Positive electrode active material, sodium ion battery, preparation method of sodium ion battery and electric equipment

CN118738347APending Publication Date: 2024-10-01SHENZHEN BAK POWER BATTERY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411002439.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Sodium-ion batteries show a problem of reduced electrochemical performance in low-temperature environments, affecting their application in extreme weather and different regions.

Method used

Polyanionic materials and Na4Fe3(PO4)2P2O7 are used as positive active materials, combined with natural graphite as negative active materials, and ether electrolyte is used. Through the preparation of composite materials and battery preparation methods, the low-temperature performance of sodium-ion batteries is improved.

Benefits of technology

It significantly improves the Na+ diffusion coefficient, energy density and cycle stability of sodium-ion batteries at low temperatures, ensuring that the battery still has excellent electrochemical performance below -40°C, broadens the operating temperature range, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738347A_ABST
    Figure CN118738347A_ABST
Patent Text Reader

Abstract

The invention provides a positive electrode active material, a sodium ion battery, a preparation method of the sodium ion battery and electric equipment, and relates to the technical field of secondary batteries. The positive electrode active material comprises a polyanion material and Na4Fe3 (PO4) 2P2O7, and the mass of the Na4Fe3 (PO4) 2P2O7 accounts for 40%-60% of the mass of the positive electrode active material. According to the invention, the polyanion material and the Na4Fe3 (PO4) 2P2O7 are compounded to serve as the positive electrode active material, and the two substances are matched with each other, so that the positive electrode active material has relatively high Na < + > diffusion coefficient, relatively high energy density and excellent cycling stability at low temperature, and the low-temperature use performance of the sodium ion battery is favorably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of secondary batteries, and in particular to a positive electrode active material, a sodium ion battery, a preparation method thereof, and an electrical device. Background Art

[0002] With the rapid growth in demand for electric two-wheeled vehicles, the demand for batteries, which are the core components of electric two-wheeled vehicles, has also risen. At present, rechargeable lithium-ion batteries (LIBs) are widely used in portable electronic devices and electric vehicles due to their long life and high energy density. However, the limited reserves of lithium have hindered the development of lithium-ion batteries, while sodium-ion batteries (SIBs) have attracted widespread attention due to the high abundance and ubiquitous distribution of sodium resources. Sodium-ion batteries have the characteristics of light weight, moderate specific energy, low cost, wide operating temperature range, and high safety, and have obvious application advantages in two-wheeled electric vehicles.

[0003] However, the electrochemical performance of sodium-ion batteries (including capacity, efficiency and energy / power density) deteriorates significantly when the temperature decreases. When the operating temperature drops below 0°C, the performance of the battery deteriorates.

[0004] The low temperature resistance of sodium ion batteries is crucial to meet the actual application needs in extreme weather and different regions (such as northern my country). However, the low temperature resistance of sodium ion batteries is currently poor, so it is necessary to improve it. Summary of the invention

[0005] The purpose of the present application is to provide a positive electrode active material, a sodium ion battery and a preparation method and an electrical device thereof to solve the above-mentioned problems.

[0006] To achieve the above objectives, this application adopts the following technical solutions:

[0007] A positive electrode active material comprises a polyanion material and Na4Fe3(PO4)2P2O7, wherein the mass of the Na4Fe3(PO4)2P2O7 accounts for 40%-60% of the mass of the positive electrode active material.

[0008] According to an embodiment of the present application, the polyanion material includes at least one of sodium iron phosphate and sodium iron pyrophosphate.

[0009] The present application also provides a sodium ion battery, comprising a positive electrode, a negative electrode and an electrolyte; the raw material for preparing the positive electrode comprises the positive electrode active material described above; the raw material for preparing the negative electrode comprises a negative electrode active material, and the negative electrode active material comprises natural graphite; the electrolyte comprises an ether electrolyte.

[0010] According to an embodiment of the present application, the ether electrolyte includes an electrolyte and a solvent; the electrolyte includes NaPF6, and the solvent includes DME, DG and TG;

[0011] And / or, in the ether electrolyte, the concentration of the electrolyte is 1 to 1.8 mol / L.

