Silicone composition and method for 3D printing based on photopolymerization

By using platinum complex-catalyzed silicone compositions to rapidly initiate and cure under short-wavelength UV, the problems of slow initiation speed and insufficient mechanical properties in the DLP method are solved, enabling efficient three-dimensional silicone elastomer part production and improving Improve manufacturing accuracy and mechanical performance.

CN118742597APending Publication Date: 2024-10-01BLUESTAR SILICONES (SHANGHAI) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180105438.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2021-12-31
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing photopolymerization-based 3D printing technologies, especially DLP and SLA methods, have slow initiation and curing speeds at wavelengths below 420nm, making it difficult to produce three-dimensional silicone elastomer parts with excellent mechanical properties and commercial raw materials. Limited and difficult to meet ideal mechanical performance requirements.

Method used

Using a photocurable silicone composition containing at least one organopolysiloxane compound, an organohydrogenpolysiloxane compound and a platinum complex catalyst, rapid initiation and curing by short-wavelength UV radiation (such as 365 or 405nm), Combined with multi-layer construction technology, manufacturing accuracy and mechanical performance are improved.

Benefits of technology

It achieves initiation and curing within seconds, improves the efficiency and manufacturing accuracy of the DLP method, obtains three-dimensional elastomer parts with excellent mechanical properties, and expands the types of raw materials available for photopolymerization-based 3D printing methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118742597A_ABST
    Figure CN118742597A_ABST
Patent Text Reader

Abstract

The present application relates to a method for producing a three-dimensional printed article, the method comprising: 1) providing a photocurable silicone composition, 2) exposing the photocurable silicone composition to actinic radiation to form a cured cross-section on a plate or a carrier or on an underlying layer, and 3) repeating steps 1) and 2) with a new layer on a previously cured cross-section to build the three-dimensional printed article, wherein the photocurable silicone composition is exposed to actinic radiation using UV radiation having a wavelength of less than 420 nm for less than 15 seconds. The invention also relates to a specific catalyst component C for the photocurable silicone composition, comprising (C-1) a ([eta]-cyclopentadienyl) tris ([sigma]-aliphatic)-platinum complex, (C-2) a thioxanthone compound having the following formula (II) and (C-3) a hydroxyl group-containing cycloaliphatic phenyl ketone having the following formula (III). And # imgabs0 # Ph-C (= O)-Cyc (III).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an organosilicon composition and a method for 3D printing a three-dimensional elastomeric organosilicon article based on photopolymerization. The elastomeric organosilicon article is constructed layer by layer by printing an organosilicon composition that can be crosslinked by a photocurable addition reaction with a 3D printer. Background of the Invention

[0003] 3D printing technology, also known as additive manufacturing (AM), can be used to prepare three-dimensional objects of complex geometry and almost any shape. Compared with molding or machining, it can obtain the target 3D object faster and using more commercially available raw materials at a low cost.

[0004] Additive manufacturing technology encompasses different techniques whose common feature is the automated additive buildup of layers of a molded part. Addition-crosslinking silicone compositions have been used in additive manufacturing processes to produce three-dimensional elastomeric silicone articles or parts.

[0005] Generally, silicone compositions can be crosslinked by addition polymerization. Direct ink writing methods have been used to print silicone compositions by extrusion technology. Silicone compositions can maintain their shape during layer-by-layer 3D printing. However, as the height of the printed object increases, it is difficult to maintain its shape. At the same time, the printing resolution and speed are still relatively low.

[0006] 3D printing technologies based on photopolymerization are now gaining more and more attention. They start with a liquid material and either deposit and solidify it locally or selectively solidify it from a liquid bath. Examples of such technologies are UV-stereolithography (SLA), UV-digital light processing (DLP), continuous liquid interface production (CLIP), UV-extrusion and inkjet deposition.

[0007] For example, UV stereolithography (SLA) is disclosed in WO2015197495. For example, UV stereolithography (SLA) uses a laser beam that is usually moved in an XY (horizontal) plane by a scanner system. A motor guided by information from a generated data source drives a mirror that sends the laser beam on a surface.

[0008] For example, UV-digital light processing (DLP) is disclosed in WO2016181149 and US20140131908. In UV-digital light processing (DLP), a 3D model is sent to a printer, and a barrel of liquid polymer is exposed to light from a DLP projector under safe light conditions. The DLP projector displays an image of the 3D model onto the liquid polymer. The DLP projector can be mounted below a window, which can be made of a transparent elastomeric film, through which the UV light from the DLP projector shines.

[0009] Continuous liquid interface production (CLIP, originally continuous liquid interphase printing) is disclosed, for example, in WO2014126837 and WO2016140891, which uses, for example, photopolymerization to produce smooth-sided solid objects of various shapes.

[0010] Since 3D photopolymerization is based on the use of liquid monomers / oligomers that can be cured / photopolymerized when exposed to a light source of a specific wavelength, photocurable silicone compositions have received great attention due to the many advantages of their cured materials, such as flexibility, insulating properties for electrical and electronic components, and good chemical resistance, temperature resistance, and weather resistance.

[0011] However, photocurable silicone compositions are a challenge because commercial raw materials are limited, such as polysiloxanes containing epoxides or acrylates, which are commonly used to obtain photocurable products but have poor mechanical properties. In addition, general DLP or SLA requires lower viscosity liquid silicone compositions, which cannot meet the ideal mechanical properties.

[0012] US Pat. No. 4,510,094 discloses an improved actinic radiation process which is carried out in the presence of a platinum complex having one cyclopentadienyl group η-bonded to the platinum atom and three aliphatic groups σ-bonded to the platinum atom.

