Method for producing active material composite particles and method for producing secondary battery

By removing SiO2 in the granules to form active material composite particles with gaps, the problem of constraint pressure and interface peeling caused by the expansion of the negative active material layer of the secondary battery during the charge and discharge process is solved, and the cycle characteristics are significantly improved.

CN118738281APending Publication Date: 2024-10-01TOYOTA JIDOSHA KK
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410310685.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-19
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

In the existing technology, there is room for improvement in the cycle characteristics of active materials containing Si. Especially in the negative active material layer of secondary batteries, the increase in constraint pressure and interfacial peeling caused by expansion during charging and discharging have not been effectively addressed. solve.

Method used

Through the manufacturing method, granules containing polymer and elemental Si are obtained, and SiO2 is removed during acid treatment to form voids and form active material composite particles with excellent cycle characteristics for use in the negative electrode active material layer of secondary batteries. The method includes step S1: obtaining granules, and step S2: forming voids by acid treatment, and hydrofluoric acid treatment may be used for the acid treatment.

Benefits of technology

Through the active material composite particles forming gaps, Si expansion is absorbed during charging, and the overall expansion amount is reduced, suppressing the increase in constraint pressure and interfacial peeling, and significantly improving the cycle characteristics of the secondary battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738281A_ABST
    Figure CN118738281A_ABST
Patent Text Reader

Abstract

Disclosed is a method for producing active material composite particles containing Si and having excellent cycle characteristics. A method for producing active material composite particles according to the present disclosure includes: obtaining a granulated body containing a polymer, elemental Si as a first component, and a component other than elemental Si as a second component (first step); and performing an acid treatment on the granulated body to remove the second component from the granulated body in a state in which the first component and the polymer remain in the granulated body, thereby forming voids in the granulated body (second step).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application discloses a method for producing active material composite particles and a method for producing a secondary battery. Background Art

[0002] Patent Document 1 discloses a granulated body of a negative electrode active material, which contains a composite of Si and carbon and a binder.

[0003] Prior art literature

[0004] Patent Document 1: Japanese Patent Application Publication No. 2019-021571 Summary of the invention

[0005] There is room for improvement in the cycle characteristics of active materials containing Si.

[0006] The present application discloses the following multiple aspects as means for solving the above-mentioned problems.

[0007] <Method 1>

[0008] A method for producing active material composite particles comprises the following steps:

[0009] obtaining granules containing a polymer, simple substance Si as a first component, and a component other than simple substance Si as a second component; and

[0010] The granules are subjected to an acid treatment to remove the second component from the granules while leaving the first component and the polymer in the granules, thereby forming voids in the granules.

[0011] <Method 2>

[0012] According to the manufacturing method described in embodiment 1,

[0013] The second component is SiO2.

[0014] <Method 3>

[0015] The manufacturing method according to embodiment 1 or 2,

[0016] The acid treatment includes hydrofluoric acid treatment.

[0017] <Method 4>

[0018] The production method according to any one of aspects 1 to 3,

[0019] The polymer contains a fluorine-containing polymer.

[0020] <Method 5>

[0021] A method for manufacturing a secondary battery comprises the following steps:

[0022] Active material composite particles are obtained by the production method described in any one of Embodiments 1 to 4; and

[0023] A negative electrode active material layer is obtained using the active material composite particles.

[0024] The active material composite particles disclosed herein have excellent cycle characteristics. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 An example of the flow of the method for producing active material composite particles is shown.

[0026] Figure 2 The states of the granules before acid treatment and the active material composite particles after acid treatment are schematically shown.

[0027] Figure 3 An example of a flow of a method for manufacturing a secondary battery is schematically shown.

[0028] Description of Reference Numerals

[0029] 1 Active material composite particles

[0030] 1a Granulation

[0031] 1ax Component 1

[0032] 1ay 2nd ingredient

[0033] 1az polymer

[0034] 1b Gap

[0035] 100 Secondary Batteries

[0036] 10 Negative electrode collector

[0037] 20 Negative electrode active material layer

[0038] 30 electrolyte layer

[0039] 40 Positive electrode active material layer

[0040] 50 Positive electrode collector DETAILED DESCRIPTION

[0041] 1. Method for producing active material composite particles

[0042] Reference Figure 1 and Figure 2 , a method for producing active material composite particles 1 according to one embodiment is described. Figure 1 and Figure 2As shown, a method for producing active material composite particles 1 according to one embodiment includes:

[0043] Step S1: obtaining granules 1a containing a polymer 1az, simple Si as a first component 1ax, and a component other than simple Si as a second component 1ay; and

[0044] Step S2: The granules 1a are subjected to an acid treatment to remove the second component 1ay from the granules 1a while leaving the first component 1ax and the polymer 1az in the granules 1a, thereby forming voids 1b in the granules 1a.

