Antibacterial and antioxidant pH indicating multifunctional medical gauze and preparation method thereof
By using dimethyl diallylammonium chloride, diallylamine, carboxyethyl acrylate and tannic acid treatment methods, medical gauze with pH indicating, antibacterial and antioxidant functions was prepared, solving the traditional problem of Gauze cannot observe wounds and infection problems in time, achieving accelerated wound healing and reduced infection.
Patent Information
- Application Number
- CN202410842076.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-08
AI Technical Summary
Traditional medical gauze cannot observe the wound condition in time, may lead to bacterial infection, and lacks antibacterial and antioxidant functions, affecting wound healing.
A terpolymer of dimethyl diallylammonium chloride, diallylamine, and carboxyethyl acrylate is used as a cationic modifier, combined with tannic acid treatment, to prepare a product with pH indicating, antibacterial and antioxidant functions. medical gauze.
It achieves non-destructive display of wound infection signals, reduces exogenous infection, accelerates wound healing, and improves the antibacterial and antioxidant properties of gauze.
Smart Images

Figure CN118743774A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of biomedical materials, and particularly relates to a pH-indicating multifunctional medical gauze with antibacterial and anti-oxidation properties and a preparation method thereof. Background Art
[0002] Skin is the largest organ in the human body and the first barrier to protect the human body. In daily life, due to some accidents, normal skin may be damaged and wounds may be formed. Skin wounds may cause a series of body problems such as bacterial infection, excessive loss of water and protein, etc. Therefore, after skin injury, medical gauze is usually needed to protect the wound, prevent wound infection and severe dehydration, provide a moist environment conducive to wound healing, and promote wound healing.
[0003] Traditional medical gauze is generally opaque, and the wound condition cannot be observed in time. The gauze needs to be uncovered, which is troublesome to operate, and bacteria may enter the wound when the gauze is uncovered, causing infection to the wound. Therefore, wound care urgently needs to develop gauze with wound infection indicator function.
[0004] In addition, bacterial infection of wounds is the most common complication of trauma, which may cause fever, redness, pain and other problems on the wound skin, and even lead to serious diseases such as swelling, suppuration, sepsis, etc. Medical gauze with certain antibacterial and antioxidant functions can not only effectively reduce exogenous infection, but also help accelerate wound healing.
[0005] Based on this, it is a technical problem that urgently needs to be solved to provide a medical gauze and its preparation method that can display visual signals of wound infection in a non-destructive way, guide medical staff to adopt timely and reasonable response measures, and at the same time play an antibacterial and antioxidant role, reduce exogenous infection, and accelerate wound healing. Summary of the invention
[0006] One of the purposes of the present invention is to provide a pH indicating multifunctional medical gauze with antibacterial and antioxidant properties and a preparation method thereof.
[0007] The second object of the present invention is to provide a pH indicating multifunctional medical gauze with antibacterial and antioxidant properties.
[0008] The technical solution adopted by the present invention to achieve one of the purposes is: to provide a method for preparing a pH-indicating multifunctional medical gauze with antibacterial and antioxidant properties, comprising the following steps: S1. Prepare a cationic modifier using dimethyldiallylammonium chloride, diallylamine and carboxyethyl acrylate as raw materials; S2, immersing the medical gauze in an aqueous solution of a cationic modifier to obtain a first product through a first modification reaction; S3, immersing the first product in a dye solution, dyeing and drying, to obtain a second product; immersing the second product in an aqueous solution of a mordant, mordanting, washing and drying, to obtain a third product; S4. Immersing the third product in an aqueous solution of tannic acid, undergoing a second modification reaction, and then washing and drying, thereby obtaining a pH indicating multifunctional medical gauze having antibacterial and antioxidant properties.
[0009] The general idea of the present invention is as follows: First, the present invention utilizes a homemade cationic modifier to perform a first modification treatment on medical gauze. Conventional cationic modifiers include quaternary ammonium compound cationic modifiers, natural cationic modifiers and the like. Quaternary ammonium compound cationic modifiers, such as 3-chloro-2-hydroxypropyltrimethylammonium chloride, have a relatively small molecular weight, can enter the interior of the fiber, and are uniformly modified, but have a relatively weak affinity with cotton fibers, resulting in very poor grafting on cotton fabrics; and natural cationic modifiers, such as chitosan, have poor water solubility, are not easy to be modified and finished by a traditional rolling and baking finishing method, and the fabric after being finished with chitosan feels hard, and the wearing properties such as whiteness and air permeability are greatly reduced, and the bonding force between the fabric and the fiber is not strong, and the washing resistance is relatively poor.
[0010] The cationic modifier used in the present invention is a terpolymer of diallyldimethylammonium chloride (DMDAAC), diallylamine (DAA), and carboxyethylacrylate (β-CEA). Considering that polydiallyldimethylammonium chloride only relies on the interaction between its positive charge and the negatively charged dye to achieve the purpose of color fixation, and its wet rubbing fastness is relatively poor, in order to improve its color fastness, the present invention introduces diallylamine and carboxyethylacrylate into the main chain of the polydiallyldimethylammonium chloride molecule for modification, which can increase the cross-linking effect between the molecular chain and the active group of the cotton fiber, thereby achieving a relatively ideal wet rubbing fastness effect.
