CN118737607A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an insulator-covered soft magnetic powder, a pressed powder magnetic core, a magnetic element and an electronic device. Background Art
[0002] Patent document 1 discloses a soft magnetic particle consisting of a particle core and an insulating film, wherein the particle core is composed of a soft magnetic metal and the insulating film is formed on the surface of the particle core. In addition, it is disclosed that the particle core has an oxide film formed by oxidizing the soft magnetic metal. In addition, it is disclosed that the insulating film is an inorganic glass coating or a sol-gel reaction product. It should be noted that it is also disclosed that the sol-gel reaction product contains a hydrocarbon group having a straight chain portion with more than 8 carbon atoms.
[0003] Patent Document 1: Japanese Patent Application Publication No. 2022-060995
[0004] In the soft magnetic particles described in patent document 1, the insulating film is made of inorganic materials such as glass or sol-gel reaction products. The insulating film made of inorganic materials has good insulation and high hygroscopicity. Therefore, when storing or transporting soft magnetic particles with insulating films, it may absorb moisture unexpectedly. If the insulating film absorbs moisture, the insulation between particles or the fluidity of the particles decreases. As a result, the insulation and the density of the pressed powder core made of soft magnetic particles decrease.
[0005] Therefore, it is an issue to realize an insulator-coated soft magnetic powder having excellent moisture resistance and in which a decrease in insulation or fluidity due to moisture absorption is suppressed. Summary of the invention
[0006] The insulator-coated soft magnetic powder according to the application example of the present invention has:
[0007] soft magnetic powder; and
[0008] an inorganic insulating film covering the particle surface of the soft magnetic powder and comprising ceramics; and
[0009] an organic film covering a surface of the inorganic insulating film and comprising a compound derived from a coupling agent having a hydrophobic functional group,
[0010] The average thickness of the inorganic insulating film is greater than or equal to 5 nm and less than or equal to 100 nm.
[0011] After being left to stand for 24 hours under an environment of atmospheric pressure, a temperature of 30° C., and a relative humidity of 80%, the moisture content measured by the Karl Fischer method at 250° C. was 30 ppm or more and 400 ppm or less.
[0012] A powder magnetic core according to an application example of the present invention includes the insulator-coated soft magnetic powder according to an application example of the present invention.
[0013] A magnetic element according to an application example of the present invention includes the powder magnetic core according to the application example of the present invention.
[0014] An electronic device according to an application example of the present invention includes the magnetic element according to the application example of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 This is a cross-sectional view schematically showing one particle of the insulator-coated soft magnetic powder according to the embodiment.
[0016] Figure 2 This is a process diagram for explaining a method for producing an insulator-coated soft magnetic powder.
[0017] Figure 3 is a top view schematically showing a torodial type coil component.
[0018] Figure 4 It is a perspective view schematically showing a closed magnetic circuit type coil component.
[0019] Figure 5 It is a perspective view showing a mobile personal computer as an electronic device including a magnetic element according to the embodiment.
[0020] Figure 6 It is a top view showing a smartphone as an electronic device including the magnetic element according to the embodiment.
[0021] Figure 7 It is a perspective view showing a digital still camera as an electronic device including a magnetic element according to the embodiment.
[0022] Description of Reference Numerals
[0023] 1: Insulator covering soft magnetic powder; 2: Soft magnetic particles; 3: Insulator coating; 4: Insulator covering soft magnetic particles; 10: Coil component; 11: Pressed powder core; 12: Wire; 20: Coil component; 21: Pressed powder core; 22: Wire; 32: Inorganic insulating film; 34: Organic film; 100: Display unit; 1000: Magnetic element; 1100: Personal computer; 1102: Keyboard; 1104: Main body; 1106: Display unit; 1200: Smart phone; 1202: Operation button; 1204: Earpiece; 1206: Microphone; 1300: Digital still camera; 1302: Housing; 1304: Light receiving unit; 1306: Shutter button; 1308: Memory; S102: Preparation process; S104: Inorganic insulating film forming process; S106: Organic film forming process. DETAILED DESCRIPTION
[0024] Hereinafter, the insulator-coated soft magnetic powder, the powder magnetic core, the magnetic element, and the electronic device of the present invention will be described in detail based on the preferred embodiments shown in the drawings.
[0025] 1. Insulation covered with soft magnetic powder
[0026] First, the insulator-coated soft magnetic powder according to the embodiment will be described. Figure 1 1 is a cross-sectional view schematically showing one particle of the insulator-coated soft magnetic powder 1 according to the embodiment. In the following description, one particle of the insulator-coated soft magnetic powder 1 is referred to as an "insulator-coated soft magnetic particle 4".
[0027] Figure 1 The insulator-covered soft magnetic particles 4 shown have soft magnetic particles 2 and an insulating coating 3 disposed on the surface of the soft magnetic particles 2. The soft magnetic particles 2 include a soft magnetic material described later. The insulating coating 3 is disposed to cover the surface of the soft magnetic particles 2 and has insulating properties. It should be noted that the covering in this specification refers to a concept including a state of covering a portion of the surface in addition to a state of covering the entire surface of the soft magnetic particles 2. In addition, in the following description, the collection of soft magnetic particles 2 is also referred to as "soft magnetic powder".
[0028] As described later, the insulator-coated soft magnetic particles 4 have excellent moisture resistance and suppress the decrease in insulation and fluidity due to moisture absorption. Therefore, the powder compact formed by compacting the insulator-coated soft magnetic powder 1 has good insulation between the insulator-coated soft magnetic particles 4 even when moisture is absorbed, and high filling properties are obtained, so that the powder compact density becomes high. Thus, a powder core with good withstand voltage and magnetic properties is obtained.
[0029] 1.1. Soft magnetic particles
[0030] The soft magnetic particles 2 are made of soft magnetic materials. As soft magnetic materials, for example, materials with at least one of Fe, Ni and Co as main components, i.e. materials containing more than 50% of these elements by atomic ratio, can be cited. In addition, the soft magnetic material, in addition to containing these elements as main components, can contain at least one selected from the group consisting of Cr, Nb, Cu, Al, Mn, Mo, Si, Sn, B, C, P, Ti and Zr according to the target characteristics. In addition, within the scope of not damaging the effect of the present embodiment, the soft magnetic material can contain inevitable impurities. Inevitable impurities refer to impurities accidentally mixed in during raw materials or manufacturing. All elements except the above-mentioned elements are included in the inevitable impurities, and as an example, O, N, S, Na, Mg, K, etc. can be cited.
[0031] Specific examples of soft magnetic materials include, in addition to Fe-Si alloys such as silicon steel and Fe-Si-Al alloys such as sendust alloy, various alloys such as Fe-Ni alloys, Fe-Co alloys, Fe-Ni-Co alloys, Fe-Si-B alloys, Fe-Si-BC alloys, Fe-Si-B-Cr-C alloys, Fe-Si-Cr alloys, Fe-B alloys, Fe-PC alloys, Fe-Co-Si-B alloys, Fe-Si-B-Nb alloys, Fe-Si-B-Nb-Cu alloys, Fe-Zr-B alloys, Fe-Cr alloys, and Fe-Cr-Al alloys; Ni alloys such as Ni-Si-B alloys and Ni-PB alloys; and Co alloys such as Co-Si-B alloys.
[0032] By using the soft magnetic material of such a composition, the insulator-coated soft magnetic particles 4 having high magnetic properties such as magnetic permeability and magnetic flux density and low coercive force can be obtained.