[0045] 1.1 Process S1

[0046] In step S1 , granules 1 a are obtained which contain a polymer 1az , simple Si as a first component 1ax , and a component other than simple Si as a second component 1ay .

[0047] 1.1.1 1st component

[0048] The first component 1ax is simple Si. Compared with the second component 1ay, simple Si as the first component 1ax is difficult to be removed by the acid treatment described later, and is likely to remain in the granules 1a after the acid treatment. Simple Si as the first component 1ax may also exist in the form of particles, for example. That is, in step S1, particles containing simple Si (Si particles) may also be used as the first component 1ax.

[0049] Si particles can exist as primary particles or as secondary particles. The chemical composition of Si particles is not particularly limited. The proportion of Si element in all elements contained in Si particles can be, for example, 50 mol% or more, 70 mol% or more, or 90 mol% or more. In addition to Si element, Si particles can also contain other elements such as alkali metal elements such as Li element. As other elements, in addition to alkali metal elements such as Li element, Sn element, Fe element, Co element, Ni element, Ti element, Cr element, B element, P element, etc. can also be cited. In addition, Si particles can also contain impurities such as oxides. The simple Si contained in Si particles can be amorphous Si or crystalline Si. The crystal phase contained in Si particles is not particularly limited.

[0050] The size of Si particles is not particularly limited. The average primary particle size of Si particles can be, for example, more than 10nm, more than 30nm, more than 50nm, more than 100nm or more than 150nm, and can be less than 10μm, less than 5μm, less than 3μm, less than 2μm or less than 1μm. In addition, the average secondary particle size of Si particles can be, for example, more than 100nm, more than 1μm or more than 2μm, and can be less than 20μm, less than 15μm or less than 10μm. Furthermore, the average primary particle size and the average secondary particle size can be obtained by electron microscope observation such as SEM, for example, as the number average of the maximum Feret diameter of each of a plurality of particles. The number of samples also depends on the number of Si particles contained in the granules 1a, but the number of samples is preferably large. The number of samples can be, for example, more than 1, more than 2, more than 5, more than 20, more than 50 or more than 100. The average primary particle size and the average secondary particle size can be appropriately adjusted, for example, by appropriately changing the manufacturing conditions of the Si particles or performing a classification process.

[0051] Si particles can be porous. Since Si particles are porous, the expansion of Si particles during charging can be alleviated by the voids in the Si particles. The form of the voids in the porous Si particles is not particularly limited. Porous Si particles can also be particles containing nanoporous silicon. Nanoporous silicon refers to silicon having multiple pores with a pore size of nanometer level (less than 1000nm, preferably less than 100nm). Porous Si particles can also contain pores with a diameter of less than 55nm. Pores with a diameter of less than 55nm are not easily crushed even by pressing. That is, porous Si particles containing pores with a diameter of less than 55nm are easy to maintain porosity even after pressing. For example, per 1g of porous Si particles, 0.21cc / g or more, 0.22cc / g or more, or 0.23cc / g or more of pores with a diameter of 55nm or less may be contained, and 0.30cc / g or less, 0.28cc / g or less, or 0.26cc / g or less of pores with a diameter of 55nm or less may be contained. The amount of pores with a diameter of 55nm or less contained in the porous Si particles can be obtained by, for example, a nitrogen adsorption method or a pore size distribution by a DFT method.

[0052] When the Si particles are porous, the porosity is not particularly limited. The porosity of the porous Si particles can be, for example, 1% or more, 5% or more, 10% or more, or 20% or more, and can be 80% or less, 70% or less, 60% or less, 50% or less, 40% or less, or 30% or less. The porosity of the Si particles can be determined, for example, by observation with a scanning electron microscope (SEM). The number of samples is preferably large, for example, 100 or more. The porosity can be an average value obtained from these samples.

[0053] When the first component 1ax is contained in the form of Si particles, the number of Si particles contained in one granule 1a is not particularly limited and may be 1 or more, 2 or more, 5 or more, 10 or more, or 50 or more, and 1000 or less, 500 or less, or 100 or less.