[0012] The present application also provides a method for preparing a sodium ion battery as described above, comprising: preparing a positive electrode slurry using a positive electrode active material, coating the positive electrode slurry on a first current collector to obtain a positive electrode; preparing a negative electrode slurry using a negative electrode active material, coating the negative electrode slurry on a second current collector to obtain a negative electrode; assembling the positive electrode, the negative electrode and an electrolyte to obtain the sodium ion battery.

[0013] According to an embodiment of the present application, preparing a positive electrode slurry using a positive electrode active material includes: mixing the positive electrode active material with a first binder, a first conductive agent, and a first solvent to obtain a positive electrode slurry;

[0014] The first binder includes polyvinylidene fluoride;

[0015] The first conductive agent includes at least one of carbon nanotubes, conductive carbon black, conductive graphite, graphene, and acetylene black;

[0016] The first solvent includes N-methylpyrrolidone.

[0017] According to an embodiment of the present application, the first current collector includes aluminum foil.

[0018] According to an embodiment of the present application, preparing negative electrode slurry using negative electrode active material includes: mixing the negative electrode active material with a second binder, a second conductive agent, and a second solvent to obtain negative electrode slurry;

[0019] The second binder includes at least one of styrene-butadiene rubber and carboxymethyl cellulose;

[0020] The second conductive agent includes at least one of carbon nanotubes, conductive carbon black, conductive graphite, graphene, and acetylene black.

[0021] According to an embodiment of the present application, the second current collector includes aluminum foil;

[0022] And / or, a positive electrode lug is welded on the positive electrode, and a negative electrode lug is welded on the negative electrode; the material of the positive electrode lug and the material of the negative electrode lug independently include aluminum, nickel or aluminum-nickel conversion.

[0023] The present application also provides an electrical device, which includes the sodium ion battery described above or includes a sodium ion battery prepared by the preparation method described above.

[0024] Compared with the prior art, the beneficial effects of this application include:

[0025] The present invention adopts a compound of polyanion materials and Na4Fe3(PO4)2P2O7 as the positive electrode active material. The two substances cooperate with each other to make the positive electrode active material have a high Na + The high diffusion coefficient, higher energy density and excellent cycle stability are beneficial to improving the low-temperature performance of sodium-ion batteries.

[0026] The present application also provides a sodium ion battery, which uses the above-mentioned positive electrode active material to enable the sodium ion battery to have excellent Na + diffusion coefficient and higher energy density; moreover, the sodium ion battery uses natural graphite as the negative electrode active material, and the natural graphite negative electrode has a solvent co-intercalation charge storage mechanism. Sodium ions can store charge without a desolvation process, which is beneficial to improve the low-temperature performance of the sodium ion battery. In addition, the sodium ion battery uses an ether electrolyte, which has a lower freezing point, can avoid the problem of electrolyte solidification at low temperatures, and can improve the low-temperature performance of the sodium ion battery. In general, the sodium ion battery of the present application has excellent low-temperature resistance, excellent cycle performance, and low production cost. The sodium ion battery of the present application has a wide operating temperature range, and even in a low temperature environment of -40°C, it still has excellent electrochemical performance and has significant market competitiveness.

[0027] The sodium ion battery prepared by the preparation method of the sodium ion battery of the present application still has excellent electrochemical performance under low temperature environment. In addition, the preparation method also has the advantages of simple operation and low production cost, which is conducive to large-scale promotion and application.

[0028] Electrical equipment using the sodium ion battery of the present application can be used at lower temperatures, broadening the operating temperature of existing electrical equipment. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope of the present application.

[0030] Figure 1 This is a scanning electron microscope image of the positive electrode sheet in Example 1. DETAILED DESCRIPTION

[0031] In order to better explain the technical solution provided by this application, before the embodiments, the technical solution is first described as a whole, as follows:

[0032] The present application provides a positive electrode active material, which includes a polyanion material and Na4Fe3(PO4)2P2O7, wherein the mass of the Na4Fe3(PO4)2P2O7 accounts for 40%-60% of the mass of the positive electrode active material.