[0013] However, for photopolymerization-based 3D printing methods such as DLP or SLA, these new Pt catalysts cannot fully initiate the polyaddition of silicone compositions at wavelengths shorter than 420 nm (such as 365 or 405 nm) based on commercial printers. Without good initiation quality and fast curing, it is difficult to carry out a smooth photopolymerization-based 3D printing method and obtain articles with satisfactory mechanical properties. In addition, there is still a need to develop photopolymerization-based 3D printing methods with more available raw materials. SUMMARY OF THE INVENTION

[0015] It is an object of the present invention to provide a method which allows time-efficient production of three-dimensional silicone elastomer parts manufactured by 3D printing based on photopolymerization.

[0016] Another object of the invention is to obtain 3D elastomeric parts with excellent manufacturing precision.

[0017] Another object of the present invention is to provide a method for manufacturing silicone elastomer objects by a 3D printing method based on photopolymerization, in particular a DLP method with faster initiation and curing, in particular at wavelengths below 420 nm, for example at 365 or 405 nm.

[0018] Another object of the present invention is to obtain 3D elastomeric parts having excellent mechanical properties.

[0019] Surprisingly, the technical solutions described below and in the independent claims can solve the above-mentioned objects. In particular, the silicone composition of the present invention is very suitable for 3D printing methods based on photopolymerization, especially DLP methods, which have faster initiation and curing. Initiation can occur within a few seconds (for example, less than 15 seconds) even at 405nm to meet the requirements of DLP printing. In addition, the silicone composition of the present invention is based on more available commercial raw materials, which are not limited to polysiloxanes containing epoxides or acrylates. Compared with conventional photocurable silicone materials through epoxides or acrylates, silicone elastomers prepared from the silicone composition of the present invention can exhibit excellent mechanical properties.

[0020] Embodiments of the invention

[0021] In a first aspect, the present invention relates to a method for producing a three-dimensional printed article, comprising:

[0022] 1) providing a photocurable silicone composition,

[0023] 2) exposing the photocurable silicone composition to actinic radiation to form a cured cross-section on a plate or carrier, and

[0024] 3) repeating steps 1) and 2) with new layers on the previously solidified cross section to build a three-dimensional printed article,

[0025] The curable silicone composition comprises:

[0026] (A) at least one organopolysiloxane compound A comprising, per molecule, at least two C2-C6 alkenyl groups bonded to silicon atoms,

[0027] (B) at least one organohydrogenpolysiloxane compound B comprising, per molecule, at least two hydrogen atoms bonded to the same or different silicon atoms, and

[0028] (C) a catalyst component C comprising a platinum complex; and

[0029] wherein the photocurable silicone composition is exposed to actinic radiation using UV radiation having a wavelength of less than 420 nm for less than 15 seconds.

[0030] In a second aspect, the present invention relates to a photocurable silicone composition comprising:

[0031] (A) at least one organopolysiloxane compound A comprising, per molecule, at least two C2-C6 alkenyl groups bonded to silicon atoms,

[0032] (B) at least one organohydrogenpolysiloxane compound B comprising, per molecule, at least two hydrogen atoms bonded to the same or different silicon atoms,

[0033] (C) a catalyst component C comprising

[0034] (C-1) (η-cyclopentadienyl)tri(σ-aliphatic)-platinum complex;

[0035] (C-2) Thioxanthone compounds having the following formula (II)

[0036]

[0037] wherein R represents a substituent at any position of the thioxanthone nucleus, which is selected from aliphatic groups having 1 to 18, preferably 2 to 12, more preferably 3 to 8 carbon atoms, preferably a linear or branched alkyl group;

[0038] n represents an integer of 1 to 8, preferably 1 to 4; and

[0039] (C-3) a hydroxyl-containing alicyclic phenyl ketone having the following formula (III):

[0040] Ph-C(=O)-Cyc(III)

[0041] wherein Ph represents a phenyl group which may be substituted or unsubstituted, and Cyc represents an alicyclic group having at least 3 carbon atoms and having at least one hydroxyl group.

[0042] The inventors believe that by selecting and modifying the platinum-containing catalyst component, faster initiation and curing can be achieved, especially at UV wavelengths below 420 nm, such as at 365 or 405 nm, and for example less than 15 seconds, while obtaining or maintaining excellent manufacturing precision and mechanical properties, which allows time-efficient photopolymerization-based 3D printing methods, especially DLP methods. In addition, more raw materials suitable for photopolymerization-based 3D printing methods can be obtained.

[0043] In this document, the term "layer" may relate to a layer at any stage of the process, the first layer or the preceding layer or the succeeding layer. The layers may have various dimensions, including thickness and width. The thickness of a layer may be uniform or may vary. The average thickness relates to the thickness of the layer immediately after printing. The cross-section of a layer may be of any shape.

[0044] In one embodiment, the layers independently have a thickness of 10 to 2000 μm, such as 50 to 1000 μm.

[0045] 3D Printing Public Content

[0046] 3D printing is often associated with a number of related technologies for manufacturing physical objects from computer-generated (eg, computer-aided design (CAD)) data sources.

[0047] "Additive Manufacturing (AM)" is defined as "the process of joining materials to make objects from 3D model data, typically layer by layer, as opposed to subtractive manufacturing methods. Synonyms associated with and covered by 3D printing include additive manufacturing, additive process, additive technology, additive layer manufacturing, layer manufacturing, and freeform manufacturing." Additive Manufacturing (AM) may also be referred to as Rapid Prototyping (RP). As used herein, "3D printing" is generally interchangeable with "additive manufacturing" and vice versa.