[0054] 1.1.2 Second component

[0055] The second component 1ay is a component other than elemental Si. The second component 1ay is removed by the acid treatment described later. That is, the second component 1ay may also be a component that dissolves in a predetermined acid. For example, the second component 1ay may also be SiO2. In the case where the second component 1ay is SiO2, most of it can be easily removed from the granules 1a by the acid treatment described later. In addition, even if a part of SiO2 remains in the granules 1a after the acid treatment, it is not easy to have an adverse effect on the electrochemical reaction (deintercalation reaction of carrier ions, etc.) as an active material. For example, the second component 1ay may also exist in the form of particles. That is, in step S1, particles (second particles) containing the second component 1ay may also be used. For example, in step S1, particles (SiO2 particles) containing SiO2 as the second component may also be used.

[0056] The second particle can exist as a primary particle or as a secondary particle. The second particle can be, for example, the SiO2 particle as described above. The SiO2 content in the SiO2 particle can be, for example, 50% by mass or more and 100% by mass or less, 70% by mass or more and 100% by mass or less, or 90% by mass or more and 100% by mass or less. In addition to SiO2, the SiO2 particle can also contain other elements, compounds and impurities.

[0057] The size of the second particle is not particularly limited. The average primary particle size of the second particle can be, for example, more than 10nm, more than 30nm, more than 50nm, more than 100nm or more than 150nm, and can be less than 10μm, less than 5μm, less than 3μm, less than 2μm or less than 1μm. In addition, the average secondary particle size of the second particle can be, for example, more than 100nm, more than 1μm or more than 2μm, and can be less than 20μm, less than 15μm or less than 10μm. Furthermore, the average primary particle size and the average secondary particle size can be obtained by observation with an electron microscope such as SEM, for example, as the number average of the maximum Feret diameter of each of a plurality of particles. The number of samples also depends on the number of the second particles contained in the granulation body 1a, but the number of samples is preferably large. The number of samples can be, for example, more than 1, more than 2, more than 5, more than 20, more than 50 or more than 100. The average primary particle size and the average secondary particle size can be appropriately adjusted, for example, by appropriately changing the manufacturing conditions of the second particle or performing a classification process.

[0058] When the second component 1ay is contained in the form of second particles, the number of second particles contained in one granule 1a is not particularly limited and may be 1 or more, 2 or more, 5 or more, 10 or more, or 50 or more, and 1000 or less, 500 or less, or 100 or less.

[0059] 1.1.3 Polymer

[0060] The polymer 1az can, for example, be used as a binder for bonding the above-mentioned first component 1ax to each other and maintaining the shape of the active material composite particle 1. In addition, the polymer 1az can also function as a buffer material. The type of polymer 1az is not particularly limited. As polymer 1az, various binders known as constituent materials of secondary batteries can also be used. For example, polymer 1az can also be selected from butadiene rubber (BR)-based binders, butyl rubber (IIR)-based binders, acrylic ester butadiene rubber (ABR)-based binders, styrene butadiene rubber (SBR)-based binders, polyvinylidene fluoride (PVdF)-based binders, polytetrafluoroethylene (PTFE)-based binders, polyimide (PI)-based binders, carboxymethyl cellulose (CMC)-based binders, polyacrylate-based binders, polyacrylate-based binders, etc. At least one of the above. In particular, when the polymer 1az contains a fluorine-containing polymer, in the case of containing one or both of a polyvinylidene fluoride (PVdF)-based binder and a polytetrafluoroethylene (PTFE)-based binder, and further in the case of containing a PVdF-based binder, it is easy to ensure higher performance. The PVdF-based binder may be a copolymer having units derived from a monomer other than VdF (Vinylidene Fluoride). The polymer 1az may be used alone or in combination of two or more.

[0061] 1.1.4 Content of each ingredient

[0062] In the granules 1a, the contents of the first component 1ax, the second component 1ay and the polymer 1az are not particularly limited. For example, the granules 1a may contain 50% by mass or more and less than 100% by mass of the first component 1ax, more than 0% by mass or less than 50% by mass of the second component 1ay, and more than 0% by mass or less than 50% by mass of the polymer 1az. Alternatively, the granules 1a may contain 60% by mass or more and less than 90% by mass of the first component 1ax, more than 5% by mass or less and less than 30% by mass of the second component 1ay, and more than 5% by mass or less and less than 30% by mass of the polymer 1az.

[0063] 1.1.5 Other ingredients

[0064] The granules 1a may be composed of only the first component 1ax, the second component 1ay and the polymer 1az, or may contain other components in addition to these. Examples of other components include various solid components and liquid components.