[0033] Na4Fe3(PO4)2P2O7 as Fe 2+ The blended phosphate compound belongs to the orthorhombic system and has a space group of Pn21a. The FeO6 octahedra are connected by sharing edges or corners, and the PO4 tetrahedra are connected to these FeO6 octahedra, thus forming layered units along the axial plane. These layered units are connected in the horizontal direction through the P2O7 group to form a three-dimensional framework structure, which means that there are diffusion channels for sodium ions in the three directions of the three-dimensional space. This structure has 4 different sodium sites, which is conducive to the insertion and extraction of sodium ions and accelerates the Na + The dissolution process reduces the polarization degree of the electrode, so that the electrode can have a sufficiently large discharge capacity and can work at a lower temperature. In other words, the structural characteristics of Na4Fe3(PO4)2P2O7 are conducive to the diffusion of sodium ions. Polyanion materials have a 3D network structure, Na + Excellent diffusion path, still has high Na under low temperature conditions + The high diffusion rate and excellent cycle stability ensure that the battery can achieve fast reaction kinetics. In a low temperature environment, Na4Fe3(PO4)2P2O7 exhibits a better discharge voltage (about 3.2V) than polyanion materials. When charging and discharging, the Na +A solid solution reaction with local lattice deformation will occur during the process of extraction or embedding. The volume change in this process is small, which helps to maintain the stability of its crystal structure. When the mass of Na4Fe3(PO4)2P2O7 accounts for 40%-60% of the mass of the positive electrode active material, the positive electrode can have excellent electrochemical properties. Specifically, the sodium ion battery can be stably operated at a low temperature of -40°C. If the content of added Na4Fe3(PO4)2P2O7 is too small, on the one hand, it cannot be guaranteed that the prepared sodium ion battery can operate at -40°C, and on the other hand, the battery cost will increase. If the content of added Na4Fe3(PO4)2P2O7 is too much, the energy density of the sodium ion battery will be low, because the theoretical specific capacity of Na4Fe3(PO4)2P2O7 is lower than the theoretical specific capacity of polyanion materials. For example, the theoretical specific capacity of Na4Fe3(PO4)2P2O7 is 129mAh / g, while the theoretical specific capacity of the polyanion material sodium iron phosphate is 154mAh / g. In addition, the structural stability of polyanion materials avoids safety issues such as overcharge and overdischarge. If the content of Na4Fe3(PO4)2P2O7 is too high, the content of polyanion materials will be relatively reduced, which may cause battery safety and other related problems. In general, the positive electrode active material of the present application has high Na at low temperature. + The high diffusion coefficient, higher energy density and excellent cycle stability are beneficial to improving the low-temperature performance of sodium-ion batteries.

[0034] Exemplarily, the mass of the Na4Fe3(PO4)2P2O7 accounts for 40%, 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49%, 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59% or 60% of the mass of the positive electrode active material.

[0035] According to an embodiment of the present application, the polyanion material includes at least one of sodium iron phosphate (NaFePO4) and sodium iron pyrophosphate (Na8Fe4(P2O7)5). When the above polyanion material is mixed with Na4Fe3(PO4)2P2O7, the framework structure of the phosphate and pyrophosphate ions can exist stably and form a sodium ion compound, which is beneficial to improving the performance of the sodium ion battery at low temperatures. Moreover, the cost of the above polyanion material is relatively low, which is beneficial to reducing the production cost of sodium ion batteries and improving market competitiveness.

[0036] The present application also provides a sodium ion battery, comprising a positive electrode, a negative electrode and an electrolyte; the raw materials for preparing the positive electrode include the positive electrode active material described above; the raw materials for preparing the negative electrode include the negative electrode active material, and the negative electrode active material includes natural graphite; the electrolyte includes an ether electrolyte.