[0011] Among them, diallylamine is composed of two allyl groups and one amino group, which can undergo oxidation reaction and addition reaction, and the amino group can also undergo all types of reactions of the amino group. Diallylamine (DAA) is mainly used as a pharmaceutical intermediate, an organic intermediate and a raw material for organic synthesis, and can also be used as a polymer monomer to prepare amphoteric polymers and crosslinking agents. In the DAA segment, the -NH- group can react with the hydroxyl group on the fiber to form a covalent bond. At the same time, the five-membered ring structure formed by DMDAAC and DAA can also be tightly bound to the fiber through van der Waals force and hydrogen bond, so that the wet fastness of the finished fabric is significantly improved compared with the single finishing of polydimethyldiallylammonium chloride (PDMDAAC). In addition, the introduction of DAA segments can also appropriately reduce the water solubility of the polymer, which has a certain effect on the improvement of the wet fastness of water immersion. Carboxyethyl acrylate adds carboxyl groups to the ternary polymer structure, which can cross-link with the hydroxyl group on the cotton fiber, improve the binding force between the dye and the fiber, and further improve the wet fastness.
[0012] Secondly, the present invention dyes and mordants the medical gauze after the first modified pretreatment, applies the color-changing textile to the medical gauze, and obtains a medical gauze based on pH color change indication. The pH value of the normal human skin surface is about 5 to 6. During the wound healing process, the pH value of the skin surface will change. When the wound is inflamed, the pH value of the skin surface is greater than 7. In the preparation process of the medical gauze, the present invention adds a dye solution with a pH indication function to obtain a color-changing medical gauze. The degree of wound healing can be understood only by observing the change in the color of the gauze, achieving the effect of displaying visual signals of wound infection in a non-destructive manner and guiding medical staff.
[0013] Finally, the present invention uses an aqueous solution of tannic acid to perform a second modification treatment on the gauze after dyeing and mordant treatment. Tannic acid is a natural plant polyphenol that contains a large amount of hydroxyl and carbonyl groups, has strong biological and surface activity, and has antioxidant, anticancer, antibacterial and disinfectant effects. The pH indicating gauze is treated with tannic acid to cause a complex reaction between its two adjacent phenolic hydroxyl groups and metal ions and dye molecules to form a stable chelate, thereby functionalizing the pH indicating gauze and giving it multiple functions of good antibacterial, antioxidant and color change indication. In addition, compared with other common plant polyphenols (such as tea polyphenols, chlorogenic acid and gallic acid, etc.), tannic acid is used in the medical gauze of the present invention, and has the following additional advantages: First, tannic acid has an amphiphilic structure and contains a large number of catechol groups in its molecules. Two adjacent phenolic hydroxyl groups can react with metal ions in the form of oxygen anions to form stable hydrophobic chelates. At the same time, tannic acid has strong interfacial adhesion, which can make the chelates formed by other metal ions adhere stably to the surface of the substrate. Second, tannic acid, tea polyphenols, chlorogenic acid and gallic acid are all polyphenol compounds, which have antioxidant and other health benefits; however, the molecular weight of tannic acid is relatively large compared to the other types, which is 1701.2. Within a certain range, polyphenols with larger molecular weight have stronger binding force with proteins and stronger antibacterial properties; Third, compared with other natural polyphenol compounds, tannic acid contains more phenolic hydroxyl groups and has better antibacterial and antioxidant properties.
[0014] Fourth, natural polyphenol tannic acid (TA), whose content in nature is second only to cellulose, is widely found in many plants such as oak, chestnut, and hemlock. It is not only cheap and harmless to the environment, but also can be widely used and has good biocompatibility.
[0015] In the present invention, the cationic modifier and tannic acid play a synergistic role: after the medical gauze is treated with the cationic modifier, the dyeing time is reduced, the wet processing fastness of the dye is improved, and the large molecular weight modifier is mainly adsorbed on the fiber surface and enters less into the fiber interior, so at the same dye concentration, the apparent color of the fiber is darker. In addition, after the cationic modification, the rate of tannic acid adsorbing on the fiber surface can also be increased, so that it can be adsorbed on the fiber faster and better, thereby giving the medical gauze better antibacterial and antioxidant effects. Further, after the tannic acid modification treatment, a network cross-linked structure is formed between the tannic acid and the dye and the mordant, which can further increase the wet processing fastness of the dye. The combined use of tannic acid and the cationic modifier improves the apparent color depth and washing fastness of the color-changing dye, so that the medical gauze has a more obvious pH color change effect, and also gives the medical gauze good antibacterial and antioxidant properties.
[0016] Furthermore, in step S1, the preparation method of the cationic modifier includes: mixing dimethyldiallylammonium chloride, diallylamine, and carboxyethyl acrylate in a certain proportion, adding a pH adjuster and a chelating agent, heating to a reaction temperature under stirring conditions, adding an initiator, and performing a polymerization reaction to obtain a cationic modifier.
