Anode-free metal halide battery

Anodeless metal halide batteries form an anode by depositing metal ions on the current collector, combined with a cathode of conductive materials and metal halide salts, to solve the energy density and stability problems of lithium-ion batteries and achieve higher energy density and cycle stability.

CN118743046APending Publication Date: 2024-10-01INTERNATIONAL BUSINESS MACHINE CORPORATION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380022686.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-02-21
Filing Date
2023-01-06
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing lithium-ion batteries are difficult to achieve higher energy density and stability due to the energy density limitations of graphite anodes and the manufacturing difficulty and sensitivity of lithium metal anodes.

Method used

An anode-less metal halide battery design is adopted. The anode is formed by depositing metal ions on the current collector. The cathode of the conductive material and metal halide salt is used, combined with the ion conductive passivation layer and the solid electrolyte, to achieve uniform plating and lithium ion plating. Stable cycle.

Benefits of technology

It improves the energy density and cycle stability of the battery, simplifies the manufacturing process, avoids the formation of lithium dendrites and the risk of short circuit, and achieves higher Coulomb efficiency and longer cycle life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118743046A_ABST
    Figure CN118743046A_ABST
Patent Text Reader

Abstract

An anodeless metal halide battery is provided. The metal halide battery includes a current collector, an electrolyte, and a cathode. The current collector includes a passivation layer of an electrically insulating material. The passivation layer allows metal ions to be transmitted. The electrolyte comprises an ion conducting material and is in contact with the current collector and the cathode. The cathode includes a metal halide salt incorporated into a conductive metal.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates generally to the field of rechargeable batteries, and more particularly to anode-less metal halide rechargeable batteries. Background Art

[0002] Rechargeable batteries are used as power sources in a wide range of applications such as industrial devices, medical devices, electronic devices, electric vehicles, and grid energy storage systems. Battery technology continues to advance to achieve higher energy density and greater efficiency, which makes it possible to use batteries as a power source for additional applications. Summary of the invention

[0003] Embodiments of the present disclosure include anode-free metal halide batteries. The metal halide battery comprises a current collector, an electrolyte, and a cathode. The current collector comprises a passivation layer of an electrically insulating material. The passivation layer allows metal ion transport. The electrolyte comprises a solvent and at least one ion-conducting salt and is in contact with the current collector and the cathode. The cathode comprises a metal halide salt incorporated into a conductive material. The anode-free metal halide battery may have a variety of advantages over alternative designs. For example, when compared to current lithium-ion batteries using graphite anodes, the disclosed anode-free metal halide batteries have a higher energy density due to the weight and volume advantages of lithium compared to graphite. In addition, these anode-free metal halide batteries may be easier to manufacture than solutions using lithium metal anodes, which require more advanced manufacturing equipment to handle the air and moisture sensitivity of lithium metal.

[0004] In some optional embodiments, the passivation layer includes an artificially formed ion-conducting material. The ion-conducting material may include, for example, polyvinyl alcohol (PVA) and / or polyethylene glycol (PEG). Including an ion-conducting passivation layer can improve the coulombic efficiency of the battery. In addition, the ion-conducting passivation layer produces more stable battery performance in cycling, with increased consistency of capacity retention during battery cycling.

[0005] Another embodiment is directed to another anode-free metal halide battery. The metal halide battery comprises a current collector, an electrolyte, and a cathode. The electrolyte comprises a solid ion conductor and is in contact with the current collector and the cathode. The cathode comprises a metal halide salt incorporated into a conductive material.

[0006] Further embodiments of the present disclosure include methods for forming an anode-free metal halide battery. The method includes forming a metal halide battery cell. The metal halide battery cell includes an anode current collector and does not include a discrete metal anode. The method further includes applying a charging voltage to the halide battery cell to cause deposition of metal ions on the anode current collector.

[0007] The above summary is not intended to describe each illustrated embodiment or every implementation of the present disclosure. BRIEF DESCRIPTION OF THE DRAWINGS

[0008] The accompanying drawings included in the present disclosure are incorporated into this specification and form a part of this specification. They illustrate embodiments of the present disclosure and, together with the description, help explain the principles of the present disclosure. The accompanying drawings are only illustrations of typical embodiments and do not limit the present disclosure.

[0009] Figure 1 A diagram of an example anode-less metal halide battery prior to initial (first) charge is shown, in accordance with an embodiment of the present disclosure.

[0010] Figure 2 An embodiment according to the present disclosure is shown. Figure 1 Figure 1. Example of an anode-less metal halide battery after initial charge.

[0011] Figure 3 An embodiment according to the present disclosure is shown. Figure 2 Figure 1. Example of an anode-less metal halide battery within an encapsulated unit cell.

[0012] Figure 4 Scanning electron microscope (SEM) images of a conventional lithium-ion anode current collector and a metal halide anode current collector constructed according to embodiments of the present disclosure are depicted.

[0013] Figure 5 is a graph showing the initial charge and discharge curves of an anode-free battery cell containing a lithium ion intercalation cathode (solid line) and a metal halide cathode constructed according to an embodiment of the present disclosure (dashed line).

[0014] Figure 6 Graphs showing charge and discharge curves for two different anode-free metal halide battery cells assembled with bare SS current collectors (hollow squares) and polymer-coated SS current collectors (solid squares) according to embodiments of the present disclosure.

[0015] Figure 7Graph showing cycling performance data for two different anode-free metal halide battery cells assembled with bare SS current collectors (open circles) and polymer-coated SS current collectors (filled circles) according to embodiments of the present disclosure.

[0016] Fig. 8A Depicted is a cross-sectional SEM image of a polymer-coated current collector of an anode-less lithium iodide cell after lithium deposition by initial charging, according to an embodiment of the present disclosure.

[0017] Figure 8B for Fig. 8A , showing circular lithium deposits on a current collector according to an embodiment of the present disclosure.

[0018] Fig. 9 Graphs showing charge and discharge curves of an anode-less metal halide battery with a Ni current collector according to an embodiment of the present disclosure.

[0019] Fig.10 Graphs showing cycling performance data for anode-free lithium iodide battery cells assembled with four different anode current collectors according to an embodiment of the present disclosure.

[0020] Fig.11 A flow chart is shown of an example method for forming an anode-less metal halide cathode cell according to an embodiment of the present disclosure.

[0021] Although the embodiments described herein are suitable for (withstand) various modifications and alternative forms, the details have been shown by way of example in the accompanying drawings and will be described in detail. However, it should be understood that the specific embodiments described should not be understood in a limiting sense. On the contrary, it is intended to cover all modifications, equivalents, and substitutes that fall within the scope of the invention. DETAILED DESCRIPTION

[0022] Aspects of the present disclosure generally relate to the field of rechargeable batteries, and more particularly to anode-free metal halide rechargeable batteries. Although the present disclosure is not necessarily limited to such applications, various aspects of the present disclosure may be understood through a discussion of various embodiments using this context.

[0023] Lithium-ion batteries are used in many applications, such as for powering small power tools, electric vehicles, and for storing energy for grid systems. As more energy storage applications are developed, the demand for higher energy density batteries continues to increase, and industry and academia have conducted intensive research and development to meet the growing demand in energy density and battery safety.

[0024] Current lithium-ion batteries based on graphite anodes have inherent capacity limitations, which limit the overall energy density of the battery. To overcome these limitations, the most common approach currently being actively studied is a lithium metal-based battery, because lithium metal has weight and volume advantages when used as an anode. The main challenge to increasing the energy density of such batteries is to make thinner lithium anodes to reduce additional lithium sources and increase volume energy density. However, due to the inherent reactivity of lithium metal to electrolyte compounds and the uneven plating properties of lithium ions, the transition to practical Li metal-based batteries is not easy. Another approach is to replace traditional graphite anodes with soft lithium metal anodes, but since lithium metal is air and moisture sensitive, this will require advanced manufacturing equipment with improved environmental control. The softness of lithium metal will also create huge challenges in processing (transportation, handling) and manufacturing.

