Positive electrode active material, all-solid-state battery, and method for producing positive electrode active material
By forming a coating film containing P, B and O on the surface of the positive active material particles, combined with the glass network structure and mixed anion effect, the composition ratio of Li and Na is optimized to solve the problem of increased battery resistance caused by the deterioration of the sulfide solid electrolyte. , achieving a significant reduction in battery resistance and improved performance.
Patent Information
- Application Number
- CN202410347064.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2024-03-26
- Publication Date
- 2024-10-01
AI Technical Summary
The sulfide solid electrolyte is prone to deterioration when the positive electrode is in direct contact with the active material particles, causing the battery resistance to increase. It is difficult to effectively reduce the battery resistance with the existing technology, especially when using low-polymerization phosphate compounds and impurity Na, it is difficult to improve ion conduction. Rate.
A coating film is formed on the surface of the active material particles. The coating film contains P, B and O. The ion conductivity is improved through the glass network structure and the mixed anion effect. Under the control of the composition ratio of Li and Na, the composition of the coating film is optimized to reduce Small battery resistance, using low polymerization degree phosphoric acid raw materials and low-priced raw materials.
It significantly reduces battery resistance, allows the use of low-price, low-purity raw materials, improves battery performance and cost-effectiveness, and ensures battery stability and performance improvement.
Smart Images

Figure CN118738313A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a positive electrode active material, an all-solid-state battery, and a method for producing the positive electrode active material. Background Art
[0002] Japanese Patent Application Laid-Open No. 2003-338321 discloses forming a film of an inorganic solid electrolyte between a positive electrode material and an organic electrolyte. Summary of the invention
[0003] Sulfide-based all-solid-state batteries (hereinafter referred to as "all-solid-state batteries") have been developed. All-solid-state batteries contain sulfide solid electrolytes. In the positive electrode, active material particles have a high potential. In the positive electrode, if the sulfide solid electrolyte is in direct contact with the active material particles, the sulfide solid electrolyte may deteriorate. Due to the deterioration of the sulfide solid electrolyte (ion conduction path), the battery resistance may increase. Therefore, it is proposed to form a coating on the surface of the active material particles. The coating hinders the direct contact between the active material particles and the sulfide solid electrolyte, thereby reducing the degradation of the sulfide solid electrolyte. In the past, it was proposed to use Li 3 PO 4 Oxide solid electrolytes such as the like are used to form a coating film (see, for example, Japanese Patent Application Laid-Open No. 2003-338321).
[0004] The present disclosure is directed to the reduction of battery resistance.
[0005] 1. The positive electrode active material includes active material particles and a coating film. The coating film covers at least a portion of the surface of the active material particles. The coating film includes P, B, and O as essential components, and further includes Li and Na as optional components.
[0006] The positive electrode active material satisfies the relationship between the following formula (1) and the following formula (2).
[0007] C Li / (C P +C B )≤1.50 (1)
[0008] C Na / (C P +C B )≤1.34 (2)
[0009] In the formula (1) and the formula (2), C Li , C P , C B and C Na They represent the element concentrations measured by X-ray photoelectron spectroscopy. Li Indicates the element concentration of lithium. P Indicates the element concentration of phosphorus.B Indicates the element concentration of boron. Na Indicates the element concentration of sodium
[0010] The left side of the above formula (1) is Li / (C P +C B )” is also referred to as “Li composition ratio”. Na / (C P +C B )" is also recorded as "Na composition ratio".
[0011] In Li 3 PO 4 The Li composition ratio is 3. 3 PO 4 (oxide solid electrolyte) promotes ion conduction (Li conduction). Therefore, the larger the Li composition ratio, the more expected the battery resistance is to be reduced. However, contrary to expectations, it was found that the battery resistance can be reduced when the Li composition ratio is small. Furthermore, as shown in the above formula (1), it was found that the battery resistance can be significantly reduced by a Li composition ratio of 1.5 or less.