[0017] Furthermore, in step S1, the mass ratio of dimethyldiallylammonium chloride, diallylamine and carboxyethyl acrylate is (90-100):(10-20):(10-20).
[0018] Furthermore, in the preparation method of the cationic modifier, the pH regulator is selected from one of acetic acid and formic acid; and the chelating agent is selected from one of tetrasodium ethylenediaminetetraacetate and disodium ethylenediaminetetraacetate.
[0019] Among them, the pH regulator adjusts the pH of the reaction system, which is beneficial to the polymerization reaction; considering that heavy metal ions may exist in the reaction system of the present invention (for example, Fe 2+ , Cu 2 + Chelating agents can form stable complexes with trace metal ions in the reaction solution, eliminating the adverse effects of trace metal ions on the polymerization reaction.
[0020] Preferably, the amount of the pH adjuster is 10%-20% of the total weight of the raw materials, and the amount of the chelating agent is 0.06‰-0.1‰ of the total weight of the raw materials.
[0021] Furthermore, in the preparation method of the cationic modifier, the initiator comprises a combination of one or more of an ammonium persulfate-sodium bisulfite system, a potassium persulfate-sodium sulfite system, and an ammonium persulfate-ascorbic acid system. Preferably, the initiator is composed of sodium bisulfite and ammonium persulfate, and the amounts of the two are 0.5%-2% of the total weight of the raw materials, respectively. The redox system of the ammonium persulfate-sodium bisulfite combination can reduce the decomposition activation energy, so that the polymerization reaction can be carried out at a relatively low temperature, which is conducive to saving energy and improving polymer properties.
[0022] Preferably, in the method for preparing the cationic modifier, the polymerization reaction temperature is 70-90° C., and the polymerization reaction time is 3-5 h.
[0023] Furthermore, in step S2, the concentration of the cationic modifier in the aqueous solution of the cationic modifier is 0.1-1.5 g / L; the bath ratio (i.e., the mass ratio of the medical gauze to the aqueous solution of the cationic modifier) is 1:(40-60). Preferably, the temperature of the first modification reaction is 20-60°C and the time is 10-30 min.
[0024] Furthermore, the dyeing process of the medical gauze of the present invention includes two steps: dyeing treatment and mordant treatment. In the dyeing treatment, dye molecules are adsorbed from the dye solution to the surface of the cationic modified cotton fiber through electrostatic attraction to color the fiber; in the mordant process, a chelate structure is formed between the mordant and the dye to improve the wet fastness of the dye.
[0025] Preferably, in step S3, the dye in the dye liquor includes one of brilliant yellow, bromothymol blue and phenol red; the bath ratio of the first product to the dye liquor is 1:(40-60); the mass ratio of the dye to the first product is (1-10):100; the temperature of the dyeing treatment is 20-90°C and the time is 5-20min.
[0026] Preferably, in step S3, the mordant includes a combination of one or more of potassium aluminum sulfate dodecahydrate, ferric sulfate, and ferrous sulfate heptahydrate; the concentration of the mordant in the aqueous solution of the mordant is 0.5-4 g / L; the temperature of the mordant treatment is 50-90° C., and the time is 20-50 min.
[0027] Furthermore, in step S4, the mass ratio of tannic acid to the third product is (10-50):100; preferably (30-50):100; the temperature of the second modification reaction is 50-80°C, and the time is 30-90 min.
[0028] In the process of modifying medical gauze with an aqueous solution of tannic acid, the adsorption of tannic acid on cotton fibers involves multiple interactions such as ionic bonds, van der Waals forces, and hydrogen bonds. Cotton fibers modified with cations are positively charged under acidic conditions, which is conducive to the adsorption of tannic acid. However, if the pH is too low, the adsorption rate may be too fast and uneven, and the glycosidic bonds in the cellulose macromolecules of the cotton fibers may be hydrolyzed, resulting in a decrease in the degree of polymerization, thereby deteriorating the strength of the cotton fibers. Preferably, in step S4, the pH value of the aqueous solution of tannic acid is controlled to be 2.5-3.5.
[0029] The technical solution adopted by the present invention to achieve the second purpose is: to provide a pH indicating multifunctional medical gauze with antibacterial and antioxidant properties, which is prepared by the preparation method according to one of the purposes of the present invention.
[0030] Compared with the prior art, the present invention has the following beneficial effects: (1) The present invention provides a method for preparing a pH-indicating multifunctional medical gauze with antibacterial and antioxidant properties. The cationic modifier used is a terpolymer of diallyldimethylammonium chloride, diallylamine, and carboxyethyl acrylate. The molecular weight is increased and reactive groups are introduced on the basis of polydiallyldimethylammonium chloride. The relative molecular weight is large, the cationic property is strong, the adsorption rate is fast, the intermolecular force between the fibers is strong, and the active groups that can react with the fibers are increased. The durability is good and the dosage is low. Moreover, the high molecular weight modifier is mainly adsorbed on the fiber surface and enters less into the fiber interior. Therefore, at the same dye concentration, the apparent color of the fiber is darker.