[0037] The raw materials for preparing the positive electrode in the sodium ion battery include the positive electrode active materials mentioned above, which is conducive to the sodium ion battery having excellent Na + Diffusion rate. The raw materials for forming the negative electrode include natural graphite, Na + and solvent molecules can be co-intercalated into natural graphite, which not only enables fast reaction kinetics but also shows the potential for low-temperature operation. + During storage, the average discharge platform of natural graphite anode is relative to Na / Na + About 0.6V, which can effectively avoid the risk of Na plating layer increased by battery polarization under low temperature conditions. In addition, natural graphite has excellent thermal stability and is more suitable for low-temperature sodium-ion batteries than conventional negative electrode active materials (such as hard carbon). In addition, the solidification of electrolytes with high freezing points at low temperatures limits the low-temperature performance of the battery. In order to improve this technical problem, the present application adopts ether electrolytes. Since ether electrolytes have lower freezing points and higher electrical conductivity than other types of electrolytes (such as ester electrolytes), they are beneficial to improving the low-temperature operation performance of sodium-ion batteries.

[0038] According to an embodiment of the present application, the ether electrolyte includes an electrolyte and a solvent; the electrolyte includes NaPF6, and the solvent includes DME, DG and TG; thereby, an efficient and stable ion conduction environment can be provided for the sodium ion battery, thereby ensuring the high performance and long life of the sodium ion battery.

[0039] Furthermore, the mass ratio of DME to DG and TG is 4:2:1.

[0040] And / or, in the ether electrolyte, the concentration of the electrolyte is 1 to 1.8 mol / L, for example, the concentration of the electrolyte can be 1 mol / L, 1.1 mol / L, 1.2 mol / L, 1.3 mol / L, 1.4 mol / L, 1.5 mol / L, 1.6 mol / L, 1.7 mol / L, 1.8 mol / L. Within the above concentration range, the ether electrolyte can provide a moderate ion mobility, which is beneficial to the rapid transmission of sodium ions in the electrolyte, thereby improving the charge and discharge efficiency and power density of the battery.

[0041] In addition to the positive electrode, the negative electrode and the electrolyte, the sodium ion battery may also include the necessary structures in the conventional sodium ion battery, for example, the sodium ion battery may also include a separator and a steel shell.

[0042] The present application also provides a method for preparing a sodium ion battery as described above, comprising: preparing a positive electrode slurry using a positive electrode active material, coating the positive electrode slurry on a first current collector to obtain a positive electrode; preparing a negative electrode slurry using a negative electrode active material, coating the negative electrode slurry on a second current collector to obtain a negative electrode; assembling the positive electrode, the negative electrode and the electrolyte to obtain a sodium ion battery.

[0043] The sodium ion battery prepared by the preparation method has excellent electrochemical performance under low temperature environment. In addition, the preparation method has the advantages of simple operation and low production cost, which is conducive to large-scale promotion and application.

[0044] According to an embodiment of the present application, preparing a positive electrode slurry using a positive electrode active material includes: mixing the positive electrode active material with a first binder, a first conductive agent, and a first solvent to obtain a positive electrode slurry;

[0045] The first binder includes polyvinylidene fluoride (PVDF);

[0046] The first conductive agent includes at least one of carbon nanotubes, conductive carbon black, conductive graphite, graphene, and acetylene black;

[0047] The first solvent includes N-methylpyrrolidone.

[0048] For example, the mass ratio of the positive electrode active material to the first binder and the first conductive agent may be 96.5:2.5:3.5, the first conductive agent may include conductive carbon black and carbon nanotubes, and the mass ratio of conductive carbon black to carbon nanotubes may be 2:1.5. The solid content of the positive electrode slurry is between 50% and 60%.

[0049] According to an embodiment of the present application, the first current collector includes aluminum foil. Further, the aluminum foil includes at least one of carbon-coated aluminum foil, corona aluminum foil, and ordinary aluminum foil.

[0050] Furthermore, after coating the positive electrode slurry on the first current collector, the preparation method further comprises: drying, rolling, and slitting to obtain a positive electrode.