[0033] In the soft magnetic material, the content of the main component is preferably 50% or more, more preferably 70% or more in terms of atomic ratio. This can particularly improve magnetic properties such as magnetic permeability and magnetic flux density of the insulator-covered soft magnetic particles 4.
[0034] The organization that constitutes the soft magnetic material is not particularly limited, and can be any one of a crystalline organization, an amorphous (amorphous) organization, or a microcrystalline (nanocrystalline) organization. Among them, the soft magnetic material preferably includes an amorphous or microcrystalline state. By including these, the coercive force becomes smaller, which helps to reduce the hysteresis loss of the magnetic element. It should be noted that organizations with different crystallinity can also be mixed in the soft magnetic material.
[0035] As amorphous materials and microcrystalline materials, there can be listed, for example, Fe-Si-B series, Fe-Si-BC series, Fe-Si-B-Cr-C series, Fe-Si-Cr series, Fe-B series, Fe-PC series, Fe-Co-Si-B series, Fe-Si-B-Nb series, Fe-Si-B-Nb-Cu series, Fe-Zr-B series such as Fe-Si-B series; Ni-Si-B series, Ni-PB series such as Ni-Si-B series; Co-Si-B series such as Co-Si-B series, etc.
[0036] The composition of the soft magnetic material is determined by the following analysis method.
[0037] Examples of the analysis method include the iron and steel atomic absorption spectrometry method specified in JIS G1257:2000, the iron and steel ICP emission spectrometry method specified in JIS G1258:2007, the iron and steel spark discharge emission spectrometry method specified in JIS G1253:2002, the iron and steel X-ray fluorescence analysis method specified in JIS G1256:1997, and the weight / titration / absorptiometry method specified in JIS G1211 to G1237.
[0038] Specifically, for example, a solid emission spectrometer manufactured by SPECTRO, in particular, a spark discharge emission spectrometer, model: SPECTROLAB, type: LAVMB08A, or an ICP device CIROS120 manufactured by Rigaku Corporation can be cited.
[0039] In particular, when determining C (carbon) and S (sulfur), the oxygen stream combustion (high frequency induction heating furnace combustion)-infrared absorption method specified in JIS G1211: 2011 may be used. Specifically, a carbon and sulfur analyzer, CS-200, manufactured by LECO Corporation may be used.
[0040] In particular, when determining N (nitrogen) and O (oxygen), the nitrogen quantitative method for iron and steel specified in JIS G1228: 1997 and the oxygen quantitative method general rules for metal materials specified in JIS Z2613: 2006 are used. Specifically, the oxygen and nitrogen analyzer TC-300 / EF-300 manufactured by LECO can be used.
[0041] In the particle size distribution of the soft magnetic powder measured on a volume basis, when the particle size at which the frequency is accumulated to 50% is taken as the average particle size, the average particle size of the soft magnetic powder is preferably greater than 1 μm and less than 20 μm, more preferably greater than 2 μm and less than 15 μm, and further preferably greater than 3 μm and less than 9 μm.
[0042] When the average particle size of the soft magnetic powder is within the above range, the eddy current loss of the magnetic element in the high-frequency region can be sufficiently reduced due to the shortened path of the eddy current within the particles of the soft magnetic particles 2. In addition, when the average particle size of the soft magnetic powder is within the above range, the filling property during powder pressing is improved, so the magnetic properties such as the magnetic permeability and saturation magnetic flux density of the powder compact can be improved.
[0043] It should be noted that when the average particle size of the soft magnetic powder is lower than the lower limit, agglomeration is likely to occur, and it may be difficult to form the insulating coating 3, and the filling property during powder pressing is reduced. On the other hand, when the average particle size of the soft magnetic powder exceeds the upper limit, the path of the eddy current in the particle becomes longer, so the eddy current loss from the eddy current in the particle may increase.
[0044] For example, a laser diffraction particle size distribution measuring device can be used to obtain the particle size distribution of the soft magnetic powder on a volume basis.
[0045] 1.2. Insulation coating
[0046] The insulating coating 3 covers the surface of the soft magnetic particles 2 . Figure 1 The insulating film 3 shown has a two-layer structure, and includes an inorganic insulating film 32 and an organic film 34. The inorganic insulating film 32 covers the surface of the soft magnetic particles 2 and contains ceramics. The organic film 34 covers the surface of the inorganic insulating film 32 and contains a compound derived from a coupling agent having a hydrophobic functional group.
[0047] 1.2.1. Inorganic insulating films
[0048] The inorganic insulating film 32 is made of ceramics, and covers the surface of the soft magnetic particles 2. As constituent components of the ceramics, for example, oxide compounds, non-oxide compounds, and the like are included.
[0049] As oxide compounds, for example, silicon oxide such as SiO2, magnesium oxide such as MgO, calcium oxide such as CaO, aluminum oxide such as Al2O3, titanium oxide such as SiO2, zirconium oxide such as ZrO2, boron oxide such as B2O3, yttrium oxide such as Y2O3, phosphorus oxide such as P2O5, bismuth oxide such as Bi2O3, zinc oxide such as ZnO, tin oxide such as SnO, lead oxide such as PbO, lithium oxide such as Li2O, sodium oxide such as Na2O, potassium oxide such as K2O, strontium oxide such as SrO, barium oxide such as BaO, gadolinium oxide such as GD2O3, lanthanum oxide such as La2O3, ytterbium oxide such as Yb2O3, etc. It should be noted that these composition formulas are examples of the composition ratios of the compounds, and the compounds may be compounds other than the above-mentioned composition ratios.
[0050] Examples of the non-oxide compound include silicon nitride such as Si 3 N 4 , aluminum nitride such as AlN, boron nitride such as BN, titanium nitride such as TiN, and tungsten nitride such as WN.
[0051] Furthermore, the ceramics in this specification are composed of one or a mixture of two or more of these constituent components. In addition, the ceramics in this specification may be crystalline, amorphous (glassy), or a mixture of these.
[0052] Among them, the ceramic preferably contains silicon oxide or aluminum oxide. They have particularly good insulation and chemical stability and are easily available. Therefore, by using ceramics containing these components, an inorganic insulating film 32 with good insulation for a long time is obtained.
[0053] The inorganic insulating film 32 may contain components other than the above components. The content of the above components in the inorganic insulating film 32 is preferably 50% by mass or more, more preferably 70% by mass or more, and further preferably 90% by mass or more. Thus, the inorganic insulating film 32 has particularly good insulating properties.
[0054] The average thickness of the inorganic insulating film 32 is 5 nm or more and 100 nm or less, preferably 10 nm or more and 70 nm or less, and more preferably 15 nm or more and 50 nm or less. If the average thickness of the inorganic insulating film 32 is within the range, the insulation of the inorganic insulating film 32 can be fully ensured, and the occupancy rate of the inorganic insulating film 32 in the pressed powder magnetic core can be reduced to improve the filling rate of the soft magnetic powder. In addition, when there are concavoconvexities on the surface of the soft magnetic particles 2, the inorganic insulating film 32 also helps to make the concavoconvexities flat and smooth while making them close to a sphere. Thus, the organic film 34 can be formed with a more uniform thickness, and the fluidity of the insulating material covering the soft magnetic powder 1 can be further improved.
[0055] When the average thickness of the inorganic insulating film 32 is lower than the lower limit, the insulating property of the inorganic insulating film 32 becomes insufficient, and the surface irregularities of the soft magnetic particles 2 cannot be sufficiently smoothed. On the other hand, when the average thickness of the inorganic insulating film 32 exceeds the upper limit, the inorganic insulating film 32 is easily peeled off, or the filling rate of the soft magnetic powder in the powder core is reduced.