[0031] (2) The present invention provides a method for preparing a pH-indicating multifunctional medical gauze with antibacterial and antioxidant properties. Before dyeing and mordanting, the medical gauze is subjected to cation modification, which exhibits positive charge and can quickly adsorb dye anions, thereby reducing dyeing time, increasing dyeing efficiency, and improving dyeing fastness.
[0032] (3) The preparation method of the pH-indicating multifunctional medical gauze with antibacterial and antioxidant properties provided by the present invention uses a cationic modifier to modify the medical gauze. During the dyeing process, no electrolyte is added, and the dyeing can be performed in a shorter time and with less energy consumption, thereby reducing wastewater discharge and achieving an ecological and environmentally friendly effect. In contrast, in the conventional dyeing process, in order to promote dyeing and improve dye utilization, a large amount of neutral electrolyte needs to be added during dyeing, but the electrolyte causes the ecological environment and water resources to be damaged, causing the soil around the river to become salinized, and it is difficult to handle and cannot be biodegraded.
[0033] (4) The preparation method of the pH indicating multifunctional medical gauze with antibacterial and antioxidant properties provided by the present invention comprises the following steps: using tannic acid to perform a second modification treatment on the medical gauze after dyeing and mordanting treatment. Tannic acid is a natural plant polyphenol, containing a large number of hydroxyl groups and carbonyl groups, having strong biological and surface activity, and having antioxidant, anticancer, antibacterial and disinfection effects. The present invention selects tannic acid to treat the pH indicating gauze. Tannic acid has a large molecular weight and can block some of the fiber pores, reducing the desorption of the dye inside the fiber. At the same time, tannic acid contains a large number of pyrogallol structures, which can provide lone pairs of electrons. During the coordination reaction, although the third phenolic hydroxyl group does not participate in the binding, this phenolic hydroxyl group can promote the dissociation of the other two phenolic hydroxyl groups, which is conducive to the formation of a stable chelate with metal ions. This chelate can form a coating on the fiber surface, increasing the fastness of dyes, tannic acid and other compounds on the fiber surface. Moreover, tannic acid can also give the pH indicating medical gauze more functions, so that it has good antibacterial, antioxidant and color change indication multiple functions.
[0034] (5) Based on the characteristics of skin pH changes during the healing process of human wounds, the present invention uses a relatively simple and cost-effective technology to prepare a pH-indicating multifunctional medical gauze with antibacterial and antioxidant properties. The medical gauze displays a visual signal in a non-destructive manner as the pH value of the external environment changes, guiding medical staff to adopt timely and reasonable response measures. At the same time, the gauze plays an antibacterial and antioxidant role, reduces exogenous infection, and accelerates wound healing. It has broad promotion and application prospects in the field of medical materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 The figures are scanning electron microscope images of the original medical gauze and the antibacterial and antioxidant pH-indicating multifunctional medical gauze prepared in Example 1 of the present invention; wherein (a) is the original medical gauze; (b) is the multifunctional medical gauze prepared in Example 1; Figure 2 This is a color diagram of the antibacterial and antioxidant pH-indicating multifunctional medical gauze prepared in Example 1 of the present invention in different pH buffer solutions. DETAILED DESCRIPTION
[0036] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0037] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other.
[0038] The embodiment of the present invention provides a method for preparing a pH-indicating multifunctional medical gauze with antibacterial and antioxidant properties, comprising the following steps: Step 1: Mix dimethyldiallylammonium chloride, diallylamine, and carboxyethyl acrylate in a mass ratio of (90-100): (10-20): (10-20), add a pH adjuster, a chelating agent, and deionized water, heat to the reaction temperature under stirring, add an initiator, and polymerize at 70-90° C. for 3-5 hours to obtain a cationic modifier.
[0039] The pH regulator is selected from a combination of one or more of acetic acid and formic acid; the chelating agent is selected from a combination of one or more of ethylenediaminetetraacetic acid tetrasodium and ethylenediaminetetraacetic acid disodium. The amount of the pH regulator is 10%-20% of the total weight of the monomer, and the amount of the chelating agent is 0.06‰-0.1‰ of the total weight of the monomer; the initiator includes sodium bisulfite and ammonium persulfate, and the amount of the two is 0.5%-2% of the total weight of the monomer.
[0040] Step 2: according to the bath ratio of medical gauze to the aqueous solution of the cationic modifier being 1:(40-60), immersing the medical gauze in an aqueous solution of the cationic modifier having a concentration of 0.1-1.5 g / L, reacting at 20-60° C. for 10-30 minutes to obtain a first product; Step 3: according to the bath ratio of the first product to the dye liquor being 1:(40-60) and the mass ratio of the dye to the first product being (1-10):100, the first product is immersed in the dye liquor, dyeing is performed at 20-90° C. for 5-20 minutes, and drying is performed to obtain a second product; the second product is immersed in an aqueous solution with a concentration of 0.5-4 g / L of a mordant, mordant-dyeing is performed at 50-90° C. for 20-50 minutes, and then washed and dried to obtain a third product; The dye in the dye solution includes one of brilliant yellow, bromothymol blue and phenol red; the mordant includes one or more of potassium aluminum sulfate dodecahydrate, ferric sulfate and ferrous sulfate heptahydrate.