[0051] According to an embodiment of the present application, preparing negative electrode slurry using negative electrode active material includes: mixing the negative electrode active material with a second binder, a second conductive agent, and a second solvent to obtain negative electrode slurry;

[0052] The second binder includes at least one of styrene-butadiene rubber (SBR) and carboxymethyl cellulose (CMC);

[0053] The second conductive agent includes at least one of carbon nanotubes, conductive carbon black, conductive graphite, graphene, and acetylene black.

[0054] Furthermore, the second solvent includes water.

[0055] Illustratively, the mass ratio of the negative electrode active material to the second binder, the second conductive agent, and the second solvent is 94.5:5.755:4.55:110, the second binder may include styrene-butadiene rubber and carboxymethyl cellulose, and the mass ratio of styrene-butadiene rubber to carboxymethyl cellulose is 4.2:1.555, and the second conductive agent may include conductive carbon black and carbon nanotubes, and the mass ratio of conductive carbon black to carbon nanotubes is 1.55:3.

[0056] Furthermore, the solid content of the negative electrode slurry is between 40% and 45%.

[0057] According to an embodiment of the present application, the second current collector includes aluminum foil;

[0058] Furthermore, after coating the negative electrode slurry on the second current collector, the preparation method further comprises: drying, rolling, and cutting to obtain a negative electrode;

[0059] And / or, a positive electrode ear is welded on the positive electrode, and a negative electrode ear is welded on the negative electrode; the material of the positive electrode ear and the material of the negative electrode ear independently include aluminum, nickel or aluminum-nickel. The positive electrode ear is connected to the positive electrode, and the negative electrode ear is connected to the negative electrode, which can ensure the smooth flow of electric energy during the charging and discharging process of the battery.

[0060] The present application also provides an electrical device, which includes the sodium ion battery described above or includes a sodium ion battery prepared by the preparation method described above.

[0061] The electrical equipment of this application includes consumer electronics, electric vehicles, portable power supplies and outdoor equipment, medical equipment, industrial equipment, etc. For example, consumer electronics include smart phones, laptops, tablets, wearable devices, etc. Electric vehicles include electric bicycles, electric cars, electric ships, and drones. Portable power supplies and outdoor equipment include mobile power supplies, camping lights, outdoor adventure equipment, etc. Medical equipment includes portable medical equipment, emergency medical equipment, etc. Industrial equipment includes industrial robots, remote monitoring systems, automatic guided vehicles, etc.

[0062] The embodiments of the present application will be described in detail below in conjunction with specific examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If specific conditions are not specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0063] Example 1

[0064] The following takes the cylindrical battery model 18650 (diameter ≤ 18mm, height ≤ 65mm) as an example.

[0065] The positive electrode active material of Example 1 includes sodium iron phosphate and Na4Fe3(PO4)2P2O7, and the mass of Na4Fe3(PO4)2P2O7 accounts for 50% of the mass of the positive electrode active material.

[0066] Preparation of positive electrode sheet: The positive electrode active material, binder PVDF, conductive carbon black, and carbon nanotubes are dispersed in N-methylpyrrolidone and mixed evenly to obtain positive electrode slurry, wherein the mass ratio of positive electrode active material to binder PVDF, conductive carbon black, and carbon nanotubes is 96.5:2.5:2:1.5. The solid content of the positive electrode slurry is between 50% and 60%, and the viscosity is between 2000 and 3000cp. The slurry to be coated is evenly coated on the positive electrode current collector, that is, aluminum foil, by a coating machine. The electrode sheet is dried, compacted by a roller press, and cut into four pieces by a slitting machine to obtain a positive electrode sheet.

[0067] Electron microscope image of the positive electrode Figure 1 As shown, it can be seen that the particles in the electron microscope image are evenly dispersed and there is no particle aggregation phenomenon, indicating that the two materials, sodium iron phosphate and Na4Fe3(PO4)2P2O7, can be evenly dispersed when mixed, indicating that the two materials have good compatibility in chemical and physical properties and can form a stable mixed system. Evenly dispersed positive electrode materials help improve the electrochemical performance of the electrode sheet.