[0065] 1.1.6 Steps for obtaining granules

[0066] In step S1, for example, the first component 1ax, the second component 1ay and the polymer 1az can be dry-mixed to adhere the components to each other, thereby obtaining granules 1a. In this case, there is no particular limitation on the mixing means, and the mixing can be performed manually using a mortar or the like, or mechanically by various mixing devices. Alternatively, in step S1, after obtaining a slurry or solution containing the first component 1ax, the second component 1ay and the polymer 1az, the granules 1a can be obtained by drying the slurry or solution. For example, a polymer 1az is dissolved in a solvent to obtain a polymer solution, Si particles as the first component 1ax and second particles (such as SiO2 particles) as the second component 1ay are dispersed in the polymer solution to obtain a slurry, and then the slurry is dried to obtain granules 1a in which the Si particles and the second particles are bonded via the polymer 1az. In this case, there is no particular limitation on the type of solvent. In addition, there is no particular limitation on the means for drying the slurry.

[0067] Step S1 may also include:

[0068] Step S1-1: forming droplets of a slurry containing the first component 1ax, the second component 1ay, and the polymer 1az into droplets to obtain slurry droplets; and

[0069] Step S1-2: The slurry droplets are dried in a heated gas in a stream to obtain granules 1a containing the first component 1ax, the second component 1ay, and the polymer 1az.

[0070] The "slurry" in step S1-1 refers to a suspension or suspension containing the first component 1ax, the second component 1ay and the polymer 1az, as long as it has fluidity that allows it to be dropletized. The "dropletization" of the slurry refers to forming the slurry containing the first component 1ax, the second component 1ay and the polymer 1az into particles containing the first component 1ax, the second component 1ay and the polymer 1az and a solvent. The method of dropletizing the slurry containing the first component 1ax, the second component 1ay and the polymer 1az is not particularly limited. For example, a method of dropletizing the slurry by spraying it can be cited. In the case of spraying the slurry, a nozzle can also be used. As a method of spraying the slurry using a spray nozzle, a pressurized nozzle method and a two-fluid nozzle method can be cited, but are not limited to this. Alternatively, the slurry can also be dropletized using a rotary atomizer.

[0071] In step S1-1, the size of the slurry droplets is not particularly limited. The diameter (equivalent spherical diameter) of the slurry droplets can be, for example, 0.5 μm or more or 5 μm or more, and can be 5000 μm or less or 1000 μm or less. The diameter of the slurry droplets can be measured, for example, using a two-dimensional image obtained by photographing the slurry droplets, or can be measured using a laser diffraction particle size distribution meter. Alternatively, the droplet diameter can also be estimated based on the operating conditions of the device that forms the slurry droplets.

[0072] "Airflow drying" in step S1-2 means drying while making the slurry droplets float in the high-temperature airflow. "Airflow drying" can include not only drying, but also incidental operations using dynamic airflow. Airflow drying allows hot air to continuously contact the slurry droplets, thereby continuously applying force to the slurry droplets. Taking advantage of this, for example, step S1-2 may also include a step of breaking (crushing) the agglomerates of the slurry droplets (or the agglomerates of the granules 1a) by airflow drying. In other words, in step S1-2, even in the case of excessive agglomeration of the slurry droplets, the agglomerates can be crushed by airflow drying. Therefore, slurry with a low solid content concentration can also be used, which makes it easy to increase the processing speed. In this way, in step S1-2, the slurry droplets are crushed by airflow drying, thereby easily shortening the manufacturing time. In step S1-2, the above-mentioned drying and crushing can be performed simultaneously or separately. In step S1-2, the first airflow drying in which the drying of the slurry droplets is dominant and the second airflow drying in which the crushing of the agglomerates is dominant can also be performed. Alternatively, the second air flow drying may be repeated.

[0073] In step S1-2, the temperature of the heating gas, the gas supply amount (flow rate) of the heating gas, the gas supply speed (flow rate) of the heating gas, and the processing time (drying time) of the heating gas can be appropriately set considering the size of the device used and the form of the slurry droplets. For example, the conditions disclosed in Japanese Patent Gazette No. 2022-047501 can also be adopted. In step S1-2, a heating gas that is substantially inert to the above-mentioned components can also be used. For example, oxygen-containing gases such as air, inert gases such as nitrogen or argon, dry air with a low dew point, etc. can be used. As a device for airflow drying, for example, a spray dryer can be used, but is not limited to this.

[0074] 1.2 Process S2

[0075] In step S2, the granules 1a are subjected to an acid treatment to remove the second component 1ay from the granules 1a while leaving the first component 1ax and the polymer 1az in the granules 1a, thereby forming voids in the granules 1a. That is, the second component 1ay is etched by subjecting the granules 1a to an acid treatment.