[0056] It should be noted that, for example, the average thickness of the inorganic insulating film 32 is measured by magnifying and observing the cross section of the insulator-covered soft magnetic particle 4. Specifically, the insulator-covered soft magnetic particle 4 is cut by a focused ion beam to prepare a cross-sectional thin-section sample. Next, the cross-sectional thin-section sample is observed with a scanning transmission electron microscope, and the thickness of the inorganic insulating film 32 is measured at five or more positions for one insulator-covered soft magnetic particle 4. And, the measured values are averaged, and the calculated result is used as the average thickness of the inorganic insulating film 32. The distribution range of the inorganic insulating film 32 in the observed image can be more clearly confirmed by using, for example, EDX analysis (energy dispersive X-ray analysis) and Auger electron spectroscopy measurement.
[0057] In addition, the inorganic insulating film 32 may include ceramic particles made of the above-mentioned ceramics. By making the diameter of the ceramic particles smaller than the diameter of the soft magnetic particles 2, the ceramic particles can be distributed in a manner covering the surface of the soft magnetic particles 2. Thus, it is easy to obtain a dense inorganic insulating film 32 with a sufficient film thickness. Such an inorganic insulating film 32 has particularly high insulation properties.
[0058] The average particle size of the ceramic particles is not particularly limited, but is preferably 1 nm or more and 50 nm or less, more preferably 3 nm or more and 30 nm or less, and further preferably 5 nm or more and 10 nm or less. Thus, it is easy to evenly distribute the ceramic particles on the surface of the soft magnetic particles 2. As a result, the thickness of the inorganic insulating film 32 becomes more uniform, which can improve the insulation.
[0059] The particle size of the ceramic particles is the equivalent circle diameter obtained by observing the cross-section thin-section sample with a scanning transmission electron microscope and from the observed image, and the average of the equivalent circle diameters obtained from five or more ceramic particles is taken as the average particle size of the ceramic particles.
[0060] 1.2.2. Organic membrane
[0061] The organic film 34 is formed by reacting a coupling agent having a hydrophobic functional group with the surface of the inorganic insulating film 32. Therefore, the organic film 34 contains a compound derived from the coupling agent having a hydrophobic functional group and exhibits properties derived from the hydrophobic functional group.
[0062] Examples of the hydrophobic functional group include a saturated hydrocarbon group, a group containing a cyclic structure, a fluoroalkyl group, a fluoroaryl group, a nitro group, an acyl group, a cyano group, etc. These groups impart good moisture resistance to the organic film 34 .
[0063] Among them, the hydrophobic functional group is preferably a saturated hydrocarbon group, and more preferably a straight-chain alkyl group having a carbon number of 1 or more and 6 or less. Thus, the organic film 34 is endowed with particularly high moisture resistance. It should be noted that when the number of carbon atoms exceeds the upper limit, it is difficult to form a state in which adjacent long-chain alkyl groups are arranged regularly. In other words, the arrangement of adjacent long-chain alkyl groups may be disordered. In this way, the moisture resistance of the organic film 34 may be reduced.
[0064] In addition, the hydrophobic functional group is preferably a group containing a cyclic structure, a fluoroalkyl group or a fluoroaryl group. They give the organic film 34 particularly high moisture resistance. In addition, the group containing a cyclic structure or the fluoroaryl group having a cyclic structure has high stability and can maintain good moisture resistance even after heating. In addition, the fluoroalkyl group or the fluoroaryl group having a fluorine atom has low surface tension due to the fluorine atom, so it has excellent hydrophobicity, and as a result, it has good moisture resistance even after heating. Therefore, even in a humid environment, an insulating material-covered soft magnetic powder 1 with excellent fluidity and good filling property during powder pressing is obtained.
[0065] The group containing a cyclic structure is a functional group having a cyclic structure. Examples of the group containing a cyclic structure include an aromatic hydrocarbon group, an alicyclic hydrocarbon group, and a cyclic ether group.
[0066] The aromatic hydrocarbon group is a residue after removing a hydrogen atom from an aromatic hydrocarbon group, and the number of carbon atoms is preferably 6 or more and 20 or less. Examples of the aromatic hydrocarbon group include aryl, alkaryl, aminoaryl, halogenated aryl, etc. Examples of the aryl group include phenyl, tolyl, xylyl, naphthyl, indenyl, etc. Examples of the alkaryl group include benzyl, methylbenzyl, phenethyl, methylphenethyl, phenylbenzyl, etc. It should be noted that the aromatic hydrocarbon group may be substituted with a substituent such as an alkyl group having 1 to 3 carbon atoms.
[0067] The alicyclic hydrocarbon group is a residue after hydrogen atoms are removed from an alicyclic hydrocarbon, and the number of carbon atoms is preferably 3 or more and 20 or less. Examples of the alicyclic hydrocarbon group include cycloalkyl and cycloalkylalkyl. Examples of the cycloalkyl group include cyclopropyl, cyclobutyl, cyclopentyl, and cyclohexyl. Examples of the cycloalkylalkyl group include cyclopentylmethyl and cyclohexylmethyl. The alicyclic hydrocarbon group may be substituted with a substituent such as an alkyl group having 1 to 3 carbon atoms.
[0068] Examples of the cyclic ether group include an epoxy group, a 3,4-epoxycyclohexyl group, an oxetanyl group, etc. The cyclic ether group may be substituted with a substituent such as an alkyl group having 1 to 3 carbon atoms.
[0069] The fluoroalkyl group is an alkyl group having 1 to 16 carbon atoms or a cycloalkyl group having 3 to 16 carbon atoms, which is substituted with one or more fluorine atoms. In particular, the fluoroalkyl group is preferably a perfluoroalkane.
[0070] The fluoroaryl group is an aryl group substituted with one or more fluorine atoms and having a carbon number of 6 to 20. In particular, the fluoroaryl group is preferably a perfluoroaryl group.
[0071] The average thickness of the organic film 34 is preferably thinner than the average thickness of the inorganic insulating film 32. Thus, the organic film 34 can be a monomolecular film or a molecular film close to a monomolecular film, and while ensuring the moisture resistance derived from the hydrophobic functional group, the occupancy rate of the organic film 34 in the insulating material-coated soft magnetic powder can be sufficiently reduced. As a result, a powder core with high magnetic properties is obtained.
[0072] The average thickness of the organic film 34 is preferably 1% or more and less than 100% of the average thickness of the inorganic insulating film 32, more preferably 3% or more and less than 50%, and further preferably 5% or more and less than 20%. Thus, it is possible to ensure that the required film thickness of the organic film 34 is maintained, while further reducing the occupancy rate of the organic film 34 in the insulating material-covered soft magnetic powder.
[0073] For example, the average thickness of the organic film 34 can be determined by qualitative and quantitative analysis in the depth direction using X-ray photoelectron spectroscopy and ion sputtering. Specifically, the concentration of the component derived from the coupling agent is studied along the depth direction. And the area where the concentration of the component derived from the coupling agent becomes high is taken as the average thickness of the organic film 34. Specifically, when the concentration changes near the boundary between the organic film 34 and the inorganic insulating film 32, half of the change in concentration, that is, the position corresponding to the midpoint between the concentration on the organic film 34 side and the concentration on the inorganic insulating film 32 side, is regarded as the boundary, and the thickness closer to the surface side than the boundary is taken as the average thickness of the organic film 34.
[0074] According to the insulating coating 3 having the two-layer structure as described above, the following effects are obtained.