[0025] Recently, an IBM-research team demonstrated a high-performance rechargeable metal halide battery using a lithium metal anode. These inventions report that the metal halide battery has a stable anode protection layer formed, which can help enhance fast charging performance and long-term battery operation. In order to further improve the weight and volume energy density of the metal halide battery while eliminating the problems associated with the above-mentioned sensitive metal anodes, a new rechargeable metal halide battery that does not use a discrete metal anode is disclosed herein. The anode-free metal halide battery can reduce side reactions from highly reactive lithium metal and impart uniform lithium ion plating under cycling. In addition, the disclosed anode-free metal halide battery can have a higher energy density than conventional batteries.

[0026] Embodiments of the present disclosure are directed to novel rechargeable metal halide batteries. In particular, some embodiments of the present disclosure include a conductive current collector in a negative electrode, an electrolyte, and a cathode. The cathode includes a metal halide and a conductive material.

[0027] Unlike conventional batteries, the disclosed battery does not require any metal anodes in the initial assembly of the unit cell. Instead, the metal halide cathode includes metal ions that can be deposited on the conductive collector in the negative electrode during the first charging step. These deposited metals then act as anode active materials, participating in sequential electrochemical reactions during cycling. By using the unique surface protection species of the metal halide battery system, uniform metal ion plating and stripping can be achieved even on the collector, and this enables the battery to operate stably. In addition, because the embodiments of the present disclosure do not use sensitive metal anodes (e.g., lithium foil), the manufacturing process of the unit cell can be simpler without any worrisome issues associated with handling soft metal foils (e.g., dents, creases, etc.) and controlling unwanted side reactions of the metal. In addition, the anode-free metal halide battery disclosed herein can suppress lithium dendrite formation, thereby preventing short circuits while maintaining improved energy density of the battery cell.

[0028] It will be understood that the foregoing advantages are example advantages and should not be construed as limiting. Implementations of the present disclosure may contain all, some, or none of the foregoing advantages while remaining within the scope of the present disclosure.

[0029] Turning now to the accompanying drawings, Figure 1 A diagram of an example anode-free metal halide battery 100 before initial charging is shown according to an embodiment of the present disclosure. As used herein, "anode-free" means that the battery 100 does not contain a lithium anode in its initial configuration (i.e., before initial or first charging). The battery 100 includes a current collector 102, a protective coating 104 formed on top of the current collector 102, and an electrolyte 106, and a cathode 108. In addition, the battery 100 includes a separator 110. In some embodiments, the battery 100 may not include a separator 110 and / or a protective coating 104 as discussed herein. The battery 100 operates via a reduction-oxidation (redox) reaction and utilizes different oxidation states and redox reactions of one or more components or elements for charging and discharging. It will be understood that the drawings are not necessarily drawn to scale so as to make it easier to visualize each component individually. For example, the protective coating 104 may be much thinner than depicted in the figure.

[0030] In some embodiments, the current collector 102 is a metal, and suitable examples include, but are not limited to, stainless steel, nickel, and mixtures and combinations thereof. In the present application, components composed of a particular material may include incidental impurities in some cases.

[0031] In some embodiments, the protective coating layer 104 is any suitable coating layer that is conductive to lithium ions. In other words, the protective coating layer 104 allows lithium ions to pass through it. The protective coating layer may be a naturally formed passivation layer called a solid-electrolyte interphase layer (SEI), or a polymer coating layer (artificial SEI) artificially applied to the collector 102. Examples of polymers that can be used include, but are not limited to, polyvinyl alcohol (PVA), poly(ethylene glycol), poly(propylene glycol), polycarbonate, polyester, polyethylene oxide (PEO), polyurethane (PU), styrene-butadiene rubber (SBR), polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), and a combination of polyethylene glycol (PEG) (poly(ethylene glycol)(PEG)copolymerized with polyhedral oligomericsilsesquioxane) copolymerized with polyhedral oligomericsilsesquioxane (POSS) (also referred to as PEG-POSS). The protective coating layer 104 may be a single ion conductor or a polymer electrolyte comprising a polymer having a sulfonic acid group, a carboxylic acid group, and a phosphonic acid group, or any strong acid group attached to a polymer matrix in the form of a lithium salt. In some embodiments, the protective coating layer 104 may comprise an inorganic metal oxide and / or a metal sulfide. In some embodiments, the protective coating layer 104 is approximately 20 μm thick and the coating layer comprises a UV-crosslinked polymer. In some embodiments, the protective coating layer 104 is electrically insulating in addition to having lithium ion conductivity. This helps prevent electrons from flowing in the electrolyte 106 while still allowing lithium ions to pass through and deposit on the current collector 102.

[0032] The electrolyte 106, which may be aqueous or non-aqueous, includes a solvent and at least one ion-conducting salt that dissociates into a corresponding metal ion and a corresponding counter anion. In some examples, which are not intended to be limiting, the metal ion includes at least one of Li, Mg, Zn, Al, and Na, and the counter anion includes nitrate (NO3 - ), hexafluorophosphate (PF6 - ), tetrafluoroborate (BF4 - ), borate oxalate (BOB - ), difluorooxalate borate (DFOB - ), trifluoromethanesulfonate (TF - ), and trifluoromethanesulfonimide (TFSI - )

[0033] In some embodiments, the electrolyte 106 is a solid electrolyte comprising an ion-conducting material. The electrolyte 106 may further be electrically insulating. For example, the electrolyte 106 may be a solid polymer electrolyte (SPE), an inorganic solid electrolyte (ISE, such as a ceramic), or a composite polymer electrolyte (CPE). In some embodiments, the ion-conducting protective coating 104, which may be a polymer, may serve as a solid electrolyte.

[0034] In some embodiments, the electrolyte 106 further includes an optional metal halide (e.g., MXn, where M is a metal, X is a halogen, and n is an integer greater than 0). In some examples, the metal halide is an electrolyte salt that dissociates into a corresponding halide ion and a corresponding metal ion. For example, the metal halide may be dissolved in a solvent including a heterocyclic compound and dissociated into a corresponding metal and halide ion. In some examples, the halide ion may include an ion of at least one of I, Br, Cl, or F (e.g., X may be I, Br, Cl, or F), and the metal ion may include an ion of at least one of Li, Mg, Zn, Al, or Na (e.g., M may be Li, Mg, Zn, Al, or Na). In other examples, the metal halide may include elements other than I, Br, Cl, F, Li, Mg, Zn, and / or Na. In some embodiments, the metal halide may provide additional ionic conductivity for the electrolyte 106.

[0035] In various embodiments, the electrolyte 106 includes one or more solvents capable of transporting metal ions and counterions. In various embodiments, which are not intended to be limiting, suitable solvents may be selected from non-aqueous organic solvents such as ethers, ethylene glycol dimethyl ether (glyme), carbonates, nitriles, amides, amines, organic sulfur solvents, organic phosphorus solvents, organic silicon solvents, fluorinated solvents, adiponitrile (ADN), propylene carbonate (PC), dimethoxyethane (DME), and mixtures and combinations thereof.

[0036] In some examples, one or more additional solvents may be included in the electrolyte 106 to further improve the electrochemical performance of the battery 100 , for example, by enhancing rechargeability, cyclability, etc.

[0037] In some embodiments that are not intended to be limiting, the solvent in the electrolyte 106 includes an optional heterocyclic compound, which in the present application refers to an aromatic or non-aromatic cyclic compound having at least two different elements as ring member atoms. Cyclic compounds (cyclic compounds) as used in the present application refer to compounds in which one or more series of atoms in the compound are connected to form a ring. In various embodiments, suitable cyclic compounds for the electrolyte 106 include 5-membered rings such as pyrrolidine, oxolane, thiolane, pyrrole, furan, and thiophene; 6-membered rings such as piperadine, alkanes (oxane), thiazane, pyridine, pyran and thiopyran; and 7-membered rings such as azepane, oxepane, thiepane, azepine, Examples of suitable heterocyclic compounds include, but are not limited to, tetrahydrofuran, tetrahydropyran, tetrahydrothiophene, oxathiolane, succinimide, The heterocyclic compounds include, but are not limited to, cyclic ethers, cyclic esters, and mixtures and combinations thereof.

[0038] In some examples, the electrolyte 106 includes substantially equal parts of a solvent including a heterocyclic compound and the one or more additional solvents.

