Composite embolism agent based on active metal microspheres, preparation method and application of composite embolism agent

By dispersing active metal microspheres or nanohydrides into lipiodol to form a composite embolic agent, the problems of hydrogen delivery and material stability in liver cancer treatment are solved, hydrogen treatment and improvement of the tumor microenvironment are achieved, and the therapeutic effect is significantly improved. and security.

CN118743779APending Publication Date: 2024-10-08CHONGQING BAIMAITENGSHI PHARMACEUTICAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410730447.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-13
Filing Date
2022-04-30
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

Traditional liver cancer treatment methods such as transcatheter arterial embolization (TAE) and chemoembolization (TACE) have poor therapeutic effects due to the vascular heterogeneity and immunosuppressive microenvironment of liver cancer, and active metal or nanohydride materials are in the aqueous system. It has poor stability and is difficult to be directly used in tumor treatment.

Method used

Develop a composite embolic agent by dispersing active metal microspheres or nano-hydride materials into lipiodol to form lipiodol-based composite embolic agent, using the dispersion function and protective effect of lipiodol to moderate its reaction rate with water, Achieve the slow release of hydrogen and hydroxide, which can be used to deliver hydrogen during interventional surgery for liver cancer and continuously generate hydrogen within the tumor to regulate the immune microenvironment.

Benefits of technology

It significantly improves the improvement effect and therapeutic effect of tumor microenvironment, solves the instability problem of active metal materials in physiological environment, and improves the safety and effect of tumor treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118743779A_ABST
    Figure CN118743779A_ABST
Patent Text Reader

Abstract

The invention provides a composite embolic agent based on active metal microspheres as well as a preparation method and application thereof, and belongs to the technical field of medicines. The composite embolization agent is composed of iodine oil and active metal microspheres or nano-hydrides, and the iodine oil serves as a dispersing agent and a protective agent and can delay the reaction rate of the active metal microspheres or the nano-hydrides and water. The preparation method of the active metal microspheres and the nano-hydrides is simple, and large-scale preparation can be achieved within a short time. The prepared composite embolism agent is locally delivered to liver cancer tissue through an interventional operation, iodophol is deposited to the liver cancer tissue to cause embolism treatment, meanwhile, active metal or hydride releases hydrogen in situ to induce hydrogen treatment, and therefore the embolism treatment effect is amplified. According to the composite embolism agent, hydrogen is released in situ through active metal or hydride, the tumor microenvironment is regulated and controlled through hydroxide and the like, and the combined embolism treatment effect better than that of pure iodine oil embolism treatment is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention is a divisional application of the invention patent with the patent name “Active metal microspheres, composite embolic agents based on active metal microspheres and their applications”, the filing date of which is April 30, 2022, and the application number is 202210469169.6 (the priority number and priority date are 202111342067.X, November 12, 2021, and 202210384584.1, April 13, 2022). Technical Field

[0002] The invention belongs to the field of medical technology, and in particular refers to a composite embolic agent based on active metal microspheres, a preparation method and an application thereof.

[0003] The invention relates to a composite embolic agent based on active metal microspheres and a composite embolic agent based on a metal composite structure. Background Art

[0004] Cancer causes millions of deaths worldwide every year and is one of the most dangerous diseases facing humanity. In particular, among many cancers, liver cancer is difficult to cure with traditional anti-tumor treatments such as surgical resection, organ transplantation, radiotherapy and chemotherapy due to its insidious onset, high malignancy, strong invasiveness, rapid growth, high recurrence rate and high mortality rate. In recent years, tumor interventional therapy has attracted widespread attention due to its excellent therapeutic effect and minimal side effects. Among them, transcatheter arterial embolization (TAE) is the most effective targeted drug delivery method that efficiently delivers vascular embolization materials and chemotherapeutic drugs to the proximal artery of the tumor through superselective arterial perfusion. It is considered to be the standard treatment for some advanced solid tumors. However, the high heterogeneity of liver cancer and its blood vessels hinders the therapeutic response of liver cancer tissues with low blood supply, and after TAE / or its combination with drugs (transcatheter chemoembolization, TACE) treatment, liver cancer lesions will accumulate a large number of hypoxia-tolerant liver cancer cells and tumor-derived stem cells (CSLCs), resulting in TAE treatment failure. In addition, the hypoxic, weakly acidic, and immunosuppressive microenvironment caused by arterial embolism will also promote the rapid proliferation, metastasis, and drug resistance of liver cancer cells, making it impossible to completely eradicate liver cancer. Therefore, TAE / TACE treatment often results in incomplete tumor necrosis, recurrence / metastasis, and low patient survival rates, which greatly limits its widespread application.

[0005] In recent years, immunotherapy, which is a therapy that fights cancer by activating the patient's immune system, has shown great promise in the field of tumor treatment. During immunotherapy, cytotoxic T lymphocytes (CTLs) play an important role in attacking tumor cells. However, the complex tumor microenvironment (TME) such as vascular abnormalities, acidic pH, hypoxia, and high concentrations of reactive oxygen species (ROS) greatly limit the activity and killing ability of CTLs in solid tumors. At the same time, the above-mentioned physiological characteristics of TME will promote the infiltration of various immunosuppressive cells such as myeloid-derived suppressor cells (MDSCs), M2 tumor-associated macrophages (TAMs), and regulatory T cells (Treg), forming an immunosuppressive microenvironment. Immunosuppressive TME is one of the main obstacles that seriously hinder tumor immunotherapy. Therefore, regulating TME through multiple pathways has been considered an attractive strategy to improve the efficacy of various cancer treatments, especially tumor immunotherapy.

[0006] Hydrogen (H2), as an endogenous gas, has significant physiological / pathological regulatory functions. In the past decade, hydrogen has been shown to have significant anti-inflammatory and anti-tumor effects due to its high biological diffusion capacity. However, due to the low solubility of hydrogen, the current mainstream hydrogen delivery methods, including oral hydrogen-rich water, injection of hydrogen-rich salts, and hydrogen inhalation therapy, are difficult to meet the dosage requirements for effective treatment. Therefore, it is necessary to develop new hydrogen carriers and their delivery strategies. Active metal (e.g., potassium, calcium, sodium, magnesium, aluminum, zinc, gallium, iron, manganese, and tin) microspheres or nanohydride materials (e.g., calcium hydride, magnesium hydride, lithium hydride, sodium hydride, potassium hydride, strontium hydride, and cerium hydride) react with water to efficiently release hydrogen. At the same time, the reaction will produce hydroxide to neutralize the acidic tumor microenvironment, activate the immune system, and achieve microenvironment regulation and synergistic hydrogen-immune synergistic therapy. However, these active metals or nano-hydride materials are too active in chemical properties and have poor stability in aqueous systems. Some active metals or nano-hydrides may even explode when in direct contact with water, and are generally considered difficult to be used directly in tumor treatment. Summary of the invention

[0007] In order to solve the above technical problems, the present invention provides a composite embolic agent and a preparation method and application thereof. After the composite embolic agent provided by the present invention is delivered to the liver cancer lesion through interventional surgery, iodized oil is deposited in the liver cancer tissue to cause embolic therapy, and at the same time, the active metal or hydride releases hydrogen in situ to induce hydrogen therapy, and the released hydroxide ions regulate the immune microenvironment, thereby amplifying the embolic therapy effect.

[0008] The present invention selects magnesium microspheres or nano calcium hydride as target preparations for research, and disperses them into lipiodol, a clinical embolic agent, to obtain a composite preparation having good chemical stability, and even when mixed with an aqueous solution, the reaction speed is relatively mild, and hydrogen can be continuously and gently generated. In the present invention, the present invention obtains lipiodol-based active metal microspheres or nano hydride composite embolic agents, which can synchronously and continuously generate hydrogen in the tumor when used for tumor interventional embolization therapy, thereby realizing the function of hydrogen therapy, and further improving the tumor microenvironment by neutralizing the tumor acidic environment, thereby obtaining a significantly improved therapeutic effect compared with lipiodol perfusion alone.

[0009] On the one hand, the present invention provides a composite embolic agent of iodized oil-based active metal microspheres or nano-hydrides, wherein the composite embolic agent comprises active metal microspheres or nano-hydrides and iodized oil; the mass percentage of the active metal microspheres or nano-hydrides in the composite embolic agent is 0.1 to 10%.

[0010] Among them, the iodized oil is a medical embolic agent. In this system, the iodized oil has a dispersing function and a protective effect. The iodized oil can protect active metals and hydrides, slowing down their reaction rate with water, thereby achieving a slow release of hydrogen and hydroxides, and playing a long-term therapeutic role.

[0011] As a preferred embodiment of the composite embolic agent of the present invention, the particle size of the active metal microspheres is 0.1-20 microns.