[0075] First, the inorganic insulating film 32 has good insulation derived from ceramics. Therefore, even if it is thin, the insulator-covered soft magnetic particles 4 are well insulated from each other. As a result, by pressing the insulator-covered soft magnetic powder 1, a powder core with good withstand voltage is obtained while suppressing the eddy current between the particles. In addition, the inorganic insulating film 32 can smooth the concavoconvexities on the surface of the soft magnetic particles 2 and make them close to a sphere. Thus, the fluidity of the insulator-covered soft magnetic powder 1 can be improved, and a powder core with a high filling rate can be manufactured. In addition, the inorganic insulating film 32 has hydroxyl groups derived from ceramics at a relatively high concentration. Therefore, the coupling agent can be combined at a high density, which helps to increase the density of the hydrophobic functional group.
[0076] On the other hand, the organic film 34 imparts hydrophobicity to the surface by covering the inorganic insulating film 32. As a result, the moisture resistance of the insulator-coated soft magnetic powder 1 can be improved. As a result, an insulator-coated soft magnetic powder 1 whose fluidity is difficult to reduce even when placed in a humid environment is obtained. In addition, by providing an inorganic insulating film 32 on the substrate, a high density of hydrophobic functional groups can be achieved, while the bonding strength of the compound derived from the coupling agent can be improved. As a result, the moisture resistance of the organic film 34 can be fully improved, and an insulator-coated soft magnetic powder 1 whose fluidity is difficult to reduce even when the particles rub against each other is obtained. In addition, when manufacturing a powder core, the closeness between the insulator-coated soft magnetic powder 1 and the binding material (adhesive) is improved. Therefore, a powder core with high mechanical strength is obtained.
[0077] 1.3. Water content
[0078] The moisture content of the insulator-coated soft magnetic powder 1 is preferably 30 ppm or more and 400 ppm or less, more preferably 40 ppm or more and 300 ppm or less, and further preferably 50 ppm or more and 200 ppm or less, by mass ratio. The moisture content of the insulator-coated soft magnetic powder 1 is within the above range, so that the insulator-coated soft magnetic powder 1 becomes a powder that is difficult to absorb moisture and has a difficult fluidity reduction. In addition, the rusting of the soft magnetic particles 2 caused by moisture can be suppressed, and thus the reduction of magnetic properties in the powder core can also be suppressed.
[0079] It should be noted that when the water content is below the lower limit, the hydrophobicity becomes excessive, and the filling property during powder compacting is sometimes reduced. On the other hand, when the water content exceeds the upper limit, the fluidity of the soft magnetic powder 1 covered by the insulator is reduced due to the excessive water content, and the soft magnetic particles 2 are likely to rust.
[0080] The moisture content of the insulator-coated soft magnetic powder 1 is measured as follows.
[0081] First, the insulator-covered soft magnetic powder 1 is left for 24 hours under an environment of atmospheric pressure, temperature of 30°C, and relative humidity of 80%. Next, the insulator-covered soft magnetic powder 1 is heated at 250°C, and the moisture content in this state is measured by the Karl Fischer method. The moisture content by the Karl Fischer method is measured using a moisture measuring device CA-310 manufactured by Nitto Seiko Analytical Science Co., Ltd., for example.
[0082] 2. Method for manufacturing soft magnetic powder covered with insulating material
[0083] Next, a method for producing the insulator-coated soft magnetic powder 1 will be described.
[0084] Figure 2It is a process diagram for explaining the method of manufacturing the insulator-coated soft magnetic powder 1.
[0085] Figure 2 The method for producing the insulator-coated soft magnetic powder shown includes a preparation step S102 , an inorganic insulating film forming step S104 , and an organic film forming step S106 .
[0086] 2.1. Preparation process
[0087] In the preparation step S102, soft magnetic powder is prepared. The soft magnetic powder can be a powder manufactured by any method. As an example of a manufacturing method, for example, in addition to various atomization methods such as water atomization, gas atomization, and rotating water flow atomization, reduction method, carbonyl method, pulverization method, etc. can also be listed. Among them, the atomization method is preferably used. That is to say, the soft magnetic powder is preferably an atomized powder. The atomized powder is small and has high sphericity, and the manufacturing efficiency is also high. In addition, in particular, the water atomized powder or the rotating water flow atomized powder has a thin oxide film on the surface because it is manufactured by contact with molten metal and water. The oxide film can become the base of the insulating coating 3. Therefore, the soft magnetic particles 2 have excellent tightness with the insulating coating 3, and finally the insulating material covering the soft magnetic particles 4 with particularly high insulation between the particles is obtained. In addition, due to the fast cooling rate, soft magnetic powders containing amorphous structures or microcrystalline structures can also be manufactured.
[0088] 2.2. Inorganic insulating film formation process
[0089] In the inorganic insulating film forming step S104 , the inorganic insulating film 32 is formed to cover the surface of the soft magnetic particles 2 .
[0090] The method for forming the inorganic insulating film 32 is not particularly limited, and examples thereof include dry formation methods such as mechanochemical method, plasma polymerization method, ALD (Atomic Layer Deposition) method, CVD (Chemical Vapor Deposition) method, ion plating method, etc.; and wet formation methods such as sol-gel method, electrolytic reduction method, etc.
[0091] Hereinafter, the mechanochemical method and the sol-gel method will be described in order as representatives.
[0092] 2.2.1. Mechanochemical method
[0093] Mechanochemical method is a method of applying mechanical stress to ceramic particles to change the physicochemical properties of ceramic particles. For example, a mechanochemical reaction device with a compression tool and a blade inside and a cylindrical chamber rotating at high speed is used, and when a mechanical interaction (mechanical chemical reaction) is generated between the soft magnetic particles 2 and the ceramic particles, an inorganic insulating film 32 can be formed on the surface of the soft magnetic particles 2. By using such a mechanical coating formation method, even when there are pollutants attached to the surface of the soft magnetic particles 2, or when the tightness is reduced, or when the surface roughness is small, the inorganic insulating film 32 can be well compacted. In addition, since the high temperature state is not experienced during the formation process of the inorganic insulating film 32, the thermal denaturation of the soft magnetic particles 2, such as unexpected crystal coarsening, can be suppressed. Thus, the soft magnetic properties of the soft magnetic particles 2 can be suppressed from being reduced.
[0094] Examples of the mechanochemical reaction apparatus include the "NOBILTA" (registered trademark) pulverizer and the "MECHANO FUSION" (registered trademark) pulverizer manufactured by Hosokawa Micron Co., Ltd. and the "HYBRIDIZER" (registered trademark) pulverizer manufactured by Nara Machinery Co., Ltd.
[0095] 2.2.3. Sol-gel method
[0096] The sol-gel method is a method of producing ceramics by hydrolyzing metal alkoxides. For example, when forming silicon oxide as the inorganic insulating film 32, the hydrolysis reaction of silicon alkoxides can be utilized. The method using silicon alkoxides will be described below.
[0097] First, the soft magnetic particles 2 are dispersed in an alcohol solution containing silicon alkoxide. Examples of the alcohol solution include lower alcohols such as ethanol and methanol. For example, 10 to 50 parts by mass of alcohol may be mixed with 1 part by mass of tetraethoxysilane.
[0098] Next, ammonia water is mixed as a catalyst for promoting the reaction, and hydrolysis is performed. Thus, a dehydration condensation reaction occurs between the hydrolyzates or between the hydrolyzates and silicon alkoxide, and -Si-O-Si- bonds are formed on the particle surface. Thus, an inorganic insulating film 32 composed of silicon oxide is formed.