[0039] In another embodiment that is not intended to be limiting, the solvent in the electrolyte 106 includes an optional nitrile compound. The nitrile compound has a chemical formula of N≡C–R or N≡C–R–C≡N, wherein R is an organic functional group. Examples of organic functional groups for the nitrile compound include ethers, alkyl ethers, thioethers, alkyl thioethers, and the like. In some examples that are not intended to be limiting, the nitrile compound is selected from valeronitrile, nononitrile, capronitrile, acetonitrile, propionitrile, glutaronitrile, methoxyacetonitrile (MAN), methoxybenzonitrile, methoxypropionitrile (e.g., 3-methoxypropionitrile (MPN)), methylglutaronitrile, butoxypropionitrile, butoxybenzonitrile, and mixtures and combinations thereof. In some examples, the nitrile compound in the electrolyte 106 can improve electrochemical performance (e.g., reversibility, rechargeability, and / or cyclability), produce fewer irreversible carbonate byproducts, or improve power density.

[0040] In some examples, the electrolyte 106 includes equal parts of a solvent including the nitrile compound and the one or more additional solvents.

[0041] The electrolyte 106 includes an oxidizing gas. In some examples, the electrolyte 106 may be in the presence of an oxidizing gas, and the phrase "including an oxidizing gas" is intended to include such a configuration. In some examples, the oxidizing gas may be dissolved in a solvent including the electrolyte 106. In some examples that are not intended to be limiting, the oxidizing gas includes at least one of oxygen, air, nitric oxide, or nitrogen dioxide. The oxidizing gas helps induce the redox reaction of the battery 100 as described above, and helps achieve a highly reversible redox reaction, which can contribute to the enhanced electrochemical performance of the battery 100. The oxidizing gas can help induce such a redox reaction, and promote the consolidation (consolidation) and stabilization of the solid-electrolyte interphase layer (SEI) on the electrode (i.e., the collector 102 and the cathode 108), but does not participate in the redox reaction of the battery 100 that produces capacity. In some examples, the electrolyte lacking the oxidizing gas may exhibit little or no rechargeability.

[0042] In the embodiments discussed below with respect to experimental results and examples, the electrolyte 106 is a mixture of about 0.2 M LiNO 3 and about 0.5 M LiTFSI (lithium bis(trifluoromethanesulfonyl)imide) in dioxolane (DOL) and also includes 1,2-dimethoxyethane (DME).

[0043] During the charge of the battery 100, the cathode 108 releases electrons through the redox reaction of the metal halide and provides a conductive path for the external circuit to which the battery 100 is connected, while the metal ions diffuse from the cathode to the current collector through the electrolyte 106, and are reduced to metal on the current collector in the negative electrode by receiving electrons transferred from the external circuit. Similarly, during the discharge of the battery 100, the deposited lithium metal is oxidized to lithium ions, releases electrons through the external circuit to which the battery 100 is connected, and a cathode redox reaction occurs on the cathode 108 by receiving electrons transferred from the external circuit.

[0044] Cathode 108 includes a conductive material and a metal halide salt incorporated into or applied to the conductive material. In various embodiments, the total amount of metal halide in cathode 108 is greater than the amount of metal halide in electrolyte 106, or at least 2 times the total amount of metal halide in electrolyte 106, or 3 times the amount, or 5 times the amount.

[0045] In some examples that are not intended to be limiting, the conductive material in the cathode 108 may include conductive powders independently selected from metal and / or carbon powders, woven or non-woven metal fibers, metal foams, woven or non-woven carbon fibers, etc. Additionally or alternatively, the cathode 108 may include a stainless steel mesh, an aluminum (Al) mesh, a nickel (Ni) foam, a carbon cloth, and / or a carbon paper. For example, in an embodiment, the cathode 108 may include a stainless steel mesh on which carbon nanoparticles are deposited.

[0046] In another embodiment, cathode 108 may be a conductive porous material. In some embodiments, cathode 108 may include a carbon material selected from amorphous carbon materials, crystalline carbon materials, and mixtures and combinations thereof. Suitable amorphous carbon materials include, but are not limited to, particles of carbon black and porous glassy carbon, and mixtures and combinations thereof. In some embodiments, the crystalline carbon material includes, but is not limited to, graphene, graphene oxide, reduced graphene oxide, carbon nanotubes, and mixtures and combinations thereof.

[0047] In some embodiments, cathode 108 may include a powder of an optional material such as lithium cobalt oxide (LCO, e.g., LiCoO2), lithium nickel cobalt aluminum oxide (NCA, e.g., LiNi x Co y Al z O2, LiNi 0.8 Co 0.15 Al 0.05 O2), lithium manganese oxide (LMO, for example, LiMn2O4), lithium nickel manganese cobalt oxide (NMC, for example, LiNiMnCoO2), nickel cobalt manganese (NCM, for example, LiNi x Co y Mn z O2, LiNi0 .33 Co 0.33 Mn 0.33 O2) or lithium iron phosphate (LFP, e.g., LiFePO4), and mixtures and combinations thereof.

[0048] The cathode 108 includes at least one metal halide salt MXn, where M is a metal, X is a halide, and n is an integer greater than 0 (e.g., 1-3). In some examples, the metal halide includes I - Br - , Cl - , or F - (For example, X may be an ion of at least one of I, Br, Cl, or F), and the metal ion may include Li + Mg 2+ 、Zn 2+ 、Al 3+ Or Na +(For example, M may be an ion of at least one of Li, Mg, Zn, Al, or Na). In other examples, the metal halide may include elements other than I, Br, Cl, F, Li, Mg, Zn, Al, and / or Na.

[0049] In some embodiments, cathode 108 may optionally include a polymer binder. Suitable polymer binders may vary widely, and examples include, but are not limited to, polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), or sulfonated tetrafluoroethylene-based fluoropolymer-copolymers (available from DowDuPont, Midland, MI under the trade name NAFION), and mixtures and combinations thereof.

[0050] In some embodiments, the cathode optionally includes a halogen diatomic molecule. Suitable halogen diatomic molecules include I2, Br2, Cl2, and F2.

[0051] In various embodiments, cathode 108 includes about 25 wt % conductive material, about 70 wt % metal halide salt, and about 5 wt % optional polymer binder, based on the total weight of cathode 108. For example, in some embodiments, cathode 108 includes about 50 wt % to about 80 wt % metal halide, or about 40 wt % to about 90 wt %, or about 30 wt % to about 100 wt %, or about 10 wt % to about 100 wt %, based on the total weight of cathode 108.

[0052] In various embodiments, the metal halide in the cathode 108 can be dispersed or distributed throughout the matrix of the conductive material and any polymer binder present. In some embodiments, the conductive material itself can be a porous material, and the metal halide salt can be located in a plurality of pores therein. In some embodiments, in addition to being located in the pores, the metal halide can also be adsorbed into the conductive material and / or the polymer binder. In some embodiments, the metal halide salt forms a gradient in the conductive matrix material, or can be concentrated near the major surface of the cathode to form one or more metal halide-rich layers.

[0053] In the embodiments discussed below with respect to experimental results and examples, the cathode 108 includes lithium-iodide deposited on a porous carbon cathode (LiI-carbon composite cathode). The porous carbon cathode includes activated carbon (host material), super-P (electronic conductive agent), and styrene butadiene rubber / carboxymethyl cellulose (SBR / CMC) binder, which is prepared by coating a slurry formed by a carbon / binder mixture in alcohol with a weight ratio of 85 / 15 on a stainless steel collector. The active cathode material, LiI in methanol, is separately prepared and dosed (dosed) onto the carbon cathode to form the LiI-carbon composite cathode. The LiI-carbon composite cathode is then dried on a hot plate at 120°C for approximately 12 hours, and all batching and drying processes are performed in an Ar-filled glove box.