[0068] Preparation of negative electrode sheet: The negative electrode sheet formula uses negative electrode active material natural graphite, binder SBR, conductive carbon black, carbon nanotubes, binder CMC and water. The mass ratio of natural graphite, SBR, conductive carbon black, carbon nanotubes, CMC and deionized water is 94.5:4.2:1.55:3:1.555:110. First, mix CMC, water and carbon nanotubes to make a glue solution (step 1). In addition, the negative electrode active material and conductive carbon black SP are mixed evenly by dry method (step 2), and the beaten glue solution is added to the mixed dry powder three times (step 2). Deionized water is added to adjust the viscosity of the slurry. Homogenize overnight, and add SBR the next day to prevent SBR from demulsifying if added too early, so that the slurry becomes jelly-like and is prepared into negative electrode slurry. The solid content of the negative electrode slurry is between 40% and 45%, and the viscosity is between 2000 and 2500cp. The slurry to be coated is evenly coated on the negative electrode collector, that is, the aluminum foil, by a coating machine. The electrode sheet is dried, compacted by a roller press, and cut into four by a slitting machine to obtain the negative electrode sheet.

[0069] Preparation of -40°C resistant sodium ion battery: The prepared positive electrode sheet and negative electrode sheet are welded to the pole ears and then wound together with the separator to obtain a battery core, which is packaged with a 18650 steel shell, spot welded, injected, pre-charged, aged, and divided into volumes to obtain a sodium ion battery; wherein, the electrolyte used in the preparation of the sodium ion battery in Example 1 is an ether electrolyte, the ether electrolyte includes an electrolyte and a solvent, the electrolyte is NaPF6, the solvent is a mixture of DME, DG, and TG, the mass ratio of DME to DG and TG is 4:2:1, and the concentration of the electrolyte in the ether electrolyte is 1.4 mol / L.

[0070] Example 2

[0071] A sodium ion battery was prepared by referring to the method of Example 1. The other steps were the same as those of Example 1, except that in the positive electrode active material of Example 2, the mass of Na4Fe3(PO4)2P2O7 accounted for 60% of the mass of the positive electrode active material.

[0072] Example 3

[0073] A sodium ion battery was prepared by referring to the method of Example 1. The other steps were the same as those of Example 1, except that in the positive electrode active material of Example 3, the mass of Na4Fe3(PO4)2P2O7 accounted for 40% of the mass of the positive electrode active material.

[0074] Example 4

[0075] A sodium ion battery was prepared by referring to the method of Example 1. The other steps were the same as those of Example 1, except that in Example 4, the positive electrode active materials were sodium iron pyrophosphate and Na4Fe3(PO4)2P2O7, and the mass of Na4Fe3(PO4)2P2O7 accounted for 50% of the mass of the positive electrode active materials.

[0076] Example 5

[0077] A sodium ion battery was prepared by referring to the method of Example 4, and the other steps were the same as those of Example 4, except that in Example 5, the mass of Na4Fe3(PO4)2P2O7 accounted for 60% of the mass of the positive electrode active material.

[0078] Example 6

[0079] A sodium ion battery was prepared by referring to the method of Example 4. The other steps were the same as those of Example 4, except that in Example 6, the mass of Na4Fe3(PO4)2P2O7 accounted for 40% of the mass of the positive electrode active material.

[0080] Comparative Example 1

[0081] A sodium ion battery was prepared by referring to the method of Example 1. The other steps were the same as those of Example 1, except that in Comparative Example 1, the mass of Na4Fe3(PO4)2P2O7 accounted for 20% of the mass of the positive electrode active material.

[0082] Comparative Example 2

[0083] A sodium ion battery was prepared by referring to the method of Example 1. The other steps were the same as those of Example 1, except that in Comparative Example 2, hard carbon was used as the negative electrode active material of the battery.

[0084] Comparative Example 3

[0085] A sodium ion battery was prepared by referring to the method of Example 1, and the other steps were the same as those of Example 1, except that: in Comparative Example 3, an ester electrolyte was used as the electrolyte in Comparative Example 3, the electrolyte was NaPF6, and the solvent of the electrolyte was a mixture of DMC, EMC, PC, and EC, wherein the mass ratio of DMC to EMC, PC, and EC was 1:1:1:2, and the concentration of the electrolyte was 1.4 mol / L.