[0012] As a preferred embodiment of the composite embolic agent of the present invention, the particle size of the active metal microspheres is 20-500 microns.

[0013] Further preferably, the size of the active metal microspheres is not less than 0.1 micron, not less than 5 microns, not less than 10 microns, not less than 20 microns, not less than 50 microns, not less than 100 microns, not less than 150 microns, not less than 200 microns, not less than 250 microns, not less than 300 microns, not less than 350 microns, not less than 400 microns, not less than 450 microns, and not more than 500 microns.

[0014] When the particle size of the microspheres is too large, they cannot be dispersed well in the dispersant and thus cannot be successfully used in clinical practice.

[0015] As a preferred embodiment of the composite embolic agent of the present invention, the particle size of the nano hydride material is 5-200 nanometers.

[0016] Among them, 5-200 nanometers is equivalent to 0.005-0.2 microns.

[0017] As a preferred embodiment of the composite embolic agent of the present invention, the particle size of the nano hydride material is 0.2-500 microns.

[0018] Further preferably, the size of the nano hydride material is not less than 0.1 micron, not less than 0.005 micron, not less than 0.01 micron, not less than 0.05 micron, not less than 0.1 micron, not less than 0.5 micron, not less than 1 micron, not less than 5 microns, not less than 10 microns, not less than 20 microns, not less than 50 microns, not less than 100 microns, not less than 150 microns, not less than 200 microns, not less than 250 microns, not less than 300 microns, not less than 350 microns, not less than 400 microns, not less than 450 microns, and not more than 500 microns.

[0019] As a preferred embodiment of the composite embolic agent of the present invention, the active metal microspheres are prepared by a gas atomization powder making method, that is, the active metal ingots are heated and melted and then atomized and cooled to obtain the active metal microspheres.

[0020] As a preferred embodiment of the composite embolic agent of the present invention, the active metal is one or more of potassium, calcium, sodium, magnesium, aluminum, zinc, gallium, iron, manganese and tin.

[0021] As a preferred embodiment of the composite embolic agent of the present invention, the nano hydride material is prepared by a liquid phase exfoliation method, that is, the nano hydride is ultrasonically dispersed in an exfoliation solvent, and the nano hydride material is obtained by centrifugation.

[0022] Preferably, the nano hydride material is prepared by liquid phase exfoliation, that is, the nano hydride is dispersed in an exfoliation solvent by ultrasonic treatment for 0.2 to 4 hours, and the nano hydride material is obtained by centrifugation. Preferably, the ultrasonic power is 50 to 100 W, and the operating temperature is 10 to 20°C.

[0023] As a preferred embodiment of the composite embolic agent of the present invention, the ratio of the amount of the nano hydride to the stripping solvent (M 质量(mg) :V 体积(mL) ) is: 0.1:1~10:1.

[0024] As a preferred embodiment of the composite embolic agent of the present invention, the nano hydride is one or more of calcium hydride, magnesium hydride, lithium hydride, sodium hydride, potassium hydride, strontium hydride and cerium hydride.

[0025] As a preferred embodiment of the composite embolic agent of the present invention, the stripping solvent is one or more of N-methylpyrrolidone, dimethyl sulfoxide or polyethylene glycol 200, pyrrole and N,N-dimethylformamide.

[0026] On the one hand, the present invention provides a method for preparing the composite embolic agent as described in the above technical solution, comprising the following steps: mixing iodized oil with active metal microspheres or nano-hydride materials and uniformly dispersing them to obtain the composite embolic agent.

[0027] Further preferably, the preparation method specifically comprises the following steps: mixing the active metal microspheres or nano-hydride material with iodized oil, and uniformly dispersing by ultrasonication to obtain the iodized oil-based active metal microspheres or nano-hydride composite embolic agent.

[0028] In one aspect, the present invention provides a use of the composite embolic agent as described in the above technical solution in the preparation of a therapeutic agent for liver cancer embolism.

[0029] In one aspect, the present invention provides a tumor preparation, comprising the composite embolic agent as described in the above technical solution.

[0030] In one aspect, the present invention provides a composite embolic agent, comprising active metal microspheres and a dispersant, wherein the metal activity of the active metal microspheres is stronger than the activity of hydrogen.

[0031] As a preferred embodiment of the composite embolic agent of the present invention, the active metal microspheres are prepared from active metals, and the active metals are selected from at least one of potassium, calcium, sodium, magnesium, aluminum, zinc, gallium, iron, manganese and tin.

[0032] As a preferred embodiment of the composite embolic agent of the present invention, the mass ratio of the active metal microspheres to the dispersant is 0.1:100 to 50:100.

[0033] As a preferred embodiment of the composite embolic agent of the present invention, the particle size of the active metal microspheres is 0.1-500 microns.

[0034] Further preferably, the short diameter of the active metal microspheres is not less than 0.1 micron, not less than 0.005 micron, not less than 0.01 micron, not less than 0.05 micron, not less than 0.1 micron, not less than 0.5 micron, not less than 1 micron, not less than 5 microns, not less than 10 microns, not less than 20 microns, not less than 50 microns, not less than 100 microns, not less than 150 microns, not less than 200 microns, not less than 250 microns, not less than 300 microns, not less than 350 microns, not less than 400 microns, not less than 450 microns, and not more than 500 microns.

[0035] As a preferred embodiment of the composite embolic agent of the present invention, the active metal microspheres are in the shape of spheres, mesoporous structures, sea urchins or polyhedrons.

[0036] As a preferred embodiment of the composite embolic agent of the present invention, the dispersant is an organic phase.

[0037] As a preferred embodiment of the composite embolic agent of the present invention, the dispersant is an oil phase.

[0038] As a preferred embodiment of the composite embolic agent of the present invention, the dispersant is selected from at least one of iodized oil, poppy seed oil, soybean oil and olive oil.

[0039] In one aspect, the present invention provides a tumor preparation, comprising the composite embolic agent as described in the above technical solution.

[0040] On the one hand, the present invention provides a composite embolic agent, which includes a metal composite structure and a dispersant, wherein the metal composite structure includes a core structure and a binding layer bound to the surface of the core structure, the core structure is a first metal, and the binding layer is a second metal; the metal composite structure is dispersed in the dispersant.

[0041] As a preferred embodiment of the composite embolic agent of the present invention, the dispersant is an organic phase.

[0042] As a preferred embodiment of the composite embolic agent of the present invention, the organic phase is an oil phase.

[0043] As a preferred embodiment of the composite embolic agent of the present invention, the oil phase is selected from at least one of iodized oil, poppy seed oil, soybean oil and olive oil.

[0044] As a preferred embodiment of the composite embolic agent of the present invention, the mass ratio of the metal composite structure to the dispersant is 0.1:100 to 50:100.

[0045] As a preferred embodiment of the composite embolic agent of the present invention, the core structure is in the shape of a sphere, a polyhedron, a porous structure or a rod.

[0046] As a preferred embodiment of the composite embolic agent of the present invention, the metal activity of the first metal is stronger than the activity of hydrogen.

[0047] As a preferred embodiment of the composite embolic agent of the present invention, the first metal is selected from at least one of potassium, calcium, sodium, magnesium, aluminum, zinc, gallium, iron, manganese and tin.

[0048] Specifically, the metal activity of the first metal is stronger than the activity of hydrogen, that is, the first metal reacts with water to generate hydrogen.

[0049] The mass ratio of the metal composite structure to the dispersant is 0.1:100 to 50:100, that is, the mass fraction of the metal composite structure in the dispersant is 0.1% to 50%.

[0050] Further preferably, the mass fraction of the metal composite structure in the organic phase is not less than 0.1%, not less than 5%, not less than 10%, not less than 15%, not less than 20%, not less than 25%, not less than 30%, and not more than 50%.

[0051] As a preferred embodiment of the composite embolic agent of the present invention, the metal activity of the second metal is weaker than the activity of hydrogen.

[0052] As a preferred embodiment of the composite embolic agent of the present invention, the second metal is selected from at least one of copper, silver, platinum and gold.

[0053] As a preferred embodiment of the composite embolic agent of the present invention, the particle size of the metal composite structure is 0.1-500 microns.

[0054] Further preferably, the short diameter of the metal composite structure is not less than 0.1 micron, not less than 0.005 micron, not less than 0.01 micron, not less than 0.05 micron, not less than 0.1 micron, not less than 0.5 micron, not less than 1 micron, not less than 5 microns, not less than 10 microns, not less than 20 microns, not less than 50 microns, not less than 100 microns, not less than 150 microns, not less than 200 microns, not less than 250 microns, not less than 300 microns, not less than 350 microns, not less than 400 microns, not less than 450 microns, and not more than 500 microns.