[0012] As a result of repeated studies on various phosphoric acid compounds, it is known that when a phosphoric acid compound with a low degree of polymerization (orthophosphoric acid) is used as a raw material, it is difficult to reduce the battery resistance. Furthermore, when impurities such as Na are contained in the raw material, it is also found that the battery resistance is difficult to reduce. Therefore, expensive raw materials (high degree of polymerization, high purity) have to be used.
[0013] In the positive electrode active material described in the above "1", the coating film contains a composite oxide. That is, the coating film contains B in addition to P and O. P, B and O can form a glass network. By containing two kinds of anions (PO-based anions and BO-based anions) in the glass network, it is expected that the mixed anion effect will be manifested. By using the mixed anion effect, the ion conductivity can be significantly increased.
[0014] Furthermore, although the details of the mechanism are not clear, the coating film containing P, B and O can be robust. That is, the coating film can slightly contain Na. Even if the coating film contains a little Na, a reduction in battery resistance can be expected. Furthermore, using a phosphoric acid raw material with a low degree of polymerization, a reduction in battery resistance can also be expected. Therefore, the use of low-priced raw materials (low degree of polymerization, low purity) can be allowed.
[0015] As shown in the above formula (2), the Na composition ratio is 1.34 or less. If the Na composition ratio exceeds 1.34, the Li composition ratio is 1.5 or less, and even if the coating film contains B, the desired battery resistance may not be obtained.
[0016] 2. The positive electrode active material described in the above “1” may include, for example, the following configuration: The coating film includes Na as an essential component.
[0017] The relationship between the following equation (3) and the following equation (4) is satisfied.
[0018] C Li / (C P +C B )≤1.27 (3)
[0019] 0.24≤C Na / (C P +C B ) (4)
[0020] 3. The positive electrode active material described in "1" or "2" above may include, for example, the following composition. The positive electrode active material has a coverage of 94% or more. The coverage is measured by X-ray photoelectron spectroscopy. When the coverage is 94% or more, it is expected that the battery resistance will be reduced.
[0021] 4. The all-solid-state battery comprises a positive electrode and a negative electrode. The positive electrode comprises the positive electrode active material according to any one of "1" to "3" above, and a sulfide solid electrolyte.
[0022] 5. The method for producing a positive electrode active material includes the following (a) and (b).
[0023] (a) A mixture is prepared by mixing a coating liquid and active material particles.
[0024] (b) The mixture is dried to produce a positive electrode active material.
[0025] The coating liquid contains a solute and a solvent. The solute contains a phosphoric acid compound and a boric acid compound as essential components and contains at least one selected from a lithium compound, a sodium salt, and an ammonium salt as an optional component.
[0026] When the coating liquid contains both a phosphoric acid compound and a boric acid compound, a coating film containing P, B, and O can be formed. When the coating liquid contains both a phosphoric acid compound and a boric acid compound, a coating film containing Na salt, NH 4 Salt raw materials. Even if the coating solution contains Na salt, NH 4 Salts are also expected to reduce battery resistance. For example, at least a portion of the phosphate compound may be a Na salt. For example, at least a portion of the boric acid compound may be NH 4 Salt. Furthermore, Na from Na salt may be contained in the coating film. 4 N in the salt can be discharged to the outside of the system during the film formation process.
[0027] Hereinafter, an embodiment of the present disclosure (hereinafter may be abbreviated as "the present embodiment") and an example of the present disclosure (hereinafter may be abbreviated as "the present example") are described. However, the present embodiment and the present example do not limit the scope of the technology of the present disclosure. The present embodiment and the present example are illustrative in all aspects. The present embodiment and the present example are non-restrictive. The scope of the technology of the present disclosure includes all variations within the meaning and scope equivalent to the records in the patent claims. For example, it was originally anticipated that any configuration would be extracted from the present embodiment and the present example and that they would be arbitrarily combined.
[0028] The above and other objects, features, aspects and advantages of the present disclosure will become apparent from the following detailed description of the present disclosure in conjunction with the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is a conceptual diagram of the positive electrode active material in this embodiment.