[0076] The acid used for the acid treatment in step S2 may be any acid that can remove the second component 1ay from the granules 1a while leaving the first component 1ax and the polymer 1az in the granules 1a. The acid treatment in step S2 may include, for example, a hydrofluoric acid treatment. That is, the first component 1ax and the polymer 1az may remain in the granules 1a by bringing hydrofluoric acid (aqueous hydrogen fluoride solution) into contact with the granules 1a, and the second component 1ay contained in the granules 1a may be dissolved, thereby removing the second component 1ay from the granules 1a. In step S2, for example, 50 mol% or more and 100 mol% or more, 70 mol% or more and 100 mol% or more, or 90 mol% or more and 100 mol% or less of the second component 1ay contained in the granules 1a may be dissolved in the acid and removed.

[0077] In step S2, the method for bringing the granules 1a into contact with the acid is not particularly limited. The granules 1a may be immersed in the acid, or the acid may be sprayed on the granules 1a. Alternatively, the granules 1a may be dispersed in a solvent to form a slurry, and the acid is added to the slurry, thereby bringing the granules 1a into contact with the acid in the slurry. In this case, water and various organic solvents can be used as solvents for dispersing the granules 1a. For example, alcohols such as ethanol may be used as solvents. In step S2, the time for the acid treatment is not particularly limited. For example, the granules 1a may be dispersed in a solvent to form a slurry, and the acid is added to the slurry, and stirred for more than 1 minute and less than 10 hours. In step S2, the temperature and atmosphere for the acid treatment are also not particularly limited.

[0078] 1.3 Active material composite particles 1

[0079] After step S2, filtration, washing and drying are optionally performed to recover the solid content, thereby obtaining an active material composite particle 1 containing the first component 1ax and the polymer 1az and having a void 1b. In the active material composite particle 1, the expansion of Si during charging is absorbed by the void 1b, and the amount of expansion of the active material composite particle 1 as a whole becomes smaller. For example, when the active material composite particle 1 is applied to the negative electrode of a secondary battery, the volume change of the negative electrode accompanying charging and discharging becomes smaller. As a result, the increase in the restraining pressure and the interface peeling can be suppressed, and the cycle characteristics are improved.

[0080] 1.3.1 Composition of active material composite particles

[0081] The active material composite particle 1 contains at least a first component 1ax and a polymer 1az. The active material composite particle 1 may contain, for example, 50% by mass or more and less than 100% by mass of the first component 1ax, 0% by mass or more and 10% by mass or less of the second component 1ay, and more than 0% by mass or less and 50% by mass or less of the polymer 1az. Alternatively, the active material composite particle 1 may contain 60% by mass or more and less than 90% by mass of the first component 1ax, 0% by mass or more and less than 5% by mass of the second component 1ay, and 10% by mass or more and less than 30% by mass of the polymer 1az.

[0082] 1.3.2 Particle size of active material composite particles

[0083] The active material composite particle 1 can be regarded as a secondary particle containing the first component 1ax, the polymer 1az and the void 1b. The average particle size of the composite particle 1 is not particularly limited. The average particle size of the composite particle 1 can be greater than 100nm, greater than 500nm, greater than 1μm, greater than 2μm or greater than 3μm, and can be less than 1mm, less than 500μm, less than 300μm, less than 100μm, less than 50μm, less than 20μm, less than 15μm or less than 10μm. The average particle size of the composite particle 1 can be obtained by observation using an electron microscope such as SEM, for example, as the numerical average of the maximum Feret diameter of multiple composite particles. The number of samples is preferably large, for example, greater than 20, greater than 50, or greater than 100. Alternatively, the average particle size (D50, median diameter) of the composite particles 1 measured using a laser diffraction particle distribution measuring device can be greater than 100 nm, greater than 500 nm, greater than 1 μm, greater than 2 μm, or greater than 3 μm, and can be less than 1 mm, less than 500 μm, less than 300 μm, less than 100 μm, less than 50 μm, less than 20 μm, less than 15 μm, or less than 10 μm.

[0084] 1.3.3 Structure and shape of active material composite particles

[0085] In the active material composite particle 1, the arrangement of the first component 1ax, the polymer 1az and the void 1b is not particularly limited. In addition, the active material composite particle 1 may have a major diameter and a minor diameter, for example, before being applied to a secondary battery. The ratio of the major diameter to the minor diameter may be, for example, 1.0 or more or 1.1 or more, and may be 1.3 or less or 1.2 or less.