[0086] Comparative Example 4

[0087] A sodium ion battery was prepared by referring to the method of Example 1. The other steps were the same as those of Example 1, except that: in Comparative Example 4, the active material of the positive electrode material was a layered O3 phase oxide material of Zhongkehai Sodium (model CFM002R) - sodium copper nickel iron manganese oxide (Na[Cu 1 / 9 Ni 2 / 9 Fe 1 / 3 Mn 1 / 3 ]O2).

[0088] Performance Testing

[0089] The sodium ion batteries of Examples 1-6 and Comparative Examples 1-4 were subjected to performance tests, and the test methods were as follows.

[0090] The sodium ion batteries of Examples 1-6 and Comparative Examples 1-4 were placed in an environment of -10°C, -20°C, and -40°C for low-rate current charge and discharge tests. The battery was first placed in a freezer at -10°C, -20°C, and -40°C for 3 hours, and then the following steps were tested. ①0.2C constant voltage charging to 3.7V, 0.01C cutoff, ② standing for 10min; ③0.2C discharge to 1.5V; ④ standing for 10min; ①-④ cycle test for 250 times, and record the capacity retention rate. The design capacity of the sodium ion battery is 1Ah. Among them, the low-rate current charge and discharge test method: the battery is in the voltage range of 1.5-3.7V, 0.2C charging, 0.2C discharge, and circulated ≥250 times at -40°C. The capacity retention rate ≥60% indicates that the test has passed. Each experimental group uses 16 batteries for parallel experiments. The consistency of the batteries used in the experiment is relatively good. The pass rate refers to the ratio of the number of batteries that passed the test to all the batteries participating in the test. The pass rates of Examples 1-6 and Comparative Examples 1-4 are shown in Table 1.

[0091] Table 1. Results of low rate current charge and discharge tests of Examples 1-6 and Comparative Examples 1-4

[0092] Experimental Group Low temperature cycle test Pass Rate Example 1 -40℃ 100% Example 2 -40℃ 94% Example 3 -40℃ 94% Example 4 -40℃ 100% Example 5 -40℃ 94% Example 6 -40℃ 94% Comparative Example 1 -40℃ 50% Comparative Example 2 -40℃ 13% Comparative Example 3 -40℃ 0 Comparative Example 4 -40℃ 31%

[0093] The pass rate of the cycle test of Examples 1-6 at -40°C is greater than that of Comparative Examples 1-4, indicating that when the positive electrode active material includes polyanion materials and Na4Fe3(PO4)2P2O7, and the mass of Na4Fe3(PO4)2P2O7 accounts for 40%-60% of the mass of the positive electrode active material, the negative electrode active material is natural graphite, and the electrolyte is an ether electrolyte, the sodium ion can have a longer service life at a low temperature of -40°C. Moreover, the pass rates of Examples 1 and 4 are greater than those of Examples 2, 3, 5, and 6, indicating that the mass of Na4Fe3(PO4)2P2O7 accounts for 50% of the mass of the positive electrode active material, and the sodium ion battery has a more excellent low-temperature cycle performance.

[0094] Table 1 discloses the statistical pass rates of 16 sets of parallel experimental tests, and Table 2 is the test data of one set of experiments.

[0095] Table 2 Cyclic test results of Examples 1-6 and Comparative Examples 1-4 at low temperature

[0096]

[0097]

[0098] It can be seen from Table 2 that Examples 1-6 can maintain a capacity retention rate of more than 60% after 250 cycles at -40°C, while Comparative Examples 1-4 have a capacity retention rate of 0 after 250 cycles at -40°C. In other words, the low-temperature performance of the sodium ion batteries of Examples 1-6 is better than that of Comparative Examples 1-4. The positive electrode active material of the present application uses a composite of a polyanion material and Na4Fe3(PO4)2P2O7, and the mass of Na4Fe3(PO4)2P2O7 accounts for 40%-60% of the mass of the positive electrode active material. The negative electrode active material uses natural graphite and an ether electrolyte, which can make the prepared sodium ion battery have excellent low-temperature resistance.