[0055] It should be noted that when the core structure of the metal composite structure is spherical, the short diameter of the metal composite structure is the particle size.

[0056] As a preferred embodiment of the composite embolic agent of the present invention, the particle size distribution of the metal composite structure is uniform.

[0057] In one aspect, the present invention provides a method for preparing the composite embolic agent described in the above technical solution, which comprises the step of combining the second metal on the surface of the first metal.

[0058] As a preferred solution of the method for preparing the composite embolic agent of the present invention, the second metal is bonded to the surface of the first metal by a physical method or a chemical method.

[0059] As a preferred embodiment of the method for preparing the composite embolic agent of the present invention, the chemical method is selected from the substitution method.

[0060] As a preferred embodiment of the method for preparing the composite embolic agent of the present invention, the replacement method comprises placing the first metal in a solution containing high-valent ions of the second metal.

[0061] As a preferred embodiment of the method for preparing the composite embolic agent of the present invention, the solution of the high-valent ions of the second metal contains at least one of chloroaurate ions, chloroplatinate ions, copper ions, and silver ions.

[0062] Preferably, in the method for preparing the metal composite structure, the efficiency of metal replacement can be accelerated by means of vibration, ultrasound, etc.

[0063] As a preferred embodiment of the method for preparing the composite embolic agent of the present invention, the physical method is a mechanical stirring method.

[0064] As a preferred embodiment of the method for preparing the composite embolic agent of the present invention, the mechanical stirring method comprises mixing and stirring the second metal in a solid state and the first metal in a liquid state.

[0065] As a preferred solution of the method for preparing the composite embolic agent of the present invention, the physical method is a vapor deposition method.

[0066] The present invention also provides a method for preparing a composite embolic agent, comprising the step of dispersing the metal composite structure in the dispersant.

[0067] Furthermore, a method for preparing a composite embolic agent also includes an ultrasonic dispersion step.

[0068] On the one hand, the present invention provides a composite embolic agent, comprising alloy metal particles and a dispersant, wherein the alloy metal particles comprise at least two metals with different activities, the two metals with different activities are mixed in the form of an alloy, and the alloy metal particles are dispersed in the dispersant.

[0069] As a preferred embodiment of the composite embolic agent of the present invention, the dispersant is an organic phase.

[0070] As a preferred embodiment of the composite embolic agent of the present invention, the organic phase is an oil phase.

[0071] As a preferred embodiment of the composite embolic agent of the present invention, the oil phase is selected from at least one of iodized oil, poppy seed oil, soybean oil and olive oil.

[0072] As a preferred embodiment of the composite embolic agent of the present invention, the alloy metal particles include at least one active metal and at least one inert metal, and the active metal element and the inert metal element are mixed in the form of an alloy.

[0073] As a preferred embodiment of the composite embolic agent of the present invention, the mass fraction of the alloy metal particles in the dispersant is 0.1% to 50%;

[0074] As a preferred embodiment of the composite embolic agent of the present invention, the alloy metal particles are uniformly dispersed in the dispersant.

[0075] As a preferred embodiment of the composite embolic agent of the present invention, the alloy metal particles are in the shape of spheres, polyhedrons, porous structures, sea urchins or rods.

[0076] As a preferred embodiment of the composite embolic agent of the present invention, the metal activity of the active metal is greater than the activity of hydrogen.

[0077] As a preferred embodiment of the composite embolic agent of the present invention, the active metal is selected from at least one of potassium, calcium, sodium, magnesium, aluminum, zinc, gallium, iron, manganese and tin.

[0078] As a preferred embodiment of the composite embolic agent of the present invention, the metal activity of the inert metal is less than that of hydrogen.

[0079] As a preferred embodiment of the composite embolic agent of the present invention, the inert metal is selected from at least one of copper, silver, platinum and gold.

[0080] As a preferred embodiment of the composite embolic agent of the present invention, the size of the alloy metal particles is 0.1-500 microns.

[0081] Further preferably, the minor diameter of the alloy metal particles is not less than 0.1 micron, not less than 0.005 micron, not less than 0.01 micron, not less than 0.05 micron, not less than 0.1 micron, not less than 0.5 micron, not less than 1 micron, not less than 5 microns, not less than 10 microns, not less than 20 microns, not less than 50 microns, not less than 100 microns, not less than 150 microns, not less than 200 microns, not less than 250 microns, not less than 300 microns, not less than 350 microns, not less than 400 microns, not less than 450 microns, and not more than 500 microns.

[0082] It should be noted that when the alloy metal particles are spherical, the short diameter of the alloy metal particles is the particle size.

[0083] The alloy metal nanoparticles can be purchased commercially or prepared using existing alloy preparation methods.

[0084] The present invention also provides a method for preparing the composite embolic agent, comprising the step of mixing the alloy metal particles with the dispersant.

[0085] Further preferably, the preparation method further comprises a step of ultrasonic dispersion.

[0086] The inventors have experimentally verified that when the mass fraction of metal microspheres, nano-hydrides, metal composite structures, and alloy metal particles in the dispersant exceeds 50%, they cannot be effectively dispersed and are difficult to be injected into the catheter for practical applications.

[0087] Compared with the prior art, the beneficial effects of the above technical solution provided by the present invention include but are not limited to:

[0088] The present invention provides a composite embolic agent and a preparation method thereof. The composite embolic agent is prepared by dispersing active metal microspheres or nano-hydrides in lipiodol embolic agents in different proportions. The obtained composite embolic agent has good chemical stability. Even when mixed with an aqueous solution, the reaction speed is relatively moderate, and hydrogen can be continuously and gently generated, thereby solving the problem that the active metal microspheres or nano-hydrides react violently with water and cannot be controlled. In the present invention, the lipiodol-based active metal microspheres or nano-metal hydrides composite embolic agent is locally delivered to liver cancer tissues through interventional surgery, and lipiodol is deposited in the liver cancer tissues to cause embolization therapy. At the same time, the active metal microspheres or nano-hydrides continuously generate hydrogen in the tumor to achieve the function of hydrogen therapy. At the same time, the released hydroxide can neutralize the weakly acidic microenvironment of the tumor to improve the tumor microenvironment, thereby amplifying the effect of embolization therapy, and obtaining a significantly improved therapeutic effect compared with lipiodol perfusion alone.

[0089] The present invention selects magnesium microspheres or nano calcium hydride as target preparations for research, and disperses them into iodized oil, a clinical embolic agent, so that the obtained composite preparation has good chemical stability.

[0090] Active metal microspheres or nano-hydrides with smaller particle sizes (less than 20 microns) help to react quickly to produce hydrogen; active metal microspheres or nano-hydrides with larger particle sizes (greater than or equal to 20 microns) can reduce the probability of escape from the lesion site, thereby reducing the risk of embolism in normal tissues and having better safety.

[0091] Structures such as mesoporous structures and sea urchin-like structures that can increase the specific surface area of ​​microspheres can help active metal microspheres of the same particle size to better react and produce hydrogen in a physiological environment.

[0092] Active metal composite structures or alloy metal particles can make active metal microspheres with larger particle sizes have higher reaction efficiency. The composite embolic agent composed of iodized oil can significantly improve the tumor microenvironment and have better embolic treatment effect. The selection of different metals to prepare metal composite structures or alloy particles has additional effects, such as enhanced improvement of the immune microenvironment and enhanced retention. Active metal composite structures or alloy metal particles are mixed with dispersants and then used for embolic therapy. They can be combined with embolization and hydrogen therapy, thereby greatly improving the effect of embolic therapy, while solving the problem of instability of active metals under physiological conditions and improving the safety of active metals in tumor treatment. The composite embolic agent preparation method of the present invention is simple and easy to use clinically. BRIEF DESCRIPTION OF THE DRAWINGS

[0093] In order to make the content of the present invention more clearly understood, the present invention is further described in detail below according to specific embodiments of the present invention in conjunction with the accompanying drawings, wherein

[0094] Figure 1 is a microscope photograph of the magnesium microspheres obtained in Example 1 of the present invention;

[0095] Figure 2 This is a photo of the evaluation of hydrogen release from magnesium microspheres in different buffers;

[0096] Figure 3 This is a transmission electron microscope (TEM) image of nano calcium hydride obtained in Example 2 of the present invention;

[0097] Figure 4 is the X-ray diffraction pattern (XRD) of nano calcium hydride obtained in Example 2 of the present invention;

[0098] Figure 5 This is an optical photograph of the metal magnesium microsphere-iodized oil composite embolic agent obtained in Example 1 of the present invention;

[0099] Figure 6 This is an optical photograph of the nano calcium hydride-iodized oil composite embolic agent obtained in Example 2 of the present invention;

[0100] Figure 7 The hydrogen release evaluation of the calcium hydride-lipiodol composite embolic agent obtained in Example 2 of the present invention;