[0086] 2. Method for manufacturing secondary battery

[0087] The active material composite particle 1 disclosed in the present invention can be used as, for example, a negative electrode active material of a secondary battery. Figure 3As shown, a method for manufacturing a secondary battery 100 according to an embodiment includes: obtaining active material composite particles 1 by the manufacturing method disclosed above; and obtaining a negative electrode active material layer 20 using the active material composite particles 1. The secondary battery 100 may be, for example, a lithium ion secondary battery.

[0088] The negative electrode active material layer 20 may also optionally contain other negative electrode active materials, electrolytes, conductive additives, and binders together with the active material composite particles 1. The electrolyte may also be, for example, an inorganic solid electrolyte. In this way, in the negative electrode active material layer 20, when an inorganic solid electrolyte is combined with the active material composite particles 1, a more excellent effect brought by the technology disclosed in the present invention can be obtained. The inorganic solid electrolyte may be a sulfide solid electrolyte or other inorganic solid electrolytes.

[0089] The secondary battery 100 can be manufactured by applying a known method except that the active material composite particles 1 are used as the negative electrode active material. For example, it can be manufactured as follows. However, the manufacturing method of the secondary battery 100 is not limited to the following method, and each layer can also be formed by dry molding, etc.

[0090] (1) Active material composite particles 1 and the like constituting the negative electrode active material layer 20 are dispersed in a solvent to obtain a negative electrode slurry. The solvent used in this case is not particularly limited, and water and various organic solvents can be used. Then, the negative electrode slurry is applied to the surface of the negative electrode collector 10 or the electrolyte layer 30 described later using a scraper or the like, and then dried, thereby forming the negative electrode active material layer 20 on the surface of the negative electrode collector 10 or the electrolyte layer 30. Here, the negative electrode active material layer 20 can also be formed by compression molding.

[0091] (2) The positive electrode active material constituting the positive electrode active material layer 40 is dispersed in a solvent to obtain a positive electrode slurry. The solvent used in this case is not particularly limited, and water and various organic solvents can be used. Then, the positive electrode slurry is applied to the surface of the positive electrode collector 50 or the electrolyte layer 30 described later using a scraper or the like, and then dried, thereby forming the positive electrode active material layer 40 on the surface of the positive electrode collector 50 or the electrolyte layer 30. Here, the positive electrode active material layer 40 can also be pressed.

[0092] (3) The layers are stacked in such a manner that the electrolyte layer 30 is sandwiched between the negative electrode active material layer 20 and the positive electrode active material layer 40, thereby obtaining a stack having the negative electrode collector 10, the negative electrode active material layer 20, the electrolyte layer 30, the positive electrode active material layer 40 and the positive electrode collector 50 in sequence. The electrolyte layer can be obtained by, for example, molding an electrolyte mixture containing a solid electrolyte and a binder, or by compression molding. Here, the stack can also be further compression molded. Other components such as terminals are installed on the stack as needed. When an electrolyte solution is used, the electrolyte layer can be a diaphragm.

[0093] (4) The stacked body is housed in a battery case and sealed to obtain a secondary battery.

[0094] [Example]

[0095] As described above, one embodiment of the technology disclosed in the present invention has been described, but the technology disclosed in the present invention can be variously modified other than the above embodiment without departing from the scope of the present invention. The following examples are shown to explain the technology disclosed in more detail, but the technology disclosed in the present invention is not limited to the following examples.

[0096] 1. Preparation of active material composite particles

[0097] 1.1 Example 1

[0098] 1.3 g of PVdF-HFP (polyvinylidene fluoride-hexafluoropropylene, manufactured by Kureha Corporation) was added to 500 mL of dimethyl carbonate and stirred to dissolve to prepare a polymer solution. 5.0 g of Si simple particles and 1.0 g of SiO2 particles (manufactured by Sigma-Aldrich Corporation, average particle size 0.1 μm to 0.2 μm) were added to the polymer solution and dispersed using an ultrasonic homogenizer to obtain a slurry. The slurry was sprayed using a spray dryer (ADL311S manufactured by YAMATO SCIENTIFIC Corporation) to dry it, thereby preparing a granulated body consisting of simple Si, SiO2 and PVdF-HFP.

[0099] 2 g of the obtained granules were dispersed in 100 mL of ethanol, and then 3 mL of a 47 wt % aqueous hydrogen fluoride solution was added thereto. After addition, the mixture was stirred for 3 hours, and then filtered under reduced pressure to recover the active material composite particles. In the active material composite particles, SiO2 contained in the granules was removed by treatment with an aqueous hydrogen fluoride solution (hydrofluoric acid treatment), forming voids. The obtained active material composite particles were vacuum dried at 120° C. for 12 hours and used as the negative electrode active material described later.