[0099] 2.3. Organic film formation process
[0100] In the organic film forming step S106 , a coupling agent having a hydrophobic functional group is reacted with the soft magnetic particles 2 . Thus, the coupling agent is attached to the surface of the inorganic insulating film 32 .
[0101] As such operations, for example, the following three operations can be cited.
[0102] The first operation may be an operation of placing both the soft magnetic particles 2 on which the inorganic insulating film 32 is formed and the coupling agent into a chamber and then heating the chamber.
[0103] The second operation may be an operation of placing the soft magnetic particles 2 on which the inorganic insulating film 32 is formed into a chamber and then spraying a coupling agent into the chamber while stirring the soft magnetic particles 2 .
[0104] The third operation includes adding water, a coupling agent, an alkaline solution such as ammonia or sodium hydroxide, and the soft magnetic particles 2 having the inorganic insulating film 32 formed thereon to a primary alcohol such as methanol, ethanol, or isopropanol, stirring, filtering, and then drying.
[0105] Examples of the coupling agent include a silane coupling agent, a titanium coupling agent, and a zirconium coupling agent.
[0106] The following chemical formula is an example of the molecular structure of a silane coupling agent.
[0107]
[0108] In the above formula, X is a functional group, Y is a spacer, and OR is a hydrolyzable group. It should be noted that R is, for example, a methyl group, an ethyl group, or the like.
[0109] Examples of the spacer group include an alkylene group, an arylene group, an aralkylene group, and an alkylene ether group.
[0110] The hydrolyzable group is, for example, an alkoxy group, a halogen atom, a cyano group, an acetoxy group, an isocyanate group, etc., wherein the alkoxy group generates silanol by hydrolysis. The silanol reacts with the hydroxyl group generated on the surface of the inorganic insulating film 32, and the coupling agent is attached to the surface of the inorganic insulating film 32.
[0111] It is sufficient that the coupling agent contains at least one such hydrolyzable group, but preferably two or more, and more preferably three hydrolyzable groups as shown in the above formula. For example, the coupling agent whose hydrolyzable group is an alkoxy group preferably contains a dialkoxy group, and more preferably contains a trialkoxy group. The coupling agent containing a trialkoxy group reacts with the three hydroxyl groups generated on the surface of the inorganic insulating film 32. Therefore, it has good tightness to the inorganic insulating film 32. In addition, the coupling agent containing a trialkoxy group also has excellent film-forming properties, so an organic film 34 with excellent continuity can be obtained. Such an organic film 34 helps to further improve the fluidity of the insulating material covering the soft magnetic powder 1.
[0112] In addition, in the coupling agent containing a trialkoxy group, even if the hydrophobic functional group is thermally decomposed after the organic film 34 is formed, the remaining part can continue to cover the surface of the inorganic insulating film 32. Therefore, it is possible to suppress a decrease in hydrophobicity.
[0113] Here, coupling agents having a hydrophobic functional group are exemplified. As coupling agents having an aromatic hydrocarbon group, for example, the following can be cited:
[0114] Phenyltrimethoxysilane represented by the following formula (A-1),
[0115]
[0116] Phenyltriethoxysilane represented by the following formula (A-2),
[0117]
[0118] Dimethoxydiphenylsilane represented by the following formula (A-3),
[0119]
[0120] 2,2-dimethoxy-1-phenyl-1-aza-2-silacyclopentane represented by the following formula (A-4),
[0121]
[0122] 3-phenoxypropyltrichlorosilane represented by the following formula (A-11),
[0123]
[0124] Phenyltriacetoxysilane represented by the following formula (A-12),
[0125]
[0126] triethoxy(p-tolyl)silane represented by the following formula (A-13),
[0127]
[0128] p-Aminophenyltrimethoxysilane represented by the following formula (A-14),
[0129]
[0130] m-Aminophenyltrimethoxysilane represented by the following formula (A-15),
[0131]
[0132] ((Chloromethyl)phenylethyl)trimethoxysilane represented by the following formula (A-16).
[0133]
[0134] Examples of the coupling agent having a cyclic ether group include:
[0135] 3-glycidoxypropylmethyldimethoxysilane represented by the following formula (A-5),
[0136]
[0137] 3-glycidoxypropyltrimethoxysilane represented by the following formula (A-6),
[0138]
[0139] 3-glycidoxypropylmethyldiethoxysilane represented by the following formula (A-7),
[0140]
[0141] 3-Glycidoxypropyltriethoxysilane represented by the following formula (A-8).
[0142]
[0143] Examples of the coupling agent having a fluoroalkyl group include:
[0144] trimethoxy(3,3,3-trifluoropropyl)silane represented by the following formula (B-1),
[0145]
[0146] trimethoxy(1H,1H,2H,2H-tridecafluoro-n-octyl)silane represented by the following formula (B-2),
[0147]
[0148] Trimethoxy(1H,1H,2H,2H-nonafluorohexyl)silane represented by the following formula (B-3).
[0149]
[0150] Examples of the coupling agent having a fluoroaryl group include:
[0151] trimethoxy(11-pentafluorophenoxyundecyl)silane represented by the following formula (C-1),
[0152]
[0153] Pentafluorophenyldimethylchlorosilane represented by the following formula (C-2).
[0154]
[0155] The amount of the coupling agent added is not particularly limited, but is preferably 0.01% by mass or more and 1.00% by mass or less, and more preferably 0.05% by mass or more and 0.50% by mass or less, based on the soft magnetic particles 2 .
[0156] Alternatively, the coupling agent may be supplied by leaving the mixture still in the chamber or by spraying the mixture into the chamber.
[0157] Then, the soft magnetic particles 2 to which the coupling agent is attached are heated. Thus, the organic film 34 is formed on the surface of the inorganic insulating film 32, and the insulating material-coated soft magnetic powder 1 is obtained. In addition, the unreacted coupling agent can be removed by heating.
[0158] The heating temperature of the soft magnetic particles 2 to which the coupling agent is attached is not particularly limited, but is preferably 50° C. or more and 300° C. or less, more preferably 100° C. or more and 250° C. or less. The heating time is preferably 10 minutes or more and 24 hours or less, more preferably 30 minutes or more and 10 hours or less. As the atmosphere for the heat treatment, for example, an air atmosphere, an inert gas atmosphere, etc. can be cited.
[0159] 3.Powder cores and magnetic components
[0160] Next, the powder magnetic core and the magnetic element according to the embodiment will be described.
[0161] The magnetic element according to the embodiment can be applied to various magnetic elements having a magnetic core, such as a choke coil, an inductor, a noise filter, a reactor, a transformer, a motor, an actuator, a solenoid valve, a generator, etc. In addition, the powder magnetic core according to the embodiment can be applied to the magnetic core of these magnetic elements.
[0162] Hereinafter, two types of coil components will be described as examples of magnetic elements.
[0163] 3.1. Ring type
[0164] First, a toroidal type coil component as an example of the magnetic element according to the embodiment will be described.
[0165] Figure 3 is a top view schematically showing a ring-type coil component.
[0166] Figure 3 The coil component 10 shown has a ring-shaped powder magnetic core 11 and a conductive wire 12 wound around the powder magnetic core 11. Such a coil component 10 is generally called a toroidal coil.