[0048] In the present invention, additive manufacturing processes refer in particular to photopolymerization-based 3D printing processes, which are based on the use of liquid monomers / oligomers that can be cured / photopolymerized when exposed to a light source of a specific wavelength.

[0049] In an advantageous embodiment, the method for producing three-dimensional printed articles is a 3D printing method based on photopolymerization, in particular a DLP method.

[0050] In an exemplary embodiment of a 3D printing method based on photopolymerization, such as a DLP method, the STL data of the 3D model is first imported into a dedicated 3D printing processing software for data preprocessing, thereby generating a specific format file containing 3D printing parameters, which is then imported into a 3D printer, and finally the article is printed layer by layer with the silicone composition according to the imported parameters. In printing, each layer with a certain cross section is printed on a layer on or below a plate or carrier, and is cured in a very short time by surface exposure, so the printing efficiency is very high.

[0051] During the printing process of the present invention, the operating parameters as required above are important to achieve fast and excellent initiation and curing. By selecting and modifying the platinum-containing catalyst component, preferably a catalyst component containing C-1 in combination with C-2 and C-3, the DLP process is allowed to be performed using the required short UV wavelength and curing time. In another preferred embodiment, the thickness of each printed layer can be in the range of 0.025mm-2mm, such as 0.030mm-1.0mm or 0.5mm. In some embodiments, the exposure intensity may be important, and for example it may be in the range of 1-100mW / cm 2 In the range of 3-80mW / cm 2 And most preferably 10-50mW / cm 2Preferably, the exposure time of the first layer printed may be in the range of 0.01 to 20 seconds, such as 0.05 to 10 or 3 seconds, and the exposure time of subsequent layers may be in the range of 0.1 to 10 seconds, such as 5 seconds. The UV wavelength used for exposure here is below 420nm, such as 365 or 405nm.

[0052] Optionally and if necessary, after photopolymerization-based 3D printing (such as DLP), the printed product can be subjected to a secondary curing or post-curing process by a UV curing box or an oven. In the post-curing process, the preferred wavelength of the UV curing box can be 405nm and the curing time can be 15s to 60s. The heating temperature of the oven can preferably be 80°C to 100°C, and the heating time is 0.01 to 4 hours.

[0053] Organopolysiloxane A

[0054] According to a particularly advantageous mode, the organopolysiloxane A comprising at least two C2-C6 alkenyl groups bonded to silicon atoms per molecule comprises:

[0055] (i) at least two siloxy units (A.1), which may be identical or different, having the following formula:

[0056]

[0057] in:

[0058] - a=1 or 2, b=0, 1 or 2 and a+b=1, 2 or 3;

[0059] - the symbol W, which may be identical or different, represents a straight chain or branched C2-C6 alkenyl group,

[0060] - and the symbols Z, which may be identical or different, represent a monovalent linear, branched or cyclic alkyl group containing from 1 to 30 carbon atoms, preferably from 1 to 8 carbon atoms, which alkyl group may be unsubstituted or substituted by one or more halogen atoms (such as fluorine, chlorine and bromine atoms) and / or by one or more aryl groups (such as phenyl), and even more preferably is chosen from the group consisting of methyl, ethyl, propyl, 3,3,3-trifluoropropyl,

[0061] (ii) and optionally at least one siloxy unit having the formula:

[0062]

[0063] in:

[0064] -c=0, 1, 2 or 3,

[0065] -Symbol Z 1, which may be identical or different, represent a monovalent linear, branched or cyclic alkyl group containing 1 to 30 carbon atoms, preferably 1 to 8 carbon atoms, which alkyl group may be unsubstituted or substituted by one or more halogen atoms (such as fluorine, chlorine and bromine atoms) and / or by one or more aryl groups (such as phenyl), and is even more preferably selected from the group consisting of methyl, ethyl, propyl, 3,3,3-trifluoropropyl.

[0066] Advantageously, Z and Z 1 is selected from the group formed by methyl, ethyl and propyl, and W is selected from the following list: vinyl, propenyl, 3-butenyl, 5-hexenyl, 9-decenyl, 10-undecenyl, 5,9-decadienyl and 6-11-dodecadienyl, and preferably, W is vinyl.

[0067] In a preferred embodiment, in formula (A.1) a=1 and a+b=2 or 3, and in formula (A.2) c=2 or 3.

[0068] These organopolysiloxanes A may have a linear, branched or cyclic structure.

[0069] When they are linear polymers, they consist essentially of siloxy units selected from W2SiO 2 / 2 、WZSiO 2 / 2 and Z 1 2SiO 2 / 2 The siloxy units "D" and the siloxy units W3SiO 1 / 2 、WZ2SiO 1 / 2 、W2ZSiO 1 / 2 and Z 1 3SiO 1 / 2 The symbols W, Z and Z 1 As mentioned above.

[0070] As examples of the terminal unit "M", there may be mentioned a trimethylsiloxy group, a dimethylvinylsiloxy group or a dimethylhexenylsiloxy group.

[0071] As examples of the unit "D", mention may be made of a dimethylsiloxy, methylvinylsiloxy, methylbutenylsiloxy, methylhexenylsiloxy, methyldecenylsiloxy or methyldecadienylsiloxy group.

[0072] The organopolysiloxane A may be an oil having a dynamic viscosity of about 1 to 10,000,000 mPa.s at 25°C, typically about 200 to 1,000,000 mPa.s at 25°C.