[0101] Figure 8 This is a schematic diagram of the interventional surgery process for rabbit liver cancer according to the present invention;

[0102] Fig. 9 This is the DSA imaging of liver cancer lesions during interventional surgery in a rabbit;

[0103] Fig.10 The magnesium microsphere-iodized oil composite embolic agent obtained in Example 1 of the present invention is used for CT imaging of liver cancer lesions before and after embolization surgery in rabbits;

[0104] Fig.11 The nano calcium hydride-iodized oil composite embolic agent obtained in Example 2 of the present invention is used for CT imaging of liver cancer lesions before and after embolization surgery in rabbits;

[0105] Fig.12 The nano calcium hydride-iodized oil composite embolic agent obtained in Example 2 of the present invention is used for embolizing liver cancer lesions before and after surgery in rabbits 18 F-FDG PET imaging;

[0106] Fig.13 The nano calcium hydride-iodized oil composite embolic agent obtained in Example 2 of the present invention is used for embolizing liver cancer lesions before and after surgery in rabbits 18 The intensity of F-FDG;

[0107] Fig.14 The nano calcium hydride-iodized oil composite embolic agent obtained in Example 2 of the present invention is used for immunohistochemical analysis of liver cancer lesions in vitro seven days after embolization in rabbits;

[0108] Fig.15 The apoptosis level of liver cancer lesions in vitro in rabbits seven days after embolization using the nano calcium hydride-iodized oil composite embolic agent obtained in Example 2 of the present invention;

[0109] Fig.16 The proliferation activity of the nano calcium hydride-iodized oil composite embolic agent obtained in Example 2 of the present invention used for the in vitro hepatic cancer lesions of rabbits seven days after embolization;

[0110] Fig.17 is a particle size distribution diagram of the magnesium-platinum metal composite structure described in Example 8 of the present invention;

[0111] Fig.18 It is a statistical graph of hydrogen production in 96% ethanol solution of the magnesium microspheres detected in Example 9 of the present invention and the Mg@Pt composite structure obtained in Example 3;

[0112] Fig.19 The Mg@Pt metal composite structure-iodized oil composite embolic agent prepared in Example 3 is used in Example 11 of the present invention to treat mouse tumors, and the mouse tumor growth curve obtained by statistics;

[0113] FIG20 is a scanning electron microscope image of raw material magnesium microspheres and Mg@Pt composite structure in Example 12 of the present invention;

[0114] Fig.21 is the XRD powder diffraction spectrum of the magnesium-platinum metal composite structure prepared in Example 13 of the present invention;

[0115] Fig. 22It is a curve chart showing the total amount of hydrogen produced by the Mg@Pt metal composite structure prepared in Example 8 in Example 14 of the present invention in a phosphate buffer solution;

[0116] Fig.23 is a statistical diagram of the particle size distribution of large-size magnesium microspheres in Example 5 of the present invention;

[0117] Fig.24 In Example 6 of the present invention, the magnesium microspheres in Example 5 are placed in buffer solutions under different pH conditions, and the total amount of hydrogen produced is measured using a gas chromatograph. DETAILED DESCRIPTION

[0118] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.

[0119] In order to describe the technical solution of the above invention in more detail, specific embodiments are listed below to demonstrate the technical effect; it should be emphasized that these embodiments are used to illustrate the present invention but are not limited to the scope of the present invention.

[0120] As shown in this specification and claims, unless the context clearly indicates an exception, the words "a", "an", "an" and / or "the" do not refer to the singular and may also include the plural, unless the context clearly indicates an exception. The terms "include" and "comprise" only indicate that the elements that have been clearly identified are included, and these elements do not constitute an exclusive list. The device may also include other elements. The term "one embodiment" means "at least one embodiment"; the term "another embodiment" means "at least one other embodiment". The relevant definitions of other terms will be given in the following description.

[0121] The detection equipment and methods used in the embodiments of this specification are:

[0122] Morphological characterization: transmission electron microscopy (FEI Tecnai F20 TEM), scanning electron microscopy (ZEISSSigma);

[0123] Elemental analysis: X-ray powder diffractometer (PANalytical X-ray diffractometer);

[0124] Determination of hydrogen production efficiency: gas chromatograph (SIEMENS MAXUMII);

[0125] In vivo angiography to detect embolism: DAS digital subtraction angiography (PHILIPS FD20);

[0126] In vivo imaging to detect tumor size:

[0127] (1) CT imaging (PHILIPS Access CT), using CT imaging combined with ioversol contrast agent to evaluate treatment efficacy;

[0128] (2) PET-CT imaging device (GEMINI TF PET / CT), 18 F-FDG is a radionuclide probe used to evaluate the effect of interventional embolization therapy with the help of positron emission tomography (PET) / CT imaging;

[0129] Evaluation method of tumor apoptosis and proliferation: Through tumor sections, use fluorescently labeled TUNEL or Ki67 protein staining to observe and count the proportion of TUNEL-positive or Ki67-positive cells in the tumor cells in the field of view, which is the tumor cell apoptosis rate or proliferation rate.

[0130] The present invention provides a composite embolic agent, comprising: active metal microspheres or nano-hydride materials and iodized oil dispersing protective agent;

[0131] The active metal microspheres are one or more of potassium, calcium, sodium, magnesium, aluminum, zinc, gallium, iron, manganese and tin. The active metal microspheres are micrometer-sized, and their particle size is 0.1-20 micrometers. The active metal microspheres are prepared from active metal ingots by aerosol powder making method. The hydride is one or more of cationic metal hydrides such as calcium hydride, magnesium hydride, lithium hydride, sodium hydride, potassium hydride, strontium hydride, cerium hydride and the like.

[0132] The above hydride materials are all nanometer-sized, with a particle size of 5-200 nanometers. The nano hydride material is obtained by stripping the hydride raw material through a liquid phase stripping method. The specific reaction conditions are to disperse the metal hydride raw material into the stripping solvent N-methylpyrrolidone, ultrasonically strip for 20 minutes, and ultracentrifuge to obtain the nano hydride product.

[0133] Subsequently, the active metal microspheres or nano hydride particles are mixed with iodized oil and uniformly dispersed by ultrasonication to obtain the composite embolic agent, wherein the mass percentage of the active metal microspheres or nano hydrides in the composite embolic agent is 0.1-10%. The prepared composite embolic agent is locally delivered to liver cancer tissues through interventional surgery, and iodized oil is deposited on the liver cancer tissues to cause embolic therapy, while the active metal microspheres or hydrides release hydrogen in situ to induce hydrogen therapy, and release hydroxides to regulate the tumor microenvironment, thereby further amplifying the embolic therapy effect. The composite embolic agent of the present invention utilizes active metals or metal hydrides to release hydrogen, hydroxides, etc. in situ to regulate the tumor microenvironment, and exhibits a better combined embolic therapy effect than simple iodized oil embolic therapy.

[0134] Example 1: Preparation of magnesium microsphere-iodized oil composite embolic agent

[0135] The metal magnesium ingot is placed in the gas atomization powder making equipment, and then the magnesium ingot temperature is heated to 700℃ to become a stable flowing liquid. Then, the liquid magnesium is atomized and cooled in a high-speed inert gas argon gas at a flow rate of 2-2.5 Mach to obtain magnesium powder, and then passed through a 1000-mesh screen to obtain 10-micron magnesium microspheres. The obtained magnesium microspheres are structurally characterized, and the results are shown in Figure 1-Figure 2 .

[0136] The magnesium microspheres prepared above are dispersed into the commercial iodized oil embolic agent at a mass fraction of 1% by mass of the magnesium microspheres. The magnesium microsphere-iodized oil composite embolic agent can be obtained by ultrasonic or shaking dispersion. The composite embolic agent can be customized according to the needs, wherein the mass ratio of the magnesium microspheres is in the range of 1%. The commercial iodized oil used as the dispersant is a light yellow clear transparent liquid, and the prepared magnesium microsphere-iodized oil composite embolic agent is a dark yellow liquid, and the optical photograph is as follows: Figure 5 shown.

[0137] Figure 1 This is a micrograph of the prepared magnesium microspheres. It can be seen that the particle size of the product is about 10 microns and the morphology and size are uniform.

[0138] Figure 2 It is the hydrogen release rate of magnesium microspheres in buffer solutions with different pH values ​​(7.4, 6.4, 5.5). It can be found that the higher the acidity of the solution, the greater the amount of bubbles produced, indicating that the hydrogen release rate is faster.