[0167] The insulator-coated soft magnetic powder and the binding material according to the embodiment are mixed, the obtained mixture is supplied to a molding die, and simultaneously pressed and molded to obtain a powder core 11. Since the powder core 11 is a powder body including the insulator-coated soft magnetic powder according to the embodiment, a coil component 10 having high magnetic permeability and high withstand voltage can be realized. Therefore, when the coil component 10 is mounted on an electronic device, etc., the electronic device, etc., can achieve high performance and miniaturization.
[0168] As the constituent materials of the binder material for making the powder magnetic core 11, organic materials such as silicone resin, epoxy resin, phenolic resin, polyamide resin, polyimide resin, polyphenylene sulfide resin, etc.; inorganic materials such as phosphates such as magnesium phosphate, calcium phosphate, zinc phosphate, manganese phosphate, cadmium phosphate, silicates such as sodium silicate, etc. can be listed, but thermosetting polyimide or epoxy resin is particularly preferred. These resin materials are materials that are easily cured by heating and have excellent heat resistance. Therefore, the manufacturing ease and heat resistance of the powder magnetic core 11 can be improved.
[0169] The ratio of the bonding material to the insulator-covered soft magnetic powder slightly varies depending on the target magnetic properties and mechanical properties of the powder core 11 to be manufactured, the allowable eddy current loss, etc., but is preferably 0.3% by mass or more and 5.0% by mass or less, more preferably 0.5% by mass or more and 3.0% by mass or less, and further preferably 0.7% by mass or more and 2.0% by mass or less. Thus, the insulator-covered soft magnetic powder particles are fully bonded to each other, and the coil component 10 having excellent magnetic properties can be obtained.
[0170] Various additives may be added to the mixture for any purpose as needed.
[0171] The conductive wire 12 may be made of a material having high conductivity, such as a metal material including Cu, Al, Ag, Au, Ni, etc. In addition, an insulating film may be provided on the surface of the conductive wire 12 as necessary.
[0172] The shape of the powder magnetic core 11 is not limited to Figure 3 The ring shape shown may be, for example, a shape in which a part of the ring is missing, a shape in which the long side direction is a straight line, a sheet shape, a film shape, or the like.
[0173] If necessary, the powder core 11 may further include soft magnetic powder or non-magnetic powder other than the insulator-coated soft magnetic powder according to the above-mentioned embodiment.
[0174] 3.2. Closed magnetic circuit type
[0175] Next, a closed magnetic circuit type coil component will be described as an example of the magnetic element according to the embodiment.
[0176] Figure 4 It is a perspective view schematically showing a closed magnetic circuit type coil component.
[0177] Hereinafter, a closed magnetic circuit type coil component will be described. However, the following description will focus on the differences from the ring type coil component, and descriptions of the same matters will be omitted.
[0178] like Figure 4 As shown, the coil component 20 involved in this embodiment is formed by burying the conductive wire 22 formed into a coil shape inside the powder core 21. That is, the coil component 20 as a magnetic element has a powder core 21 including the above-mentioned insulator-covered soft magnetic powder, and the conductive wire 22 is molded by the powder core 21. The powder core 21 has the same structure as the above-mentioned powder core 11. As a result, the coil component 20 with high magnetic permeability and high withstand voltage can be realized.
[0179] In addition, with this type of coil component 20, it is relatively easy to reduce the size of the device. Therefore, when the coil component 20 is mounted on an electronic device or the like, the electronic device or the like can achieve higher performance and smaller size.
[0180] Furthermore, since the lead wire 22 is buried inside the powder core 21, a gap is unlikely to be generated between the lead wire 22 and the powder core 21. Therefore, vibration caused by magnetostriction of the powder core 21 can be suppressed, and noise associated with the vibration can also be suppressed.
[0181] It should be noted that the shape of the powder core 21 is not limited to Figure 4 The shape shown can also be a sheet, a film, etc.
[0182] Furthermore, the powder core 21 may contain soft magnetic powder or non-magnetic powder other than the insulator-coated soft magnetic powder according to the above-mentioned embodiment, as necessary.
[0183] 4. Electronic devices
[0184] Next, based on Figure 5 to Figure 7 An electronic device including the magnetic element according to the embodiment will be described.
[0185] Figure 5 It is a perspective view showing a mobile personal computer as an electronic device including a magnetic element according to the embodiment. Figure 5The personal computer 1100 shown in the figure includes a main body 1104 including a keyboard 1102 and a display unit 1106 including a display unit 100. The display unit 1106 is rotatably supported by the main body 1104 via a hinge structure. Such a personal computer 1100 has a built-in magnetic element 1000, such as a choke coil, an inductor, a motor, etc. used for a switching power supply.
[0186] Figure 6 It is a top view showing a smartphone as an electronic device including the magnetic element according to the embodiment. Figure 6 The smartphone 1200 shown includes a plurality of operation buttons 1202, an earpiece 1204, and a microphone 1206. The display unit 100 is disposed between the operation buttons 1202 and the earpiece 1204. Such a smartphone 1200 has a built-in magnetic element 1000 such as an inductor, a noise filter, a motor, and the like.
[0187] Figure 7 13 is a perspective view showing a digital still camera as an electronic device including a magnetic element according to an embodiment. The digital still camera 1300 generates an imaging signal by photoelectrically converting an optical image of a subject using an imaging element such as a CCD (Charge Coupled Device).
[0188] Figure 7 The digital still camera 1300 shown in the figure has a display unit 100 provided on the back side of a housing 1302. The display unit 100 functions as a viewfinder for displaying an electronic image of a subject. In addition, a light receiving unit 1304 including an optical lens or a CCD is provided on the front side of the housing 1302, that is, the back side in the figure.
[0189] When the photographer checks the subject image displayed on the display unit 100 and presses the shutter button 1306, the CCD shooting signal at that moment is transmitted and stored in the memory 1308. Such a digital still camera 1300 also has a built-in magnetic element 1000 such as an inductor, a noise filter, etc.
[0190] As an electronic device according to an embodiment of the present invention, in addition to Figure 5 Personal computers, Figure 6 Smartphones, Figure 7In addition to digital still cameras, examples include mobile phones, tablet terminals, watches, inkjet ejection devices (inkjet printers), laptop personal computers, televisions, cameras, video recorders, car navigation devices, pagers, electronic notepads, electronic dictionaries, calculators, electronic game equipment, word processors, workstations, videophones, crime prevention TV monitors, electronic binoculars, POS terminals, medical equipment (such as electronic thermometers, blood pressure monitors, blood glucose meters, electrocardiogram measuring devices, ultrasonic diagnostic equipment, electronic endoscopes), fish finders, various measuring equipment, measuring instruments (such as measuring instruments for vehicles, aircraft, and ships), mobile body control equipment (such as automobile control equipment, aircraft control equipment, railway vehicle control equipment, ship control equipment), flight simulators, etc.
[0191] As described above, such an electronic device includes the magnetic element according to the embodiment. Thus, the effect of the magnetic element according to the embodiment having high magnetic permeability and high withstand voltage can be enjoyed, and the performance and miniaturization of the electronic device can be improved.
[0192] 5. Effects of the Implementation Methods
[0193] As described above, the insulator-coated soft magnetic powder 1 involved in this embodiment has soft magnetic powder, an inorganic insulating film 32 and an organic film 34. The inorganic insulating film 32 covers the particle surface of the soft magnetic powder (the surface of the soft magnetic particle 2) and contains ceramics. The organic film 34 covers the surface of the inorganic insulating film 32 and contains a compound derived from a coupling agent having a hydrophobic functional group. In addition, in the insulator-coated soft magnetic powder 1, the average thickness of the inorganic insulating film 32 is greater than 5nm and less than 100nm. In addition, after the insulator-coated soft magnetic powder 1 is placed for 24 hours under an environment of atmospheric pressure, an air temperature of 30°C, and a relative humidity of 80%, the moisture content measured by the Karl Fischer method at 250°C is greater than 30ppm and less than 400ppm.