[0054] In some examples, the battery 100 includes an optional separator 110. The separator 110 forces electrons to pass through an external circuit to which the battery 100 is connected, so that the electrons do not travel through the battery 100 (e.g., through the electrolyte 106 of the battery 100), while still allowing metal ions to flow through the electrolyte 106 of the battery 100 during charging and discharging. In some examples, the separator 110 can be soaked with the electrolyte 106, soaked within the electrolyte 106, surrounded by the electrolyte 106, etc. The separator 110 can include a non-conductive material to prevent electrons from moving through the battery 100, so that the electrons instead move through the external circuit through the battery terminals. For example, the separator 110 can include glass, non-woven fibers, polymer films, rubber, etc. In the embodiments discussed below with respect to experimental results and examples, the separator 110 is placed between the cathode and the anode. 2325 Partition.

[0055] In some examples, the battery 100 has a closed or substantially closed volume. For example, the current collector 102, the protective coating 104, the electrolyte 106, the cathode 108, and the separator 110 can be in a closed or substantially closed unit cell or other enclosure. In this way, the oxidizing gas of the electrolyte 106 remains within the battery 100, so that the battery 100 has a relatively fast charging rate, high energy efficiency, high power density, high reversibility, high cyclability, and / or combinations thereof as described herein.

[0056] Reference now Figure 2 , which shows an embodiment according to the present disclosure, Figure 1 FIG. 1 is an example of an anode-less metal halide battery 100 after initial charging. Figure 2 Except that the initial charging of the battery 100 causes the lithium ions to be reduced to metallic lithium 202 plated on the current collector 102, the battery 100 is substantially the same as shown in FIG. Figure 1106 . In other words, charging of the battery 100 causes the lithium ions initially present in the cathode 108 to move through the electrolyte 106 and through the protective coating 104, and then to be plated on top of the current collector 102 in the form of metallic lithium 202 by receiving electrons transferred through the external circuit and the current collector. During subsequent operation, the metallic lithium 202 can effectively serve as the anode of the battery 100. In other words, the metal 202 can absorb metal ions from the electrolyte 106 during charging and release the metal ions into the electrolyte 106 during discharge. In this way, the battery 100 can be assembled without a separate anode (e.g., without a lithium foil anode), and the anode can be subsequently formed by depositing lithium 202 on the current collector 102 during the initial charge.

[0057] Even at relatively high charge current densities, battery 100 is capable of undergoing many charge and discharge cycles (e.g., exhibiting good rechargeability). In some examples, battery 100 is capable of undergoing many charge and discharge cycles at greater than or equal to about 1 mA / cm 2 , about 5mA / cm 2 , about 10mA / cm 2 , or about 20mA / cm 2 As an example, the battery 100 may be capable of performing at least 100 charge and discharge cycles at a current density of about 1 mA / cm 2 , about 5mA / cm 2 , about 10mA / cm 2 , or about 20mA / cm 2 At least 1000 charge and discharge cycles were completed at a current density of .

[0058] Additionally or alternatively, the battery 100 may exhibit relatively high energy efficiency. For example, the battery 100 may exhibit a relatively high energy efficiency of greater than or equal to about 1 mA / cm 2 , about 5mA / cm 2 , about 10mA / cm 2 , or about 20mA / cm 2 At a current density of greater than or equal to about 1 mA / cm, the battery 100 exhibits an energy efficiency of greater than or equal to 90%. In some examples, the battery 100 may be greater than or equal to about 1 mA / cm 2 , about 5mA / cm 2 , about 10mA / cm 2 , or about 20mA / cm 2 At a current density of 1.5 MW, it exhibits an energy efficiency greater than or equal to 99%.

[0059] Reference now Figure 3 , which shows an embodiment according to the present disclosure, Figure 2FIG. 3 shows an example of an anode-free metal halide battery 100 within an encapsulated cell 300. The encapsulated cell 300 may include a cell that houses the battery 100 during operation of the battery 100, a cell for assembling the battery 100, or both. For example, the encapsulated cell 300 may include a cell available from Swagelok of Solon, OH under the trade name SWAGELOK and may be used to assemble the battery 100. In some examples, the encapsulated cell 300 may include an inlet tube 302 and / or an outlet tube 304. The inlet tube 302 and the outlet tube 304 may be used to introduce air or other gases (e.g., the oxidizing gas of the electrolyte 106) into and out of the encapsulated cell.

[0060] In one example embodiment, to assemble the cathode 108, powders of conductive materials, metal halides, lithium ions, and any optional polymer binder are simply mixed together to form a slurry. In some embodiments, an optional solvent may be used to fully disperse the powder. The slurry is then cast on the surface of a separator 110 or any type of mesh (which may be referred to herein as a gas diffusion layer (GDL)) and dried to form the cathode 108. In another embodiment, the slurry is cast on the surface of an optional current collector (e.g., a metal foil) in the positive electrode. In various non-limiting embodiments, the slurry may be air-dried, dried in an oven, or a combination thereof.

[0061] In some examples, the metal halide itself can be dried prior to being incorporated into the slurry. In a non-limiting example, the metal halide can be dried on a hot plate in an argon-filled glove box at about 120° C. for greater than 12 hours.

[0062] To make a battery cell, the current collector 102 and the optional separator 110 having the cathode 108 formed thereon are stacked together. In some embodiments, the optional separator 110 is soaked with the electrolyte solution 106, or the electrolyte solution 106 is placed in the cell between the current collector 102 and the cathode 108, or both. After stacking the current collector 102, the separator 110 soaked with the solution, and the cathode 108, the encapsulated unit cell 300 can be closed or substantially closed to form a closed or substantially closed volume around the stack.

[0063] The oxidizing gas is then introduced into the encapsulated unit cell 300 to assemble the battery 100. In some examples, the introduction of the oxidizing gas into the encapsulated unit cell 300 includes introducing the oxidizing gas into the encapsulated unit cell 300 via the inlet tube 302. In some examples, the encapsulated unit cell 300 may include an inert gas (e.g., argon), or be in the presence of an inert gas, before the oxidizing gas is introduced into the encapsulated unit cell 300. In some such examples, the introduction of the oxidizing gas may purge and completely replace the inert gas within the encapsulated unit cell 300 with the oxidizing gas. For example, the oxidizing gas may be introduced into the encapsulated unit cell 300 via the inlet tube 302, and the inert gas may be purged through the outlet tube 304. In some examples, the concentration of the oxidizing gas in the encapsulated unit cell 300 may be about 5 weight percent to about 100 weight percent, about 20 weight percent to about 100 weight percent, about 50 weight percent to about 100 weight percent, or about 80 weight percent to about 100 weight percent of the total amount of gas in the encapsulated unit cell 300 (e.g., compared to the total amount of the oxidizing gas and the inert gas in the encapsulated unit cell 300).

[0064] Now refer to Figure 4-10 The present disclosure is described with respect to some non-limiting examples. In particular, a diagram showing images and resulting data collected from some embodiments studied by the inventors of the present disclosure will first be described. Figure 4-10 , and then discuss the resulting Figure 4-10 The experimental details of the data shown in . However, it will be understood in advance that these examples are only illustrative examples, and they are not intended to be limiting. As will be appreciated by those of ordinary skill in the art, many modifications may be made to the specific examples without departing from the scope of the invention, and such modifications are contemplated by the present disclosure. For example, alternative materials, compositions of materials, and arrangements of materials that are not inconsistent with the present disclosure may be considered.

[0065] In particular, Figure 4 and 5 Two different anode-free cells were compared: one with a conventional lithium-ion cathode and the other with a metal halide cathode constructed according to an embodiment of the present disclosure. Figure 4 , depicted are scanning electron microscope (SEM) images 400, 450 of lithium-deposited current collectors obtained from anode-free battery cells having a conventional lithium-ion cathode (400) and a metal halide cathode (450) constructed according to embodiments of the present disclosure. In particular, the SEM images 400, 450 show the plating behavior of lithium, which has a very strong impact on the electrochemical performance of lithium batteries, such as rate capability and long-term cycle life. Figure 4In the present invention, stainless steel (SS) current collectors are used for both anode-less lithium-ion cells and anode-less metal halide cells because the commonly used aluminum and copper current collectors tend to become corroded in electrolytes containing halide ions.