[0030] Figure 2 This is a schematic flowchart of the method for producing the positive electrode active material in this embodiment.
[0031] Figure 3 This is a conceptual diagram of the all-solid-state battery in this embodiment.
[0032] Figure 4 The table shows the experimental results. DETAILED DESCRIPTION
[0033] <Explanation of terms>
[0034] “Element concentration (C Li , C P , C B , C Na )" indicates the value measured by the following steps. The element concentration is measured by X-ray photoelectron spectroscopy (XPS). XPS obtains the most surface composition information in the measured object. For example, an XPS device manufactured by ULVAC-PHI (product name "PHI X-tool") and its equivalent can be used. The positive electrode active material (powder) is set in the XPS device. A narrow scan analysis is performed using a pass energy of 224 eV. The measured data is processed using analytical software. For example, analytical software manufactured by ULVAC-PHI (product name "MulTiPak") and its equivalent can be used. The peak area (integral value) of the Li1s spectrum is converted into the element concentration (C Li ). The peak area of the P2p spectrum is converted into the element concentration of P (C P ). The peak area of the B1s spectrum is converted into the element concentration of B (CB ). The peak area of the Na1s spectrum is converted into the element concentration of Na (C Na ).
[0035] The "coverage rate" is a value measured by the following procedure. The XPS data obtained above are analyzed to determine the element concentration from the peak areas of C1s, O1s, B1s, P2p, M2p3, etc. The coverage rate is determined by the following formula (5).
[0036] θ=(P+B) / (P+B+M) (5)
[0037] In the above formula (5), θ represents the coverage. The coverage is expressed as a percentage (%). P, B, and M represent the element concentration of each element. M represents the element concentration of the constituent elements of the active material particles (however, excluding Li and O). M may include, for example, at least one selected from Ni, Co, Mn, and Al. For example, the active material particles are "LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O 2 ”, the right side of the above formula (5) can be transformed into “(P+B) / (P+B+Ni+Co+Mn)”. For example, when the active material particles are “LiNi 0.8 Co 0.15 Al 0.05 O 2 ", the right side of the above formula (5) can be transformed into "(P+B) / (P+B+Ni+Co+Al)".
[0038] Unless otherwise specified, a numerical range such as "m to n%" includes an upper limit and a lower limit. That is, "m to n%" means a numerical range of "m% or more and n% or less". In addition, "m% or more and n% or less" includes "more than m% and less than n%".
[0039] <Positive electrode active material>
[0040] The positive electrode active material may be composed of one particle. The positive electrode active material may contain two or more particles. That is, the positive electrode active material may be a powder (an aggregate of particles). The positive electrode active material may have a D50 of, for example, 1 to 30 μm, 10 to 20 μm, or 1 to 10 μm. "D50" represents the particle size that accumulates to 50% in the volume-based particle size distribution (cumulative distribution). The particle size distribution can be measured by laser diffraction.
[0041] Figure 1 : is a conceptual diagram of the positive electrode active material in this embodiment. The positive electrode active material 5 includes composite particles. The composite particles have a core-shell structure. That is, the positive electrode active material 5 includes active material particles 1 and a coating film 2. The positive electrode active material 5 can be referred to as a "coated active material" or the like.
[0042] <Coating>
[0043] The coating 2 is a shell of the positive electrode active material 5. The coating 2 covers at least a portion of the surface of the active material particle 1 (core). The coverage rate may be, for example, 93% or more. The coverage rate may be, for example, 94% or more, 95% or more, 96% or more, or 97% or more. The coverage rate may be, for example, 100% or less, 97% or less, 96% or less, or 95% or less.
[0044] The thickness of the coating film 2 can be, for example, 5 to 100 nm, 5 to 50 nm, 10 to 30 nm, or 20 to 30 nm. The thickness of the coating film 2 can be measured, for example, by cross-sectional observation of the composite particles. Cross-sectional observation can be performed, for example, using a SEM (Scanning Electron Microscope).