[0194] According to such a configuration, an insulator-coated soft magnetic powder 1 having excellent moisture resistance and suppressing the decrease in insulation or fluidity due to moisture absorption is obtained. Thus, a powder magnetic core having suppressed eddy current between particles and good withstand voltage is obtained. In addition, the filling rate of the powder magnetic core can be increased, and a powder magnetic core having high magnetic permeability and mechanical strength can be obtained. In addition, the mechanical strength of the powder magnetic core can be further improved by the compactness of the organic film 34 and the high density of the hydrophobic functional group.
[0195] In addition, the ceramic preferably contains silicon oxide or aluminum oxide.
[0196] These have particularly good insulating properties and chemical stability and are easily available. Therefore, by using ceramics containing these components, an inorganic insulating film 32 having excellent insulating properties for a long period of time can be obtained.
[0197] In addition, the inorganic insulating film 32 may include ceramic particles which have a smaller diameter than the soft magnetic particles 2 (particles of soft magnetic powder) and are made of ceramic.
[0198] This allows the inorganic insulating film 32 to be distributed so as to cover the surface of the soft magnetic particles 2. As a result, a dense inorganic insulating film 32 having a sufficient film thickness can be easily obtained. Such an inorganic insulating film 32 has particularly high insulating properties.
[0199] In addition, the average thickness of the organic film 34 is preferably thinner than the average thickness of the inorganic insulating film 32 .
[0200] Thus, by making the organic film 34 a monomolecular film or a molecular film close to a monomolecular film, the occupancy rate of the organic film 34 in the insulator-coated soft magnetic powder can be sufficiently reduced while ensuring moisture resistance derived from the hydrophobic functional group. As a result, a powder core with high magnetic properties can be obtained.
[0201] In addition, the hydrophobic functional group may be a linear alkyl group having 1 to 6 carbon atoms.
[0202] This can provide the organic film 34 with particularly high moisture resistance.
[0203] In addition, the hydrophobic functional group may be a group containing a cyclic structure, a fluoroalkyl group, or a fluoroaryl group.
[0204] Thus, the organic film 34 can be endowed with particularly high moisture resistance. In addition, the group containing a ring structure or the fluorinated aryl group having a ring structure can maintain good moisture resistance even after heating due to its high stability. In addition, the fluorinated alkyl group or the fluorinated aryl group having a fluorine atom has low surface tension due to the fluorine atom, and thus has excellent hydrophobicity, and as a result, has good moisture resistance even after heating. Therefore, even in a humid environment, an insulating material-coated soft magnetic powder 1 having excellent fluidity and good filling properties during powder pressing is obtained.
[0205] In addition, the powder magnetic core according to the embodiment includes the insulator-coated soft magnetic powder according to the embodiment, thereby obtaining a powder magnetic core having a high withstand voltage and high mechanical strength and relative density.
[0206] Furthermore, the magnetic element according to the embodiment includes the powder magnetic core according to the embodiment. Thus, a magnetic element having high withstand voltage and high magnetic permeability is obtained.
[0207] Furthermore, the electronic device according to the embodiment includes the magnetic element according to the embodiment. Thus, an electronic device with improved performance and reduced size is obtained.
[0208] As mentioned above, the insulator-coated soft magnetic powder, the powder magnetic core, the magnetic element, and the electronic device of the present invention have been described based on the preferred embodiments, but the present invention is not limited thereto.
[0209] For example, in the above-mentioned embodiment, a powder core is cited as an application example of the insulator-covered soft magnetic powder of the present invention, but the application example is not limited thereto, and may be a magnetic device, such as a magnetic fluid, a magnetic head, a magnetic shielding sheet, etc. In addition, the shape of the powder core or magnetic element may be any shape, and is not limited to the shape shown in the figure.
[0210] The powder magnetic core and the magnetic element according to the present invention may be the powder magnetic core and the magnetic element in the above-described embodiment to which any arbitrary components are added.
[0211] Example
[0212] Next, specific examples of the present invention will be described.
[0213] 6. Preparation of soft magnetic powder covered with insulation
[0214] 6.1. Sample No.1
[0215] First, a soft magnetic powder composed of the soft magnetic material shown in Table 1 was prepared. The composition of the soft magnetic material and the method for producing the soft magnetic powder are shown in Table 1. It should be noted that the composition formula shown in Table 1 represents the ratio of each element in terms of atomic ratio. In addition, the average particle size of the soft magnetic powder is shown in Table 2.
[0216] Next, an inorganic insulating film was formed on the surface of the soft magnetic powder particles. The constituent materials of the inorganic insulating film, the average thickness, and the average particle size of the ceramic particles used are shown in Table 2. A mechanochemical reaction device was used to form the inorganic insulating film.
[0217] Next, an organic film was formed on the surface of the inorganic insulating film. Table 2 shows the ratio of the hydrophobic functional group of the coupling agent used in forming the organic film, the number of carbon atoms when the hydrophobic functional group is an alkyl group, and the average thickness.
[0218] Insulator-coated soft magnetic powder of Sample No. 1 was obtained as described above. Then, the moisture content of the obtained insulator-coated soft magnetic powder was measured. The measurement results are shown in Table 2.
[0219] 6.2. Sample No. 2 to 40
[0220] Insulator-coated soft magnetic powders of Samples Nos. 2 to 40 were obtained in the same manner as Sample No. 1 except that the composition of the insulator-coated soft magnetic powder was changed as shown in Tables 1 to 3.
[0221]
Table 1
[0222] Soft magnetic materials Composition Manufacturing method Crystalline Materials 1 <![CDATA[Fe 88.6 Yes 6.7 Cr 4.7 ]]> Water atomization method Crystalline Materials 2 <![CDATA[Fe 84.7 Yeah 9.4 To the 5.9 ]]> Water atomization method Amorphous materials1 <![CDATA[(Fe 0.97 Cr 0.03 ) 76 (Yes 0.5 B 0.5 ) 22 C2]]> Water atomization method Amorphous Materials2 <![CDATA[(Fe 0.97 Cr 0.03 ) 76 (Yes 0.5 B 0.5 ) 22 C2]]> Rotating water atomization method
[0223] In Tables 2 and 3 shown later, among the insulator-coated soft magnetic powders of each sample No., those corresponding to the present invention are referred to as “Examples”, and those not corresponding to the present invention are referred to as “Comparative Examples”.
[0224] In addition, the symbols of the chemical formulas shown in Tables 2 and 3 correspond to the following compounds.
[0225] A-1: Phenyltrimethoxysilane
[0226] B-1: Trimethoxy (3,3,3-trifluoropropyl) silane
[0227] C-1: Trimethoxy(11-pentafluorophenoxyundecyl)silane
[0228] D-1: Methyltrimethoxysilane
[0229] D-2: Ethyltrimethoxysilane
[0230] D-3: Propyltrimethoxysilane
[0231] D-4: Hexyltrimethoxysilane
[0232] D-5: Octyltrimethoxysilane
[0233] 7. Evaluation of soft magnetic powder covered with insulation
[0234] 7.1. DC insulation withstand voltage (withstand voltage)
[0235] First, an exposure test was conducted in which each insulator was covered with soft magnetic powder and left for 24 hours in a high humidity environment at atmospheric pressure, a temperature of 30°C, and a relative humidity of 80%.