[0139] Example 2: Preparation of calcium hydride-lipiodol composite embolic agent

[0140] Calcium hydride powder and organic solvent N-methylpyrrolidone were added into the reactor. The ratio of calcium hydride powder to N-methylpyrrolidone (M 质量(mg) :V 体积(mL) ) is 10:1. Vigorously shake to evenly disperse the calcium hydride powder in N-methylpyrrolidone. Place the mixed dispersion system in an ultrasonic cleaner and treat the dispersion system with ultrasound for 0.3 hours. The working power of the ultrasonic cleaner is 100W and the working temperature is 15°C. The treated reaction system is ultracentrifuged to obtain the precipitate, and then washed with ethanol several times to obtain calcium hydride nanoparticles. The obtained calcium hydride nanoparticles were structurally characterized, and the results are shown in Figure 3-Figure 4 .

[0141] in, Figure 3 This is a transmission electron microscope image of the prepared calcium hydride nanoparticles. It can be seen that the particle size of the prepared product is about 7.9 nanometers and the morphology and size are uniform.

[0142] Figure 4The X-ray diffraction spectrum of synthesized nano calcium hydride is shown in the figure. The horizontal axis is the degree of 2θ angle and the vertical axis is the intensity. The 2θ angles of the characteristic diffraction peaks of the calcium hydride nanoparticles are 28.18, 30.38, 32.04, 41.72, and 47.56, respectively corresponding to (011), (102), (111), (211), and (013) diffraction crystal planes. The above diffraction peak data are consistent with the standard X-ray diffraction data of calcium hydride (JCPDS no. 31-0266), which can prove that the synthesis method described in the present invention can successfully prepare calcium hydride nanoparticles.

[0143] The nano calcium hydride powder prepared above is dispersed into the commercial iodized oil embolic agent according to the mass percentage of the nano calcium hydride powder of 0.4%, and the calcium hydride-iodized oil composite embolic agent can be obtained by ultrasonic or shaking dispersion. According to the needs, the composite embolic agent can be customized, wherein the mass ratio of the nano calcium hydride is in the range of 0.4%. The dispersant commercial iodized oil used is a light yellow clear transparent liquid, and the optical photo is as follows Figure 6 As shown in (left), the prepared nano calcium hydride-iodized oil composite embolic agent is a milky white liquid, and the optical photo is as follows Figure 6 (right) shown.

[0144] Test Example: The hydrogen release performance of the nano calcium hydride-iodized oil composite embolic agent obtained in Example 2 was tested.

[0145] Take 50 μl of the composite embolic agent and drop it into the EP tube containing 3 ml of water, and monitor the generation of hydrogen in real time. Figure 7 As shown in the optical photographs, a large number of bubbles are generated in the EP tube, indicating that the nano-calcium hydride-iodized oil composite embolic agent has good hydrogen in situ release performance, confirming the stability and practicality of the composite embolic agent.

[0146] Application Example 1: The magnesium microsphere-iodized oil composite embolic agent obtained in Example 1 is used for interventional embolization treatment of rabbit liver cancer

[0147] With the help of CT imaging guidance, VX2 liver cancer tissue was directly implanted into the left lobe of the liver. After two weeks, a tumor was formed, and an in situ rabbit liver cancer tumor model was obtained. The tumor-bearing rabbits were randomly divided into three groups: (1) control group; (2) iodized oil group; (3) magnesium microsphere-iodized oil composite embolic agent group. Figure 8As shown in the figure, a 2.0-F microcatheter and a coaxial guidewire cannula were inserted into the left hepatic artery containing the tumor lesion through the femoral artery under the guidance of DSA fluoroscopy. Then, 0.3 ml of iodized oil or magnesium microsphere-iodized oil composite embolic agent was slowly injected into the left hepatic artery through the microcatheter while avoiding reflux. After surgery, CT imaging and enhanced CT were used to monitor the treatment effect. As iodized oil was deposited in the liver cancer lesion, the magnesium microspheres were locally delivered to the lesion. In the liver tumor, the magnesium microspheres slowly reacted with water to release hydrogen and magnesium hydroxide. Magnesium hydroxide can neutralize the weakly acidic tumor microenvironment, and hydrogen can trigger hydrogen therapy. The combination of the two can enhance the effect of iodized oil embolization therapy.

[0148] The specific experimental results are as follows Fig. 9 and Fig.10 First, by Fig. 9 It can be seen that the size of the liver cancer lesions in the left lobe of the liver of the tumor-bearing rabbits is 1.0 to 1.5 cm, indicating that the liver cancer model was successfully established. After the femoral artery interventional surgery, it was found that a large amount of iodized oil was deposited in the liver tumor part of the rabbits in the iodized oil group and the magnesium microsphere-iodized oil composite embolic agent group, indicating that the interventional embolization surgery was very successful. One week after the interventional surgery, the present invention used CT imaging combined with ioversol contrast agent to evaluate the treatment effect. The results are as follows Fig.10 As shown, the tumor in the control group grows rapidly, and the volume increases by 3.3 times. The CT signal intensity of the lesion area shown by CT subtraction imaging is 26.68, and the tumor efficacy evaluation standard (mRECIST) evaluates it as progressive disease. The tumor growth in the simple iodized oil embolization group is suppressed, and the volume does not increase, but the enhanced CT imaging shows that the lesion still has some tissues enhanced (CT subtraction finds that the lesion still has some white enhancement, and its CT signal intensity is 3.63), indicating that the simple iodized oil embolization at this dosage cannot achieve complete tumor killing, and mRECIST evaluates it as partial remission. However, the present invention does not find that the tumor site is enhanced in the magnesium microsphere-iodized oil composite embolic agent group (CT subtraction does not find that the lesion has white enhancement, and its CT signal intensity is 0.86), indicating that the composite embolic agent has a good therapeutic effect, and mRECIST evaluates it as complete remission.

[0149] Application Example 2: The calcium hydride-iodized oil composite embolic agent obtained in Example 2 is used for interventional embolization treatment of liver cancer in rabbits

[0150] Following the above modeling scheme, VX2 liver cancer tissue was directly implanted into the left lobe of the liver with the help of CT imaging guidance. After two weeks, a tumor was formed, and an in situ model of rabbit liver cancer tumor was obtained. The tumor-bearing rabbits were randomly divided into three groups: (1) control group; (2) iodized oil group; (3) nano-calcium hydride-iodized oil composite embolic agent group. Subsequently, a 2.0-F microcatheter and a coaxial guidewire cannula were used to enter the left hepatic artery containing the tumor lesion through the femoral artery under the guidance of DSA fluoroscopy. Then, 0.3 ml of iodized oil or nano-calcium hydride-iodized oil composite embolic agent was slowly injected into the left hepatic artery through the microcatheter while avoiding reflux. After surgery, CT imaging was used to monitor the treatment effect.

[0151] The size of the liver cancer lesions in the left lobe of the liver of the tumor-bearing rabbits was 1.0 to 1.5 cm. After the interventional surgery, it was found that a large amount of iodized oil was deposited in the liver tumor of the rabbits in the iodized oil group and the nano-calcium hydride-iodized oil composite embolic agent group, indicating that the interventional embolization surgery was very successful. One week after the interventional surgery, the present invention used CT imaging combined with ioversol contrast agent to evaluate the treatment effect. The results are as follows Fig.11 As shown, the tumor growth in the control group is rapid, and the volume increases by 10 times, and the CT signal intensity of CT subtraction imaging showing the lesion area is 21.46, and mRECIST evaluates it as progressive disease. The tumor growth in the simple iodized oil embolization group is suppressed, and the volume does not increase, but the enhanced CT imaging shows that the lesion still has some tissues to be enhanced (CT subtraction finds that the lesion still has some white enhancement, and its CT signal intensity is 3.86), indicating that the simple iodized oil embolization under this dosage cannot achieve tumor complete killing, and mRECIST evaluates it as partial remission. However, the present invention does not find that the tumor site has enhancement (CT subtraction does not find that the lesion has white enhancement, and its CT signal intensity is 1.35) in the nanometer calcium hydride-iodized oil composite embolic agent group, indicating that the composite embolic agent has good therapeutic effect, and mRECIST evaluates it as complete remission.

[0152] Since the surface of tumor cells overexpresses glucose transporter-3, fluorinated glucose will significantly accumulate in tumor tissues, providing a strong guarantee for the clinical diagnosis of tumors. 18 F-FDG is a radionuclide probe used to evaluate the effect of interventional embolization therapy with the help of positron emission tomography (PET) / CT imaging. Fig.12 and Fig.13 As shown, PET / CT imaging showed that preoperative liver cancer lesions had strong 18 F-FDG signal, average 18 The F intensity was 6.95, indicating that it has high biological activity. Seven days after surgery, the tumor volume of the untreated control group increased, and the high metabolic area increased. 18 The F intensity increased to 9.64; while the iodized oil group 18 The F-FDG signal was significantly reduced, with an average 18The F intensity dropped to 5.26, but it was still at a medium level. 18 The F-FDG signal completely disappeared, and the average 18 The F intensity is 2.40, which is the same as normal tissue (normal tissue 18 The average F intensity was 2.20), which confirmed that the nano-calcium hydride-iodized oil composite embolic agent had the best combined treatment effect. With the deposition of iodized oil, the nano-calcium hydride was delivered to the tumor site in situ, and the in situ slow release of hydrogen and calcium hydroxide enhanced the interventional embolic treatment effect, indicating that the nano-calcium hydride-iodized oil composite embolic agent is an embolic agent with transformation potential.