[0073] All viscosities considered in this description correspond to the magnitude of the “Newtonian” dynamic viscosity at 25° C., ie the dynamic viscosity measured in a manner known per se with a Brookfield viscometer at a sufficiently low shear rate gradient that the measured viscosity is independent of the rate gradient.

[0074] When they are cyclic organopolysiloxanes, they are formed from siloxy units "D" having the formula: W2SiO 2 / 2 , Z 1 2SiO 2 / 2 or WZSiO 2 / 2 , which may be of dialkylsiloxy, alkylvinylsiloxy or alkylsiloxy type. Examples of such siloxy units have been mentioned above. The cyclic organopolysiloxane A has a viscosity of about 1-5000 mPa.s at 25°C.

[0075] Organohydrogenpolysiloxane B

[0076] According to a preferred embodiment, the organohydrogenpolysiloxane compound B is an organopolysiloxane containing at least two hydrogen atoms per molecule bonded to the same or different silicon atoms, and preferably at least three hydrogen atoms per molecule directly bonded to the same or different silicon atoms.

[0077] Advantageously, the organohydrogenpolysiloxane compound B is an organopolysiloxane comprising:

[0078] (i) at least two and preferably at least three siloxy units having the formula:

[0079]

[0080] in:

[0081] - d = 1 or 2, e = 0, 1 or 2 and d + e = 1, 2 or 3,

[0082] -Symbol Z 3 , which may be identical or different, represent a monovalent linear, branched or cyclic alkyl group containing 1 to 30 carbon atoms, preferably 1 to 8 carbon atoms, which alkyl group may be unsubstituted or substituted by one or more halogen atoms (such as fluorine, chlorine and bromine atoms) and / or by one or more aryl groups (such as phenyl), and even more preferably is selected from the group consisting of methyl, ethyl, propyl, 3,3,3-trifluoropropyl, and

[0083] (ii) optionally at least one siloxy unit having the formula:

[0084]

[0085] in:

[0086] -c=0, 1, 2 or 3,

[0087] -Symbol Z 2 , which may be identical or different, represent a monovalent linear, branched or cyclic alkyl group containing 1 to 30 carbon atoms, preferably 1 to 8 carbon atoms, which alkyl group may be unsubstituted or substituted by one or more halogen atoms (such as fluorine, chlorine and bromine atoms) and / or by one or more aryl groups (such as phenyl), and is even more preferably selected from the group consisting of methyl, ethyl, propyl, 3,3,3-trifluoropropyl.

[0088] The organohydrogenpolysiloxane compound B may consist only of the siloxy units of formula (B.1) or may also contain units of formula (B.2). It may have a linear, branched or cyclic structure.

[0089] Examples of siloxy units of formula (B.1) are in particular the following units: H(CH3)2SiO 1 / 2 and HCH3SiO 2 / 2 .

[0090] When they are linear polymers, they are formed essentially from:

[0091] - siloxy units "D" selected from the group consisting of Z 2 2SiO 2 / 2 or Z 3 HSiO 2 / 2 units, and

[0092] - siloxy units "M" selected from the group consisting of Z 2 3SiO 1 / 2 or Z 3 2HSiO 1 / 2 unit.

[0093] These linear organopolysiloxanes may be oils having a dynamic viscosity of about 1 to 1,000,000 mPa.s at 25°C, typically about 10 to 500,000 mPa.s at 25°C or preferably about 15 to 10,000 or 5,000 mPa.s at 25°C, or gums having a molecular weight of about 1,000,000 mPa.s or more at 25°C.

[0094] When they are cyclic organopolysiloxanes, they are composed of compounds having the formula Z 2 2SiO 2 / 2 and Z 3 HSiO 2 / 2 The siloxy units "D" are formed, which can be dialkylsiloxy type or a single unit Z 3 HSiO 2 / 2They have a viscosity of about 1-5000 mPa.s.

[0095] Examples of the linear organohydrogenpolysiloxane compound B are: dimethylpolysiloxane with hydrodimethylsilyl terminal groups, dimethylhydrogenmethylpolysiloxane with trimethylsilyl terminal groups, dimethylhydrogenmethylpolysiloxane with hydrodimethylsilyl terminal groups, hydromethylpolysiloxane with trimethylsilyl terminal groups and cyclic hydromethylpolysiloxanes.

[0096] Particularly preferred are oligomers and polymers corresponding to the general formula (B.3) as organohydrogenpolysiloxane compounds B:

[0097]

[0098] in:

[0099] - x and y are integers ranging between 0 and 10000,

[0100] -Symbol R 1 Can be the same or different, independently of each other:

[0101] a linear or branched alkyl group containing 1 to 8 carbon atoms, which is optionally substituted by at least one halogen, preferably fluorine, the alkyl group being preferably methyl, ethyl, propyl, octyl and 3,3,3-trifluoropropyl, or

[0102] - Cycloalkyl groups containing 5 to 8 ring carbon atoms.

[0103] Aralkyl groups having an alkyl moiety containing 5 to 14 carbon atoms and an aryl moiety containing 6 to 12 carbon atoms.

[0104] The following compounds are particularly suitable for the present invention as organohydrogenpolysiloxane compound B:

[0105]

[0106] where a', b', c', d' and e' are defined as follows:

[0107] - In the polymer of formula S1:

[0108] 0≤a'≤150, preferably 0≤a'≤100 and in particular 0≤a'≤20, and

[0109] -1≤b'≤90, preferably 10≤b'≤80 and in particular 30≤b'≤70,

[0110] - In the polymer of formula S2: 0≤c'≤15

[0111] - In the polymer of formula S3: 5≤d'≤200, preferably 20≤d'≤100, and 2≤e'≤90, preferably 10≤e'≤70.