[0100] 1.2 Comparative Example 1: No Acid Treatment

[0101] In Example 1, the acid treatment with the aqueous hydrogen fluoride solution was not performed, and the granules composed of simple Si, SiO 2 and PVdF-HFP were used as the negative electrode active material as it was.

[0102] 1.3 Comparative Example 2: No SiO2

[0103] 5.0 g of Si simple substance particles were added to the polymer solution prepared in the same manner as in Example 1, and dispersed using an ultrasonic homogenizer to obtain a slurry. The slurry was sprayed and dried using a spray dryer (ADL311S manufactured by YAMATO SCIENTIFIC Co., Ltd.) to prepare granules composed of simple substance Si and PVdF-HFP, which were used as negative electrode active materials.

[0104] 2. Fabrication of all-solid-state batteries

[0105] 2.1 Preparation of positive electrode active material layer

[0106] In a PP container, butyl butyrate as a solvent, a 5 wt% butyl butyrate solution of a PVDF-based binder, and LiNi as a positive electrode active material were placed. 1 / 3 Co 1 / 3 Mn 1 / 3 O2 particles (average particle size 6 μm), Li2S-P2S5 glass ceramics as sulfide solid electrolyte and VGCF (vapor grown carbon fiber) as conductive additive are stirred for 30 seconds with an ultrasonic disperser (UH-50 made by SMT). Next, the container is oscillated for 3 minutes with an oscillator (TTM-1 made by Shibata Science Co., Ltd.), and then stirred for 30 seconds with an ultrasonic disperser. Then, the positive electrode slurry is obtained by oscillating with an oscillator for 3 minutes. Using an applicator, the positive electrode slurry is applied to Al foil (made by Showa Denko) by a scraper method and dried on a hot plate at 100°C for 30 minutes, thereby forming a positive electrode active material layer on the Al foil.

[0107] 2.2 Fabrication of negative electrode active material layer

[0108] In a PP container, dibutyl ether and mesitylene as solvents, a 5 wt% mesitylene solution of a PVDF-based binder, VGCF as a conductive aid, Li2S-P2S5-based glass ceramics as a solid electrolyte, and the above-mentioned active material composite particles or granules as a negative electrode active material are added to the container and stirred for 30 seconds using an ultrasonic disperser (UH-50 manufactured by SMT). Next, the container is oscillated for 30 minutes with an oscillator (TTM-1 manufactured by Shibata Science Co., Ltd.) to obtain a negative electrode slurry. Using an applicator, the negative electrode slurry is applied to a Cu foil (manufactured by UACJ) by a scraper method and dried on a hot plate at 100°C for 30 minutes, thereby forming a negative electrode active material layer on the Cu foil.

[0109] 2.3 Fabrication of solid electrolyte layer

[0110] Heptane as a solvent, a 5 wt% heptane solution of an SBR-based binder, and Li2S-P2S5-based glass ceramics as a solid electrolyte were added to a PP container and stirred for 30 seconds using an ultrasonic dispersing device (UH-50 manufactured by SMT). Next, the container was vibrated for 30 minutes using an oscillator (TTM-1 manufactured by Shibata Science Co., Ltd.) to obtain an electrolyte slurry. Using an applicator, the electrolyte slurry was applied to an Al foil as a substrate by a scraper method and dried on a hot plate at 100°C for 30 minutes, thereby forming a solid electrolyte layer on the Al foil.

[0111] 2.4 Stacking of layers

[0112] The positive electrode active material layer and the solid electrolyte layer are stacked to obtain a first stack having Al foil / positive electrode active material layer / solid electrolyte layer / Al foil. The first stack is placed on a roller press and pressed at a pressing pressure of 100 kN / cm and a pressing temperature of 165° C. Then, the Al foil as a substrate is removed from the first stack to obtain a positive electrode stack having Al foil / positive electrode active material layer / solid electrolyte layer.

[0113] The negative electrode active material layer and the solid electrolyte layer are stacked to obtain a second stack having Cu foil / negative electrode active material layer / solid electrolyte layer / Al foil. The second stack is placed on a roller press and pressed at a pressing pressure of 60 kN / cm and a pressing temperature of 25° C. Then, the Al foil as a substrate is removed from the second stack to obtain a first negative electrode stack having Cu foil / negative electrode active material layer / solid electrolyte layer.