[0099] In addition, the batteries of Example 1 and Comparative Example 1 were disassembled after 5 cycles of low-temperature cycling. After disassembly, it can be seen that there is no sodium precipitation on the surface of the negative electrode sheet of Example 1. It can be preliminarily determined that the insertion and extraction of sodium ions are normal during the initial cycle of the battery of Example 1 at low temperature. There are dense white spots on the negative electrode sheet of Comparative Example 1, indicating that sodium precipitation is serious, which affects the later cycle of the battery. The negative electrode sheets of Examples 2-6 after 5 cycles of low-temperature cycling have similar conditions to those of Example 1, and the negative electrode sheets of Comparative Examples 2-3 after 5 cycles of low-temperature cycling have similar conditions to those of Comparative Example 1, indicating that the batteries of the embodiments have better electrochemical properties and cycle performance than the comparative examples.

[0100] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.

Claims

1. A positive electrode active material, characterized in that: The positive electrode active material comprises a polyanion material and Na4Fe3(PO4)2P2O7, and the mass of the Na4Fe3(PO4)2P2O7 accounts for 40%-60% of the mass of the positive electrode active material.

2. The positive electrode active material according to claim 1, characterized in that The polyanion material includes at least one of sodium iron phosphate and sodium iron pyrophosphate.

3. A sodium ion battery, characterized in that: including a positive electrode, a negative electrode and an electrolyte; The raw material for preparing the positive electrode includes the positive electrode active material according to claim 1 or 2; The raw material for preparing the negative electrode includes a negative electrode active material, and the negative electrode active material includes natural graphite; The electrolyte includes an ether electrolyte.

4. The sodium ion battery according to claim 3, characterized in that: The ether electrolyte includes an electrolyte and a solvent; the electrolyte includes NaPF6, and the solvent includes DME, DG and TG; And / or, in the ether electrolyte, the concentration of the electrolyte is 1 to 1.8 mol / L.

5. A method for preparing a sodium ion battery as claimed in claim 3 or 4, characterized in that: include: Prepare a positive electrode slurry using a positive electrode active material, and apply the positive electrode slurry on a first current collector to obtain a positive electrode; Prepare negative electrode slurry by using negative electrode active material, and apply the negative electrode slurry on the second current collector to obtain a negative electrode; The positive electrode, the negative electrode and the electrolyte are assembled to obtain the sodium ion battery.

6. The preparation method according to claim 5, characterized in that: The method of preparing positive electrode slurry by using positive electrode active material comprises: mixing the positive electrode active material with a first binder, a first conductive agent and a first solvent to obtain positive electrode slurry; The first binder includes polyvinylidene fluoride; The first conductive agent includes at least one of carbon nanotubes, conductive carbon black, conductive graphite, graphene, and acetylene black; The first solvent includes N-methylpyrrolidone.

7. The preparation method according to claim 6, characterized in that: The first current collector includes aluminum foil.

8. The preparation method according to claim 5, characterized in that: The method of preparing negative electrode slurry by using negative electrode active material includes: mixing the negative electrode active material with a second binder, a second conductive agent and a second solvent to obtain negative electrode slurry; The second binder includes at least one of styrene-butadiene rubber and carboxymethyl cellulose; The second conductive agent includes at least one of carbon nanotubes, conductive carbon black, conductive graphite, graphene, and acetylene black.

9. The preparation method according to claim 8, characterized in that: The second current collector comprises aluminum foil; And / or, a positive electrode lug is welded on the positive electrode, and a negative electrode lug is welded on the negative electrode; the material of the positive electrode lug and the material of the negative electrode lug independently include aluminum, nickel or aluminum-nickel conversion.

10. An electrical device, characterized in that: The electrical equipment includes the sodium ion battery according to claim 3 or 4, or includes a sodium ion battery prepared by the preparation method according to any one of claims 5-9.