[0153] In order to further confirm the effect of embolization therapy, the present invention isolated liver cancer tissue, stained tissue sections with H&E, TUNEL and Ki67, and performed histopathological analysis to evaluate tumor tissue damage, cell apoptosis and cell proliferation. Fig.14 As shown in the results, compared with the simple iodized oil and the control group, the nano-calcium hydride-iodized oil composite embolic agent group had the highest tumor cell apoptosis rate (control group: 2.1%; simple iodized oil group: 62.7%; nano-calcium hydride-iodized oil composite embolic agent group: 87.6%) and the lowest cell proliferation level (control group: 87.5%; simple iodized oil group: 26.1%; nano-calcium hydride-iodized oil composite embolic agent group: 2.9%). Fig.15 and Fig.16 ), which confirmed that the composite embolic agent, as a new type of embolic agent, has excellent therapeutic effects and is a drug with great potential for clinical transformation.

[0154] Example 3: An active metal microsphere is prepared by the preparation method of magnesium microsphere in Example 1, except that the magnesium microsphere is filtered through a sieve of about 240 meshes and has a particle size of about 60 microns.

[0155] Example 4: A composite embolic agent, comprising lipiodol embolic agent (commercially available) and microspheres with a particle size of about 60 microns prepared in Example 3. The embolic agent and microspheres are mixed and then shaken briefly to obtain a uniformly dispersed emulsion.

[0156] Compared with magnesium microspheres with larger particle sizes (350 microns and 500 microns), active metal microspheres with a particle size of about 60 microns have a significant size effect and can react with physiological solutions faster to produce hydrogen; at the same time, compared with 10-micron microspheres, the probability of them being free from the lesion site is lower and the safety is better. According to data verification, theoretical analysis and speculation, active metal microspheres with a particle size between 50-150 microns have similar effects to magnesium microspheres of about 60 microns described in this embodiment, can meet the needs of active metal microspheres for tumor treatment, and have the potential to be further prepared with embolic agents as composite embolic agents for application.

[0157] Example 5: An active metal microsphere is prepared by the preparation method described in Example 1, except that a 42-mesh screen is used for filtration. Specifically, taking the active metal magnesium microsphere as an example, the particle size distribution is as follows: Fig.23 As shown, the particle size is about 350±45 microns.

[0158] Example 6: The effect of the large-sized microspheres described in Example 5 on generating hydrogen in buffers under different pH conditions was investigated. 20 mg of magnesium microspheres were placed in 4 mL of phosphate buffers at different pH values, and a gas chromatograph was used to quantitatively measure the cumulative amount of hydrogen generated by the magnesium microspheres in the buffers of different concentrations in real time.

[0159] The results of hydrogen generation of magnesium microspheres with a particle size of about 350±45 microns at different pH values ​​are as follows Fig.24 As shown in the figure, when pH = 7.4, almost no hydrogen is produced in the buffer; when pH = 6.4, hydrogen can be produced compared to pH = 7.4, but the amount of hydrogen produced is less and the rate of production is slower; when pH = 5.5, after 350 seconds of reaction, the cumulative content of hydrogen produced by magnesium microspheres reaches about 3.5 times that of pH = 6.4, indicating that magnesium microspheres can produce hydrogen in a slightly acidic environment, and the rate of hydrogen production increases as the pH value decreases. This indicates that large-size magnesium microspheres can produce hydrogen in the slightly acidic physiological environment of tumors, and have the potential to be further applied in hydrogen therapy for tumors.

[0160] Example 7: A composite embolic agent containing active metal microspheres with large particle size, comprising the large particle size magnesium microspheres (particle size is about 350±45 microns) and lipiodol embolic agent (commercially purchased) described in Example 5. The large particle size magnesium microspheres and lipiodol are mixed, and the mass ratio of magnesium microspheres to lipiodol is 10:100. After simple shaking, a uniformly dispersed emulsion can be obtained by ultrasound.

[0161] Example 8: A magnesium-platinum metal composite structure (Mg@Pt composite structure)

[0162] A magnesium-platinum metal composite structure comprises a magnesium core structure and platinum particles bonded to the surface of the magnesium core structure. Fig.17 The particle size distribution diagram of the magnesium-platinum metal composite structure is shown in FIG. The particle size distribution of the magnesium-platinum metal composite microspheres is about 25 microns. The preparation method of the magnesium-platinum metal composite structure is as follows:

[0163] 100 mg of magnesium microspheres (24 μm in diameter) were added to a 0.1% chloroplatinic acid ethanol solution. After ultrasonic treatment, the originally grayish white magnesium microspheres turned dark brown. When the ethanol evaporated completely, a magnesium-platinum metal composite structure (Mg@Pt composite structure) was obtained.

[0164] The corresponding concentration of chloroplatinic acid is matched according to the number, shape and particle size of the magnesium core structure particles.

[0165] Example 9: Testing the rate of hydrogen generation of the magnesium-platinum metal composite structure of Example 8

[0166] In order to compare the efficiency of hydrogen generation of magnesium microspheres and magnesium-platinum composite structures, 20 mg of magnesium microspheres and the magnesium-platinum metal composite structure obtained in Example 3 were weighed and placed in 96% ethanol solution respectively. The hydrogen generation in the two samples was observed. The hydrogen bubbles were observed for about 10 seconds. The results are as follows: Fig.18 As shown in the figure, a large number of bubbles appear in the ethanol solution of the magnesium-platinum metal composite structure. The number of bubbles generated in the same time period is counted, and it is found that the efficiency of the magnesium-platinum metal composite structure in generating gas in the ethanol solution is about 200 times that of the simple Mg microspheres. The efficiency of the magnesium-platinum metal composite structure in generating hydrogen is much greater than that of the magnesium microspheres, indicating that the magnesium-platinum metal composite structure has a higher hydrogen production efficiency than the active metal single substance. The reason is that in the magnesium-platinum metal composite structure, a galvanic cell composite structure is formed between the inert metal platinum and the active metal magnesium, thereby increasing the efficiency of the active metal magnesium in generating hydrogen.

[0167] Hydrogen can selectively remove highly cytotoxic oxygen free radicals [hydroxyl radicals (·OH) and peroxynitrite anions (ONOO-)], disrupt the intracellular redox balance, induce tumor cell apoptosis, and retain the physiologically required ROS for normal cell signal transduction, with low toxic side effects. Therefore, the magnesium-platinum metal composite structure has a higher efficiency in generating hydrogen, which helps to increase the hydrogen content in the tumor microenvironment, thereby more effectively regulating the tumor microenvironment. The composite embolic agent prepared with the magnesium-platinum metal composite structure will have a better therapeutic effect on tumors.

[0168] Example 10: A composite embolic agent

[0169] A composite embolic agent includes the magnesium-platinum metal composite structure of Example 8 and iodized oil. The appearance of simple iodized oil is a light yellow clear transparent liquid, and the composite embolic agent is a milky white liquid. The composite embolic agent is prepared by the following method: the magnesium-platinum metal composite structure prepared in Example 8 is dispersed in iodized oil (commercially purchased), and dispersed evenly by ultrasound or shaking to obtain a magnesium-platinum metal composite structure-iodized oil composite embolic agent, and the mass fraction of the magnesium-platinum metal composite structure in the iodized oil is 6.0%.

[0170] Example 11: A composite embolic agent for treating tumors in mice

[0171] The magnesium-platinum metal composite structure-iodized oil composite embolic agent prepared in Example 10 was used to treat mouse tumors.

[0172] First, H22 tumor cells were inoculated on the right back of the mouse to establish a mouse subcutaneous liver cancer tumor model. 3 Around 14:00 p.m., the mice were randomly divided into two groups and received iodized oil embolization therapy and magnesium-platinum metal composite structure-iodized oil composite embolization therapy respectively. The tumor growth of the mice was measured and recorded, and a mouse tumor growth curve was made.

[0173] Comparative Example 1: Iodized oil embolic agent for tumor treatment in mice

[0174] The difference between Comparative Example 1 and Example 11 is that the mice received iodized oil embolization treatment, the tumor growth of the mice was measured and recorded, and the treatment method and testing method were the same as those in Example 6.