[0045] The coating 2 contains P, B and O as essential components. P, B and O can form oxide glass. The oxide glass can contain a glass network structure. Through the coexistence of P and B, it is expected that the mixed anion effect will be manifested. The oxide glass can contain, for example, a phosphate skeleton and a boric acid skeleton. For example, the TOF-SIMS (Time-of-Flight Secondary Ion Mass Spectrometry) spectrum of the positive electrode active material 5 can contain ions from phosphate ions (such as PO 2 - ,PO 3 - The fragment peaks from borate ions (such as BO 2 - , BO 3 - Fragment peaks of
[0046] The coating film 2 contains Li as an optional component. Li may also be an essential component. In the present embodiment, the relationship of the following formula (1) is satisfied.
[0047] C Li / (C P +C B )≤1.50 (1)
[0048] By satisfying the relationship of the above formula (1), it is expected that the battery resistance will be reduced. In addition, it is considered that the origin of Li in the coating film 2 is two or more. For example, the coating film 2 may contain Li from the lithium compound contained in the coating liquid. For example, the coating film 2 may contain Li diffused from the active material particles 1 when the coating film 2 is formed.
[0049] For example, the relationship of the following formula (3) may be satisfied.
[0050] CLi / (C P +C B )≤1.27 (3)
[0051] The Li composition ratio may be, for example, 1.11 or less, 1.01 or less, 1.00 or less, 0.89 or less, 0.82 or less, or 0.5 or less. The Li composition ratio may be, for example, 0.5 or more, 0.82 or more, 0.89 or more, 1.00 or more, 1.01 or more, 1.11 or more, or 1.27 or more.
[0052] As long as the relationship of the above formula (1) is satisfied, the relationship between the quantities of P and B is arbitrary. For example, "C P / C B =99 / 1~1 / 99", "C P / C B =9 / 1~1 / 9" or "C P / C B =7 / 3~3 / 7”. For example, it can satisfy “1≤C P / C B ” or “2≤C P / C B "And so on.
[0053] The coating film 2 further contains Na as an optional component. Na may also be an essential component. In this embodiment, the relationship of the following formula (2) is satisfied.
[0054] C Na / (C P +C B )≤1.34 (2)
[0055] If the Na composition ratio exceeds 1.34, for example, there may be disadvantages such as an increase in battery resistance. The Na composition ratio may be, for example, 0.84 or less, 0.61 or less, 0.43 or less, 0.37 or less, 0.27 or less, 0.24 or less, or 0.05 or less.
[0056] For example, the relationship of the following formula (4) may be satisfied.
[0057] 0.24≤C Na / (C P +C B ) (4)
[0058] The Na composition ratio may be, for example, 0.05 or more, 0.27 or more, 0.37 or more, 0.43 or more, 0.61 or more, or 0.84 or more.
[0059] <Active material particles>
[0060] The active material particle 1 is the core of the positive electrode active material 5. The active material particle 1 may have a D50 of, for example, 1 to 30 μm, 10 to 20 μm, or 1 to 10 μm. The active material particle 1 may reversibly accommodate Li ions. The active material particle 1 may have any crystal structure. The active material particle 1 may include, for example, a layered rock salt structure.
[0061] The active material particles 1 may have any composition. For example, the active material particles 1 may have a composition represented by the following formula (6).
[0062] Li 1-a Ni x M 1-x O 2 (6)
[0063] In the above formula (6), the relationship of -0.5≤a≤0.5 and 0<x<1 is satisfied. M is at least one selected from Co, Mn and Al. For example, the relationship of 0.5≤x<1 or 0.6≤x≤0.9 can be satisfied.
[0064] A dopant may be added to the active material particles 1. The dopant may diffuse throughout the particles or may be locally distributed. For example, the dopant may be localized on the surface of the particles. The dopant may be a substitutional solid solution atom or an intrusive solid solution atom. The amount of dopant added (molar fraction relative to the total amount of the active material particles 1) may be, for example, 0.01 to 5%, 0.1 to 3%, or 0.1 to 1%. The dopant may include, for example, at least one selected from B, C, N, halogen, Si, Na, Mg, Al, Mn, Co, Cr, Sc, Ti, V, Cu, Zn, Ga, Ge, Se, Sr, Y, Zr, Nb, Mo, In, Pb, Bi, Sb, Sn, W, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, and actinide elements.