[0066] like Figure 4 As shown in , the lithium plating behavior between the two battery chemistries differs greatly. In particular, the metal halide cathode plates lithium more uniformly and is better at stripping and plating during cycling because it has a relatively uniform current distribution. This is reflected by Figure 4 This is illustrated by the large, granular lithium deposits shown in the second SEM image 450 in FIG. 4. In contrast, the SEM image 400 of the lithium deposit produced by the lithium-ion cathode cell shows needle-shaped lithium dendrites 402. These dendrites 402 tend to form dead lithium sheets during cycling, which significantly reduces the overall capacity of the cell. The sharp dendrites also cause short circuits in the battery, leading to cell failure. Therefore, Figure 4 It is demonstrated that the metal halide cell chemistry results in more uniform lithium plating on stainless steel current collectors.

[0067] As discussed, lithium morphology affects the cycling efficiency of the battery. Figure 4 The initial charge and discharge curves obtained for the battery without an anode are shown in Figure 5 In particular, Figure 5 Graph 500 showing initial charge 502, 504 and discharge 506, 508 curves at 0.5 mAh cutoff capacity for anode-less lithium ion cells (502, 506) and anode-less metal halide cells (504, 508) constructed in accordance with embodiments of the present disclosure.

[0068] As shown in graph 500, at its operating voltage, the anode-free lithium-ion cell has a coulombic efficiency (CE) of 49%. In contrast, the anode-free metal halide cell shows a coulombic efficiency of 73%, which means that uniform lithium plating is closely related to higher lithium stripping in the cell. In other words, the discharge curve 506 of the lithium-ion cell drops at a capacity of about 0.25 mAh (indicating a rapidly falling voltage), which is about 49% of the cell charging to 0.5 mAh capacity (as shown in charging curve 502). In contrast, the discharge curve 508 of the SS-metal halide cathode cell shows a voltage drop point of about 0.365 mAh, or about 73% of the cell charging to 0.5 mAh capacity (as shown in charging curve 504). This also shows that the anode-free metal halide cell has more promising results than the anode-free lithium-ion cell, which may be a result of the stable, uniform SEI layer formed on the current collector.

[0069] Figure 6 and7 The properties of anode-free metal halide cells including a bare stainless steel current collector were compared with those of anode-free metal halide cells with an artificial SEI (polymer-based protective coating layer) on top of the stainless steel current collector. UV-crosslinked polyethylene glycol reinforced by polyhedral oligomeric silsesquioxane (POSS-PEG) was used as the artificial SEI layer. Figure 5 As shown in , the anode-free metal halide battery charges and discharges normally with relatively high coulombic efficiency. In the case of confirming the morphological benefits of lithium plating from the metal halide cathode, adding an artificial protective layer on the current collector can help prevent the loss of active materials for SEI formation and produce higher capacity and cycle life. For this reason, the lithium ion conductive polymer coating layer is applied to the current collector and used as the anode of the battery together with the current collector and lithium deposit. In some embodiments, the thickness of the polymer coating layer is approximately 20 μm, and the coating layer is polymerized by UV light.

[0070] Figure 6 Shown are the charge and discharge curves after aging cycles from a metal halide cell without an anode having a stainless steel (SS) current collector. In particular, Figure 6 600 is a graph showing the charge 602, 604 and discharge 606, 608 curves of a metal halide cell using a bare metal (in this case, stainless steel) current collector (604, 608) and a metal halide cell including a polymer coating layer on top of the stainless steel current collector (602, 606). Below the cut-off capacity, the polymer coated SS cell shows a higher discharge capacity and coulombic efficiency (as shown by its discharge curve 606) than the bare SS cell (as shown by its discharge curve 608).

[0071] in addition, Figure 6 It is shown that in terms of overpotentials during charge and discharge reactions, the charge overpotential of the polymer coated SS cell is higher than that of the bare SS cell due to the thick polymer coating layer. This is illustrated by the charge curve 602 of the polymer coated SS cell being above the charge curve 604 of the bare-metal SS cell. Likewise, the discharge overpotential of the polymer coated SS cell is higher, and this indicates that the lithium ion conductive polymer coating layer is resistant to lithium ion stripping from the anode. The resistance caused by the ion conductive polymer coating layer can be reduced by increasing the ion conductivity and / or reducing the thickness of the polymer coating layer.

[0072] Reference now Figure 7, shown is a graph 700 showing cycling performance data for two different anode-free metal halide battery cells according to embodiments of the present disclosure. As can be seen in graph 700, the polymer-coated SS cell has higher capacity and stable cyclability after initial stable cycling. In contrast, the bare SS cell has a slightly unstable cycle life during 40 cycles. This suggests that the artificial polymer coating increases the consistency of charge capacity in the anode-free metal halide battery over repeated cycles.

[0073] Fig. 8A and 8B Depicted are SEM images 800, 850 of polymer-coated current collectors obtained from anode-free metal halide battery cells after lithium deposition by initial charging according to embodiments of the present disclosure. In particular, Figure 8B Shows Fig. 8A An enlarged portion 850 of the SEM image 800 is shown. Fig. 8A and 8B It is generated for a battery cell using a cut-off capacity of 0.1 mAh.

[0074] Fig. 8A and 8B A stainless steel current collector 802 is shown with a polymer 804 deposited thereon. During the initial charging run, lithium ions permeate the polymer 804 and are deposited on the current collector 802 as lithium metal 806. The lithium metal 806 is deposited substantially uniformly below the polymer 804 and on top of the current collector 802. This indicates that the polymer layer is a lithium ion conductor and that the charging reaction occurs normally below this artificial polymer SEI layer. Unlike the needle-like dendrites that form on lithium-ion battery cells without an anode, Figure 8B The enlarged image in further shows a circular lithium deposit 806 uniformly disposed on the current collector. Thus, it is possible to reversibly operate a metal halide lithium battery without an anode.

[0075] Fig. 9 and 10 Electrochemical properties of anode-free lithium iodide cells assembled with different metal current collectors and artificial SEI layers (e.g., bare metal or polymer coated) are shown. For these experiments, anode-free lithium iodide cells were assembled in a dry air atmosphere, Ni foil and SS foil were used as anode current collectors, and a polyvinyl alcohol (PVA) coating layer was applied to the current collector as an artificial SEI layer.

[0076] First reference Fig. 9, shown is a graph 900 showing the charge 902 and discharge 904 curves of an anode-free lithium iodide battery cell assembled with a PVA-coated Ni substrate according to an embodiment of the present disclosure. The charge-discharge performance was evaluated under a cut-off voltage condition of 2.0 V to 3.5 V. It shows a higher coulombic efficiency (CE) of more than 80%, and good charge and discharge behavior without any voltage spikes.

[0077] In addition, this result shows that the anode-free metal halide battery disclosed herein can be operated in a dry air atmosphere, similar to Figure 6 The cell shown in FIG. 1 is operated in a pure oxygen atmosphere. It is worth noting that when the cell is tested in an oxygen atmosphere, the oxygen reduction reaction can occur at about 2.5 V, so lower voltages are affected. Figure 6 However, if the same battery cell is tested in dry air, the voltage of the battery cell can be extended to 2.0V ( Fig. 9 ), which allows for higher battery cell capacities.

[0078] Reference now Fig.10 , shown is a graph 1000 showing cycle performance data of four different anode-free lithium iodide battery cells assembled with current collectors of bare SS (grey squares) and bare Ni (black circles) and current collectors using PVA-coated SS (grey diamonds) and PVA-coated Ni (black triangles) according to an embodiment of the present disclosure. The cycle performance data was obtained at 0.3C in a dry air atmosphere. As shown in FIG. 1000, the cell with the Ni current collector has a higher capacity retention throughout the cycle than the cell with the SS current collector. In addition, in terms of the number of cycles, the cell with the SS current collector has a shorter cycle life than the cell with the Ni current collector. In the case of a Ni substrate, applying a PVA coating on the substrate improves the cycle stability in a dry air atmosphere by up to 30 times. As shown, the use of Ni foil as a current collector and a PVA coating as an artificial SEI layer further improves the electrochemical performance of the anode-free metal halide cell.