[0041] Step 4: According to the mass ratio of tannic acid to the third product being (10-50):100, the third product is immersed in an aqueous solution of tannic acid with a pH value of 2.5-3.5, and reacted at 50-80° C. for 30-90 minutes. The product is washed and dried to obtain a pH indicating multifunctional medical gauze with antibacterial and antioxidant properties.
[0042] The present invention will be further described below in conjunction with specific embodiments, but the present invention is not limited thereto.
[0043] Example 1 The preparation process of antibacterial and antioxidant pH-indicating multifunctional medical gauze is as follows: Step 1: According to the mass ratio of monomers being 100:15:10, add dimethyldiallylammonium chloride aqueous solution (60wt%), diallylamine, and carboxyethyl acrylate into a three-necked flask, followed by adding 10% (owm) acetic acid, 0.1‰ (owm) tetrasodium ethylenediaminetetraacetate and deionized water, stirring evenly on a magnetic stirrer and heating to 80°C, then adding initiators 0.6% (owm) ammonium persulfate and 0.6% (owm) sodium bisulfite in batches, and reacting at 80°C for 4h to obtain a cationic modifier.
[0044] Step 2: Weigh the cationic modifier, add deionized water to dissolve it, and then transfer it to a volumetric flask to make a cationic modifier solution with a concentration of 1g / L; pour 50ml of the cationic modifier solution into a conical flask, add 1g of medical gauze, and react in a room temperature oscillation dyeing machine at 60℃ for 30min. After the reaction, take out the medical gauze and dry it.
[0045] Step 3: weigh the dye brilliant yellow and add deionized water to prepare a mother liquor, prepare 50 ml of dye solution with the mother liquor and deionized water according to a certain bath ratio, and the dye dosage is 5% owf; immerse the medical gauze in step 2 in the dye solution, react at 90° C. in a normal temperature oscillation dyeing machine for 20 minutes, take out the medical gauze and dry it; weigh the mordant potassium aluminum sulfate dodecahydrate, add deionized water to prepare a mordant solution with a concentration of 3g / L, immerse the dyed medical gauze in the mordant solution, react at 80° C. in a normal temperature oscillation dyeing machine for 20 minutes, take out the medical gauze after the reaction, wash it with water, soap it, and dry it.
[0046] Step 4: Weigh 50% (owf) tannic acid into a conical flask, add deionized water, adjust the pH value of the solution to 3, and prepare a tannic acid solution; immerse the medical gauze in step 3 in the tannic acid solution, react at 70°C in a normal temperature oscillating dyeing machine for 60 minutes, take out the medical gauze after the reaction, wash with water, soap, and dry, and prepare a pH indicating multifunctional medical gauze with antibacterial and antioxidant properties.
[0047] Figure 1The following are scanning electron microscope images of the original medical gauze and the antibacterial and antioxidant pH-indicating multifunctional medical gauze prepared in Example 1 of the present invention. Figure 1 It can be seen that the medical gauze is Figure 1 The fiber surface of (a) is relatively smooth, with clear texture and natural curl; the multifunctional medical gauze prepared in Example 1 Figure 1 (b) There is a coating and a small amount of fine particles on the fiber surface. This is because tannic acid can be deposited on the fiber surface to form a strong adhesion layer. At the same time, tannic acid contains a large amount of pyrogallol structure, which can provide lone pair electrons, which is conducive to the formation of stable chelates with metal ions and dyes. This chelate can form a coating on the fiber surface.
[0048] Figure 2 This is a color diagram of the antibacterial and antioxidant pH-indicating multifunctional medical gauze prepared in Example 1 of the present invention in different pH buffer solutions. Figure 2 It can be seen that the medical gauze has a more obvious color change between pH 5-8. When the pH is less than 7, the gauze is yellow. When the pH is greater than or equal to 7, the gauze changes from yellow to red, with a relatively obvious color change perceptible to the naked eye, indicating that the medical gauze prepared in this embodiment has good pH indicating performance.
[0049] Example 2 The preparation process of antibacterial and antioxidant pH-indicating multifunctional medical gauze is as follows: Step 1: According to the mass ratio of monomers of 100:10:15, add dimethyldiallylammonium chloride aqueous solution (60wt%), diallylamine, and carboxyethyl acrylate into a three-necked flask, then add 10% (owm) acetic acid, 0.1‰ (owm) tetrasodium ethylenediaminetetraacetate and deionized water, stir evenly on a magnetic stirrer and heat to 85°C, then add initiators 0.6% (owm) ammonium persulfate and 0.6% (owm) sodium bisulfite in batches, and react at 85°C for 3h to obtain a cationic modifier.