[0065] <Method for producing positive electrode active material>
[0066] Figure 2 : is a schematic flow chart of the method for producing the positive electrode active material in the present embodiment. Hereinafter, the "method for producing the positive electrode active material in the present embodiment" may be referred to as "the present production method". The present production method includes "(a) preparation of a mixture" and "(b) drying". The present production method may further include, for example, "(c) heat treatment" and the like.
[0067] <(a) Preparation of mixture>
[0068] The present manufacturing method includes preparing a mixture by mixing a coating liquid and active material particles 1. The details of the active material particles 1 are as described above. The mixture may be, for example, a suspension or a wet powder. For example, a suspension may be formed by dispersing active material particles 1 (powder) in a coating liquid. For example, a wet powder may be formed by spraying a coating liquid in a powder. In the present manufacturing method, any mixing device, granulating device, etc. may be used.
[0069] The coating liquid contains a solute and a solvent. The coating liquid may further contain suspended matter (insoluble components), precipitates, etc. As for the solvent, any component may be contained as long as it can dissolve the solute. The solvent may contain water, alcohol, etc. The solvent may contain ion exchange water, methanol, ethanol, etc.
[0070] The solute contains the raw material of the coating 2. The amount of the solute can be, for example, 0.1 to 20 parts by mass relative to 100 parts by mass of the solvent. The solute contains a phosphate compound and a boric acid compound as essential components. The phosphate compound is a P source of the coating 2. The boric acid compound is a B source of the coating 2. The solute contains a lithium compound, a Na salt, and NH 4 At least one of the salts can be used as an optional component. For example, the solute can include phosphoric acid and boric acid. For example, the solute can include phosphoric acid and boric acid, and in addition to these, it can further include sodium phosphate, sodium borate, NH phosphate, 4 Salt, boric acid NH 4 Phosphate sodium salts and the like may also function as excipients, etc. In the solute, all or part of the phosphate compound and the boric acid compound may form Na salts, NH 4 Salt, etc. By replacing all or part of the raw materials with Na salts, etc., it is expected that the cost of raw materials will be reduced. For example, a mixture of metaphosphoric acid and Na orthophosphate can be used. For example, in condensed phosphoric acid (metaphosphoric acid, etc.), all or part of the phosphate groups can form Na salts, etc. Phosphoric acid compounds, for example, may include orthophosphoric acid, etc. By using a phosphate compound with a low degree of polymerization, it is expected that the cost of raw materials will be reduced. Solutes, for example, may include orthophosphoric acid, polyphosphoric acid, metaphosphoric acid, Na orthophosphate, Na polyphosphate, Na metaphosphate, Na hexametaphosphate, 2Na phosphate, 3Na phosphate, boric acid, Na metaborate, and NH boric acid. 4 At least one of Na salt and NH 4 The salt may be, for example, a hydrate.
[0071] The solute may contain a lithium compound as long as the Li composition ratio in the positive electrode active material 5 can be 1.5 or less. The lithium compound may contain, for example, lithium hydroxide, lithium nitrate, lithium carbonate, or the like.
[0072] <(b) Drying>
[0073] The present manufacturing method includes manufacturing a positive electrode active material 5 by drying the mixture. The coating film 2 is formed by drying the coating liquid attached to the surface of the active material particle 1. In the present manufacturing method, any drying method can be used. For example, the mixture can be dried using a spray dryer. That is, droplets are formed by spraying the suspension from a nozzle. The droplets contain the active material particles 1 and the coating liquid. For example, by using hot air, the droplets are dried to form the positive electrode active material 5. By using the spray drying method, for example, it is expected that the coverage rate will be improved.
[0074] For example, the positive electrode active material 5 can be produced by using a tumbling fluidized bed coating apparatus. In the tumbling fluidized bed coating apparatus, "(a) preparation of the mixture" and "(b) drying" can be performed substantially simultaneously.