[0175] Please refer to Fig.19 In Example 11, mice were treated with Mg@Pt metal composite structure-lipiodol composite embolic agent for tumors, and the average tumor volume of the mice on the 10th day after treatment was about 50 cubic millimeters, while in Comparative Example 1, mice were treated with lipiodol embolic agent, and the average tumor volume of the mice on the 10th day was close to 400 cubic millimeters;

[0176] Therefore, compared with Comparative Example 1, the Mg@Pt metal composite structure-iodized oil composite embolic agent of Example 11 has significantly improved therapeutic effect on tumors. Fig.19 The *** shown in the table indicates a statistically significant p value < 0.001, and the p value represents a significant difference. The smaller the p value, the more significant the difference between the groups. The p value calculation results here show that there is a significant difference between Example 11 and Comparative Example 1, and the Mg@Pt metal composite structure-iodized oil composite embolic agent has a significantly enhanced tumor embolization therapeutic effect compared with the traditional iodized oil embolic agent.

[0177] Example 12: A magnesium-platinum metal composite structure and its preparation method

[0178] A magnesium-platinum metal composite structure includes a magnesium core structure and platinum particles bonded to the surface of the magnesium core structure, wherein the core structure is spherical, and the particle size distribution of the magnesium-platinum metal composite microspheres is about 350 microns. The preparation method of the magnesium-platinum metal composite structure is as follows:

[0179] Prepare a 0.1% chloroplatinic acid ethanol solution, add 100 mg of magnesium microspheres (particle size of about 350 μm) to the chloroplatinic acid ethanol solution, and after ultrasonic treatment, observe that the originally grayish white magnesium microspheres turn into dark brown. After the reaction is completed, remove the liquid, and wait until the residual ethanol evaporates completely to obtain a magnesium-platinum metal composite structure.

[0180] The raw material magnesium microspheres and magnesium-platinum metal composite structure in Example 4 were characterized by optical microscopy. Fig.20a , Fig.20b , Fig.20a This is a scanning electron microscope image of the raw magnesium microspheres; Fig.20b This is a scanning electron microscope image of a magnesium-platinum metal composite structure.

[0181] contrast Fig.20a , Fig.20b It can be seen that the surface of the microspheres of the magnesium-platinum metal composite structure is rougher. The rough surface is the platinum attached to the surface of the magnesium microspheres, indicating that the platinum is attached to the surface of the magnesium microspheres through a reduction reaction, thereby forming a magnesium-platinum metal composite structure.

[0182] Example 13: A magnesium-platinum metal composite structure

[0183] The difference between Example 13 and Example 12 is that the particle size of the raw material magnesium microspheres is about 500 microns, and the magnesium-platinum metal composite structure is prepared by the preparation method of Example 12.

[0184] Example 14: A magnesium-platinum metal composite structure

[0185] A magnesium-platinum metal composite structure includes a magnesium core structure and platinum particles bonded to the surface of the magnesium core structure, wherein the core structure is rod-shaped. The preparation method of the rod-shaped magnesium-platinum metal composite structure is as follows:

[0186] A magnesium rod (diameter: 0.5 mm, length: 2 mm, commercially available) was placed in 2 mL of 0.3% chloroplatinic acid ion (PtCl6 2- ) in a neutral solution (sodium chloroplatinate solution), react for 1 minute, take out the rod-shaped magnesium-platinum metal composite structure, wash it with anhydrous ethanol three times to remove the unreacted ions on the surface, and seal the prepared magnesium-platinum composite rod structure in anhydrous ethanol for storage. According to the principle of in situ replacement reduction, a magnesium-platinum metal composite structure is formed on the surface of magnesium, PtCl6 2- Platinum nanoparticles will be reduced on the surface of the magnesium rod, thus obtaining a rod-shaped magnesium-platinum metal composite structure.

[0187] Fig.21 is the XRD diffraction pattern of the rod-shaped magnesium-platinum metal composite structure prepared in Example 14, Fig.21 The vertical line on the horizontal axis is the standard XRD signal peak position and relative intensity of magnesium element, the curve is the XRD signal spectrum of the rod-shaped magnesium-platinum metal composite structure, and the diamond is marked as the XRD signal peak position of platinum element. Fig.21It can be seen that in the XRD spectrum of the magnesium-platinum metal composite rod-like structure, the signal of elemental magnesium is consistent with the standard signal peak position of elemental magnesium. In addition to the strong magnesium signal, a platinum signal peak also appears, further proving that platinum nanoparticles have successfully grown on the surface of the magnesium rod to obtain the rod-shaped magnesium-platinum metal composite structure.

[0188] Example 15: Testing the rate of hydrogen generation from the rod-shaped magnesium-platinum metal composite structure obtained in Example 14

[0189] In order to explore the hydrogen production ability of the rod-shaped magnesium-platinum metal composite structure, the rod-shaped magnesium-platinum metal composite structure prepared in Example 14 and a simple magnesium rod of the same size were placed in 50 mL of phosphate buffer, respectively, and gas chromatography was further used to quantitatively determine the hydrogen production of the rod-shaped magnesium-platinum metal composite structure and the simple magnesium rod at different times.

[0190] The total amount of hydrogen produced is measured as follows: Fig. 22 As shown, from Fig. 22 The results show that when the magnesium rod is placed in the buffer solution, only a small amount of hydrogen can be produced in the initial stage, while the rod-shaped magnesium-platinum metal composite structure can last longer and continuously produce a large amount of hydrogen, and the rate and total amount of hydrogen produced are much greater than that of a simple magnesium rod. This experimental result directly proves that the magnesium-platinum metal composite structure described in the present invention has excellent hydrogen production ability and has the potential to be further used in tumor treatment.

[0191] Example 16: A composite embolic agent

[0192] A composite embolic agent comprises the magnesium-platinum metal composite structure of Example 14 and iodized oil.

[0193] The rod-shaped metal composite structure can achieve better fixation of the metal composite structure at the site of action by adjusting the aspect ratio, thereby avoiding the blockage of blood vessels in other normal tissues caused by the metal composite structure entering the blood circulation when using the magnesium-platinum metal composite rod structure and the iodized oil composite embolic agent.

[0194] Example 17: Aluminum-gallium metal composite structure

[0195] An aluminum-gallium metal composite structure includes an aluminum core structure and gallium particles bonded to the surface of the aluminum core structure. The aluminum-gallium metal composite structure is prepared as follows:

[0196] At room temperature, 200 mg of aluminum powder (300 mesh, about 48 microns) was placed in a 4 mL centrifuge tube, 200 mg of liquid metal gallium was added dropwise, and magnetic stirring was performed for 10 minutes to prepare an aluminum-gallium metal composite structure by utilizing the strong fusion ability of gallium to aluminum. After stirring, the mixture was washed several times with anhydrous ethanol, and then sealed and stored in anhydrous ethanol for later use.

[0197] Example 18: A composite embolic agent

[0198] A composite embolic agent includes the aluminum-gallium metal composite structure of Example 17 and iodized oil. The composite embolic agent is obtained by mixing the aluminum-gallium metal composite structure with iodized oil, and dispersing the aluminum-gallium metal composite structure more evenly in the iodized oil by ultrasound. Metal aluminum reacts with water to generate aluminum hydroxide, which can be used as an immune adjuvant to regulate the immune microenvironment of the tumor site and enhance the effect of immunotherapy.

[0199] Example 19: A composite embolic agent containing alloy metal particles

[0200] An alloy metal particle composite embolic agent comprises platinum-gold alloy metal particles and iodized oil, wherein the platinum-gold alloy metal particles are commercially purchased. The alloy metal particles can be further doped with other ions and may have the function of providing trace elements.

[0201] The magnesium-platinum composite structure can produce hydrogen in physiological solutions under neutral pH conditions, and the active metal microspheres can produce hydrogen in physiological solutions under slightly acidic pH conditions. As the particle size of the active metal microspheres changes, each particle size range has corresponding advantages; the composite embolic agents formed by these microspheres and iodized oil can play the role of delivering hydrogen in tumor embolization therapy, thereby achieving enhanced tumor embolization therapy.

[0202] Obviously, the above embodiments are merely examples for clear description and are not limitations of the implementation methods.

[0203] Although the above disclosure discusses some of the invention embodiments currently considered useful through various examples, it should be understood that such details are for illustrative purposes only, and the appended claims are not limited to the disclosed embodiments. On the contrary, the claims are intended to cover all modifications and equivalent combinations that are consistent with the essence and scope of the embodiments of the present application.