[0050] Step 2: Weigh the cationic modifier, add deionized water to dissolve it, and then transfer it into a volumetric flask to make a cationic modifier solution with a concentration of 0.5g / L; pour 40ml of the cationic modifier solution into a conical flask, add 1g of medical gauze, and react in a room temperature oscillation dyeing machine at 50℃ for 10min. After the reaction, take out the medical gauze and dry it.
[0051] Step 3: weigh the dye brilliant yellow and add deionized water to prepare a mother liquor, prepare 50 ml of dye liquor with the mother liquor and deionized water according to a certain bath ratio, and the dye dosage is 8% owf; immerse the medical gauze in step 2 in the dye liquor, react at 40°C in a normal temperature oscillation dyeing machine for 15 minutes, take out the medical gauze and dry it; weigh the mordant potassium aluminum sulfate dodecahydrate, add deionized water to prepare a mordant solution with a concentration of 1g / L, immerse the dyed medical gauze in the mordant solution, react at 65°C in a normal temperature oscillation dyeing machine for 40 minutes, and take out the medical gauze after the reaction, wash it with water, soap it, and dry it.
[0052] Step 4: Weigh 40% (owf) tannic acid into a conical flask, add deionized water, adjust the pH value of the solution to 3.5, and prepare a tannic acid solution. Immerse the medical gauze in step 3 in the tannic acid solution, react at 50°C in a normal temperature oscillating dyeing machine for 70 minutes, take out the medical gauze after the reaction, wash with water, soap, and dry, and prepare a pH indicating multifunctional medical gauze with antibacterial and antioxidant properties.
[0053] Example 3 The preparation process of antibacterial and antioxidant pH-indicating multifunctional medical gauze is as follows: Step 1: According to the mass ratio of monomers being 100:20:10, add dimethyldiallylammonium chloride aqueous solution (60wt%), diallylamine, and carboxyethyl acrylate into a three-necked flask, followed by adding 10% (owm) acetic acid, 0.1‰ (owm) tetrasodium ethylenediaminetetraacetate and deionized water, stirring evenly on a magnetic stirrer and heating to 80°C, then adding initiators 0.6% (owm) ammonium persulfate and 0.6% (owm) sodium bisulfite in batches, and reacting at 80°C for 4h to obtain a cationic modifier.
[0054] Step 2: Weigh the cationic modifier, add deionized water to dissolve it, and then transfer it into a volumetric flask to make a cationic modifier solution with a concentration of 1.5g / L; pour 60ml of the cationic modifier solution into a conical flask, add 1g of medical gauze, and react in a room temperature oscillation dyeing machine at 45℃ for 15min. After the reaction, take out the medical gauze and dry it.
[0055] Step 3: weigh the dye brilliant yellow and add deionized water to prepare a mother liquor, prepare 50 ml of dye liquor with the mother liquor and deionized water according to a certain bath ratio, and the dye dosage is 12% owf; immerse the medical gauze in step 2 in the dye liquor, react at 60° C. in a normal temperature oscillation dyeing machine for 10 minutes, take out the medical gauze and dry it; weigh the mordant potassium aluminum sulfate dodecahydrate, add deionized water to prepare a mordant solution with a concentration of 2g / L, immerse the dyed medical gauze in the mordant solution, react at 70° C. in a normal temperature oscillation dyeing machine for 35 minutes, and take out the medical gauze after the reaction, wash it with water, soap it, and dry it.
[0056] Step 4: Weigh 30% (owf) tannic acid into a conical flask, add deionized water, adjust the pH value of the solution to 3, and prepare a tannic acid solution; immerse the medical gauze in step 3 in the tannic acid solution, react at 70°C in a room temperature oscillation dyeing machine for 55 minutes, take out the medical gauze after the reaction, wash with water, wash with soap, and dry it to prepare a pH indicating multifunctional medical gauze with antibacterial and antioxidant properties.
[0057] Example 4 The preparation process of antibacterial and antioxidant pH-indicating multifunctional medical gauze is as follows: Step 1: Add dimethyldiallylammonium chloride aqueous solution (60wt%), diallylamine, and carboxyethyl acrylate into a three-necked flask according to the mass ratio of the monomers of 90:10:15, and then add 10% (owm) acetic acid, 0.1‰ (owm) tetrasodium ethylenediaminetetraacetate and deionized water, stir evenly on a magnetic stirrer and heat to 80°C, then add initiators 0.6% (owm) ammonium persulfate and 0.6% (owm) sodium bisulfite in batches, and react at 80°C for 5h to obtain a cationic modifier.
[0058] Step 2: Weigh the cationic modifier, add deionized water to dissolve it, and then transfer it into a volumetric flask to make a cationic modifier solution with a concentration of 0.1g / L; pour 50ml of the cationic modifier solution into a conical flask, add 1g of medical gauze, and react in a room temperature oscillation dyeing machine at 20℃ for 30min. After the reaction, take out the medical gauze and dry it.