[0112] Catalyst component C

[0113] The selected platinum-containing catalyst component C of the present invention is essential for the quality of the photocuring or photopolymerization of the silicone composition. According to the present invention, the catalyst component C comprises (C-1) (η-cyclopentadienyl) tris(σ-aliphatic)-platinum complex, (C-2) thioxanthone compound and (C-3) a hydroxyl-containing alicyclic phenyl ketone. Surprisingly, it was found that the use of the platinum complex (C-1) in combination with compounds (C-2) and (C-3) makes it possible to effectively initiate the photopolymerization of the photocurable silicone composition using a wavelength of 420 nm or less.

[0114] The platinum complex (C-1) is a (η5-cyclopentadienyl)tri(α-aliphatic)platinum complex having the formula (I)

[0115]

[0116] in

[0117] Cp represents a cyclopentadienyl group η-bonded to a platinum atom, said cyclopentadienyl group being unsubstituted or substituted with one or more groups which do not interfere with the hydrosilylation reaction, and

[0118] Each of R1, R2 and R3

[0119] represents a hydrocarbon or acyl group having 1 to 30, preferably 1 to 18 carbon atoms, said R1, R2 and R3 groups being sigma-bonded to the platinum atom.

[0120] In an exemplary embodiment, the group represented by R1, R2 and R3 can be an unsubstituted or substituted, linear, branched or cyclic alkyl or aryl, alkylaryl or arylalkyl, in particular an alkyl or aryl group. The substituent groups that can be on the groups Cp, R1, R2 and R3 are one or more groups that do not interfere with the hydrosilation reaction, such as alkyl and silyl groups or halogens such as F, Cl or Br.

[0121] In an exemplary embodiment, the radicals R1, R2 and R3 can independently of one another be unsubstituted or substituted phenyl or alkyl radicals, such as methyl, ethyl, propyl or butyl radicals, or acetyl radicals.

[0122] The preparation of platinum complex (C-1) is known in the art and is commercially available. 5(η-cyclopentadienyl)trimethylplatinum can be prepared by adding a solution of cyclopentadienyl sodium in tetrahydrofuran to an equimolar amount of trimethylplatinum iodide dissolved in benzene and isolating the product complex from the reaction mixture according to the procedure of SD Robinson and BL Shaw, J. Chem. Soc., 1965, 1529. Other platinum complexes such as (η 5 -cyclopentadienyl) trialiphatic platinum complexes can be prepared by using corresponding amounts of substituted cyclopentadienyl sodium instead of cyclopentadienyl sodium and various trialiphatic platinum halides instead of iodotrimethylplatinum. If necessary and in some commercial products, a solvent can be used to disperse the platinum complex (C-1).

[0123] Suitable for implementing the present invention 5 Representative examples of trialiphatic platinum complexes of (Cp) (η 5 -cyclopentadienyl) group: (Cp) trimethyl platinum, (Cp) ethyl dimethyl platinum, (Cp) triethyl platinum, (Cp) triallyl platinum, (Cp) tripentyl platinum, (Cp) trihexyl platinum, (methyl-Cp) trimethyl platinum, (trimethylsilyl-Cp) trimethyl platinum, (phenyldimethylsilyl-Cp) trimethyl platinum, (Cp) acetyl dimethyl platinum, etc. Other suitable (η) groups suitable for the present invention are: 5 -cyclopentadienyl)trialiphatic platinum complexes are described, for example, in U.S. Pat. No. 4,510,094.

[0124] In an advantageous embodiment, the substituent groups on the cyclopentadienyl group are hydrocarbon groups consisting of C and H atoms, including alkyl or aryl groups, preferably having 1 to 18, such as 2 to 12 or 6 to 8 carbon atoms.

[0125] The catalyst component (C) contains (C-2) a thioxanthone compound having the following formula (II):

[0126]

[0127] wherein R represents a substituent at any position of the thioxanthone nucleus selected from aliphatic groups having 1 to 18, preferably 2 to 12, more preferably 3 to 8 carbon atoms, preferably a linear or branched alkyl group; and

[0128] n represents an integer from 1 to 8, preferably from 1 to 4;

[0129] Optionally and preferably, the catalyst component C may further contain (C-3) a hydroxyl-containing alicyclic phenyl ketone having the following formula (III):

[0130] Ph-C(=O)-Cyc(III)

[0131] wherein Ph represents a phenyl group which may be substituted or unsubstituted, and Cyc represents an alicyclic group having at least 3 carbon atoms and having at least one hydroxyl group.

[0132] According to the present invention, the amount of (C-1) may advantageously be 20-50000 ppm, preferably 300-10000 ppm, more preferably 500-8000 ppm, based on the total amount of the silicone composition. In another advantageous embodiment, the weight ratio of (C-1): (C-2) may be 1:0.1-1:10, preferably 5:1-1:5, more preferably 3:1-1:3. Furthermore, it may also be advantageous that the weight ratio of (C-1): (C-3) is 1:0.1 to 1:10, preferably 5:1 to 1:5, more preferably 3:1 to 1:3. The combination of (C-1), (C-2) and (C-3) in the desired ratio can further ensure that the photocurable silicone composition is fully and effectively initiated at a shorter wavelength in a short time, such as less than 15 seconds or even less than 10 seconds.