[0075] <(c) Heat treatment>
[0076] The present manufacturing method may include subjecting the positive electrode active material 5 to heat treatment. The coating 2 may be fixed by heat treatment. Heat treatment may also be referred to as "firing". In the present manufacturing method, any heat treatment device may be used. The treatment temperature may be, for example, 150 to 300° C. The treatment time may be, for example, 1 to 10 hours. The heat treatment atmosphere may be, for example, an air atmosphere or an inert atmosphere.
[0077] <All-solid-state battery>
[0078] Figure 3 This is a conceptual diagram of an all-solid-state battery in this embodiment. The battery 100 may have any shape. For example, the battery 100 may have a plate-like shape. The battery 100 includes a power generation element 50. The battery 100 may include an outer package (not shown). The outer package may accommodate the power generation element 50. The outer package may be, for example, a bag made of an Al laminated film. The power generation element 50 includes a positive electrode 10 and a negative electrode 20. The power generation element 50 may further include a separator layer 30. The separator layer 30 is arranged between the positive electrode 10 and the negative electrode 20. The power generation element 50 may have any form. For example, the power generation element 50 may have either a monopolar structure or a bipolar structure.
[0079] The positive electrode 10 may include, for example, a positive electrode current collector and a positive electrode active material layer. The positive electrode current collector may include, for example, Al foil or the like. The positive electrode active material layer is disposed on the surface of the positive electrode current collector. The positive electrode active material layer includes a positive electrode active material and a sulfide solid electrolyte. The details of the positive electrode active material are as described above.
[0080] The amount of the sulfide solid electrolyte may be, for example, 1 to 200 parts by volume relative to 100 parts by volume of the positive electrode active material. The sulfide solid electrolyte may be, for example, glass ceramic or argyrodite. The sulfide solid electrolyte may include, for example, a LiI-LiBr-Li 3 PS4 , Li 2 S-SiS 2 、LiI-Li 2 S-SiS 2 、LiI-Li 2 SP 2 S 5 、LiI-Li 2 O-Li 2 SP 2 S 5 、LiI-Li 2 SP 2 O 5 、LiI-Li 3 PO 4 -P 2 S 5 , Li 2 S-GeS 2 -P 2 S 5 , Li 2 SP 2 S 5 , Li 10 G 2 S 12 , Li 4 P 2 S 6 , Li 7 P 3 S 11 , Li 3 PS 4 , Li 7 PS 6 , and Li 6 PS 5 At least one of X (X=Cl, Br, I).
[0081] For example, "LiI-LiBr-Li 3 PS 4 " means that by mixing LiI, LiBr and Li 3 PS 4 Sulfide solid electrolytes are produced by mixing in any molar ratio. For example, sulfide solid electrolytes can be produced by mechanochemical methods. By marking numbers before each raw material, the mixing ratio can be limited. For example, "10LiI-15LiBr-75Li 3 PS 4 " indicates that the mixing ratio of the raw materials is "LiI / LiBr / Li 3 PS 4 =10 / 15 / 75 (molar ratio)".
[0082] The positive electrode active material layer may further include a conductive material and a binder, for example. The amount of the conductive material and the binder may be, for example, 0.1 to 10 parts by mass, respectively, independently relative to 100 parts by mass of the positive electrode active material. The conductive material may include, for example, acetylene black, vapor grown carbon fiber (VGCF), etc. The binder may include, for example, polyvinylidene fluoride (PVDF), styrene butadiene rubber (SBR), etc.
[0083] Example
[0084] <Sample>
[0085] Figure 4 TABLE 1 is a table showing the experimental results. Positive electrode active materials and all-solid batteries according to No. 1 to No. 14 were produced as follows.
[0086] No.1
[0087] A coating liquid was prepared by dissolving 10.8 parts by mass of orthophosphoric acid (content 85%, manufactured by KISHIDA Chemical Co., Ltd.) in 166 parts by mass of ion-exchanged water.