[0079] Reference now Fig.11 , a flow chart of an example method 1100 of forming an anode-free metal halide battery cell according to an embodiment of the present disclosure is shown. The method 1100 may be performed by hardware, firmware, software executed on a processor, or any combination thereof. For example, the method 1100 may be performed by a computer system (e.g., having a processor and a memory) configured to control a robot and / or other device for assembling a battery. The method 1100 may begin at operation 1102, where components of an anode-free battery cell are formed.

[0080] As disclosed herein, the anode-free battery cell assembly comprises a cathode, a separator, an electrolyte, and a current collector for one or both electrodes. The anode-free metal halide battery demonstrated in the present disclosure does not include a lithium anode in the initial unit cell, but only includes an anode current collector. Instead, the cathode may be composed of an active cathode material containing lithium (e.g., a carbon cathode, such as a LiI-carbon composite cathode) deposited on a porous cathode. In some embodiments, a passivation layer, also referred to as a solid electrolyte interphase layer, is formed on top of the current collector in the negative electrode. In other embodiments, a polymer coating layer (artificial SEI) is deposited on top of the current collector in the negative electrode.

[0081] In some embodiments, the porous carbon cathode includes activated carbon (host material), super-P (electronic conductive agent), and styrene butadiene rubber / carboxymethyl cellulose (SBR / CMC) binder, which is prepared by coating a slurry of carbon / binder mixture in alcohol with a weight ratio of 85 / 15 on a stainless steel current collector. The active cathode material, LiI in methanol, is separately formulated and dosed onto the carbon cathode to form a LiI-carbon composite cathode. The LiI-carbon composite cathode is then dried on a hot plate at 120° C. for approximately 12 hours, and all batching and drying processes are performed in an Ar-filled glove box.

[0082] In some embodiments, the electrolyte is a mixture of about 0.2M LiNO3 and about 0.5M LiTFSI (lithium bis(trifluoromethanesulfonyl)imide) in dioxolane (DOL), and also includes 1,2-dimethoxyethane (DME). The separator can be, for example, a Celgard 2325 separator, and can be placed between the cathode and the current collector.

[0083] To form the anode-free battery cell assembly, the current collector and optional separator and cathode formed thereon may be stacked together. In some embodiments, the optional separator is soaked with an electrolyte solution, or the electrolyte solution is placed in the unit cell between the current collector and the cathode, or both. After stacking the current collector, the separator soaked with the solution, and the cathode, the battery cell may be closed or substantially closed to form a closed or substantially closed volume around the stack.

[0084] The oxidizing gas may then be introduced into the encapsulated unit cell to assemble the battery 100. In some examples, introducing the oxidizing gas into the encapsulated unit cell includes introducing the oxidizing gas into the encapsulated unit cell via an inlet tube. In some examples, before the oxidizing gas is introduced into the encapsulated unit cell, the encapsulated unit cell may include an inert gas (e.g., argon), or in the presence of an inert gas. In some such examples, the introduction of the oxidizing gas may purge and completely replace the inert gas within the encapsulated unit cell with the oxidizing gas. For example, the oxidizing gas may be introduced into the encapsulated unit cell via the inlet tube, and the inert gas may be purged through the outlet tube. In some examples, the concentration of the oxidizing gas in the encapsulated unit cell 300 may be about 5% to about 100% by weight, about 20% to about 100% by weight, about 50% to about 100% by weight, or about 80% to about 100% by weight of the total amount of gas in the encapsulated unit cell.

[0085] After forming the anode-free battery cell assembly, a charging voltage may be applied to the cell assembly at operation 1104. The application of the charging voltage may cause lithium ions that may initially be in the cathode, electrolyte, or both to move toward the current collector and deposit as metallic lithium that will serve as an anode on top of the current collector. In embodiments including a passivation layer (SEI layer) naturally formed on a bare metal current collector, lithium ions may pass through the passivation layer and deposit on top of the bare metal current collector to form a metallic lithium layer that serves as an anode of the resulting battery. In embodiments having a polymer-coated current collector, the polymer coating layer may serve as an artificial SEI. In these embodiments, lithium ions may penetrate the polymer coating layer and deposit on top of the current collector to form a metallic lithium layer. As lithium is deposited on the current collector, the current collector, together with the lithium deposit and the polymer coating layer, may be substantially converted into and serve as an anode of the battery. After applying the initial charging voltage for a sufficiently long time to enable lithium ions to migrate to the current collector, method 1100 may be terminated.

[0086] Some example embodiments of anode-less metal halide cells will now be discussed in detail. These example embodiments are non-limiting examples that the inventors have successfully fabricated and tested using the methods disclosed herein.

[0087] Example 1: Anode-less metal halide cells assembled with LiI-carbon composite cathode and stainless steel (SS) current collector operated under oxygen and dry air.

[0088] According to the general procedure of anode-free metal halide cells discussed above, the cells were assembled in an argon-filled glove box or a dry air-filled glove box. For SEM analysis, the SS-LiI / C composite cells in Swagelok cells were assembled in an argon-filled glove box, and oxygen was bubbled into the assembled cells for 30 seconds. After closing the inlet / outlet valves, the cells were then started to operate under an oxygen atmosphere. After the first charge up to 1 mAh, the cells were disassembled and the SS current collectors were carefully rinsed with a DOL / DME solvent mixture and then dried under vacuum at room temperature. Figure 4 As shown in (on the right), smooth and uniform lithium deposition was observed on the SS current collector. In addition, the SS-LiI / C composite unit cell was operated at a capacity of 0.5 mAh under an oxygen atmosphere, and the charge-discharge curves showed much better coulombic efficiency (in Figure 5 -73% in the dashed line graph).

[0089] Coin-type cells were also assembled in a dry air filled glove box. For this, the electrolyte was a mixture of 0.2M LiNO3, 0.2M LiBOB and 0.5M LiTFSI in DOL / DME. The experiment had a cut-off voltage condition of 2.0 to 3.5V at 0.3C and the cyclability of the cell was plotted at Figure 7 (SS) in.

[0090] Example 2: Anode-free metal halide cell assembled with LiI-carbon composite cathode and Ni current collector operated under dry air.

[0091] The same cell parts (components) and assembly method described in the general procedure were applied, except that the current collector was Ni instead of SS. Using Ni current collector, the coin-type cell was assembled with an electrolyte having 0.2M LiNO3, 0.2M LiBOB (lithium bis(oxalato)borate) and 0.5M LiTFSI in DOL / DME solution. The assembled cell was operated at 0.3C with a cutoff voltage of 2.0 to 3.5V. The charge and discharge curves and cyclability are plotted in Fig. 9 and Fig.10 (Ni) in.

[0092] Example 3: Anode-free metal halide cell assembled with LiI-carbon composite cathode and SS current collector coated with PEG-POSS operated under oxygen.

[0093] The unit cell was assembled by following the general method described above. As an artificial protective layer, a cross-linked PEG-POSS (PEG: PEG-methyl ether acrylate, POSS: methacrylic acid polyhedral oligomeric silsesquioxane) film was applied to the SS metal current collector. The cross-linked coating process was carried out in an argon-filled glove box. The PEG was freeze-dried under vacuum for 2 days and then stored on molecular sieves. PEG, POSS, and a photoinitiator (Darocur 1173) were all mixed together based on a weight ratio of PEG:POSS of 10:1 and 0.1 wt % of UV initiator of the total solution. The resulting solution was stirred for 10 minutes before the solution was applied to the current collector by doctor blade coating, and the coating was polymerized by UV light exposure for up to 2 minutes.

[0094] For electrochemical testing and SEM analysis, since the experiment was conducted under oxygen atmosphere, the Swagelok unit cell was assembled and oxygen was purged for 30 seconds. Initial cycling was performed at 0.5 mA current ( Figure 6 ) and long-term circulation ( Figure 7 ) for 30 minutes with a cut-off capacity of 0.25 mAh. To observe lithium deposits on the current collector, a cell with a PEG / POSS-coated stainless steel current collector was assembled and charged to a capacity of 0.1 mAh. After disassembly of the cell, the POSS-PEG-coated current collector was carefully rinsed with a DOL / DME solvent mixture and then dried under vacuum at room temperature. The SEM image of the cross-section of the POSS-PEG-coated current collector is shown in Figure 2. Fig. 8A and Figure 8B As shown in . Lithium is deposited below the POSS-PEG artificial SEI layer and directly on the SS current collector.