[0133] Reinforced silica filler D

[0134] In order to allow sufficiently high mechanical strength, it is advantageous to include fine particles of silica as reinforcing filler D in the silicone composition of the invention, which may be at least partially surface-treated. Precipitated and fumed silica or mixtures thereof may be used. The specific surface area of ​​these active reinforcing fillers should be at least 50 m 2 / g, preferably 100-400m 2 / g, determined by the BET method. Such active reinforcing fillers are very well known materials in the field of silicone rubber. The silica filler may have hydrophilic properties or may have been hydrophobized by known methods. Advantageously, the silica reinforcing filler is subjected to an overall surface treatment. This means that at least 50%, more preferably at least 80% or at least 90% or especially preferably all of the surface of the silica reinforcing filler is preferably treated with hydrophobicity.

[0135] In a preferred embodiment, the silica reinforcing filler has a specific surface area of ​​at least 50 m2 as determined by the BET method. 2 / g and preferably 100-400m 2 / g of fumed silica. Fumed silica with a hydrophobic surface treatment can be used. In those cases where a fumed silica with a hydrophobic surface treatment is used, a fumed silica with a preliminary hydrophobic surface treatment can be used. Alternatively, a surface treatment agent can be added during mixing of the fumed silica with the organopolysiloxane compound A, thereby treating the fumed silica in situ.

[0136] The surface treatment agent may be selected from one or more conventionally used agents such as alkylalkoxysilanes, alkylchlorosilanes, alkylsilazanes, silane coupling agents, titanate-based treatment agents and fatty acid esters. These surface treatment agents may be used simultaneously or sequentially.

[0137] The amount of the silica reinforcing filler D in the silicone composition of the present invention is 0.5 to 40 wt %, preferably 2 to 20 wt %, more preferably 3 to 15 wt % of the total composition.

[0138] Cross-linking inhibitor G

[0139] Crosslinking inhibitors are optional components. However, they are usually used in addition-crosslinking silicone compositions to slow down the curing of the composition at ambient temperature. The crosslinking inhibitor F can be selected from the following compounds:

[0140] - acetylenic alcohols, such as ethynylcyclohexanol,

[0141] - tetramethylvinyltetrasiloxane, such as 2,4,6,8-tetramethyl-2,4,6,8-tetravinylcyclotetrasiloxane,

[0142] - pyridine,

[0143] - organic phosphines and phosphites,

[0144] - unsaturated amides, and

[0145] -Alkyl maleates.

[0146] These acetylenic alcohols, which belong to the preferred hydrosilylation reaction heat blocking agents and are described, for example, in FR-B-1 528 464 and FR-A-2 372 874, have the following formula:

[0147] (R”)(R”')(OH)CC≡CH

[0148] Wherein: R" is a linear or branched alkyl group, or a phenyl group; R"' is H or a linear or branched alkyl group, or a phenyl group; and the groups R" and R"' and the carbon atom located at the triple bond position may form a ring.

[0149] The total number of carbon atoms contained in R" and R'" is at least 5, preferably 9 to 20. As for the alkynol, examples that may be mentioned include:

[0150] -1-ethynyl-1-cyclohexanol;

[0151] -3-methyl-1-dodecyne-3-ol;

[0152] -3,7,11-trimethyl-1-dodecyne-3-ol;

[0153] -1,1-diphenyl-2-propyn-1-ol;

[0154] -3-ethyl-6-ethyl-1-nonyn-3-ol;

[0155] -2-methyl-3-butyn-2-ol;

[0156] -3-methyl-1-pentadecyn-3-ol; and

[0157] - diallyl maleate or a diallyl maleate derivative.

[0158] In a preferred embodiment, the cross-linking inhibitor is 1-ethynyl-1-cyclohexanol.

[0159] Advantageously, the amount of crosslinking inhibitor F in the silicone composition of the invention is from 0.01% to 2% by weight, preferably from 0.03% to 1% by weight, relative to the total weight of the silicone composition.

[0160] The use of the inhibitor effectively avoids premature curing of the silicone composition on the nozzle tip and subsequent deformation of the printed layer.

[0161] Other components H:

[0162] The silicone composition according to the invention may optionally further comprise other additives, such as standard semi-reinforcing or filling fillers, other functional silicone resins such as silicone resins or cyclosiloxanes having vinyl groups, non-reactive methylpolysiloxanes, pigments, organic solvents or adhesion promoters.

[0163] Non-siliceous minerals that may be included as semi-reinforcing or filling mineral fillers may be selected from carbon black, titanium dioxide, alumina, hydrated alumina, calcium carbonate, quartz powder, diatomaceous earth, zinc oxide, mica, talc, iron oxide, barium sulfate and slaked lime.

[0164] In the context of the present invention, the molar ratio of hydrogen atoms bonded to silicon (SiH) to alkenyl groups bonded to silicon (e.g. Si-CH=CH2) in the entire composition is between 0.2 and 20, preferably between 0.5 and 15, more preferably between 0.5 and 10, even more preferably between 0.5 and 5. The Si-H and alkenyl groups in the entire composition refer to those contained in components A, B and possible other components.

[0165] In an exemplary embodiment, the mass content of alkenyl units (preferably vinyl units) in the entire composition is 0.001% to 30%, preferably 0.01% to 10%.

[0166] In another exemplary embodiment, the mass content of SiH units in the entire composition is 0.2-91%, preferably 0.5-80%, and more preferably 1.0-50%. The curing rate of the photocurable silicone composition depends at least in part on the SiH content in the composition. The required SiH unit content can promote the photocuring reaction.