[0114] The Al foil and solid electrolyte layer as the substrate and the first negative electrode laminate are stacked in the order of Al foil / solid electrolyte layer / solid electrolyte layer / negative electrode active material layer / Cu foil to obtain a third laminate. The third laminate is placed on a flat uniaxial press and temporarily pressed at 100 MPa and 25° C. for 10 seconds. Then, the Al foil is peeled off from the third laminate to obtain a second negative electrode laminate having a solid electrolyte layer / solid electrolyte layer / negative electrode active material layer / Cu foil. Furthermore, the area of ​​the second negative electrode laminate is larger than that of the above-mentioned positive electrode laminate.

[0115] The positive electrode laminate and the second negative electrode laminate were stacked in the order of Al foil / positive electrode active material layer / solid electrolyte layer / solid electrolyte layer / solid electrolyte layer / negative electrode active material layer / Cu foil to obtain a fourth laminate. The fourth laminate was placed on a flat uniaxial press and pressed at 200 MPa and 120° C. for 1 minute. Thus, an all-solid battery for evaluation was obtained.

[0116] 3. Evaluation of all-solid-state batteries

[0117] The all-solid battery was made by using a constraint fixture to constrain the predetermined constraint pressure, and then charged to 4.55V at 1 / 10C constant current, discharged to 3.0V at 1C, charged to 4.35V at 1 / 3C constant current-constant voltage, discharged to 3.00V at 1 / 3C constant current-constant voltage, and then repeated 200 constant current charge and discharge tests at 2C as a cycle test. The ratio of the discharge capacity of the 200th cycle of the cycle test to the initial discharge capacity ([200th cycle discharge capacity / initial discharge capacity]×100) was calculated as the discharge capacity maintenance rate.

[0118] 4. Evaluation results

[0119] Table 1 below shows the discharge capacity maintenance ratios of all-solid batteries of Example 1 and Comparative Examples 1 and 2. In Table 1 below, the discharge capacity maintenance ratio of Comparative Example 2 is set to 100, and the discharge capacity maintenance ratios of Example 1 and Comparative Example 1 are shown relative to each other.

[0120] Table 1

[0121] Discharge capacity maintenance rate Example 1 122 Comparative Example 1 72 Comparative Example 2 100

[0122] As shown in Table 1, the all-solid battery of Example 1 has excellent cycle characteristics compared with the all-solid batteries of Comparative Examples 1 and 2. It is believed that in the all-solid battery of Example 1, by removing SiO2 from the granules, voids are formed in the active material composite particles, and the Si expansion during charging is absorbed by the voids, so that the expansion amount of the active material composite particles as a whole becomes smaller. That is, it is believed that the volume change of the negative electrode accompanying charging and discharging becomes smaller, and the increase of the restraining pressure and the interface peeling can be suppressed, and the cycle characteristics are improved.

[0123] Furthermore, in the above-mentioned embodiment, when manufacturing active material composite particles, SiO2 is used as the second component, a fluorinated polymer is used as the polymer, and hydrofluoric acid treatment is used as the acid treatment, but it is believed that the same active material composite particles can be formed by acid treatment when using materials other than these. In addition, in the above-mentioned embodiment, as a secondary battery for evaluation, the case of making a full solid battery is exemplified, but in secondary batteries other than these, the effect brought by the active material composite particles can also be expected.

[0124] As described above, active material composite particles having excellent cycle characteristics can be produced according to the following method. That is, the method for producing active material composite particles of the present disclosure includes:

[0125] Step S1: obtaining granules containing a polymer, simple Si as a first component, and a component other than simple Si as a second component; and

[0126] Step S2: The granules are subjected to an acid treatment to remove the second component from the granules while leaving the first component and the polymer in the granules, thereby forming voids in the granules.

Claims

1. A method for producing active material composite particles, comprising the following steps: obtaining granules containing a polymer, simple substance Si as a first component, and a component other than simple substance Si as a second component; and The granules are subjected to an acid treatment to remove the second component from the granules while leaving the first component and the polymer in the granules, thereby forming voids in the granules.

2. The method for producing active material composite particles according to claim 1, The second component is SiO2.

3. The method for producing active material composite particles according to claim 1 or 2, The acid treatment includes hydrofluoric acid treatment.

4. The method for producing active material composite particles according to any one of claims 1 to 3, The polymer contains a fluorine-containing polymer.

5. A method for manufacturing a secondary battery, comprising the following steps: Active material composite particles are obtained by the production method according to any one of claims 1 to 4; and A negative electrode active material layer is obtained using the active material composite particles.