[0095] Example 4: Anode-free metal halide cell assembled with LiI-carbon composite cathode and PVA-coated SS current collector operated under dry air.

[0096] Anode-free metal halide cells with LiI / C composite cathode and SS current collector were prepared using the general procedure discussed above. An artificial SEI layer of polyvinyl alcohol (PVA) polymer was applied to the SS current collector. For this test, 5 wt % PVA in deionized water solution was applied to the SS current collector by a doctor blade method. After drying in an oven at 60°C for 12 hours, the polymer-coated SS was used as the current collector. The assembled coin unit cells were operated with an electrolyte having 0.2 M LiNO3, 0.2 M LiBOB and 0.5 M LiTFSI in DOL / DME solvent at 0.3C in a dry air atmosphere and the resulting cycle life is plotted in Fig.10 middle.

[0097] Example 5: Anode-free metal halide cell assembled with LiI-carbon composite cathode and Ni current collector coated with PVA operated under dry air.

[0098] Anode-free square metal halide cells with LiI / C composite cathode and Ni current collector were prepared by the general procedure discussed above. To create an artificial SEI layer, a PVA polymer coating layer was applied to the Ni current collector. Coin cell cells with electrolytes having 0.2 M LiNO3, 0.2 M LiBOB, and 0.5 M LiTFSI in DOL / DME solvent were assembled in a dry air-filled glove box and operated at 0.3C with a cutoff voltage condition of 2.0 to 3.5 V. The resulting cycle life is plotted in Fig.10 middle.

[0099] Comparative Example 1: Anode-free lithium-ion battery assembled with NMC622 cathode operated under oxygen.

[0100] For comparison, a conventional Li(Ni0.6Mn0.2Co0.2)O2(NMC622) cathode was obtained, along with 1M LiPF6 in EC / DEC (ethylene carbonate / diethyl carbonate) electrolyte, Celgard 2325 separator, and SS current collector. The SS-NMC cell was assembled in a Swagelok cell configuration in an argon-filled glove box. Prior to the charge / discharge test, oxygen was passed into the assembled cell for 30 seconds, and after closing the inlet valve / outlet valve, the cell began to operate under an oxygen environment. In order to deposit lithium on the SS current collector, the cell was charged to a capacity of 1 mAh, and after rinsing the SS substrate with DMC solvent and subsequently drying in vacuo at room temperature for 1 hour, the surface morphology of the deposited lithium was observed by scanning electron microscopy (SEM). Figure 4 As shown in (on the left), sharp needle-like structures (lithium dendrite growth) are formed by lithium deposition, which eventually leads to a short circuit in the battery. Figure 5 As shown in (solid line), the unit cell operated at 0.5 mA for 1 hour showed a low Coulombic efficiency (49%).

[0101] The terms used herein are only used for the purpose of describing specific embodiments and are not intended to limit various embodiments. As used herein, the singular forms "one (kind) (indefinite articles a, an)" and "said (the)" are intended to include plural forms unless the context clearly indicates otherwise. It will be further understood that when used in this specification, the terms "include" and / or "include" indicate the existence of the stated features, wholes, steps, operations, elements, and / or parts (components), but do not exclude the existence of one or more other features, wholes, steps, operations, elements, parts, and / or their groups. In the previous detailed description of the example embodiments of various embodiments, reference was made to the accompanying drawings (where the same numbers represent the same elements), which constitute part thereof, and in which specific example embodiments are shown schematically, in which various embodiments can be practiced. These embodiments are described in sufficient detail so that those skilled in the art can practice these embodiments, but other embodiments may also be used, and logical, mechanical, electrical, and other changes may be made without departing from the scope of various embodiments. In the previous description, many specific details are set forth to provide a thorough understanding of various embodiments. However, various embodiments may also be practiced without these specific details. In other instances, well-known circuits, structures, and techniques have not been shown in detail in order not to obscure the embodiments.

[0102] As used herein, when "plurality" is used in reference to an item, it means one or more items. For example, "plurality of different types of networks" refers to one or more different types of networks.

[0103] When different reference numerals include the same number followed by different letters (e.g., 100a, 100b, 100c) or a punctuation mark followed by different numbers (e.g., 100-1, 100-2, or 100.1, 100.2), the reference character alone, without a letter or a following number (e.g., 100), may refer to the entire group of elements, any subset of the group, or an example sample of the group.

[0104] In addition, the phrase "at least one", when used with a list of items, means that different combinations of one or more of the listed items can be used, and only one of each item in the list may be required. In other words, "at least one" means that any combination of items and numbers of items from the list can be used, but not all items in the list are required. The item can be a specific object, thing, or category.

[0105] For example, without limitation, "at least one of item A, item B, or item C" may include item A, item A and item B, or item B. This example may also include item A, item B, and item C, or item B and item C. Of course, there may be any combination of these items. In some illustrative examples, "at least one" may be, for example, without limitation, two of item A; one of item B; and ten of item C; four of item B; and seven of item C; or other suitable combinations.

[0106] In the above, reference is made to various embodiments. However, it should be understood that the present disclosure is not limited to the specifically described embodiments. On the contrary, any combination of the described features and elements, whether or not related to different embodiments, may be considered for implementation and practice of the present disclosure. Without departing from the scope of the described embodiments, many modifications, changes, and variations may be clear to those of ordinary skill in the art. In addition, although the embodiments of the present disclosure may achieve advantages relative to other possible solutions or relative to the prior art, whether a specific advantage is achieved by a given embodiment is not a limitation of the present disclosure. Therefore, the described aspects, features, embodiments, and advantages are merely illustrative and are not considered as elements or limitations of the appended claims unless expressly stated in the claims. In addition, it is intended that the following statements be interpreted as covering all such changes and modifications falling within the scope of the present invention.

[0107] A non-limiting list of example implementations is provided below to illustrate some aspects of the present disclosure.

[0108] Example embodiment 1 is an anode-free metal halide battery. The anode-free metal halide battery includes: a negative electrode current collector including a passivation layer of an electrically insulating material that allows metal ion transport, an electrolyte including an ion-conducting material, and a cathode including a metal halide salt incorporated into a conductive material, wherein the electrolyte is in contact with the negative electrode current collector and the cathode.

[0109] Example embodiment 2 includes the anode-less metal halide battery of example embodiment 1, including or excluding the optional features. In this example embodiment, the anode-less metal halide battery includes an oxidizing gas.

[0110] Example embodiment 3 includes the anode-less metal halide battery of any one of example embodiments 1 to 2, including or excluding the optional features. In this example embodiment, the passivation layer is naturally generated on the negative electrode current collector in contact with the electrolyte.

[0111] Example embodiment 4 includes the anode-less metal halide battery of any one of example embodiments 1 to 3, including or excluding the optional features. In this example embodiment, the conductive material is a porous carbon material, forming a metal halide-carbon composite cathode.

[0112] Example embodiment 5 includes the anode-free metal halide battery of any one of example embodiments 1 to 4, including or excluding the optional features. In this example embodiment, the electrolyte is selected from a liquid electrolyte, a gel polymer electrolyte, a solid polymer electrolyte, a ceramic-based electrolyte, a polymer-ceramic composite electrolyte, and combinations thereof.

[0113] Example embodiment 6 includes the anode-free metal halide battery described in any of example embodiments 1 to 5, including or excluding the optional features. In this example embodiment, the passivation layer includes an artificially formed ion-conducting material. Optionally, the ion-conducting material is selected from linear polymers, cross-linked polymers, star polymers, block copolymers, metal oxides, and combinations thereof. Optionally, the ion-conducting material further comprises an inorganic filler selected from carbon nanotubes, nanoparticles, polyhedral oligomeric silsesquioxane (POSS) compounds, and combinations thereof.

[0114] Example embodiment 7 includes the anode-free metal halide battery of any one of example embodiments 1 to 6, including or excluding the optional features. In this example embodiment, the anode-free metal halide battery includes a non-conductive separator between the negative electrode current collector and the cathode.