[0167] In a preferred embodiment, the silicone composition of the present invention comprises, per 100 wt % of the silicone composition:

[0168] - 10 to 95% by weight of at least one organopolysiloxane compound A;

[0169] - 0.1 to 40% by weight of at least one organohydrogenpolysiloxane compound B; and

[0170] - 300-40000 ppm of catalyst component C.

[0171] It should be noted that the various quantities shown in the above two preferred embodiments and within the above ranges in this application are merely exemplary, and thus each of them can be arbitrarily combined in any manner well understood by those skilled in the art.

[0172] Multi-part compositions

[0173] The composition can be a one-part composition comprising the components in a single part, or alternatively, a multi-part composition comprising these components in two or more parts, provided that components B and C are not present in the same part. For example, a multi-part composition can comprise a first part comprising a portion of component A and all of component C, and a second part comprising the remainder of component A and all of component B. In certain embodiments, component A is in the first part, component B is in the second part separate from the first part, and component C is in the first part, the second part, and / or a third part separate from the first and second parts. Other components such as D, E, and F can be present in the corresponding part (or parts) together with at least one of component B or C, and / or can be present in a separate part (or parts).

[0174] One-part compositions are typically prepared by mixing the principal components and any optional ingredients in the stated proportions at ambient temperature. Although the order of addition of the various components is not critical if the composition is to be used immediately, the hydrosilylation catalyst is typically added last at a temperature below about 30°C to prevent premature curing of the composition.

[0175] In addition, multi-part compositions can be prepared by combining the components in each part. Combining can be accomplished by any technique known in the art such as blending or stirring in a batch or continuous process in a specific apparatus. The specific apparatus is determined by the viscosity of the components and the viscosity of the final composition.

[0176] In an advantageous embodiment, the photocurable silicone composition of the present invention is formulated as a two-part composition. In a photopolymerization-based 3D printing method, the formulated two-part silicone composition stored in two separate compartments can be mixed before entering or within a mixing barrel, or combined immediately before printing, and then printed layer by layer, wherein each layer is first applied and then exposed to actinic radiation to form a cured cross-section on a plate or carrier or on an underlying layer.

[0177] Another aspect of the invention is a silicone elastomeric article produced by the process according to the invention.

[0178] Another aspect of the present invention is the use of a silicone composition as described above for a 3D printing method based on photopolymerization.

[0179] Another aspect of the invention is a catalyst component as defined above for use in an organosilicon component.

[0180] The following examples are intended to illustrate but not to limit the present invention. Example

[0181] raw material

[0182] Table 1

[0183]

[0184]

[0185] Preparation of basic silicone composition

[0186] Each photocurable silicone composition for all the inventive examples and comparative examples was formulated according to the amounts and ingredients shown in Table 2. The ingredients were placed in a container under stirring at ambient temperature to obtain a silicone composition after thorough mixing. Some of the formulated silicone compositions were used for additional 3D printing processes as follows, and others were used for property evaluation.

[0187] 3D Printing Process

[0188] The photopolymerization-based 3D printing method is performed as follows:

[0189] 1. First, completely remove the bubbles in each freshly prepared organosilicon composition material in the examples;

[0190] 2. Install the forming table and barrel securely, and confirm that the peeling film on the barrel and the bottom transparent glass are clean and free of foreign matter;

[0191] 3. Check and install scraper;

[0192] 4. Pour the silicone material into the scraper groove and adjust the gap between the scraper and the peeling film in the range of about 0.2-0.3mm.

[0193] 5. Import the printing model, set the slicing parameters and export the printing file to the printer;

[0194] 6. Set the exposure intensity and time of each layer according to the optimized single-layer exposure parameters, and then start printing layer by layer;

[0195] 7. Remove the printed object after printing is completed.

[0196] 8. Place the printed object in an oven at 80℃~150℃ for secondary curing until the surface is completely cured.

[0197] Performance Evaluation

[0198] The evaluation results of the samples prepared according to the present invention are listed in Table 2.

[0199] Viscosity: The viscosity of the sample mixture was tested according to ASTM D445 at 25° C. The test conditions can be found in Table 2, where for example the expression Viscosity-20 (7#, 20 rpm) means the viscosity measured by using Spindle 7 at 20 rpm, and similarly, Viscosity-2 (7#, 2 rpm) means the viscosity measured by using Spindle 7 at 2 rpm.

[0200] Gel time: The curing speed at 405 nm and the pot life in the dark at 23°C were evaluated by different gel times. The power of the LED light source was 3 W. The distance between the light source and the sample was 10 cm. The test conditions can be found in Table 2. Fast curing speed and sufficiently long pot life are necessary for photopolymerization-based 3D printing by light irradiation. The gel time is obtained by the change in viscosity. As the reaction progresses, the viscosity gradually increases due to the increase in the degree of crosslinking. As the degree of crosslinking increases, the sample becomes a gel state. The gel time is determined by the time the sample can be stretched in the form of thin filaments but the filaments can remain unbroken.