[0236] Next, each insulating material subjected to the exposure test was coated with soft magnetic powder, and the DC dielectric withstand voltage was measured at room temperature of 25° C. and relative humidity of 45% by the following method.
[0237] First, 0.15 g of the insulator-coated soft magnetic powder was filled into an alumina cylinder with an inner diameter of 8 mm, and brass electrodes were placed at both ends of the cylinder. Then, a digital force gauge was used to apply a force of 20 kgf to the insulator-coated soft magnetic powder using the electrodes at both ends of the cylinder, and a DC voltage of 50 V was applied between the electrodes for two seconds, and the resistance between the electrodes was measured using a digital multimeter.
[0238] Next, the DC voltage applied between the electrodes was boosted by 50V each time while the resistance value between the electrodes was measured to confirm whether there was insulation breakdown. Furthermore, the boost and resistance value were measured repeatedly until insulation breakdown occurred. Furthermore, the lowest DC voltage value when insulation breakdown occurred was obtained. It should be noted that the state where the resistance value is less than 1MΩ is regarded as insulation breakdown. The measurement was performed more than three times, and the average value of the measured values was used as the DC insulation withstand voltage. Furthermore, the DC insulation withstand voltage (withstand voltage) obtained was evaluated according to the following evaluation criteria. The evaluation results are shown in Tables 2 and 3.
[0239] A: Withstand voltage is 400V or more
[0240] B: Withstand voltage is 350V or more and less than 400V
[0241] C: Withstand voltage is 300V or more and less than 350V
[0242] D: Withstand voltage is 250V or more and less than 300V
[0243] E: Withstand voltage is 200V or more and less than 250V
[0244] F: Withstand voltage less than 200V
[0245] 7.2. Radial compressive strength of molded body
[0246] First, an exposure test was conducted in which each insulator was covered with soft magnetic powder and left for 24 hours in a high humidity environment at atmospheric pressure, a temperature of 30°C, and a relative humidity of 80%.
[0247] Next, each insulator-coated soft magnetic powder subjected to the exposure test was mixed with epoxy resin as a binder and toluene as an organic solvent to obtain a mixture. The amount of epoxy resin added was set to 2 parts by mass per 100 parts by mass of the insulator-coated soft magnetic powder.
[0248] Next, the obtained mixture was stirred and immediately dried at 50° C. for 1 hour in an air atmosphere to obtain a block-like dried product. Next, the dried product was sieved with a mesh size of 400 μm and pulverized to obtain a granulated powder.
[0249] Next, the obtained granulated powder was filled into a molding die to obtain a green compact under the following molding conditions.
[0250] Molding method: pressing
[0251] Shape of the molded body: Ring
[0252] · Molded body dimensions: outer diameter 14mm, inner diameter 8mm, thickness 3mm
[0253] Molding pressure: 3t / cm 2 (294.2MPa)
[0254] Next, the powder compact was heated at 150° C. for 3 hours in an air atmosphere to solidify the binder, thereby obtaining a ring-shaped molded body.
[0255] Next, the radial compressive strength of the obtained molded body was measured according to the radial compressive strength test method specified in JIS Z2507:2000. Specifically, when the radial compressive strength is K, the outer diameter is D, the wall thickness in the radial direction (half the difference between the outer diameter and the inner diameter) is t, the thickness is L, and the breaking load is F, K=F(Dt) / (Lt 2 ) The radial compressive strength K was obtained. And the obtained radial compressive strength was evaluated according to the following evaluation criteria. The evaluation results are shown in Tables 2 and 3.
[0256] A: Radial compressive strength is above 50MPa
[0257] B: Radial compressive strength is 45MPa or more and less than 50MPa
[0258] C: Radial compressive strength is 40MPa or more and less than 45MPa
[0259] D: Radial compressive strength is 35MPa or more and less than 40MPa
[0260] E: Radial compressive strength is 30MPa or more and less than 35MPa
[0261] F: Radial compressive strength is less than 30MPa
[0262] 7.3. Relative density of molded body
[0263] First, an exposure test was conducted in which each insulator was covered with soft magnetic powder and left for 24 hours in a high humidity environment at atmospheric pressure, a temperature of 30°C, and a relative humidity of 80%.
[0264] Next, the insulator-coated soft magnetic powders subjected to the exposure test were molded in the same manner as in 7.2 to obtain a molded body. Next, the density of the powder compact was measured. Next, the density of the powder compact was divided by the true density of the soft magnetic powder to calculate the relative density. And, the calculated relative density was evaluated according to the following evaluation criteria. The evaluation results are shown in Tables 2 and 3.
[0265] A: Relative density is more than 67%
[0266] B: Relative density is 66% or more and less than 67%
[0267] C: Relative density is 65% or more and less than 66%
[0268] D: Relative density is 64% or more and less than 65%
[0269] E: Relative density is 63% or more and less than 64%
[0270] F: Relative density less than 63%
[0271]
Table 2
[0272]
[0273]
Table 3
[0274]
[0275] As shown in Tables 2 and 3, the insulator-coated soft magnetic powder of each embodiment has good voltage resistance and high radial compressive strength and relative density of the molded body even after exposure to a humid environment, compared with the insulator-coated soft magnetic powder of the comparative example.
[0276] In contrast, it is known that when the insulating film is only an inorganic insulating film or only an organic film, any one of the withstand voltage, radial compressive strength and relative density will decrease. In addition, it is also known that the thickness or water content of the inorganic insulating film is important for improving the withstand voltage, radial compressive strength and relative density.
[0277] From the above results, it is understood that according to the present invention, an insulator-coated soft magnetic powder can be obtained which is excellent in moisture resistance and in which a decrease in insulation or fluidity due to moisture absorption is suppressed.
Claims
1. An insulator-covered soft magnetic powder, characterized in that: The insulator-covered soft magnetic powder has: Soft magnetic powder; an inorganic insulating film covering the particle surface of the soft magnetic powder and comprising ceramics; and an organic film covering a surface of the inorganic insulating film and comprising a compound derived from a coupling agent having a hydrophobic functional group, The average thickness of the inorganic insulating film is greater than or equal to 5 nm and less than or equal to 100 nm. After being left to stand for 24 hours under an environment of atmospheric pressure, a temperature of 30° C., and a relative humidity of 80%, the moisture content measured by the Karl Fischer method at 250° C. was 30 ppm or more and 400 ppm or less.
2. The insulator-coated soft magnetic powder according to claim 1, wherein: The ceramic includes silicon oxide or aluminum oxide.
3. The insulator-coated soft magnetic powder according to claim 1 or 2, wherein: The inorganic insulating film has ceramic particles having a smaller diameter than particles of the soft magnetic powder and composed of the ceramic.
4. The insulator-coated soft magnetic powder according to claim 1 or 2, wherein: An average thickness of the organic film is thinner than an average thickness of the inorganic insulating film.
5. The insulator-coated soft magnetic powder according to claim 1 or 2, wherein: The hydrophobic functional group is a linear alkyl group having 1 to 6 carbon atoms.
6. The insulator-coated soft magnetic powder according to claim 1 or 2, wherein: The hydrophobic functional group is a group containing a cyclic structure, a fluoroalkyl group or a fluoroaryl group.
7. A powder magnetic core, characterized in that: Contains the insulator-coated soft magnetic powder according to claim 1 or 2.
8. A magnetic element, characterized in that: A powder magnetic core according to claim 7 is provided.
9. An electronic device, characterized in that: A magnetic element according to claim 8.