[0088] By mixing 50 parts by mass of active material particles (LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O 2 ) was dispersed in 53.7 parts by mass of the coating liquid to prepare a suspension. The suspension was supplied to a spray dryer (product name "Mini Spray Dryer B-290", manufactured by BUCHI) to produce a positive electrode active material. The air supply temperature of the spray dryer was 200°C, and the air supply volume was 0.45 m 3 / min. The positive electrode active material was heat treated in air at a temperature of 200°C.
[0089] By combining the positive electrode active material, sulfide solid electrolyte (10LiI-15LiBr-75Li 3 PS 4 ), a conductive material (VGCF), a binder (SBR) and a dispersion medium (heptane) are mixed to prepare a positive electrode slurry. The mixing ratio of the positive electrode active material and the sulfide solid electrolyte is "positive electrode active material / sulfide solid electrolyte = 6 / 4 (volume ratio)". The amount of the conductive material and the binder is 3 parts by mass, respectively, relative to 100 parts by mass of the positive electrode active material. The positive electrode slurry is fully stirred using an ultrasonic homogenizer. A coating is formed by applying the positive electrode slurry to the surface of the positive electrode collector (Al foil). The coating is dried at 100°C for 30 minutes using a hot plate. A positive electrode raw sheet is thus manufactured. A disc-shaped positive electrode is cut out from the positive electrode raw sheet. The area of the positive electrode is 1cm 2.
[0090] A negative electrode and a separator layer are prepared. The negative electrode active material is graphite. The same type of sulfide solid electrolyte is used between the positive electrode, the separator layer and the negative electrode. In a cylindrical fixture, the positive electrode, the separator layer and the negative electrode are stacked in sequence to form a laminate. The laminate is pressed to form a power generation element. A fully solid battery is manufactured by connecting terminals to the power generation element.
[0091] No.2
[0092] A positive electrode active material and an all-solid-state battery were produced in the same manner as in No. 1 except that polyphosphoric acid (product name "polyphosphoric acid-116T", manufactured by Nippon Chemical Industry Co., Ltd.) was used instead of orthophosphoric acid.
[0093] No.3、No.4
[0094] The coating solution is prepared by dissolving 10.8 parts by mass of metaphosphoric acid (containing Na) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) in 166 parts by mass of ion exchange water. In addition, the positive electrode active materials and all-solid-state batteries involved in No. 3 and No. 4 are manufactured in the same manner as No. 1. In addition, "metaphosphoric acid (containing Na)" means a mixture of metaphosphoric acid and sodium metaphosphate (excipient). The molar ratio "Na / P" in metaphosphoric acid (containing Na) is 0.5. The molar ratio "Na / P" represents the ratio of the amount of Na to the amount of P.
[0095] No.5
[0096] A solution is formed by dissolving 10.8 parts by mass of orthophosphoric acid (content 85%, manufactured by KISHIDA Chemical Co., Ltd.) in 166 parts by mass of ion exchange water. Boric acid (manufactured by NACALAI TESQUE Co., Ltd.) is then dissolved in the solution in such a manner that the molar ratio "P / B" becomes 1.0, thereby preparing a coating solution. Otherwise, a positive electrode active material and an all-solid-state battery are manufactured in the same manner as in No. 1. The molar ratio "P / B" represents the ratio of the amount of P to the amount of B.
[0097] No.6
[0098] A positive electrode active material and an all-solid-state battery were produced in the same manner as in No. 5 except that polyphosphoric acid (product name "polyphosphoric acid-116T", manufactured by Nippon Chemical Industry Co., Ltd.) was used instead of orthophosphoric acid.
[0099] No.7
[0100] A positive electrode active material and an all-solid-state battery were produced in the same manner as in No. 5, except that metaphosphoric acid (containing Na) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used instead of orthophosphoric acid.
[0101] No.8
[0102] A positive electrode active material and an all-solid-state battery were produced in the same manner as in No. 5, except that sodium hexametaphosphate (manufactured by Yoneyama Chemical Industry Co., Ltd.) was used instead of orthophosphoric acid.