[0115] Example embodiment 8 includes the anode-less metal halide battery of any one of example embodiments 1 to 7, including or excluding the optional features. In this example embodiment, the thickness of the passivation layer is in the range of 0.1 nanometers to 20 micrometers.

[0116] Example embodiment 9 includes the anode-less metal halide battery of any one of example embodiments 1 to 8, including or excluding the optional features. In this example embodiment, the thickness of the passivation layer is 0.1 nanometers to 1 micrometer.

[0117] Example embodiment 10 includes the anode-less metal halide battery of any one of example embodiments 1 to 9, including or excluding the optional features. In this example embodiment, the negative electrode current collector acts as an anode when a metal is deposited thereon.

[0118] Example embodiment 11 includes the anode-less metal halide battery of any one of example embodiments 1 to 10, including or excluding the optional features. In this example embodiment, the negative electrode current collector is a metal foil located at the negative terminal of the battery.

[0119] Example embodiment 12 includes the anode-free metal halide battery of any one of example embodiments 1 to 11, including or excluding the optional features. In this example embodiment, the anode-free metal halide battery includes a positive electrode current collector.

[0120] Example embodiment 13 is an anode-free metal halide battery. The anode-free metal halide battery includes a negative electrode current collector, an electrolyte comprising a solvent and at least one ion-conducting salt, and a cathode comprising a metal halide compound deposited on a conductive carbon material, wherein the electrolyte is in contact with the negative electrode current collector and the cathode.

[0121] Example embodiment 14 includes the anode-free metal halide battery of example embodiment 13, including or excluding the optional features. In this example embodiment, the cathode includes lithium ions deposited on a porous carbon material. Optionally, the porous carbon material is a LiI-carbon composite.

[0122] Example embodiment 15 includes the anode-free metal halide battery of any of example embodiments 13 to 14, including or excluding the optional features. In this example embodiment, the passivation layer includes an artificially formed ion-conducting material. Optionally, the ion-conducting material is selected from polyvinyl alcohol (PVA) and poly(ethylene glycol) (PEG) copolymerized with polyhedral oligomeric silsesquioxane (POSS).

[0123] Example embodiment 16 includes the anode-free metal halide battery of any one of example embodiments 13 to 15, including or excluding the optional features. In this example embodiment, the anode-free metal halide battery includes a separator between the negative current collector and the cathode.

[0124] Example embodiment 17 includes the anode-less metal halide battery of any one of example embodiments 13 to 16, including or excluding the optional features. In this example embodiment, the thickness of the passivation layer is in the range of 0.1 nanometers to 20 micrometers.

[0125] Example embodiment 18 is a method of forming an anode-free metal halide battery. The method includes forming a metal halide battery cell, wherein the metal halide battery cell includes a negative current collector and does not include a separate anode. The method further includes applying a charging voltage to the metal halide battery cell to cause metal ions to be reduced to corresponding metals on the negative current collector.

[0126] Example embodiment 19 includes the method of example embodiment 18, including or excluding optional features. In this example embodiment, the metal halide battery cell further includes a passivation layer on top of the negative current collector, an electrolyte comprising a solvent and at least one ion-conducting salt, and a cathode comprising a metal halide compound deposited on a conductive material, wherein the electrolyte is in contact with the negative current collector and the cathode. Optionally, the passivation layer comprises an artificially formed ion-conducting material selected from polyvinyl alcohol (PVA) and poly(ethylene glycol) (PEG) copolymerized with polyhedral oligomeric silsesquioxane (POSS). Optionally, the cathode comprises lithium iodide deposited on a porous carbon material, and wherein applying a charging voltage to the battery cell causes lithium ions released from the cathode to be reduced to lithium metal on the negative current collector.

Claims

1. Anode-free metal halide battery comprising: a negative electrode current collector comprising a passivation layer of an electrically insulating material that allows for the transport of metal ions; an electrolyte comprising an ion-conducting material; and A cathode comprising a metal halide salt incorporated into a conductive material, wherein the electrolyte is in contact with the negative current collector and the cathode.

2. The battery of claim 1, further comprising an oxidizing gas. 3 . The battery of claim 1 , wherein the passivation layer is naturally generated on the negative electrode current collector in contact with the electrolyte.

4. The battery of claim 1, wherein the conductive material is a porous carbon material forming a metal halide-carbon composite cathode.

5. The battery of claim 1, wherein the electrolyte is selected from the group consisting of a liquid electrolyte, a gel polymer electrolyte, a solid polymer electrolyte, a ceramic-based electrolyte, a polymer-ceramic composite electrolyte, and combinations thereof.

6. The battery of claim 1, wherein the passivation layer comprises an artificially formed ion-conducting material.

7. The battery of claim 6, wherein the ion-conducting material is selected from the group consisting of linear polymers, cross-linked polymers, star polymers, block copolymers, metal oxides, and combinations thereof.

8. The battery of claim 6, wherein the ion-conducting material further comprises an inorganic filler selected from the group consisting of carbon nanotubes, nanoparticles, polyhedral oligomeric silsesquioxane (POSS) compounds, and combinations thereof.

9. The battery of claim 1, further comprising: A non-conductive separator is interposed between the negative electrode current collector and the cathode.

10. The battery of claim 1, wherein the thickness of the passivation layer is in the range of 0.1 nanometers to 20 micrometers.

11. The battery of claim 1, wherein the thickness of the passivation layer is between 0.1 nanometers and 1 micrometer.

12. The battery of claim 1, wherein the negative current collector acts as an anode when a metal is deposited thereon.

13. The battery of claim 1, wherein the negative current collector is a metal foil located at the negative terminal of the battery.

14. The battery of claim 1, further comprising a positive current collector.

15. Anode-less metal halide battery, comprising: Anode current collector; an electrolyte comprising a solvent and at least one ion-conducting salt; and A cathode comprising a metal halide compound deposited on a conductive carbon material, wherein the electrolyte is in contact with the negative current collector and the cathode.

16. The battery of claim 15, wherein the cathode comprises lithium ions deposited on a porous carbon material.

17. The battery according to claim 16, wherein the porous carbon material is a LiI-carbon composite.

18. The battery of claim 15, wherein the passivation layer comprises an artificially formed ion-conducting material.

19. The battery of claim 18, wherein the ion-conducting material is selected from: Polyvinyl alcohol (PVA); polyethylene glycol (PEG) copolymerized with polyhedral oligomeric silsesquioxane (POSS); Polyethylene glycol; Polypropylene glycol; Polycarbonate; Polyester; Polyethylene oxide (PEO); Polyurethane (PU); Styrene-butadiene rubber (SBR); Polyvinylidene fluoride (PVDF); and Polytetrafluoroethylene (PTFE).

20. The battery of claim 15, further comprising: A separator is disposed between the negative electrode collector and the cathode.

21. The battery of claim 15, wherein the thickness of the passivation layer is in the range of 0.1 nm to 20 μm.

22. A method of forming an anode-less metal halide battery, the method comprising: forming a metal halide battery cell, wherein the metal halide battery cell includes a negative current collector and does not include a separate anode; as well as A charging voltage is applied to the metal halide battery cell to cause metal ions to be reduced to corresponding metals on the negative current collector.

23. The method of claim 22, wherein the metal halide battery cell further comprises: a passivation layer on top of the negative electrode current collector; an electrolyte comprising a solvent and at least one ion-conducting salt; as well as A cathode comprising a metal halide compound deposited on a conductive material, wherein the electrolyte is in contact with the negative current collector and the cathode.

24. The method of claim 23, wherein the passivation layer comprises an artificially formed ion-conducting material selected from the group consisting of: Polyvinyl alcohol (PVA); polyethylene glycol (PEG) copolymerized with polyhedral oligomeric silsesquioxane (POSS); Polyethylene glycol; Polypropylene glycol; Polycarbonate; Polyester; Polyethylene oxide (PEO); Polyurethane (PU); Styrene-butadiene rubber (SBR); Polyvinylidene fluoride (PVDF); and Polytetrafluoroethylene (PTFE).

25. The method of claim 23, wherein the cathode comprises lithium iodide deposited on a porous carbon material, and wherein applying a charging voltage to the battery cell causes lithium ions released from the cathode to be reduced to lithium metal at the negative current collector.