[0201] The mechanical properties were measured by the following procedure: a mixture of the silicone composition was poured into a mold and cured by UV light irradiation and heated at 150°C for 60 minutes. The conditions for UV curing were performed by irradiating the sample composition with a UV Hg lamp with the following parameters:

[0202] Optical power: 120w / cm 20m / min,

[0203] UV A: 147.7mJ / cm2 1417.9mw / cm2

[0204] UV B: 112.8mJ / cm2 1092.8mw / cm2

[0205] UV C:33.4mJ / cm2 321.9mw / cm2

[0206] UV V: 192.7mJ / cm2 1840.7mw / cm2

[0207] The distance between the light source and the sample is 10 cm. When the sample is irradiated for 3 seconds, the sample loses fluidity and quickly forms. The resulting sample is then used to measure the hardness, tensile strength, elongation at break, and tear strength as follows:

[0208] Hardness: The hardness of the cured samples was tested at 25° C. according to ASTM D 2240. The photocured samples were further heated to 150° C. for 60 minutes before measurement.

[0209] Tensile Strength and Elongation at Break: The tensile strength and elongation at break of the cured samples were tested according to ASTM D412 at 25° C. The photocured samples were further heated to 150° C. for 60 minutes before measurement.

[0210] Tear Strength: Tear strength of cured samples was tested according to ASTM D642 at 25° C. Prior to measurement, the photocured samples were heated to 150° C. for 60 minutes.

[0211] Table 2. Formulations and test results of curable silicone compositions

[0212]

Claims

1. A method for producing a three-dimensional printed product, comprising: 1) providing a photocurable silicone composition, 2) exposing the photocurable silicone composition to actinic radiation to form a cured cross-section on a plate or carrier or on an underlying layer, and 3) repeating steps 1) and 2) with new layers on the previously solidified cross section to build a three-dimensional printed article, The curable silicone composition comprises: (A) at least one organopolysiloxane compound A comprising, per molecule, at least two C2-C6 alkenyl groups bonded to silicon atoms, (B) at least one organohydrogenpolysiloxane compound B comprising, per molecule, at least two hydrogen atoms bonded to the same or different silicon atoms, and (C) a catalyst component C comprising a platinum complex; and wherein the photocurable silicone composition is exposed to actinic radiation using UV radiation having a wavelength of less than 420 nm for less than 15 seconds.

2. The method of claim 1, wherein the photocurable silicone composition is exposed to actinic radiation using UV radiation having a wavelength less than 410 nm, such as 365 nm or 406 nm, for example for less than 10 s.

3. The process according to any one of the preceding claims, wherein the catalyst component C comprises: (C-1) (η-cyclopentadienyl)tri(σ-aliphatic)-platinum complex, (C-2) a thioxanthone compound having the following formula (II), wherein R represents a substituent at any position of the thioxanthone nucleus selected from aliphatic groups having 1 to 18, preferably 2 to 12, more preferably 3 to 8 carbon atoms, Preferably a linear or branched alkyl group; and n represents an integer of 1 to 8, preferably 1 to 4; and (C-3) a hydroxyl-containing alicyclic phenyl ketone having the following formula (III): Ph-C(=O)-Cyc(III) wherein Ph represents a phenyl group which may be substituted or unsubstituted, and Cyc represents an alicyclic group having at least 3 carbon atoms and having at least one hydroxyl group.

4. The method according to claim 3, wherein the mass content of SiH units in the entire composition is 0.2 to 91%, preferably 0.5 to 80%, more preferably 1.0 to 50%.

5. The method according to claim 3, wherein the amount of (C-1) is 20-50000 ppm, preferably 300-10000 ppm, more preferably 500-8000 ppm, based on the total amount of the silicone composition.

6. The method according to claim 3, wherein the weight ratio of (C-1):(C-2) can be 1:0.1 to 1:10, preferably 5:1 to 1:5 or 3:1 to 1:

3.

7. The method according to claim 3, wherein the weight ratio of (C-1):(C-3) can be 1:0.1 to 1:10, preferably 5:1 to 1:5, more preferably 3:1 to 1:

3.

8. An organosilicon composition comprising: (A) at least one organopolysiloxane compound A comprising, per molecule, at least two C2-C6 alkenyl groups bonded to silicon atoms, (B) at least one organohydrogenpolysiloxane compound B comprising, per molecule, at least two hydrogen atoms bonded to the same or different silicon atoms, (C) a catalyst component C comprising (C-1) (η-cyclopentadienyl)tri(σ-aliphatic)-platinum complex, (C-2) Thioxanthone compounds having the following formula (II) wherein R represents a substituent at any position of the thioxanthone nucleus selected from aliphatic groups having 1 to 18, preferably 2 to 12, more preferably 3 to 8 carbon atoms, preferably straight or branched chain alkyl groups; and n represents an integer of 1 to 8, preferably 1 to 4; and (C-3) a hydroxyl-containing alicyclic phenyl ketone having the following formula (III): Ph-C(=O)-Cyc(III) wherein Ph represents a phenyl group which may be substituted or unsubstituted, and Cyc represents an alicyclic group having at least 3 carbon atoms and having at least one hydroxyl group.

9. The organosilicon composition according to claim 8, wherein the mass content of SiH units in the entire composition is 0.2 to 91%, preferably 0.5 to 80%, more preferably 1.0 to 50%.

10. The silicone composition according to claim 8, wherein the amount of (C-1) is in the range of 20-50000 ppm, preferably 300-10000 ppm, more preferably 500-8000 ppm, based on the total amount of the silicone composition.

11. The organosilicon composition according to claim 8, wherein the weight ratio of (C-1):(C-2) is 1:0.1 to 1:10, preferably 5:1 to 1:5, more preferably 3:1 to 1:

3. 12 . The organosilicon composition according to claim 8 , wherein the weight ratio of (C-1):(C-3) is 1:0.1 to 1:10, preferably 5:1 to 1:5, and more preferably 3:1 to 1:

3.

13. An article prepared by the method according to any one of claims 1 to 7.