[0059] Step 3: weigh the dye brilliant yellow and add deionized water to prepare a mother liquor, prepare 40 ml of dye liquor with the mother liquor and deionized water according to a certain bath ratio, and the dye dosage is 2.5% owf; immerse the medical gauze in step 2 in the dye liquor, react at 20° C. in a normal temperature oscillation dyeing machine for 20 minutes, take out the medical gauze and dry it; weigh the mordant ferric sulfate, add deionized water to prepare a mordant solution with a concentration of 4 g / L, immerse the dyed medical gauze in the mordant solution, react at 50° C. in a normal temperature oscillation dyeing machine for 50 minutes, and take out the medical gauze after the reaction, wash it with water, soap it, and dry it.
[0060] Step 4: Weigh 10% (owf) tannic acid into a conical flask, add deionized water, adjust the pH value of the solution to 2.5, and prepare a tannic acid solution; immerse the medical gauze in step 3 in the tannic acid solution, react at 80°C in a normal temperature oscillating dyeing machine for 30 minutes, take out the medical gauze after the reaction, wash with water, wash with soap, and dry it to prepare a pH indicating multifunctional medical gauze with antibacterial and antioxidant properties.
[0061] Example 5 The preparation process of antibacterial and antioxidant pH-indicating multifunctional medical gauze is as follows: Step 1: Add dimethyldiallylammonium chloride aqueous solution (60wt%), diallylamine, and carboxyethyl acrylate into a three-necked flask according to the mass ratio of the monomers of 90:15:20, and then add 10% (owm) acetic acid, 0.1‰ (owm) tetrasodium ethylenediaminetetraacetate and deionized water, stir evenly on a magnetic stirrer and heat to 75°C, then add initiators 0.6% (owm) ammonium persulfate and 0.6% (owm) sodium bisulfite in batches, and react at 75°C for 4h to obtain a cationic modifier.
[0062] Step 2: Weigh the cationic modifier, add deionized water to dissolve it, and then transfer it into a volumetric flask to make a cationic modifier solution with a concentration of 0.31g / L; pour 50ml of the cationic modifier solution into a conical flask, add 1g of medical gauze, and react in a room temperature oscillation dyeing machine at 60℃ for 30min. After the reaction, take out the medical gauze and dry it.
[0063] Step 3: weigh the dye brilliant yellow and add deionized water to prepare a mother liquor, prepare 60 ml of dye liquor with the mother liquor and deionized water according to a certain bath ratio, and the dye dosage is 10% owf; immerse the medical gauze in step 2 in the dye liquor, react at 90° C. for 5 min in a normal temperature oscillation dyeing machine, take out the medical gauze and dry it; weigh the mordant ferrous sulfate heptahydrate, add deionized water to prepare a mordant solution with a concentration of 0.5 g / L, immerse the dyed medical gauze in the mordant solution, react at 90° C. for 30 min in a normal temperature oscillation dyeing machine, take out the medical gauze after the reaction, wash it with water, soap it, and dry it.
[0064] Step 4: Weigh 20% (owf) tannic acid into a conical flask, add deionized water, adjust the pH value of the solution to 2.5, and prepare a tannic acid solution; immerse the medical gauze in step 3 in the tannic acid solution, react at 75°C in a room temperature oscillation dyeing machine for 60 minutes, take out the medical gauze after the reaction, wash with water, soap, and dry, and prepare a pH indicating multifunctional medical gauze with antibacterial and antioxidant properties.
[0065] Comparative Example 1 In this comparative example, the medical gauze was not subjected to cation modification and tannic acid treatment, and the other steps were the same as those in Example 1.
[0066] Comparative Example 2 In this comparative example, the medical gauze was not treated with tannic acid, and the other steps were the same as those in Example 1.
[0067] Performance Testing 1. Dyeing effect test The dyeing effects of Example 1 and Comparative Examples 1 and 2 were tested to obtain the apparent color depth values (K / S values) of the samples, as shown in Table 1.
[0068] Table 1
[0069] As can be seen from Table 1, the K / S value of Comparative Example 1 is 2.89, and the K / S value of Comparative Example 2 is 6.83, indicating that the cationic modifier can effectively promote the dyeing of the dye and increase the color depth of the gauze. The K / S value of Example 1 is 8.50, indicating that after being treated with tannic acid, the dye fastness on the gauze is better and the color is darker. This is because the tannic acid molecule contains a large number of catechol groups, and two adjacent phenolic hydroxyl groups can react with metal ions and dyes in the form of oxygen anions to form a stable chelate. At the same time, tannic acid has strong interfacial adhesion, which can make the chelate formed by the remaining metal ions stably adhere to the fiber surface, thereby improving the color fastness of the dye.
[0070] (II) Antioxidant performance test The antioxidant properties of the original medical gauze, Example 1 and Comparative Example 2 were tested, as shown in Table 2.
[0071] Table 2
[0072] As shown in Table 2, the DPPH free radical scavenging rates of the original medical gauze, comparative example 2 and embodiment 1 are 2%, 13% and 93% respectively, the antioxidant grade of the original medical gauze and comparative example 2 is level 0, which means that they have no antioxidant capacity, and the antioxidant grade of embodiment 1 is level 3, which means that they have extremely strong antioxidant capacity. The results show that after the medical gauze is treated with tannic acid, the gauze has extremely strong antioxidant capacity.