[0103] No.9
[0104] A positive electrode active material and an all-solid-state battery were produced in the same manner as in No. 5, except that sodium metaphosphate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used instead of orthophosphoric acid.
[0105] No.10
[0106] A positive electrode active material and an all-solid-state battery were produced in the same manner as in No. 5 except that sodium metaborate (manufactured by Yoneyama Chemical Industry Co., Ltd.) was used instead of boric acid.
[0107] No.11
[0108] A positive electrode active material and an all-solid-state battery were produced in the same manner as in No. 5, except that ammonium borate (manufactured by Yoneyama Chemical Industry Co., Ltd.) was used instead of boric acid.
[0109] No.12
[0110] A positive electrode active material and an all-solid-state battery were produced in the same manner as in No. 5 except that disodium hydrogen phosphate 12 hydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used instead of orthophosphoric acid. The molar ratio "Na / P" in disodium hydrogen phosphate 12 hydrate was 2.0.
[0111] No.13
[0112] A positive electrode active material and an all-solid-state battery were produced in the same manner as in No. 5 except that sodium polyphosphate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used instead of orthophosphoric acid. The molar ratio "Na / P" in the sodium polyphosphate was 1.0.
[0113] No.14
[0114] A positive electrode active material and an all-solid-state battery were produced in the same manner as in No. 5 except that trisodium phosphate 12 hydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used instead of orthophosphoric acid. The molar ratio "Na / P" in trisodium phosphate 12 hydrate was 3.0.
[0115] <Evaluation>
[0116] The XPS device was used to measure the Li composition ratio, Na composition ratio and coverage in each positive electrode active material. The resistance was measured in each all-solid-state battery. The measurement results are shown in Figure 4 .
[0117] <Results>
[0118] In the Li composition ratio "C Li / (C P +C B )" is 1.5 or less, a tendency of significantly lowering battery resistance is found. Na / (C P +C B )" is 1.34 or less, a tendency is found that the battery resistance is stabilized at a low value (No. 5 to No. 13).
[0119] In the case where the coating film does not contain B, even if the Li composition ratio is 1.5 or less and the Na composition ratio is 1.34 or less, a tendency of high battery resistance is observed (No. 4).
[0120] When the coating film contained B and the Li composition ratio was 1.5 or less, and the Na composition ratio exceeded 1.34, a tendency was observed that the battery resistance increased (No. 14).
Claims
1. A positive electrode active material comprising active material particles and a coating film, wherein the coating film covers at least a portion of the surface of the active material particles, the coating film comprising P, B and O as essential components, and further comprising Li and Na as optional components, and satisfying the relationship between formula (1) and formula (2): C Li / (C P +C B ) ≤1.50 (1) C Na / (C P +C B ) ≤1.34 (2), In the formula (1) and the formula (2), C Li , C P , C B and C Na represent the element concentrations measured by X-ray photoelectron spectroscopy, C Li Represents the element concentration of lithium, C P Represents the elemental concentration of phosphorus, C B represents the element concentration of boron, and C Na Indicates the element concentration of sodium.
2. The positive electrode active material according to claim 1, in, The coating film contains Na as an essential component and satisfies the relationship between formula (3) and formula (4): C Li / (C P +C B )≤1.27 (3) 0.24≤C Na / (C P +C B ) (4)。 3. The positive electrode active material according to claim 1 or 2, in, The coating has a coverage of 94% or more, which is measured by X-ray photoelectron spectroscopy.
4. An all-solid-state battery comprising a positive electrode and a negative electrode, wherein the positive electrode comprises the positive electrode active material according to claim 1 or 2, and a sulfide solid electrolyte.
5. A method for producing a positive electrode active material, include: (a) preparing a mixture by mixing a coating liquid and active material particles, and (b) producing a positive electrode active material by drying the mixture, The coating liquid contains a solute and a solvent, wherein the solute contains a phosphoric acid compound and a boric acid compound as essential components and contains at least one selected from a lithium compound, a sodium salt, and an ammonium salt as an optional component.