[0204] Similarly, it should be noted that in order to simplify the description of the disclosure of this application and thus help understand one or more embodiments of the invention, in the above description of the embodiments of this application, multiple features are sometimes combined into one embodiment, figure or description thereof. However, this disclosure method does not mean that the features required by the object of this application are more than the features mentioned in the claims. In fact, the features of the embodiments are less than all the features of the single embodiment disclosed above.

[0205] In some embodiments, numbers describing the number of components and attributes are used. It should be understood that such numbers used in the description of the embodiments are modified by the modifiers "about", "approximately" or "substantially" in some examples. Unless otherwise specified, "about", "approximately" or "substantially" indicate that the numbers are allowed to vary by ±. Accordingly, in some embodiments, the numerical parameters used in the specification and claims are approximate values, which may vary according to the required features of individual embodiments.

[0206] Finally, it should be understood that the embodiments described in this application are only used to illustrate the principles of the embodiments of the present application. Other variations may also fall within the scope of the present application. Therefore, as an example and not a limitation, the alternative configurations of the embodiments of the present application may be considered to be consistent with the teachings of the present application. Accordingly, the embodiments of the present application are not limited to the embodiments explicitly introduced and described in the present application.

Claims

1. A composite embolic agent of iodized oil-based active metal microspheres, characterized in that: The composite embolic agent comprises active metal microspheres and iodized oil; the mass percentage of the active metal microspheres in the composite embolic agent is 0.1-10%.

2. The composite embolic agent according to claim 1, characterized in that: The particle size of the active metal microspheres is 0.1-20 microns.

3. The composite embolic agent according to claim 1, characterized in that: The active metal microspheres are prepared by a gas atomization powder making method, that is, the active metal ingots are heated and melted and then atomized and cooled to obtain the active metal microspheres.

4. The composite embolic agent according to claim 3, characterized in that: The active metal is one or more of potassium, calcium, sodium, magnesium, aluminum, zinc, gallium, iron, manganese and tin.

5. The method for preparing the composite embolic agent according to any one of claims 1 to 4, characterized in that: The method comprises the following steps: mixing iodized oil and active metal microspheres and uniformly dispersing them to obtain the composite embolic agent.

6. Use of the composite embolic agent according to any one of claims 1 to 4 in the preparation of a therapeutic agent for liver cancer embolism.

7. The composite embolic agent according to claim 1, characterized in that: The particle size of the active metal microspheres is 20-500 microns.

8. A composite embolic agent, characterized in that: The invention comprises active metal microspheres and a dispersant, wherein the metal activity of the active metal microspheres is stronger than the activity of hydrogen.

9. The composite embolic agent according to claim 8, characterized in that: The dispersant is an organic phase.

10. The composite embolic agent according to claim 8, characterized in that: The dispersant is an oil phase.

11. The composite embolic agent according to claim 8, characterized in that: The dispersant is selected from at least one of iodized oil, poppy seed oil, soybean oil and olive oil.

12. The composite embolic agent according to any one of claims 8 to 11, characterized in that: The active metal microspheres are prepared from active metals, and the active metals are selected from at least one of potassium, calcium, sodium, magnesium, aluminum, zinc, gallium, iron, manganese and tin; and / or The particle size of the active metal microspheres is 0.1-500 microns.

13. The composite embolic agent according to any one of claims 8 to 11, characterized in that: The active metal microspheres are in the shape of spheres, mesoporous structures, sea urchins or polyhedrons; and / or The mass ratio of the active metal microspheres to the dispersant is 0.1:100 to 50:

100.

14. A tumor preparation comprising the composite embolic agent according to any one of claims 1 to 4.

15. A tumor preparation comprising the composite embolic agent according to any one of claims 8 to 13.

16. A tumor preparation comprising active metal microspheres, wherein the metal activity of the active metal microspheres is stronger than the activity of hydrogen.

17. The tumor preparation according to claim 16, characterized in that The particle size of the active metal microspheres is 0.1-500 microns; and / or The active metal microspheres are in the shape of spheres, mesoporous structures, sea urchins or polyhedrons.

18. The tumor preparation according to claim 16 or 17, characterized in that: The active metal microspheres are prepared from active metals, and the active metals are selected from at least one of potassium, calcium, sodium, magnesium, aluminum, zinc, gallium, iron, manganese and tin.

19. A composite embolic agent, characterized in that: The invention comprises a metal composite structure and a dispersant. The metal composite structure comprises a core structure and a bonding layer bonded to the surface of the core structure. The core structure is a first metal, the bonding layer is a second metal, and the metal composite structure is dispersed in the dispersant.

20. The composite embolic agent according to claim 19, characterized in that: The dispersant is an organic phase; and / or The mass ratio of the metal composite structure to the dispersant is 0.1:100 to 50:

100.

21. The composite embolic agent according to claim 19, characterized in that: The organic phase is an oil phase.

22. The composite embolic agent according to claim 19, characterized in that: The oil phase is selected from at least one of iodized oil, poppy seed oil, soybean oil and olive oil.

23. The composite embolic agent according to any one of claims 19 to 22, characterized in that: The core structure is in the shape of a sphere, a polyhedron, a porous structure or a rod; and / or The particle size distribution of the metal composite structure is uniform.

24. The composite embolic agent according to any one of claims 19 to 22, characterized in that: The metal activity of the first metal is stronger than the activity of hydrogen.

25. The composite embolic agent according to claim 24, characterized in that: The first metal is selected from at least one of potassium, calcium, sodium, magnesium, aluminum, zinc, gallium, iron, manganese and tin.

26. The composite embolic agent according to any one of claims 19 to 22, characterized in that: The metal activity of the second metal is weaker than the activity of hydrogen.

27. The composite embolic agent according to claim 26, characterized in that: The second metal is selected from at least one of copper, silver, platinum and gold.

28. The composite embolic agent according to any one of claims 19 to 22, characterized in that: The particle size of the metal composite structure is 0.1-500 microns; and / or The metal composite structure is uniformly dispersed in the dispersant.

29. A method for preparing the composite embolic agent according to any one of claims 19 to 28, characterized in that: The method comprises the step of bonding the second metal to the surface of the first metal.

30. The method for preparing the composite embolic agent according to claim 29, characterized in that: The second metal is bonded to the surface of the first metal by a physical method or a chemical method.

31. The method for preparing the composite embolic agent according to claim 30, characterized in that: The chemical method is selected from the group consisting of a displacement method.

32. The method for preparing the composite embolic agent according to claim 31, characterized in that: The replacement method includes placing the first metal in a solution containing high-valent ions of the second metal.

33. The method for preparing the composite embolic agent according to claim 32, characterized in that: The solution of high-valent ions of the second metal contains at least one of chloroaurate ions, chloroplatinate ions, copper ions, and silver ions.

34. The method for preparing the composite embolic agent according to claim 30, characterized in that: The physical method is a mechanical stirring method or a vapor deposition method.

35. The method for preparing the composite embolic agent according to claim 34, characterized in that: The mechanical stirring method includes mixing and stirring the second metal in a solid state and the first metal in a liquid state.

36. A composite embolic agent, characterized in that: The invention comprises alloy metal particles and a dispersant. The alloy metal particles comprise at least two metals with different activities, and the two metals with different activities are mixed in the form of an alloy. The alloy metal particles are dispersed in the dispersant.

37. The composite embolic agent according to claim 36, characterized in that: The dispersant is an organic phase.

38. The composite embolic agent according to claim 36, characterized in that: The organic phase is an oil phase.

39. The composite embolic agent according to claim 36, characterized in that: The oil phase is selected from at least one of iodized oil, poppy seed oil, soybean oil and olive oil.

40. The composite embolic agent according to any one of claims 36 to 39, characterized in that: The alloy metal particles are in the shape of spheres, polyhedrons, porous structures, sea urchins or rods; and / or The mass fraction of the alloy metal particles in the dispersant is 0.1% to 50%.

41. The composite embolic agent according to any one of claims 36 to 39, characterized in that: The metal activity of the active metal is greater than the activity of hydrogen.

42. The composite embolic agent according to claim 41, characterized in that: The active metal is selected from at least one of potassium, calcium, sodium, magnesium, aluminum, zinc, gallium, iron, manganese and tin.

43. The composite embolic agent according to any one of claims 36 to 39, characterized in that: The metallic activity of the inert metal is less than the activity of hydrogen.

44. The composite embolic agent according to any one of claims 43, characterized in that: The inert metal is selected from at least one of copper, silver, platinum and gold.

45. The composite embolic agent according to any one of claims 36 to 39, characterized in that: The alloy metal particles include at least one active metal and at least one inert metal, and the active metal element and the inert metal element are mixed in the form of an alloy; and / or The alloy metal particles are uniformly dispersed in the dispersant.

46. ​​The composite embolic agent according to any one of claims 36 to 39, characterized in that: The size of the alloy metal particles is 0.1-500 microns.