[0073] (III) Antibacterial performance test The antibacterial properties of the original medical gauze, Example 1 and Comparative Example 2 were tested, as shown in Table 3.
[0074] Table 3
[0075] As shown in Table 3, the antibacterial rates of the original medical gauze, comparative example 2, and embodiment 1 against Staphylococcus aureus and Escherichia coli are 0.00% and 0.00%, 83.72% and 0.00%, and 100.00% and 100.00%, respectively. The results show that the original medical gauze has no antibacterial effect, comparative example 2 has a certain antibacterial effect on Staphylococcus aureus, has no antibacterial effect on Escherichia coli, and embodiment 1 has good antibacterial effects on both Staphylococcus aureus and Escherichia coli.
[0076] In summary, the pH-indicating multifunctional medical gauze with antibacterial and antioxidant properties provided by the present invention is simple to operate and cost-effective based on the characteristics of skin pH changes during human wound healing. The multifunctional medical gauze provided by the present invention displays a visual signal in a non-destructive manner as the pH value of the external environment changes, guiding medical staff to adopt timely and reasonable response measures. At the same time, the gauze plays an antibacterial and antioxidant role, reduces exogenous infection, and accelerates wound healing. It has broad promotion and application prospects in the field of medical materials.
[0077] The above are only preferred embodiments of the present invention, and are not intended to limit the implementation methods and protection scope of the present invention. Those skilled in the art should be aware that all solutions obtained by equivalent substitutions and obvious changes made using the contents of the specification of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a pH-indicating multifunctional medical gauze with antibacterial and antioxidant properties, characterized in that: The following steps are involved: S1. Prepare a cationic modifier using dimethyldiallylammonium chloride, diallylamine and carboxyethyl acrylate as raw materials; S2, immersing the medical gauze in an aqueous solution of a cationic modifier to obtain a first product through a first modification reaction; S3, immersing the first product in a dye solution, dyeing and drying, to obtain a second product; The second product is immersed in an aqueous solution of a mordant, subjected to mordant treatment, washed and dried to obtain a third product; S4. Immersing the third product in an aqueous solution of tannic acid, undergoing a second modification reaction, and then washing and drying, thereby obtaining a pH indicating multifunctional medical gauze having antibacterial and antioxidant properties.
2. The preparation method according to claim 1, characterized in that: In step S1, the preparation method of the cationic modifier includes: mixing dimethyldiallylammonium chloride, diallylamine, and carboxyethyl acrylate in a certain proportion, adding a pH adjuster and a chelating agent, heating to a reaction temperature under stirring conditions, adding an initiator, and performing a polymerization reaction to obtain a cationic modifier.
3. The preparation method according to claim 1 or 2, characterized in that: In step S1, the mass ratio of dimethyldiallylammonium chloride, diallylamine and carboxyethyl acrylate is (90-100):(10-20):(10-20).
4. The preparation method according to claim 2, characterized in that: In step S1, the pH regulator is selected from one of acetic acid and formic acid; the chelating agent is selected from one of tetrasodium ethylenediaminetetraacetate and disodium ethylenediaminetetraacetate.
5. The preparation method according to claim 2, characterized in that: In step S1, the initiator includes one or more combinations of an ammonium persulfate-sodium bisulfite system, a potassium persulfate-sodium sulfite system, and an ammonium persulfate-ascorbic acid system.
6. The preparation method according to claim 1, characterized in that: In step S2, the concentration of the cationic modifier in the aqueous solution of the cationic modifier is 0.1-1.5 g / L; the bath ratio of the medical gauze to the aqueous solution of the cationic modifier is 1:(40-60); the temperature of the first modification reaction is 20-60°C, and the time is 10-30 min.
7. The preparation method according to claim 1, characterized in that: In step S3, the dye in the dye solution includes one of brilliant yellow, bromothymol blue, and phenol red; the bath ratio of the first product to the dye solution is 1:(40-60); the mass ratio of the dye to the first product is (1-10):100; the temperature of the dyeing treatment is 20-90°C, and the time is 5-20min.
8. The preparation method according to claim 1, characterized in that: In step S3, the mordant includes a combination of one or more of potassium aluminum sulfate dodecahydrate, ferrous sulfate, and ferrous sulfate heptahydrate; the concentration of the mordant in the aqueous solution of the mordant is 0.5-4 g / L; the temperature of the mordant treatment is 50-90° C., and the time is 20-50 min.
9. The preparation method according to claim 1, characterized in that: In step S4, the mass ratio of tannic acid to the third product is (10-50):100; the pH value of the aqueous solution of tannic acid is 2.5-3.5; the temperature of the second modification reaction is 50-80°C, and the time is 30-90 minutes.
10. A pH indicating multifunctional medical gauze with antibacterial and antioxidant properties, characterized in that: Prepared by the preparation method according to any one of claims 1 to 9.
Citation Information
Cited By
Detection method for efficacy of hygienic product and application of detection method
CN120992529A
Antibacterial breathable medical gauze swab
CN121781417A